Multilayer ceramic capacitor and method for manufacturing the same
By controlling the stacking direction distance ratio and dielectric layer thickness of the ceramic main body, combined with different dielectric materials and adhesive content, the problems of moisture-proof reliability and voltage resistance in multi-layer ceramic capacitors are solved, and high capacity and high resistance are achieved Take into account both voltage.
Patent Information
- Application Number
- CN202010830259.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-29
- Filing Date
- 2020-08-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-08-18
AI Technical Summary
In miniaturized and high capacity multi-layer ceramic capacitors, the prior art is difficult to improve moisture resistance and withstand voltage simultaneously, especially in the voids at the side edges that lead to moisture permeation and excessive firing. question.
By controlling the ratio of the distance between the stacking direction of the central region of the ceramic body and the distance between the edge region of the side edge part between 1.00 and 1.07, the thickness of the dielectric layer and the inner electrode is adjusted, and different dielectric materials and bonds are used in the firing process. The agent content is to form the side edge portion, and the shrinkage rate of the side edge portion is reduced to improve moisture resistance and voltage tolerance.
It is achieved to improve moisture-proof reliability and voltage withstand characteristics in ultra-small and high-capacity multi-layer ceramic capacitors, increase the breakdown voltage and improve the concentrated easing effect of electric field.
Smart Images

Figure CN112885600B_ABST
Abstract
Description
[0001] This application claims the benefit of priority from Korean Patent Application No. 10-2019-0156838 filed on November 29, 2019, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field
[0002] The present disclosure relates to a multilayer ceramic capacitor and a method of manufacturing the multilayer ceramic capacitor, in which moisture-proof reliability can be improved while a withstand voltage can be improved. Background Art
[0003] Generally, an electronic component using a ceramic material, such as a capacitor, an inductor, a piezoelectric element, a varistor, or a thermistor, includes a ceramic body formed using the ceramic material, an internal electrode formed inside the ceramic body, and an external electrode disposed on a surface of the ceramic body to be connected to the internal electrode.
[0004] Recently, as electronic products have become miniaturized and multifunctional, chip components have also become miniaturized and highly functional. Therefore, multilayer ceramic capacitors are required to have high capacitance and small size.
[0005] As described above, for small and high capacity products, it is necessary to ensure reliability and high withstand voltage characteristics.
[0006] Miniaturization and high capacitance of multilayer ceramic capacitors require a significant increase in the active electrode area (increasing the active volume fraction required to achieve capacitance).
[0007] In order to realize a small and high-capacity multilayer ceramic capacitor as described above, when manufacturing the multilayer ceramic capacitor, the inner electrode can be exposed in the width direction of the body, thereby significantly increasing the inner electrode area in the width direction through a marginless design. For example, in the pre-firing stage, after manufacturing such a sheet, a method of separately attaching the side edge portion to the electrode exposed surface in the width direction of the sheet to complete the multilayer ceramic capacitor is adopted.
[0008] However, in the process of forming the side margin portion according to the above method, voids in the side margin portion increase, and moisture may penetrate the voids, thereby reducing moisture-proof reliability.
[0009] Increasing the firing temperature to remove the voids may cause a problem in that a withstand voltage may be reduced due to over-firing of the internal electrodes adjacent to the side margin portions.
[0010] Therefore, research is required to improve moisture resistance reliability and ensure high breakdown voltage (BDV) in ultra-small and high-capacity products. Summary of the invention
[0011] This summary is provided to introduce selected concepts in a simplified form, and the concepts are further described in the following detailed description. This summary is neither intended to identify key features or essential features of the claimed subject matter, nor is it intended to be used as an aid in determining the scope of the claimed subject matter.
[0012] An aspect of the present disclosure is to provide a multilayer ceramic capacitor that can improve moisture-proof reliability while improving withstand voltage and a method of manufacturing the multilayer ceramic capacitor.
[0013] According to one aspect of the present disclosure, a multilayer ceramic capacitor includes: a ceramic body including a dielectric layer, the ceramic body having a first surface and a second surface opposite to each other, a third surface and a fourth surface connecting the first surface and the second surface, and a fifth surface and a sixth surface connected to the first surface, the second surface, the third surface and the fourth surface and opposite to each other; a plurality of first internal electrodes and a plurality of second internal electrodes disposed inside the ceramic body, exposed to the first surface and the second surface, and having an end exposed to the third surface or the fourth surface; and a first side edge portion and a second side edge portion, respectively disposed on the side portions of the plurality of first internal electrodes and the plurality of second internal electrodes exposed to the first surface and the second surface. The ratio Db / Da satisfies greater than or equal to 1.00 and less than or equal to 1.07, wherein "Db" is the distance between the two ends of the corresponding edge regions of the first side edge portion and the second side edge portion in the stacking direction of the dielectric layer, and "Da" is the distance in the stacking direction of the central region of the ceramic body.
[0014] According to one aspect of the present disclosure, a method for manufacturing a multilayer ceramic capacitor includes: preparing a first ceramic green sheet and a second ceramic green sheet, forming a plurality of first internal electrode patterns at predetermined intervals on the first ceramic green sheet, and forming a plurality of second internal electrode patterns at predetermined intervals on the second ceramic green sheet; stacking the first ceramic green sheet and the second ceramic green sheet in such a manner that the plurality of first internal electrode patterns and the plurality of second internal electrode patterns are staggered and overlapped with each other to form a ceramic green sheet stacking body; cutting the ceramic green sheet stacking body to have side surfaces with edges of the plurality of first internal electrode patterns and edges of the plurality of second internal electrode patterns exposed in a width direction; forming a first side edge portion and a second side edge portion on the side surfaces of the cut stacking body, respectively; and firing the cut stacking body to provide a ceramic body including a dielectric layer and first and second internal electrodes. The ratio Db / Da satisfies greater than or equal to 1.00 and less than or equal to 1.07, wherein "Db" is the distance between the two ends of the corresponding edge areas of the first side edge portion and the second side edge portion in the stacking direction of the dielectric layer, and "Da" is the distance in the central area of the ceramic body in the stacking direction. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] The above and other aspects, features and advantages of the present disclosure will be more clearly understood through the following detailed description taken in conjunction with the accompanying drawings, in which:
[0016] Figure 1 is a schematic perspective view showing a multilayer ceramic capacitor according to an exemplary embodiment;
[0017] Figure 2 It is shown Figure 1 A perspective view of the appearance of the ceramic body;
[0018] Figure 3 It is shown Figure 2 A perspective view of a ceramic green sheet stacked body before firing of the ceramic body;
[0019] Figure 4 It is along Figure 1 A cross-sectional view taken along line II';
[0020] Figure 5 yes Figure 4 A magnified view of region B; and
[0021] 6A to 6F are cross-sectional views and perspective views schematically illustrating a method of manufacturing a multilayer ceramic capacitor according to another exemplary embodiment. DETAILED DESCRIPTION
[0022] The following detailed description is provided to help the reader gain a comprehensive understanding of the methods, devices and / or systems described herein. However, various variations, modifications and equivalents of the methods, devices and / or systems described herein will be apparent to those of ordinary skill in the art. The order of operations described herein is merely exemplary and is not limited to the order set forth herein, but changes may be made that will be apparent to those of ordinary skill in the art, except for operations that must occur in a particular order. In addition, descriptions of functions and configurations that will be well known to those of ordinary skill in the art may be omitted for clarity and brevity.
