Positive electrode active material for secondary battery and secondary battery

By using the cathode active material LiaNixCoyMnzMbO2 containing specific elements in aqueous lithium secondary batteries, the problem of battery degradation during charging and storage is solved, the potential window of the electrolyte is expanded, and the durability and stability of the battery are improved.

CN112673497BActive Publication Date: 2024-10-25PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980058891.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-09-27
Filing Date
2019-08-01
Publication Date
2024-10-25
Estimated Expiration
2039-08-01

AI Technical Summary

Technical Problem

Existing aqueous lithium secondary batteries are prone to deterioration during charging and storage, and the potential range of the electrolyte is limited, making it difficult to operate stably at high voltages.

Method used

The specific cathode active material LiaNixCoyMnzMbO2 is used. The element M includes Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Ga, In, etc. By using these elements as the cathode active material in the aqueous electrolyte, Suppresses battery deterioration during charging and storage, and expands the potential window of the electrolyte.

Benefits of technology

It effectively suppresses battery degradation during charging and storage, improves the durability and voltage stability of secondary batteries, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112673497B_ABST
    Figure CN112673497B_ABST
Patent Text Reader

Abstract

The positive electrode active material is Li a Ni x Co y Mn z M b O 2 Indicates that it satisfies 0.9
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a positive electrode active material for a secondary battery and a secondary battery. Background Art

[0002] Aqueous lithium secondary batteries using aqueous solutions as electrolytes are known. Aqueous lithium secondary batteries are required to be used within a potential range where no electrolysis reaction of water occurs. It is necessary to use an active material that is stable in an aqueous solution and can reversibly absorb and detach a large amount of lithium within a potential range where oxygen and hydrogen are not produced by the electrolysis of water. In other words, it is necessary to use an active material that can exert a large capacity within a specific potential range. In addition, as an electrolyte, it is desirable to use a neutral to alkaline electrolyte. When a neutral, i.e., pH=7, electrolyte is used, the decomposition voltage of water is as follows: hydrogen evolution potential is 2.62V, and oxygen evolution potential is 3.85V. In addition, when a strongly alkaline, i.e., pH=14, electrolyte is used, the decomposition voltage of water is as follows: hydrogen evolution potential is 2.21V, and oxygen evolution potential is 3.44V.

[0003] Therefore, as a positive electrode active material, a material that can absorb more Li up to a minimum of 3.85 V (pH=7) is desired, and as a negative electrode active material, a material that can absorb more Li up to 2.21 V (pH=14) is desired.

[0004] Patent Document 1 describes a positive electrode active material having the general formula Li s Ni x Co y Mn z M t A layered structure compound represented by O2 (0.9≤s≤1.2, 0.25≤x≤0.4, 0.25≤y≤0.4, 0.25≤z≤0.4, 0≤t≤0.25; M is one or more selected from Mg, Al, Fe, Ti, Ga, Cu, V and Nb) is used as the main component.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 4581524 Summary of the invention

[0008] For secondary batteries using aqueous electrolyte solutions, there is a demand for a technology that can expand the potential region where electrolysis does not occur and improve the durability, that is, suppress battery degradation during charged storage.

[0009] The present application aims to provide a positive electrode active material for a secondary battery using an aqueous electrolyte and a secondary battery using an aqueous electrolyte, wherein battery degradation during charged storage is suppressed, and a secondary battery is provided.

[0010] The secondary battery positive electrode active material according to one embodiment of the present application is a secondary battery positive electrode active material having an electrolyte solution prepared by dissolving a lithium salt in water, and is represented by the general formula Li a Ni x Co y Mn z M b O2 represents and satisfies:

[0011] 0.9 <a<1.1、

[0012] 0.4 <x<1、

[0013] 0≤y<0.4,

[0014] 0≤z<0.4,

[0015] 0≤b<0.2,

[0016] 0.9<(x+y+z+b)<1.1,

[0017] The element M includes at least one selected from the group consisting of Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Al, Ga, and In.

[0018] According to the present application, it is possible to suppress battery degradation during charged storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a diagram for explaining the function of the implementation method. DETAILED DESCRIPTION

[0020] As a result of intensive studies, the present inventors have found that battery degradation during charged storage can be suppressed by using a specific material as a positive electrode active material in an electrolyte solution containing water as a solvent and a lithium salt as an electrolyte salt.

[0021] Hereinafter, an embodiment of a positive electrode active material and a secondary battery according to one embodiment of the present application will be described. However, the embodiment described below is an example, and the present application is not limited thereto.

[0022] [Aqueous electrolyte]

[0023] The aqueous electrolyte described in this embodiment contains at least water and a lithium salt. It should be noted that when using an electrolyte containing water as a solvent, since water theoretically decomposes at a voltage of 1.23V, it is also desired to develop a secondary battery that can work stably without decomposing water even when a higher voltage is applied.