[0023] The features described herein may be presented in different forms and should not be construed as limited to the examples described herein. Rather, the examples described herein have been provided so that this disclosure will be thorough and complete, and will fully convey the scope of the disclosure to those skilled in the art.
[0024] Here, it is noted that the use of the term "may" with respect to an example or embodiment (e.g., with respect to what an example or embodiment may include or implement) means that there is at least one example or embodiment that includes or implements such features, and all examples and embodiments are not limited thereto.
[0025] Throughout the specification, when an element (such as a layer, a region, or a substrate) is described as being “on”, “connected to”, or “coupled to” another element, the element may be directly “on”, “connected to”, or “coupled to” the other element, or one or more other elements may be present between them. In contrast, when an element is described as being “directly on”, “directly connected to”, or “directly coupled to” another element, there may be no other elements present between them.
[0026] As used herein, the term "and / or" includes any one of the associated listed items and any combination of any two or more items.
[0027] Although terms such as "first", "second", and "third" may be used herein to describe various members, components, regions, layers, or portions, these members, components, regions, layers, or portions are not limited to these terms. Rather, these terms are only used to distinguish one member, component, region, layer, or portion from another member, component, region, layer, or portion. Therefore, without departing from the teachings of the examples described herein, the first member, first component, first region, first layer, or first portion referred to in the examples may also be referred to as the second member, second component, second region, second layer, or second portion.
[0028] For ease of description, spatially relative terms such as "above," "above," "below," and "below" may be used herein to describe the relationship of one element to another element as shown in the accompanying drawings. Such spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientations depicted in the accompanying drawings. For example, if the device in the accompanying drawings is turned over, an element described as being "above" or "above" relative to another element will then be "below" or "below" relative to the other element. Therefore, the term "above" includes both above and below orientations depending on the spatial orientation of the device. The device may also be positioned in other ways (e.g., rotated 90 degrees or in other orientations), and the spatially relative terms used herein will be interpreted accordingly.
[0029] The terms used herein are only used to describe various examples and are not intended to limit the present disclosure. Unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. The terms "comprise", "include" and "have" list the existence of the stated features, quantities, operations, components, elements and / or their combinations, but do not exclude the existence or addition of one or more other features, quantities, operations, components, elements and / or their combinations.
[0030] Variations in the shapes shown in the drawings may occur due to manufacturing techniques and / or tolerances. Therefore, the examples described herein are not limited to the specific shapes shown in the drawings but include variations in shapes that occur during manufacturing.
[0031] The features of the examples described herein can be combined in various ways that will be apparent after understanding the disclosure of the present application. In addition, although the examples described herein have various configurations, other configurations that will be apparent after understanding the disclosure of the present application are feasible.
[0032] The drawings may not be drawn to scale, and the relative size, proportions, and depiction of elements in the drawings may be exaggerated for clarity, illustration, and convenience.
[0033] Subsequently, examples are described in further detail with reference to the accompanying drawings.
[0034] Figure 1 is a schematic perspective view illustrating a multilayer ceramic capacitor according to an exemplary embodiment.
[0035] Figure 2 It is shown Figure 1 A perspective view of the exterior shape of a ceramic body.
[0036] Figure 3 It is shown Figure 2 A perspective view of a ceramic green sheet stacked body before firing of a ceramic body.
[0037] Figure 4 It is along Figure 1 A cross-sectional view taken along line II'.
[0038] Reference Figures 1 to 4 , a multilayer ceramic capacitor 100 according to an exemplary embodiment includes: a ceramic body 110 ; a plurality of internal electrodes 121 and 122 formed in the ceramic body 110 ; and external electrodes 131 and 132 formed on an outer surface of the ceramic body 110 .
[0039] The ceramic body 110 may have first and second surfaces 1 and 2 opposite to each other, third and fourth surfaces 3 and 4 connecting the first and second surfaces, and a fifth surface 5 as an upper surface and a sixth surface 6 as a lower surface.
[0040] The first surface 1 and the second surface 2 may be surfaces opposite to each other in the width direction of the ceramic body 110 as the second direction, the third surface 3 and the fourth surface 4 may be surfaces opposite to each other in the length direction as the first direction, and the fifth surface 5 and the sixth surface 6 may be surfaces opposite to each other in the thickness direction as the third direction.
[0041] The shape of the ceramic body 110 is not particularly limited, but may be a rectangular parallelepiped shape as shown in the drawings.
[0042] One ends of the plurality of internal electrodes 121 and 122 formed in the ceramic body 110 are exposed to the third surface 3 or the fourth surface 4 of the ceramic body.
[0043] The internal electrodes 121 and 122 may be provided as a pair of first and second internal electrodes 121 and 122 having different polarities.
[0044] One end of the first internal electrode 121 may be exposed to the third surface 3 , and one end of the second internal electrode 122 may be exposed to the fourth surface 4 .
[0045] The other end of the first internal electrode 121 is formed to be spaced a predetermined distance from the fourth surface 4 , and the other end of the second internal electrode 122 is formed to be spaced a predetermined distance from the third surface 3 .
[0046] The first external electrode 131 may be formed on the third surface 3 of the ceramic body, and the second external electrode 132 may be formed on the fourth surface 4 of the ceramic body to be electrically connected to the internal electrode.
[0047] According to an exemplary embodiment, a multilayer ceramic capacitor 100 includes: a plurality of internal electrodes 121 and 122, which are arranged inside a ceramic body 110, exposed to a first surface 1 and a second surface 2, and have one end exposed to a third surface 3 or one end exposed to a fourth surface 4; and a first side edge portion 112 and a second side edge portion 113, which are respectively arranged on the sides of the internal electrodes 121 and 122 exposed on the first surface 1 and the second surface 2.
[0048] A plurality of internal electrodes 121 and 122 are formed in the ceramic body 110, and respective side portions of the plurality of internal electrodes 121 and 122 are exposed to first and second surfaces, which are surfaces in a width direction of the ceramic body 110. First and second side margin portions 112 and 113 are disposed on the exposed side portions of the internal electrodes 121 and 122.
[0049] An average thickness of the first side margin portion 112 and the second side margin portion 113 may be greater than or equal to 10 μm and less than 45 μm.
[0050] According to an exemplary embodiment, the ceramic body 110 may include a laminated body in which a plurality of dielectric layers 111 are stacked, and first and second side margin parts 112 and 113 disposed on both sides of the laminated body.
[0051] The plurality of dielectric layers 111 may be in a sintered state, and may be integrated such that a boundary between adjacent dielectric layers cannot be recognized.
[0052] The length of the ceramic body 110 corresponds to the distance from the third surface 3 to the fourth surface 4 of the ceramic body.
[0053] The length of the dielectric layer 111 forms the distance between the third surface 3 and the fourth surface 4 of the ceramic body.
[0054] According to an exemplary embodiment, the length of the ceramic body may be 400 μm to 1400 μm, specifically, the length of the ceramic body may be 400 μm to 800 μm or 600 μm to 1400 μm, but is not limited thereto.
[0055] The internal electrodes 121 and 122 may be formed on the dielectric layer 111 , and the internal electrodes 121 and 122 may be formed in the ceramic body through sintering with one dielectric layer interposed therebetween.
[0056] Reference Figure 3 , the first internal electrode 121 is formed on the dielectric layer 111. The first internal electrode 121 is not formed in the entire length direction of the dielectric layer. For example, one end of the first internal electrode 121 is formed to the third surface 3 to be exposed to the third surface 3, and the other end of the first internal electrode 121 may be formed to be a predetermined distance from the fourth surface 4 of the ceramic body.
[0057] An end portion of the first internal electrode exposed to the third surface 3 of the ceramic body is connected to the first external electrode 131 .
[0058] Compared with the first internal electrode, one end of the second internal electrode 122 is exposed to the fourth surface 4 to be connected to the second external electrode 132 , and the other end of the second internal electrode 122 is formed to be spaced a predetermined distance from the third surface 3 .
[0059] The internal electrodes may be stacked in an amount of 400 layers or more to implement a high-capacitance multilayer ceramic capacitor, but the embodiment is not limited thereto.
[0060] The dielectric layer 111 may have the same width as that of the first internal electrode 121. For example, the first internal electrode 121 may be formed in the entire width direction of the dielectric layer 111.
[0061] According to an exemplary embodiment, the width of the dielectric layer and the width of the internal electrode may be 100 μm to 900 μm, but are not limited thereto. Specifically, the width of the dielectric layer and the width of the internal electrode may be 100 μm to 500 μm or 100 μm to 900 μm.
[0062] The ceramic body 110 may include an effective portion A as a portion contributing to the capacitance formation of the capacitor, and an upper cover portion 114 and a lower cover portion 115 as an upper edge portion and a lower edge portion formed on an upper portion and a lower portion of the effective portion A, respectively.
[0063] The active portion A may be formed by repeatedly stacking a plurality of first internal electrodes 121 and a plurality of second internal electrodes 122 with the dielectric layer 111 interposed between the first internal electrodes 121 and the second internal electrodes 122 .
[0064] The upper cover 114 and the lower cover 115 may have the same material and configuration as those of the dielectric layer 111 except that the internal electrodes are not included.
[0065] For example, the upper cover 114 and the lower cover 115 may include a ceramic material such as barium titanate (BaTiO 3 ) based ceramic materials.
[0066] The upper cover 114 and the lower cover 115 may each have a thickness of 20 μm or less, but are not necessarily limited thereto.
[0067] According to an exemplary embodiment, in order to improve moisture-proof reliability and ensure high BDV in ultra-small and high-capacity products, the present disclosure may be characterized in that the ratio of the stacking direction distance of the ceramic body in the central area to the distance between the two ends of the corresponding edge areas of the first side edge portion and the second side edge portion in the stacking direction of the ceramic body is controlled.
[0068] For example, as an exemplary embodiment of the present disclosure, in a case where the upper covering portion 114 and the lower covering portion 115 both have a thickness less than or equal to 20 μm, there may be a problem of deteriorated moisture resistance, whereas in the case of the prior art where the thickness of the upper covering portion and the lower covering portion is greater than 20 μm, there is no problem of moisture resistance reliability due to the thickness of the covering portion.
[0069] In an exemplary embodiment, the internal electrode and the dielectric layer are formed by being cut at the same time, and the width of the internal electrode and the width of the dielectric layer may be the same, which will be described in more detail below.
[0070] In order to significantly increase the capacitance of a multilayer ceramic capacitor, a method of thinning the dielectric layer, a method of stacking the thinned dielectric layer to a higher degree, a method of increasing the coverage of the internal electrode, and the like can be considered.
[0071] In addition, a method of increasing the overlapping area of internal electrodes forming a capacitor may be considered.
[0072] In order to increase the overlapping area of the internal electrodes, the edge area in which the internal electrodes are not formed should be significantly reduced.
[0073] In particular, as the size of the multilayer ceramic capacitor is further reduced, the edge area should be significantly reduced to increase the overlapping area of the internal electrodes.
[0074] Generally, in order to realize a small and high-capacity multilayer ceramic capacitor, when manufacturing a multilayer ceramic capacitor, the inner electrode is exposed in the width direction of the body, thereby significantly increasing the inner electrode area in the width direction through a marginless design. For example, in the pre-firing stage, after manufacturing such a sheet, a method of attaching the side edge portion separately to the electrode exposed surface in the width direction of the sheet to complete the multilayer ceramic capacitor is applied.
[0075] However, in the process of forming the side margin portion according to the above method, voids in the side margin portion increase, and moisture may penetrate the voids, thereby reducing moisture-proof reliability.
[0076] Increasing the firing temperature to remove the voids may cause a problem in that a withstand voltage may be reduced due to over-firing of the internal electrodes adjacent to the side margin portions.
[0077] According to an exemplary embodiment of the present disclosure, a ratio Db / Da of a distance Db between both ends of the corresponding edge regions of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to a distance Da in the stacking direction of the central region of the ceramic body 110 satisfies 1.00 to 1.07 (i.e., greater than or equal to 1.00 and less than or equal to 1.07). The distances Da and Db may be measured by standard methods that will be apparent to and understood by a person of ordinary skill in the art. For example, referring to Figure 4 The distances Da and Db can be measured in the WT cross section at the center in the length direction of the ceramic body by a known standard method. Hereinafter, as an example, the distance Da may be expressed as the distance between two end points in the WT cross section of the corresponding edge region.