[0024] (Solvent)

[0025] The aqueous electrolyte contains water as the main solvent. Here, containing water as the main solvent means that the content of water is 50% or more by volume relative to the total amount of solvent contained in the electrolyte. The content of water contained in the electrolyte is preferably 90% or more by volume relative to the total amount of solvent. The solvent contained in the electrolyte can be a mixed solvent containing water and a non-aqueous solvent. Examples of the non-aqueous solvent include alcohols such as methanol; carbonates such as dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, ethylene carbonate, and propylene carbonate; acetone; acetonitrile; and non-protonic polar solvents such as dimethyl sulfoxide.

[0026] The aqueous electrolyte contains non-flammable water as the main solvent, so the safety of the secondary battery using the aqueous electrolyte can be improved. From this viewpoint, the content of water is preferably 8% by mass or more, more preferably 10% by mass or more relative to the total amount of the electrolyte. In addition, the content of water is preferably 50% by mass or less, more preferably 20% by mass or less relative to the total amount of the electrolyte.

[0027] (Lithium Salt)

[0028] The lithium salt contained in the aqueous electrolyte can be used as long as it is a compound that can be dissolved in a solvent containing water and dissociated so that lithium ions are present in the aqueous electrolyte. The lithium salt preferably does not cause deterioration of battery characteristics due to its reaction with the materials constituting the positive electrode and the negative electrode. Examples of such lithium salts include salts formed with inorganic acids such as perchloric acid, sulfuric acid and nitric acid; salts formed with halide ions such as chloride ions and bromide ions; and salts formed with organic anions containing carbon atoms in the structure.

[0029] Examples of the organic anions constituting the lithium salt include anions represented by the following general formulae (i) to (iii).

[0030] (R 1 SO2)(R 2 SO2)N - (i)

[0031] (R 1 , R 2 R is independently selected from a halogen atom, an alkyl group or a halogen-substituted alkyl group. 1 and R 2 They are optionally bonded to each other to form a ring.)

[0032] R 3 SO3 - (ii)

[0033] (R 3 is selected from a halogen atom, an alkyl group or a halogen-substituted alkyl group. )

[0034] R 4 CO2 - (iii)

[0035] (R 4 is selected from alkyl or halogen-substituted alkyl. )

[0036] In the above general formulae (i) to (iii), the number of carbon atoms in the alkyl group or the halogen-substituted alkyl group is preferably 1 to 6, more preferably 1 to 3, and even more preferably 1 to 2. The halogen in the halogen-substituted alkyl group is preferably fluorine. The number of halogen substitutions in the halogen-substituted alkyl group is less than the number of hydrogen atoms in the original alkyl group. The halogen atom in the above general formulae (i) to (ii) is preferably a fluorine atom.

[0037] R 1 ~R 4 are, for example, saturated alkyl or saturated halogen-substituted alkyl and R 1 ~R 2 When they are not bonded to each other to form a ring, they may be a group represented by the following general formula (iv).

[0038] C n H a F b Cl c Br d I e (iv)

[0039] (n is an integer greater than or equal to 1, a, b, c, d, and e are integers greater than or equal to 0, and 2n+1=a+b+c+d+e is satisfied.)

[0040] In the above general formula (iv), from the viewpoint of oxidation resistance, a is preferably smaller, more preferably a=0, and most preferably 2n+1=b.

[0041] Specific examples of the organic anion represented by the general formula (i) include bis(fluorosulfonyl)imide (FSI; [N(FSO2)2] - ), bis(trifluoromethanesulfonyl)imide (TFSI; [N(CF3SO2)2] - ), bis(perfluoroethanesulfonyl)imide (BETI; [N(C2F5SO2)2] - ), (perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide ([N(C2F5SO2)(CF3SO2)]- ) etc. In addition, as R 1 ~R 2 Specific examples of organic anions that are bonded to each other to form a ring include cTFSI; ([N(CF2SO2)2] - ) etc. Specific examples of organic anions represented by the general formula (ii) include FSO3 - CF3SO3 - 、C2F5SO3 - As specific examples of the organic anion represented by the general formula (iii), for example, CF3CO2 - 、C2F5CO2 - wait.

[0042] Examples of organic anions other than those of the general formula (i) include bis(1,2-benzenediol (2-)-O,O')borate, bis(2,3-naphthalenediol (2-)-O,O')borate, bis(2,2'-biphenylenediol (2-)-O,O')borate, and bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O')borate.

[0043] As the anion constituting the lithium salt, the imide anion is preferably used. As suitable specific examples of the imide anion, in addition to the imide anion exemplified as the organic anion represented by the general formula (i), (fluorosulfonyl) (trifluoromethanesulfonyl) imide (FTI; [N(FSO2)(CF3SO2)] - )wait.

[0044] Specific examples of lithium salts having lithium ions and imide anions include lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(perfluoroethanesulfonyl)imide (LiBETI), lithium (perfluoroethanesulfonyl)(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide (LiFSI), and lithium (fluorosulfonyl)(trifluoromethanesulfonyl)imide (LiFTI).

[0045] Specific examples of other lithium salts include CF3SO3Li, C2F5SO3Li, CF3CO2Li, C2F5CO2Li, bis(1,2-benzenediol (2-)-O,O') lithium borate, bis(2,3-naphthalenediol (2-)-O,O') lithium borate, bis(2,2'-biphenylenediol (2-)-O,O') lithium borate, bis(5-fluoro-2-ol-1-benzenesulfonic acid-O,O') lithium borate, lithium perchlorate (LiClO4), lithium chloride (LiCl), lithium bromide (LiBr), lithium hydroxide (LiOH), lithium nitrate (LiNO3), lithium sulfate (Li2SO4), lithium sulfide (Li2S), lithium hydroxide (LiOH), etc.

[0046] In the aqueous electrolyte described in the present embodiment, the ratio of water to lithium salt is preferably 15:1 or less, more preferably 4:1 or less in terms of molar ratio. This is because: if the ratio of water to lithium salt is within these ranges, the potential window of the aqueous electrolyte is expanded, and the applied voltage to the secondary battery can be further increased. From the perspective of the safety of the secondary battery, the ratio of water to lithium salt is preferably 1.5:1 or more in terms of molar ratio.

[0047] (additive)

[0048] The aqueous electrolyte solution described in this embodiment may further contain additives or other electrolytes known in the art. As other electrolytes, a lithium ion conductive solid electrolyte may be further contained.

[0049] As additives, for example, fluorophosphates, carboxylic anhydrides, alkaline earth metal salts, sulfur compounds, acids and bases can be cited. The aqueous electrolyte preferably further contains at least one of fluorophosphates, carboxylic anhydrides, alkaline earth metal salts and sulfur compounds. The content of these additives is, for example, 0.1% by mass or more and 5.0% by mass or less relative to the total amount of the aqueous electrolyte.

[0050] Examples of the fluorophosphate that can be added to the aqueous electrolyte include, for example, lithium fluorophosphate salts represented by the general formula LixPFyOz (1 ≤ x < 3, 0 < y ≤ 2, 2 ≤ z < 4). By making the aqueous electrolyte contain the fluorophosphate, the electrolysis of water can be inhibited. Specific examples of the lithium fluorophosphate salt include, for example, lithium difluorophosphate (LiPF2O2) and lithium monofluorophosphate (Li2PFO3), and LiPF2O2 is preferred. It should be noted that the fluorophosphate represented by the general formula LixPFyOz may be a mixture of multiple ones selected from LiPF2O2, Li2PFO3, and Li3PO4. In this case, x, y, and z may be values other than integers. The content of the fluorophosphate is, for example, preferably 0.1% by mass or more based on the total amount of the aqueous electrolyte, and more preferably 0.3% by mass or more. In addition, the content of the lithium fluorophosphate salt is, for example, preferably 3.0% by mass or less based on the total amount of the aqueous electrolyte, and more preferably 2.0% by mass or less.

[0051] The alkaline earth metal salt that can be added to the aqueous electrolyte is a salt having an ion of an alkaline earth metal (Group 2 element) and an anion such as an organic anion. Examples of the alkaline earth metal include, for example, beryllium (Be), magnesium (Mg), calcium (Ca), and strontium (Sr), and magnesium and calcium are preferred.

[0052] Examples of the organic anion constituting the alkaline earth metal salt include, for example, the organic anions represented by the general formulas (i) to (iii) described as the organic anions constituting the above lithium salts. However, the anion constituting the alkaline earth metal salt may be an organic anion other than the organic anions represented by the general formulas (i) to (iii), or may be an inorganic anion.

[0053] The dissociation constant of the alkaline earth metal salt in the aqueous electrolyte is preferably large. For example, suitable examples include alkaline earth metal salts of perfluoroalkanesulfonic acid imides such as Ca[N(CF3SO3)2]2(CaTFSI), Ca[N(CF3CF3SO2)2]2(CaBETI), Mg[N(CF3SO3)2]2(MgTFSI), and Mg[N(CF3CF3SO2)2]2(MgBETI); alkaline earth metal salts of trifluoromethanesulfonic acid such as Ca(CF3SO3)2 and Mg(CF3SO3)2; alkaline earth metal salts of perchloric acid such as Ca[ClO4]2 and Mg[ClO4]2; and tetrafluoroborates such as Ca[BF4]2 and Mg[BF4]2. Among these, alkaline earth metal salts of perfluoroalkanesulfonic acid imides are more preferred from the viewpoint of plasticizing effect, and CaTFSI and CaBETI are particularly preferred. In addition, as alkaline earth metal salt, it is also preferred to have an alkaline earth metal salt with the same anion as the Li salt contained in the electrolyte. The alkaline earth metal salt can be used alone or in combination with two or more. From the viewpoint of the potential window expanding to the low potential side, the content of the alkaline earth metal salt is, for example, 0.5 mass % or more and 3 mass % or less relative to the total amount of the aqueous electrolyte, preferably 1.0 mass % or more and 2 mass % or less.