[0078] By controlling the ratio of the stacking direction distance of the ceramic body in the central area to the distance between the two end points of the corresponding edge areas of the first side edge portion and the second side edge portion, an ultra-small and high-capacity multilayer ceramic capacitor can be achieved, and the withstand voltage can be improved while improving moisture-proof reliability.
[0079] Specifically, according to an exemplary embodiment of the present disclosure, an ultra-small and high-capacity multilayer ceramic capacitor can be provided in which the thickness of the dielectric layer 111 is less than or equal to 0.6 μm and the thickness of the internal electrodes 121 and 122 is less than or equal to 0.4 μm. The thickness of the dielectric layer 111 and the internal electrodes 121 and 122 can be measured by a standard method that will be apparent to and understood by a person of ordinary skill in the art.
[0080] As in the embodiment, in the case of an ultra-small and high-capacity multilayer ceramic capacitor in which a thin film dielectric layer and an internal electrode are applied and in which the thickness of the dielectric layer 111 is less than or equal to 0.6 μm and the thickness of the internal electrodes 121 and 122 is less than or equal to 0.4 μm, moisture penetration into the side edge portion resulting in reduced moisture resistance is a very important problem.
[0081] For example, in an exemplary embodiment of the present disclosure, since a technology in which the dielectric layer 111 has a thickness of less than or equal to 0.6 μm and the internal electrodes 121 and 122 have a thickness of less than or equal to 0.4 μm is applied to an ultra-small and high-capacity multilayer ceramic capacitor, the thickness of the dielectric layer and the internal electrodes can be relatively thin, and therefore, there is a possibility that the moisture-proof reliability may be reduced due to moisture infiltration.
[0082] However, in the ultra-small and high-capacity multilayer ceramic capacitor having separate side margin portions as in the exemplary embodiment of the present disclosure, the ratio Db / Da of the distance Db between the two end points in the stacking direction of the ceramic body 110 of the corresponding edge regions of the first side margin portion 112 and the second side margin portion 113 relative to the stacking direction distance Da in the central region of the ceramic body 110 can be controlled to satisfy 1.00 to 1.07. Therefore, even in the case of a thin film in which the thickness of the dielectric layer 111 is less than or equal to 0.6 μm and the thickness of the internal electrodes 121 and 122 is less than or equal to 0.4 μm, moisture-proof reliability can be improved, and withstand voltage characteristics can also be improved.
[0083] However, the meaning of thin film does not necessarily mean that the thickness of the dielectric layer 111 is less than or equal to 0.6 μm and the thickness of the internal electrodes 121 and 122 is less than or equal to 0.4 μm, but can be understood as including dielectric layers and internal electrodes thinner than those of related art products.
[0084] Although there is no particular limitation on the method of adjusting the ratio Db / Da of the distance Db between the two end points of the corresponding edge areas of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to the stacking direction distance Da in the central area of the ceramic body 110 to satisfy 1.00 to 1.07, for example, the dielectric material and composition used to form the first side edge portion 112 and the second side edge portion 113 may be implemented to be different from the dielectric material and composition of the dielectric layer 111 used to form the effective portion A.
[0085] For example, in the related art, since the dielectric material and composition used to form the side margin portion are the same as those used to form the dielectric layer of the effective portion, voids are formed in the side margin portion during firing, and thus there is a problem of relatively low moisture resistance.
[0086] Furthermore, when the firing temperature is increased to remove the side edge portion voids to improve moisture resistance, the withstand voltage of the multilayer ceramic capacitor is reduced.
[0087] However, according to an exemplary embodiment of the present disclosure, the dielectric material and composition used to form the first side edge portion 112 and the second side edge portion 113 may be applied differently from the dielectric material and composition used to form the dielectric layer 111 of the effective portion A, thereby obtaining the two effects of improving moisture-proof reliability and improving withstand voltage characteristics.
[0088] For example, the content of the binder included in the dielectric material for forming the first and second side margin parts 112 and 113 may be different from the content of the binder included in the dielectric material for forming the dielectric layer 111 of the active part A, thereby achieving features according to an exemplary embodiment of the present disclosure.
[0089] The higher the binder content, the greater the shrinkage during firing. Conversely, the lower the binder content, the lower the shrinkage.
[0090] Therefore, when the content of the adhesive included in the dielectric material used to form the first side edge portion 112 and the second side edge portion 113 is less than the content of the adhesive included in the dielectric material used to form the dielectric layer 111 of the effective portion A, the shrinkage rate of the side edge portion during the firing process is lower than the shrinkage rate of the dielectric layer of the effective portion, so that the above-mentioned features can be achieved according to an exemplary embodiment.
[0091] For example, refer to Figure 4, a ratio Db / Da of a distance Db between two end points of the corresponding edge regions of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to a distance Da in the stacking direction of the central region of the ceramic body 110 satisfies 1.00 to 1.07. In this case, the edge regions of the first side edge portion 112 and the second side edge portion 113 have a protruding shape compared to the central region of the ceramic body 110.
[0092] When the ratio Db / Da of the distance Db between the two end points of the corresponding edge areas of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to the stacking direction distance Da in the central area of the ceramic body 110 satisfies 1.00 to 1.07, the two effects of improving moisture-proof reliability and improving withstand voltage characteristics can be obtained.
[0093] The case where the ratio Db / Da of the distance Db between the two end points in the stacking direction of the ceramic body 110 of the respective edge regions of the first side edge portion 112 and the second side edge portion 113 relative to the stacking direction distance Da in the central region of the ceramic body 110 is less than 1.00 is the case of the prior art. In this case, the central portion of the ceramic body has an upwardly protruding shape compared to the edge portions of the side edges. In this case, the distance between the ends of the internal electrodes is relatively short, so that the withstand voltage characteristics are deteriorated, and the high temperature load characteristics are deteriorated.
[0094] If the ratio Db / Da of the distance Db between the two end points of the corresponding edge areas of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 to the stacking direction distance Da in the central area of the ceramic body 110 is greater than 1.07, the shrinkage degree of the side edge portion is relatively small, and the protrusion of the edge area of the side edge portion is aggravated, which may form an uncoated area of the external electrode or may reduce the thickness of the external electrode coating, thereby deteriorating the moisture resistance.
[0095] More specifically, according to an exemplary embodiment of the present disclosure, when the ratio Db / Da of the distance Db between the two end points of the corresponding edge areas of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to the stacking direction distance Da in the central area of the ceramic body 110 satisfies greater than 1.00 and less than or equal to 1.07, the two more excellent effects of improving moisture-proof reliability and improving withstand voltage characteristics can be obtained.