[0054] The carboxylic anhydride that can be added to the aqueous electrolyte includes cyclic carboxylic anhydride and chain carboxylic anhydride. As cyclic carboxylic anhydride, for example, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, diglycolic anhydride, cyclohexane dicarboxylic anhydride, cyclopentane tetracarboxylic anhydride, phenyl succinic anhydride, etc. can be listed. Chain carboxylic anhydride is an anhydride of two identical or different carboxylic acids selected from carboxylic acids having 1 to 12 carbon atoms such as acetic acid, propionic acid, butyric acid, isobutyric acid, etc. As a specific example thereof, acetic anhydride, propionic anhydride, etc. can be listed. When added to the aqueous electrolyte, the carboxylic anhydride can be used alone or in combination of two or more. The content of the carboxylic anhydride is, for example, 0.1% by mass or more and 5.0% by mass or less relative to the total amount of the aqueous electrolyte, preferably 0.3% by mass or more and 2.0% by mass or less.

[0055] As sulfur compounds that can be added to the aqueous electrolyte, there can be listed, for example, organic compounds containing sulfur atoms in the molecule, and the compound does not contain the above-mentioned lithium salts, carboxylic acids and alkaline earth metal salts. By including the sulfur compound in the aqueous electrolyte, it is possible to compensate for the coating containing components derived from the reduction reaction of anions represented by general formulas (i) to (iii) such as TFSI and BETI, and it is possible to efficiently block the parasitic hydrogen evolution in the negative electrode. As specific examples of sulfur compounds, there can be listed, for example, cyclic sulfur compounds such as ethylene sulfite, 1,3-propane sultone, 1,4-butane sultone, cyclopentane sulfone, cyclobutene sulfone; sulfonic acid esters such as methyl methanesulfonate and busulfan; sulfones such as dimethyl sulfone, diphenyl sulfone, and methyl phenyl sulfone; sulfides or disulfides such as dibutyl disulfide, dicyclohexyl disulfide, and tetramethylthiuram monosulfide; sulfonamides such as N,N-dimethylmethanesulfonamide and N,N-diethylmethanesulfonamide, etc. Among these sulfur compounds, ethylene sulfite, 1,3-propane sultone, 1,4-butane sultone, cyclopentane sulfone, etc. are preferred, and ethylene sulfite is particularly preferred. When added to the aqueous electrolyte, the sulfur compound can be used alone or in combination of two or more. The content of the sulfur compound can be, for example, 0.1% by mass or more and 5.0% by mass or less relative to the total amount of the aqueous electrolyte, preferably 0.3% by mass or more and 2.0% by mass or less.

[0056] The method for preparing the aqueous electrolyte according to the present embodiment is not particularly limited, and the aqueous electrolyte may be prepared by, for example, appropriately mixing water, a lithium salt, and the above-mentioned additives when adding.

[0057] The pH of the aqueous electrolyte is not particularly limited, for example, as long as it is greater than 3 and less than 14, preferably greater than 10. This is because: when the pH of the aqueous electrolyte is within these ranges, the stability of the positive electrode active material in the positive electrode and the negative electrode active material in the negative electrode in the aqueous solution can be improved, and the absorption and desorption reactions of lithium ions in the positive electrode active material and the negative electrode active material can become smoother.

[0058] [Secondary battery]

[0059] Hereinafter, a secondary battery described in an example of an embodiment of the present application will be described. A secondary battery as an example of an embodiment comprises the above-mentioned aqueous electrolyte, a positive electrode and a negative electrode. The secondary battery has a structure in which, for example, an electrode body comprising a positive electrode, a negative electrode and a separator and an aqueous electrolyte are contained in a battery case. As the electrode body, for example, a wound electrode body in which a positive electrode and a negative electrode are wound with a separator therebetween, a stacked electrode body in which a positive electrode and a negative electrode are stacked with a separator therebetween, etc. can be cited, and the form of the electrode body is not limited thereto.

[0060] Battery cases for housing the electrode bodies and aqueous electrolytes include cylindrical, square, coin-shaped, button-shaped, and other metal or resin cases; and resin cases formed by laminating metal foils with resin sheets (laminated batteries).

[0061] The secondary battery described in this embodiment can be manufactured using a known method, for example, by housing a wound or stacked electrode body in a battery case body, injecting an aqueous electrolyte, and then sealing the opening of the battery case body with a gasket and a sealing body.

[0062] [positive electrode]

[0063] The positive electrode constituting the secondary battery described in this embodiment is composed of, for example, a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector. The positive electrode active material layer can be formed on one surface of the positive electrode collector or on both surfaces. The positive electrode active material layer includes, for example, a positive electrode active material, a binding material, a conductive material, etc.

[0064] As the positive electrode current collector, a foil of a metal that is stable within the potential range of the positive electrode and a thin film of the metal disposed on the surface layer can be used. As the positive electrode current collector, a porous body such as a mesh body, a punched sheet, and a metal plate net of the metal can be used. As the material of the positive electrode current collector, stainless steel, aluminum, aluminum alloy, titanium, etc. can be used. From the viewpoints of current collection, mechanical strength, etc., the thickness of the positive electrode current collector is preferably, for example, 3 μm or more and 50 μm or less.

[0065] The positive electrode can be obtained by, for example, coating a positive electrode composite material slurry containing a positive electrode active material, a conductive material, a binding material, etc. on a positive electrode collector and drying it, thereby forming a positive electrode active material layer on the positive electrode collector, and rolling the positive electrode active material layer. As a dispersion medium used in the positive electrode composite material slurry, for example, water, ethanol and other alcohols, ethers such as tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), etc. can be used. The thickness of the positive electrode active material layer is not particularly limited, for example, 10 μm or more and 100 μm or less.

[0066] The positive electrode active material is a lithium transition metal oxide containing lithium (Li) and transition metal elements such as cobalt (Co), manganese (Mn) and nickel (Ni). As a specific example of the lithium transition metal oxide, Li a Ni x Co y Mn z M b O2 represents and satisfies:

[0067] 0.9 <a<1.1

[0068] 0.4 <x<1

[0069] 0 ≤ y < 0.4

[0070] 0 ≤ z < 0.4

[0071] 0 ≤ b < 0.2

[0072] 0.9 < (x + y + z + b) < 1.1。

[0073] Element M preferably contains at least one selected from the group consisting of titanium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), tungsten (W), aluminum (Al), gallium (Ga), and indium (In).

[0074] From the viewpoint of high capacity, the lithium transition metal oxide preferably contains Ni in an amount exceeding 40 mol% relative to the total amount of transition metals other than lithium, and more preferably exceeding 50 mol%. Specifically, 0.4 < x < 1.0, and more preferably 0.5 < x < 1.0. In addition, from the viewpoint of crystal structure stability, 0 ≤ y < 0.4, 0 ≤ z < 0.4, 0 ≤ b < 0.2, and 0.9 < (x + y + z + b) < 1.1 are preferred.

[0075] Figure 1 Schematic explanatory diagram showing the positive electrode active material 10 according to the present embodiment. In a secondary battery using an aqueous electrolyte, self-discharge is achieved by embedding protons from the electrolyte into the positive electrode active material 10, and the battery voltage can be reduced, especially the voltage when using a positive electrode active material with a high Ni ratio. In contrast, by the presence of element M such as Al, Ti, Zr, W, etc. in the positive electrode active material, proton insertion is suppressed, and thus voltage reduction is suppressed.

[0076] Here, as the existence form of element M in the positive electrode active material, there may be a mode of solid solution in the positive electrode active material and a mode of existing in the form of a compound on the surface of the positive electrode active material. Element M in the present embodiment only needs to exist in at least one of these two modes. Whether element M is solid-solved in the positive electrode active material or concentrated on the surface of the positive electrode active material can be determined according to the size of element M and the calcination temperature during the production of the positive electrode. It should be noted that when existing in the form of a compound on the surface of the positive electrode active material, element M exists in the form of polyanions such as oxides, carbonates, phosphates, and sulfates.

[0077] That is, the size of the added element M determines whether it is a solid solution (mixing different metals into the transition metal site of the positive electrode active material) or a tendency to be biased on the surface of the positive electrode active material. Generally speaking, the elements of the 3rd and 4th periods (small elements) tend to be solid solutions, and the elements of the 5th period and later (large elements) tend to be biased on the surface. The 3rd period element is Al, and the 4th period elements are Ti, V, Cr, and Ga. The 5th period elements are Zr, Nb, Mo, and In, and the 6th period elements are Hf, Ta, and W.

[0078] In addition, whether the added element M is solid-dissolved or partial to the surface also changes with the calcination temperature. The higher the calcination temperature, the easier it is to solid-dissolve, but other elements such as Li volatilize and cause the ratio of Li to decrease, which may cause an increase in resistance and a decrease in capacity. If the calcination temperature is low, crystallization of the active material will not occur and it will not work as an active material. Therefore, it can be said that 500°C to 900°C is a suitable temperature for the calcination temperature.

[0079] More specifically, in order to make the element M solid solution, the smaller elements of the 3rd and 4th periods are used as the element M, and the calcination temperature is as high as possible and the calcination is carried out for a long time. If the calcination temperature is too high or the calcination time is too long, sintering is aggravated, the particle size becomes too large, Li volatilizes and causes the Li ratio to decrease, which becomes the reason for the increase in resistance and the decrease in battery capacity. Therefore, it is preferably, for example, below 900°C and below 24 hours. In addition, in order to make the element M partial to the surface, the larger elements of the 5th period and thereafter are used as the element M, and the calcination temperature is as low as possible and the calcination is carried out for a short time. If the calcination temperature is too low or the calcination time is too short, the crystallization of the positive active material becomes insufficient and the battery characteristics deteriorate. Therefore, it is preferably, for example, above 700°C and above 6 hours.

[0080] It should be noted that in the mode of making the element M biased on the surface, there can be a mode that is biased only on the surface of the secondary particles composed of the aggregation of primary particles and a mode that is biased on the surface of the primary particles (inside the secondary particles) and the surface of the secondary particles. In the mode that is biased only on the surface of the secondary particles, for example, after the precursor is mixed with the Li raw material and baked to make the active material of the secondary particles without adding a metal compound, the metal compound (element M additive material) is mixed and heat-treated at a low temperature (about 700°C) for a short time, so that it can be biased only on the surface of the secondary particles. Here, when the element M is a larger element of the 5th period and later, it is necessary to pay attention to the fact that it is difficult to dissolve and is easy to be biased on the surface. On the other hand, in the mode that is biased on the surface of the primary particles (inside the secondary particles) and the surface of the secondary particles, after mixing the precursor (transition metal hydroxide), the metal compound (element M additive material) and the Li raw material (LiOH or Li2CO3), it can be biased on the surface of the primary particles (inside the secondary particles) and the surface of the secondary particles by baking at a low temperature (about 700°C) for a short time.