[0096] For example, in a case where a ratio Db / Da of a distance Db between two end points of corresponding edge regions of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to a distance Da in the stacking direction of the central region of the ceramic body 110 is 1.00, it may be difficult to realize an actual product, and when Db / Da exceeds 1.00 as in the embodiment, the above two effects can be improved.
[0097] Reference Figure 4 In the multilayer ceramic capacitor according to the exemplary embodiment, a ratio d2 / d1 of an interval d2 between the first internal electrode 121 and the second internal electrode 122 in an end portion of the ceramic body 110 adjacent to the first side edge portion 112 or the second side edge portion 113 relative to an interval d1 between the first internal electrode 121 and the second internal electrode 122 in a central region of the ceramic body 110 may satisfy greater than 1.00 and less than or equal to 1.05. Therefore, when the interval d2 between the first internal electrode 121 and the second internal electrode 122 in the end portion of the ceramic body 110 increases, an electric field concentration relaxation effect may be obtained, and a breakdown voltage (BDV) may be increased. The intervals d1 and d2 may be measured by a standard method that will be apparent to and understood by a person of ordinary skill in the art.
[0098] In a general multilayer ceramic capacitor, due to a pressing process of the ceramic body, an interval between the first and second internal electrodes in an end portion of the ceramic body becomes smaller than a distance between the first and second internal electrodes in a central region of the ceramic body.
[0099] In this case, when the interval between the first and second internal electrodes is narrowed in the end portion of the ceramic body, the electric field is concentrated, and thus a breakdown voltage (BDV) is reduced.
[0100] According to an exemplary embodiment of the present disclosure, when the shrinkage ratio of the side edge portion is controlled to be lower than the shrinkage ratio of the dielectric layer of the effective portion during the firing process, the interval d2 between the first internal electrode 121 and the second internal electrode 122 in the end portion of the ceramic body 110 may be greater than the interval d1 between the first internal electrode 121 and the second internal electrode 122 in the central region of the ceramic body 110. Therefore, the concentration of the electric field between the first internal electrode and the second internal electrode in the end portion of the ceramic body may be alleviated.
[0101] For this reason, in the multilayer ceramic capacitor according to the exemplary embodiment, the breakdown voltage (BDV) may be increased, thereby improving reliability.
[0102] If a ratio d2 / d1 of an interval d2 between the first internal electrode 121 and the second internal electrode 122 in the end of the ceramic body 110 relative to an interval d1 between the first internal electrode 121 and the second internal electrode 122 in the central region of the ceramic body 110 is less than or equal to 1.00, a breakdown voltage (BDV) is reduced due to the concentration of an electric field between the internal electrodes in the end of the ceramic body.
[0103] If a ratio d2 / d1 of an interval d2 between the first and second internal electrodes 121 and 122 in the end of the ceramic body 110 relative to an interval d1 between the first and second internal electrodes 121 and 122 in the central region of the ceramic body 110 exceeds 1.05, moisture resistance reliability may be deteriorated.
[0104] Figure 5 yes Figure 4 Magnified view of area B.
[0105] Reference Figure 5 , the ratio of the number of pores in the first side edge portion 112 and the second side edge portion 113 to the number of pores in the dielectric layer 111 of the effective portion A may satisfy 0.9 to 1.1 (i.e., greater than or equal to 0.9 and less than or equal to 1.1). As an example, in the same cross section (e.g., Figure 5 The number of pores P per unit area of the corresponding parts is measured in the LT cross section shown in FIG. 1 , and then the number of pores P per unit area is compared.
[0106] According to an exemplary embodiment, a ratio Db / Da of a distance Db between two end points of corresponding edge regions of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to a stacking direction distance Da in the central region of the ceramic body 110 satisfies 1.00 to 1.07, and a ratio of the number of pores in the first side edge portion 112 and the second side edge portion 113 to the number of pores in the dielectric layer 111 of the effective portion A satisfies 0.9 to 1.1, thereby improving moisture-proof reliability and withstand voltage characteristics.
[0107] Although there is no particular limitation on the method of controlling the ratio of the number of pores in the first side edge portion 112 and the second side edge portion 113 to the number of pores in the dielectric layer 111 of the effective portion A to satisfy 0.9 to 1.1, the method can be achieved, for example, by adjusting the particle size of the raw material of the ceramic powder introduced in the process of forming the dielectric layer 111 of the effective portion A, the first side edge portion 112, and the second side edge portion 113.
[0108] For example, barium titanate (BaTiO 3The average particle size of the powder may be larger than that of the barium titanate (BaTiO 3 )The average particle size of the powder can achieve the method of controlling the ratio of the number of pores as described above.
[0109] Although not particularly limited, for example, barium titanate (BaTiO 3 ) powder has an average particle size of about 100 nm, and the barium titanate (BaTiO 3 )The average particle size of the powder is about 70 nm.
[0110] 6A to 6F are cross-sectional views and perspective views schematically illustrating a method of manufacturing a multilayer ceramic capacitor according to another exemplary embodiment.
[0111] According to another exemplary embodiment, a method for manufacturing a multilayer ceramic capacitor includes: preparing a first ceramic green sheet and a second ceramic green sheet, forming a plurality of first internal electrode patterns at predetermined intervals on the first ceramic green sheet, and forming a plurality of second internal electrode patterns at predetermined intervals on the second ceramic green sheet; stacking the first ceramic green sheet and the second ceramic green sheet in such a manner that the first internal electrode patterns and the second internal electrode patterns are staggered and overlapped with each other to form a ceramic green sheet stacking body; cutting the ceramic green sheet stacking body to have a side surface where edges of the first internal electrode patterns and the second internal electrode patterns are exposed in a width direction; forming a first side edge portion and a second side edge portion on side surfaces of the cut stacking body, respectively; and firing the cut stacking body to provide a ceramic body including a dielectric layer and first and second internal electrodes. In this case, a ratio Db / Da of a distance Db between both ends of respective edge regions of the first side edge portion and the second side edge portion in a stacking direction of the ceramic body relative to a stacking direction distance Da in a central region of the ceramic body satisfies 1.00 to 1.07.
[0112] Hereinafter, a method of manufacturing a multilayer ceramic capacitor according to another exemplary embodiment will be described.
[0113] like Fig. 6A As shown in FIG. 1 , a plurality of stripe-type first internal electrode patterns 221 are formed at predetermined intervals on a ceramic green sheet 211. The plurality of stripe-type first internal electrode patterns 221 may be formed in parallel with each other.
[0114] The ceramic green sheet 211 may be formed using a ceramic paste including ceramic powder, an organic solvent, and an organic binder.
[0115] Ceramic powder is a material with a high dielectric constant and may be barium titanate (BaTiO 3)-based materials, lead composite perovskite-based materials, strontium titanate (SrTiO 3 )-based materials, but not limited thereto. Specifically, barium titanate (BaTiO 3 When the ceramic green sheet 211 is fired, the ceramic green sheet 211 becomes the dielectric layer 111 constituting the ceramic body 110.
[0116] The stripe-type first internal electrode pattern 221 may be formed by an internal electrode paste including a conductive metal, and the conductive metal may be nickel (Ni), copper (Cu), palladium (Pd), or an alloy thereof, but is not limited thereto.
[0117] A method of forming the stripe-type first internal electrode pattern 221 on the ceramic green sheet 211 is not particularly limited, but may be formed by, for example, a printing method such as a screen printing method or a gravure printing method.
[0118] Although not shown, a plurality of stripe-type second internal electrode patterns 222 may be formed on the ceramic green sheet 211 at predetermined intervals.
[0119] Hereinafter, the ceramic green sheet having the first internal electrode pattern 221 formed thereon may be referred to as a first ceramic green sheet, and the ceramic green sheet having the second internal electrode pattern 222 formed thereon may be referred to as a second ceramic green sheet.
[0120] Next, if Figure 6B As shown in , the first ceramic green sheets and the second ceramic green sheets may be alternately stacked in such a manner that the stripe-type first internal electrode patterns 221 and the stripe-type second internal electrode patterns 222 are alternately stacked.
[0121] Thereafter, the stripe-type first internal electrode patterns 221 may be the first internal electrodes 121 , and the stripe-type second internal electrode patterns 222 may be the second internal electrodes 122 .
[0122] According to another exemplary embodiment, a thickness td of each of the first and second ceramic green sheets is equal to or less than 1.0 μm, and a thickness te of each of the first and second internal electrode patterns is equal to or less than 0.5 μm.
[0123] Since an exemplary embodiment of the present disclosure is characterized by an ultra-small and high-capacity multilayer ceramic capacitor having a thin film including a dielectric layer having a thickness of less than or equal to 0.6 μm and an internal electrode having a thickness of less than or equal to 0.4 μm, the thickness td of each of the first ceramic green sheet and the second ceramic green sheet is less than or equal to 1.0 μm, and the thickness te of each of the first internal electrode pattern and the second internal electrode pattern is less than or equal to 0.5 μm.
[0124] Figure 6C is a cross-sectional view showing a ceramic green sheet stack body 220 in which a first ceramic green sheet and a second ceramic green sheet are stacked according to an exemplary embodiment, Fig.6D is a perspective view showing a ceramic green sheet stack body 220 in which first and second ceramic green sheets are stacked.
[0125] Reference Figure 6C and Fig.6D , first ceramic green sheets having a plurality of parallel stripe-type first internal electrode patterns 221 printed thereon and second ceramic green sheets having a plurality of parallel stripe-type second internal electrode patterns 222 printed thereon are alternately stacked.
[0126] Specifically, the first and second ceramic green sheets may be stacked in such a manner that central portions of the stripe-type first internal electrode patterns 221 printed on the first ceramic green sheet and central portions of gaps between the stripe-type second internal electrode patterns 222 printed on the second ceramic green sheet overlap each other.
[0127] Next, if Fig.6D As shown in FIG. 1 , the ceramic green sheet stack body 220 may be cut across a plurality of stripe-type first internal electrode patterns 221 and a plurality of stripe-type second internal electrode patterns 222. For example, the ceramic green sheet stack body 220 may be cut along C1-C1 cutting lines and C2-C2 cutting lines orthogonal to each other to form the provided stack body 210.
[0128] More specifically, the stripe-type first and second inner electrode patterns 221 and 222 may be cut along the longitudinal direction (C1-C1) and divided into a plurality of inner electrodes having a predetermined width. At this time, the stacked ceramic green sheets are also cut together with the inner electrode patterns. Therefore, the dielectric layer may be formed to have the same width as that of the inner electrode. Fig.6D The width (the distance between the cutting lines C1 - C1 ) shown in FIG. 1 is merely an example and is not limited thereto.
[0129] Cutting along the C2-C2 cutting line may be performed to fit individual ceramic body sizes. For example, before forming the first and second side margin portions, the rod-shaped stacked body may be cut into individual ceramic body sizes along the C2-C2 cutting line to form a plurality of stacked bodies 210.
[0130] For example, the rod-shaped laminate may be cut in such a manner that the central portion of the overlapped first internal electrodes and the central portion of the predetermined gap formed between the second internal electrodes are cut by the same cutting line. Thus, one end of the first internal electrode and one end of the second internal electrode may be alternately exposed on the cut surface.
[0131] Thereafter, a first side margin portion and a second side margin portion may be formed on the first side surface and the second side surface of the stack body 210 , respectively.
[0132] Next, if Fig. 6E As shown in FIG. 2 , a first side margin portion and a second side margin portion (not shown) may be formed on a first side surface and a second side surface of the stacked body 210 , respectively.
[0133] Specifically, in the method of forming the first side margin part, the side ceramic green sheet 212 coated with an adhesive (not shown) is disposed on the stamping elastic material 300 formed using rubber.
[0134] Next, the stacked body 210 is rotated 90 degrees so that the first side surface of the stacked body 210 faces the side ceramic green sheet 212 coated with an adhesive (not shown), and then the stacked body 210 is pressed and adhered to the side ceramic green sheet 212 coated with an adhesive (not shown).
[0135] When the stacking body 210 is pressed and adhered to the side ceramic raw sheet 212 coated with an adhesive (not shown) to transfer the side ceramic raw sheet 212 to the stacking body 210, due to the stamping elastic material 300 formed using a rubber material, the side ceramic raw sheet 212 is formed as a first side edge portion of the stacking body 210, and the remaining portion can be cut.
[0136] Fig. 6F It is shown that the side ceramic green sheet 212 is formed as a first side edge portion of the stacked body 210 .
[0137] Thereafter, by rotating the stacked body 210 , a second side margin portion may be formed on the second side surface of the stacked body 210 .
[0138] Next, a ceramic body including a dielectric layer and first and second internal electrodes may be formed by calcining and firing the stacked body having the first and second side margin parts formed on both side surfaces of the stacked body 210 .
[0139] According to an exemplary embodiment of the present disclosure, since an adhesive is applied on an upper portion of the side ceramic green sheet 212 , the side ceramic green sheet 212 may be transferred to the stacked body 210 under relatively low temperature and low pressure conditions unlike the related art.
[0140] As a result, damage to the stacked body 210 may be significantly reduced, thereby preventing degradation of electrical characteristics of the multilayer ceramic capacitor after firing and improving reliability.