[0081] The element M dissolved in the lithium transition metal oxide and the element M present on the surface of the active material particles can be of the same type or different elements. Even if the dissolved element M and the element M present on the surface are the same element, they are clearly distinguished due to differences in crystal structure, etc. The element M that is biased on the surface of the active material mainly constitutes an oxide having a crystal structure different from that of the lithium transition metal oxide. The dissolved element M and the element M biased on the surface can be distinguished by various analysis methods such as element mapping based on EPMA (Electron Probe Micro-Analysis), analysis of chemical bond states based on XPS (X-ray Photoelectron Spectroscopy), and SIMS (Secondary Ionization Mass Spectroscopy).

[0082] The average particle size (D50) of the lithium transition metal oxide particles is preferably, for example, 2 μm or more and 20 μm or less. When the average particle size (D50) is less than 2 μm and exceeds 20 μm, the packing density in the positive electrode active material layer is sometimes reduced and the capacity is reduced compared to the case where the above range is satisfied. The average particle size (D50) of the positive electrode active material can be measured by using, for example, MT3000II manufactured by MICROTRAC BELL and by laser diffraction.

[0083] Examples of the conductive material contained in the positive electrode active material layer include carbon black, acetylene black, Ketjen black, graphite and other carbon powders, etc. These may be used alone or in combination of two or more.

[0084] As the binding material contained in the positive electrode active material layer, for example, fluorine-based polymers, rubber-based polymers, etc. can be listed. As fluorine-based polymers, for example, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF) or their modified bodies can be listed, and as rubber-based polymers, for example, ethylene-propylene-isoprene copolymers, ethylene-propylene-butadiene copolymers, etc. can be listed. They can be a single one, or two or more can be used in combination.

[0085] The positive electrode of the present embodiment can be obtained by, for example, applying a positive electrode composite material slurry containing a positive electrode active material, a conductive material, a binder, etc., on a positive electrode current collector, drying the slurry to form a positive electrode active material layer, and rolling the positive electrode composite material layer.

[0086] [negative electrode]

[0087] The negative electrode constituting the secondary battery described in this embodiment is composed of, for example, a negative electrode current collector and a negative electrode active material layer formed on the negative electrode current collector. The negative electrode active material layer may be formed on one surface of the negative electrode current collector or on both surfaces. The negative electrode active material layer includes, for example, a negative electrode active material, a binding material, and the like.

[0088] As the negative electrode current collector, a foil of a metal that is stable within the potential range of the negative electrode, and a thin film of the metal disposed on the surface layer, etc. can be used. As the negative electrode current collector, a porous body such as a mesh body, a punched sheet, and a metal plate net of the metal can be used. As the material of the negative electrode current collector, copper, copper alloy, aluminum, aluminum alloy, stainless steel, nickel, etc. can be used. From the viewpoints of current collection, mechanical strength, etc., the thickness of the negative electrode current collector is preferably, for example, 3 μm or more and 50 μm or less.

[0089] The negative electrode can be prepared by, for example, coating a negative electrode composite material slurry containing a negative electrode active material, a binding material and a dispersion medium on a negative electrode collector and drying the coating film, and then rolling to form a negative electrode active material layer on one or both sides of the negative electrode collector. The negative electrode active material layer may contain any component such as a conductive agent as needed. The thickness of the negative electrode active material layer is not particularly limited, for example, 10 μm or more and 100 μm or less.

[0090] The negative electrode active material is not particularly limited as long as it is a material that can absorb / release lithium ions. The material constituting the negative electrode active material may be a non-carbon material, a carbon material, or a combination thereof. Examples of non-carbon materials include lithium metal, alloys containing lithium elements, and metal compounds such as metal oxides, metal sulfides, and metal nitrides containing lithium. Examples of alloys containing lithium elements include lithium aluminum alloys, lithium tin alloys, lithium lead alloys, and lithium silicon alloys. Examples of metal oxides containing lithium include metal oxides containing lithium and containing titanium, tantalum, or niobium, preferably lithium titanate (Li4Ti5O 12 wait).

[0091] As carbon materials used as negative electrode active materials, for example, graphite and hard carbon can be listed. Among them, graphite is preferred due to its high capacity and small irreversible capacity. Graphite is a general term for carbon materials with a graphite structure, including natural graphite, artificial graphite, expanded graphite, graphitized mesophase carbon particles, etc. When graphite is used as a negative electrode active material, in order to reduce the activity of reduction and decomposition of aqueous electrolytes, it is preferred to cover the surface of the negative electrode active material layer with a coating. These negative electrode active materials can be used alone or in combination of two or more.