[0141] In addition, by transferring the side ceramic green sheet 212 coated with an adhesive to the side of the stacked body 210 and then pressing it in a firing process, the adhesive force between the stacked body and the ceramic green sheet may be improved.
[0142] Thereafter, external electrodes may be formed on the third side surface of the ceramic body to which the first internal electrode is exposed and on the fourth side surface of the ceramic body to which the second internal electrode is exposed, respectively.
[0143] According to another exemplary embodiment, since the ratio Db / Da of the distance Db between the two end points of the corresponding edge areas of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to the stacking direction distance Da in the central area of the ceramic body 110 satisfies 1.00 to 1.07, the moisture-proof reliability and withstand voltage characteristics can be improved.
[0144] Furthermore, descriptions of the same features as those in the above-described embodiments will be omitted here to avoid redundancy.
[0145] Hereinafter, exemplary embodiments of the present disclosure will be described in more detail with reference to experimental examples, but the scope is not limited by the experimental examples.
[0146] Experimental Example
[0147] Use BaTiO with a thickness of 100nm or less 3 The powder is used as a main component of the ceramic body, and at least one of Mn, V, Si, Al, Ba and Dy, an organic binder, an organic solvent, a plasticizer and a dispersant are added to the main component at a predetermined ratio to prepare a ceramic slurry.
[0148] When preparing the slurry, zirconia balls are used as a mixture / dispersion medium in the main component powder and the sub-component powder, and mechanical grinding is performed after mixing ethanol / toluene and a dispersant, and then a binder mixing process is performed to achieve dielectric sheet strength.
[0149] The prepared slurry was manufactured into a sheet having a thickness of 1.0 μm using a blade type coater. Ni inner electrode printing was performed on the molded sheet. As a printing method, a method such as screen printing, inkjet printing, and gravure printing can be used.
[0150] The upper and lower covers were manufactured by laminating cover sheets having a thickness of 2 to 3 μm in 10 to 20 layers, and a pressed bar was manufactured by pressing an active sheet having an internal electrode printed thereon. The pressed bar was cut into 3216 (length×width×thickness: 3.2 mm×1.6 mm×1.6 mm) sheets using a cutter.
[0151] Use BaTiO with a thickness of 100nm or less 3The powder is used as a matrix material component of the side edge portion, and at least one of Mg, Ba and Si, an organic binder, an organic solvent, a plasticizer and a dispersant are mixed in a predetermined ratio to prepare a ceramic slurry. The slurry is manufactured in the same manner as the ceramic main body dielectric layer, and a sheet is formed into a thickness of 10 μm to 20 μm using an on-roll forming coater using a head discharge method to form the side edge portion.
[0152] Next, the internal electrodes are exposed in the width direction of the body, and a molded sheet is attached to the electrode exposed portion of the edgeless green sheet where the internal electrodes are exposed in the width direction of the body, and then the molded sheet is cut into a predetermined size to form a side edge portion thereon.
[0153] A 0603 size (length×width×height: 0.6 mm×0.3 mm×0.3 mm) multilayer ceramic capacitor green sheet was manufactured by attaching molded sheets to both sides of the green sheet by applying a predetermined temperature and a predetermined pressure under conditions that significantly reduced deformation of the green sheet.
[0154] The multilayer ceramic capacitor samples manufactured as described above were subjected to a calcination process at a temperature of 400° C. or less in a nitrogen atmosphere, and a firing process at a firing temperature of 1200° C. or less in a 0.5% H 2 The samples were fired at a hydrogen concentration of 0.1477 or lower, and then the electrical characteristics, edge length, withstand voltage, and moisture resistance were fully inspected.
[0155] The room temperature capacitance and dielectric loss of the multilayer ceramic capacitor (MLCC) were measured using an LCR meter at 1 kHz and 0.5 V AC, and 50 samples were taken to measure the breakdown voltage (BDV) at which insulation breakdown occurred at room temperature of 25° C.
[0156] High temperature withstand voltage refers to the IR withstand voltage greater than or equal to 10 when a voltage step of 5V / μm is applied for 1 hour at 105°C and the voltage step is continuously increased for measurement. 5 The voltage when Ω.
[0157] Furthermore, microstructures such as edge density and edge length were compared with respect to the fractured and polished surfaces of the sheets.
[0158] Relative to the surface formed by the stacking direction (T) and the width direction (W), after polishing the ceramic body to 1 / 2 length in the vertical direction, the number of pores in the dielectric layer and the side edge portion of the effective part was confirmed by measuring and counting within an area range of 30μm×30μm using a scanning electron microscope (SEM) with a magnification of 5000 times.
[0159] Next, a moisture resistance test was performed on each sample of the example and the comparative example. The moisture resistance test was performed on 40 samples at a relative humidity of 85% and a temperature of 85°C, and the insulation resistance was measured while applying a rated voltage of 4V for 24 hours. At this time, when the resistance of all samples remained greater than or equal to 10 during the test, the insulation resistance was measured. 5 Ω is OK, when the resistance of one or more samples is less than 10 5 Ω, it is determined as NG.
[0160] [Table 1]
[0161]
[0162]
[0163] *: Comparative example
[0164] In the case of Comparative Examples 1 to 4, the ratio Db / Da of the distance Db between the two end points of the corresponding edge regions of the first side edge portion and the second side edge portion in the stacking direction of the ceramic body relative to the stacking direction distance Da of the central region of the ceramic body is less than 1.00. In this case, the moisture resistance is satisfied, but there is a problem that the room temperature withstand voltage is reduced to less than 100 V / μm.
[0165] On the other hand, in the case of samples 5 to 7 according to the exemplary embodiment of the present disclosure, the ratio Db / Da of the distance Db between the two end points in the stacking direction of the ceramic body of the corresponding edge regions of the first side edge portion and the second side edge portion relative to the stacking direction distance Da of the central region of the ceramic body satisfies 1.00 to 1.07. In this case, the room temperature withstand voltage of 100 V / μm or more, the high temperature withstand voltage of 70 V / μm or more, and the moisture-proof load characteristic are OK (three characteristics according to the exemplary embodiment of the present disclosure).
[0166] On the other hand, in the case of Comparative Example 8, the ratio Db / Da of the distance Db between the two end points in the stacking direction of the ceramic body of the corresponding edge regions of the first side edge portion and the second side edge portion relative to the stacking direction distance Da of the central region of the ceramic body is 1.10 (greater than 1.07). In this case, the room temperature withstand voltage and the high temperature withstand voltage are satisfied, but the moisture-proof property is not satisfied.