[0092] As the binding material contained in the negative electrode active material layer, for example, fluorine-based polymers, rubber-based polymers, etc. can be used in the same manner as in the case of the positive electrode. In addition, styrene-butadiene copolymer (SBR) or its modified body can also be used. The content of the binding material contained in the negative electrode active material layer is preferably 0.1% by mass or more and 20% by mass or less relative to the total amount of the negative electrode active material, more preferably 1% by mass or more and 5% by mass or less. As the thickener contained in the negative electrode active material layer, for example, carboxymethyl cellulose (CMC), polyethylene oxide (PEO), etc. can be listed. They can be a single kind, or two or more kinds can be used in combination.

[0093] [Separator]

[0094] As a separator, there is no particular limitation as long as it has the function of passing lithium ions and electrically separating the positive electrode from the negative electrode, and for example, a porous sheet composed of a resin, an inorganic material, etc. can be used. Specific examples of porous sheets include microporous films, woven fabrics, non-woven fabrics, etc. As resin materials constituting the separator, olefin resins such as polyethylene and polypropylene; polyamide, polyamide-imide, cellulose, etc. can be listed. As inorganic materials constituting the separator, glasses and ceramics such as borosilicate glass, silica, alumina, and titanium dioxide can be listed. The separator can be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, it can be a multilayer separator comprising a polyethylene layer and a polypropylene layer, and a separator coated with a material such as an aromatic polyamide resin, ceramic, etc. on the surface of the separator can also be used.

[0095] It should be noted that, in the above embodiment, a secondary battery having an aqueous electrolyte is described, but the aqueous electrolyte described in one example of this embodiment can be used in a storage device other than a secondary battery, and can be used in, for example, a capacitor. In this case, the capacitor has, for example, an aqueous electrolyte described in one example of this embodiment and two electrodes. The electrode material constituting the electrode can be any material that can be used in a capacitor and can absorb and release lithium ions, and materials such as graphite-containing materials such as natural graphite or artificial graphite, and materials such as lithium titanate can be listed.

[0096] Example

[0097] Hereinafter, examples and comparative examples of the present application will be described in detail, but the present application is not limited to the following examples.

[0098] (Example 1)

[0099] A secondary battery was manufactured according to the following steps.

[0100] [Production of positive electrode]

[0101] As the positive electrode active material, the precursor [(Ni 0.55 Co 0.30 Mn 0.15 )(OH)2], LiOH and Al2O3 were mixed in a predetermined amount ratio and calcined at 850°C for 7 hours in the atmosphere to prepare a lithium transition metal oxide (LiNi 0.55 Co 0.30 Mn 0.15 Al 0.0015 O2). The lithium transition metal oxide, acetylene black (AB) as a conductive material and polyvinylidene fluoride (PVdF) as a binder were mixed in a mass ratio of NCA:AB:PVdF=100:1:0.9, and then an appropriate amount of N-methyl-2-pyrrolidone (NMP) was added and stirred to prepare a positive electrode slurry. Then, the obtained positive electrode slurry was applied to both sides of an aluminum foil (positive electrode collector), dried, and the coating of the positive electrode composite material was rolled using a roller to prepare the positive electrode of Example 1.

[0102] [Production of negative electrode]

[0103] Graphite as a negative electrode active material, styrene-butadiene copolymer (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener were mixed in a mass ratio of 100:1:1, and water was added to prepare a negative electrode slurry. Next, the negative electrode slurry was applied to both sides of a negative electrode collector formed of copper foil, dried, and then rolled using a calendering roller to produce a negative electrode having a negative electrode active material layer formed on both sides of the negative electrode collector.

[0104] [Preparation of aqueous electrolyte]

[0105] LiN(SO2CF3)2, LiN(SO2C2F5)2, LiOH·H2O and water (ultrapure water) were mixed in a molar ratio of 0.7:0.3:0.034:1.923.

[0106] [Manufacturing of Secondary Batteries]

[0107] The electrode body is made by winding the positive electrode and the negative electrode with a separator, and the electrode body is housed in a battery case with a bottomed cylindrical shape together with the aqueous electrolyte, and the opening of the battery case is sealed with a gasket and a sealing body. It is used as the secondary battery of Example 1. For the secondary battery of Example 1, the stability during charging and storage is evaluated. In Table 1, the change in open circuit voltage is recorded as the evaluation result of the stability during charging and storage. In Table 1, the change in open circuit voltage is referred to as the voltage change.

[0108] [Evaluation of Stability during Charge Storage]

[0109] After charging at a constant current of 0.1C until the closed circuit voltage of the battery reaches 2.75V, the battery is stored at 25°C for 72 hours. After storage, the change in the open circuit voltage of the battery (V) is calculated. The charging storage test is performed in an environment of 25°C. The change in the open circuit voltage (V) is used as an evaluation of the stability during charging storage.

[0110] (Comparative Example 1)

[0111] When preparing the positive electrode active material, the positive electrode was prepared by the same method as in Example 1 except that Al2O3 was not added. A secondary battery was prepared using the prepared positive electrode and evaluated in the same manner as in Example 1. That is, in the secondary battery of Comparative Example 1, LiNi 0.55 Co 0.30 Mn 0.15 O2 is used as the positive electrode active material.