[0167] In addition, in Comparative Examples 9 and 10, the ratio Db / Da of the distance Db between the two end points of the corresponding edge regions of the first side edge portion and the second side edge portion in the stacking direction of the ceramic body relative to the stacking direction distance Da of the central region of the ceramic body is greater than 1.07. In this case, the room temperature withstand voltage is less than 100 V / μm, the high temperature withstand voltage is reduced to less than 70 V / μm, and the moisture resistance is not satisfied.
[0168] As a result of experimental measurement, it can be seen that when the ratio Db / Da of the distance Db between the two end points of the corresponding edge areas of the first side edge portion 112 and the second side edge portion 113 in the stacking direction of the ceramic body 110 relative to the stacking direction distance Da in the central area of the ceramic body 110 satisfies 1.00 to 1.07, both moisture-proof reliability and withstand voltage characteristics can be met.
[0169] As described above, according to an exemplary embodiment, by adjusting the ratio of the stacking direction distance of the ceramic body in the central area to the distance between the two end points of the corresponding edge areas of the first side edge portion and the second side edge portion in the stacking direction of the ceramic body, the moisture-proof reliability can be improved and the breakdown voltage can also be improved.
[0170] In addition, in the multilayer ceramic capacitor according to the exemplary embodiment, the breakdown voltage (BDV) may be increased, thereby improving reliability.
[0171] Although the present disclosure includes specific examples, it will be apparent to those of ordinary skill in the art that various changes in form and detail may be made in these examples without departing from the spirit and scope of the claims and their equivalents. The examples described herein are to be considered as descriptive only and not for limiting purposes. The description of the features or aspects in each example will be considered to be applicable to similar features or aspects in other examples. If the described techniques are performed in a different order, and / or if the components in the described systems, architectures, devices, or circuits are combined in different ways and / or the components in the described systems, architectures, devices, or circuits are replaced or supplemented with other components or their equivalents, appropriate results may be obtained. Therefore, the scope of the present disclosure is not limited by specific embodiments, but by the claims and their equivalents, and all variations within the scope of the claims and their equivalents will be interpreted as being included in the present disclosure.
Claims
1. A multilayer ceramic capacitor comprising: A ceramic body including a dielectric layer, the ceramic body having a first surface and a second surface opposite to each other, a third surface and a fourth surface connecting the first surface and the second surface, and a fifth surface and a sixth surface connected to the first surface, the second surface, the third surface and the fourth surface and opposite to each other; a plurality of first internal electrodes and a plurality of second internal electrodes disposed inside the ceramic body, exposed to the first surface and the second surface, and having ends exposed to the third surface or the fourth surface; and The first side edge portion and the second side edge portion are respectively disposed on the first surface and the second surface of the ceramic body, Wherein, the ratio Db / Da satisfies greater than 1.00 and less than or equal to 1.07, wherein "Db" is the distance between the two ends of the edge area of the first side edge portion and the second side edge portion respectively away from the ceramic body in the stacking direction of the dielectric layer, and "Da" is the distance in the central area of the ceramic body in the stacking direction.
2. The multilayer ceramic capacitor according to claim 1, wherein: The ceramic body comprises: an effective portion including the plurality of first internal electrodes and the plurality of second internal electrodes, the first internal electrodes and the second internal electrodes being arranged to face each other with the dielectric layer interposed therebetween to form a capacitor; and a covering portion provided on an upper portion and a lower portion of the effective portion in the stacking direction, and A ratio of the number of pores in the first side margin portion and the second side margin portion to the number of pores in the dielectric layer of the effective portion satisfies greater than or equal to 0.9 and less than or equal to 1.
1.
3. The multilayer ceramic capacitor according to claim 1, wherein: The ratio Db / Da is greater than 1.00 and less than or equal to 1.
04.
4. The multilayer ceramic capacitor according to claim 1, wherein: The dielectric layer has a thickness of 0.6 μm or less, and each of the plurality of first internal electrodes and the plurality of second internal electrodes has a thickness of 0.4 μm or less.
5. The multilayer ceramic capacitor according to any one of claims 1 to 4, wherein The ratio d2 / d1 is greater than 1.00 and less than or equal to 1.05, wherein "d2" is a spacing between the first internal electrode and the second internal electrode at an end portion of the ceramic body adjacent to the first side edge portion or the second side edge portion, and "d1" is a spacing between the first internal electrode and the second internal electrode in a central region of the ceramic body.
6. A method for manufacturing a multilayer ceramic capacitor, comprising: preparing a first ceramic green sheet and a second ceramic green sheet, forming a plurality of first internal electrode patterns at predetermined intervals on the first ceramic green sheet, and forming a plurality of second internal electrode patterns at predetermined intervals on the second ceramic green sheet; stacking the first ceramic green sheets and the second ceramic green sheets in such a manner that the plurality of first internal electrode patterns and the plurality of second internal electrode patterns alternately overlap each other to form a ceramic green sheet stacked body; cutting the ceramic green sheet stacked body to have side surfaces where edges of the plurality of first internal electrode patterns and edges of the plurality of second internal electrode patterns are exposed in a width direction; forming first and second side margin portions on the side surfaces of the cut stacked body, respectively; and firing the cut stacked body to provide a ceramic body including a dielectric layer and first and second internal electrodes, Wherein, the ratio Db / Da satisfies greater than 1.00 and less than or equal to 1.07, wherein "Db" is the distance between the two ends of the edge area of the first side edge portion and the second side edge portion respectively away from the ceramic body in the stacking direction of the dielectric layer, and "Da" is the distance in the central area of the ceramic body in the stacking direction.
7. The method of claim 6, wherein: A thickness of each of the first and second ceramic green sheets is equal to or less than 1.0 μm, and a thickness of each of the first and second internal electrode patterns is equal to or less than 0.5 μm.
8. The method of claim 6, wherein: The ceramic body comprises: an effective portion including a plurality of first internal electrodes and a plurality of second internal electrodes, the first internal electrodes and the second internal electrodes are arranged to face each other with the dielectric layer interposed therebetween to form a capacitor; and a covering portion provided on an upper portion and a lower portion of the effective portion in the stacking direction, and A ratio of the number of pores in the first side margin portion and the second side margin portion to the number of pores in the dielectric layer of the effective portion satisfies greater than or equal to 0.9 and less than or equal to 1.
1.
9. The method of claim 6, wherein: The ratio Db / Da is greater than or equal to 1.01 and less than or equal to 1.
07.
10. The method according to claim 8 or 9, wherein: The ratio d2 / d1 is greater than 1.00 and less than or equal to 1.05, wherein "d2" is a spacing between the first internal electrode and the second internal electrode at an end portion of the ceramic body adjacent to the first side edge portion or the second side edge portion, and "d1" is a spacing between the first internal electrode and the second internal electrode in a central region of the ceramic body.