[0112] (Example 2)

[0113] As the positive electrode active material, the precursor [(Ni 0.55 Co 0.30 Mn 0.15 )(OH)2], LiOH and TiO2 were mixed in a predetermined amount ratio and calcined at 850°C for 7 hours in the atmosphere to produce lithium transition metal oxide (LiNi 0.55 Co 0.30 Mn 0.15 Ti 0.0015 O2). In addition to using LiNi 0.55 Co 0.30Mn 0.15 Ti 0.0015 A secondary battery of Example 2 was produced in the same manner as in Example 1 except that O 2 was used as the positive electrode active material, and was evaluated in the same manner as in Example 1.

[0114] (Example 3)

[0115] As the positive electrode active material, the precursor [(Ni 0.55 Co 0.30 Mn 0.15 )(OH)2], LiOH and ZrO2 were mixed in a predetermined amount ratio and calcined at 850°C for 7 hours in the atmosphere to produce a lithium transition metal oxide (LiNi 0.55 Co 0.30 Mn 0.15 Zr 0.0005 O2). In addition to using LiNi 0.55 Co 0.30 Mn 0.15 Zr 0.0005 A secondary battery of Example 3 was produced in the same manner as in Example 1 except that O 2 was used as the positive electrode active material, and was evaluated in the same manner as in Example 1.

[0116] Table 1 summarizes the evaluation results.

[0117] [Table 1]

[0118]

[0119] As shown in Table 1, compared with the secondary battery of Comparative Example 1, the secondary batteries of Examples 1 to 3 can suppress the voltage drop during charge storage by adding Al, Ti, and Zr to the positive electrode active material, respectively. That is, compared with the secondary battery of Comparative Example 1, the charge storage stability of the secondary batteries of Examples 1 to 3 is improved. It can be inferred that the reason why the charge storage stability of the secondary battery of Example 1 is improved is that the interlayer of the layered structure of the positive electrode active material is narrowed by solid solution of Al, and proton embedding is suppressed. It can be inferred that the reason why the charge storage stability of the secondary battery of Example 2 is improved is that the interlayer of the layered structure of the positive electrode active material is narrowed by solid solution of Ti, and proton embedding is suppressed. It can be inferred that the reason why the charge storage stability of the secondary battery of Example 3 is improved is that the interlayer of the layered structure of the positive electrode active material is narrowed by solid solution of Zr, and proton embedding is suppressed. On this basis, the proton embedding into the interlayer of the positive electrode active material at the interface between the positive electrode active material and the aqueous electrolyte is hindered.

[0120] In addition, the negative electrode of the manufactured battery is lithium titanate, which is a material with almost no potential change at the negative electrode. Therefore, suppressing the decrease in open circuit voltage means suppressing the decrease in the potential of the positive electrode. Therefore, it can be seen that by adding different elements to the positive electrode active material and dissolving them, the decrease in the potential of the positive electrode is suppressed, and the charging storage stability of the battery can be improved.

[0121] The effect of adding element M is manifested by suppressing proton embedding in this way. When the added element M is dissolved in the crystal of the active material, the proton embedding is suppressed due to the reduction of the lattice. In addition, even if the added element M is not dissolved in the crystal but is biased on the surface of the active material, it will present a form of different elements covering the surface of the active material, suppressing the embedding of protons. In summary, the solid solution and surface bias of the added element M can also occur simultaneously.

Claims

1. A secondary battery comprising: a positive electrode containing a positive electrode active material for a secondary battery, a negative electrode containing a negative electrode active material, and an electrolyte solution formed by dissolving a lithium salt in water, The positive electrode active material for the secondary battery is generally Li a Ni x Co y Mn z M b O2 represents and satisfies: 0.9<a<1.1、 0.4<x<1、 0≤y<0.4、 0≤z<0.4、 0<b<0.2、 0.9<(x+y+z+b)<1.1, The element M includes at least one selected from the group consisting of Ti and Zr, The water content is 8 mass % or more and 50 mass % or less relative to the total amount of the electrolyte solution, The pH of the electrolyte is greater than 10.

2. The secondary battery according to claim 1, wherein The element M includes Zr.

3. The secondary battery according to claim 1, wherein The element M includes Ti.

4. The secondary battery according to claim 1, wherein In the general formula, x satisfies x>0.

5.

5. The secondary battery according to claim 1, wherein b in the general formula satisfies 0 <b<0.03。 6. The secondary battery according to claim 2, wherein The element M is concentrated in the surface layer of the positive electrode active material.

7. The secondary battery according to claim 6, wherein The element M is concentrated in the surface layer portion of the primary particles and the surface layer portion of the secondary particles of the positive electrode active material.

8. The secondary battery according to claim 3, wherein The element M is solid-dissolved in the positive electrode active material.

9. The secondary battery according to claim 1, wherein The element M exists in the surface layer of the positive electrode active material and is solid-dissolved in the positive electrode active material.

10. The secondary battery according to claim 1, wherein The amount of water is less than 4 mol relative to 1 mol of the lithium salt in the electrolyte.