Lead zirconate-based anti-ferroelectric ceramic material and preparation and application thereof
Through doping and component regulation of lead zirconate-based antiferroelectric ceramic materials, high dielectric constant and ultra-low phase transition electric field are achieved under low electric field, and the existing antiferroelectric ceramic materials are solved by dielectric under low electric field The problem of low constants has expanded its application range and is especially suitable for power semiconductor devices.
Patent Information
- Application Number
- CN202411092952.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-12-03
AI Technical Summary
The existing antiferroelectric ceramic materials have a low dielectric constant under low electric fields, which limits their application in many fields. After the phase transition electric field is increased, the ferroelectricity of the material weakens, affecting the energy storage density and efficiency.
Using lead zirconate antiferroelectric ceramic material, through partial element doping and component regulation, a material with ultra-low phase transition electric field and room temperature high dielectric constant is prepared, suitable for energy storage and charging with good performance under low electric fields. Discharge performance.
The application range of antiferroelectric ceramic capacitors has been expanded, especially in the fields of power semiconductor devices and fast power semiconductors, improving the stability and performance of materials.
Smart Images

Figure CN119072220A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electronic functional materials and devices, and in particular to a lead zirconate-based antiferroelectric ceramic material and a preparation method and application thereof. Background Art
[0002] There are many ways to store energy. The mainstream energy storage devices on the market include dielectric capacitors, supercapacitors, batteries, and fuel cells. Among them, dielectric capacitors have the advantages of fast charging and discharging speed, high power density, high utilization efficiency, and stable performance. Its working principle is that under the action of the external electric field, the dipole positive and negative charge centers inside the dielectric layer gradually separate and gather on the two plates. In order to offset the charge on the surface of the dielectric, the two ends of the metal plate will adsorb equal amounts of positive and negative charges, thereby achieving the purpose of storing charge. Dielectric capacitors can be divided into two categories according to the dielectric materials in them: organic polymer capacitors and ceramic capacitors. Although organic polymer capacitors have high breakdown field strength, their dielectric constant is low and thermal stability is poor, which limits their application in many fields. Ceramic capacitors have the advantages of high dielectric constant, high temperature resistance, long cycle life, and small size. They have played an important role in information electronics, medical care, energy, national defense and other fields.
[0003] There are three main types of dielectric materials used for ceramic capacitors: linear ceramics, ferroelectric ceramics, and antiferroelectric ceramics. Linear ceramic capacitors do not have spontaneous polarization. Under the action of an electric field, the polarization intensity changes linearly, and the dielectric constant remains constant. After the electric field is removed, it can return to a non-polar state; ferroelectric ceramic capacitors have spontaneous polarization and polarized domains, and the adjacent dipoles in the domain are arranged in a directional manner. Under the action of an external electric field, the spontaneous polarization can change nonlinearly with the electric field, and the dielectric constant decreases with the increase of the electric field. After the electric field is removed, there is residual spontaneous polarization; antiferroelectric ceramic materials also have spontaneous polarization, but the arrangement directions between adjacent dipoles are opposite, and they are in an antiferroelectric state, so they do not show spontaneous polarization to the outside, but under the action of an electric field, the antiferroelectric state can change to a ferroelectric state, and the electric field can be removed and it can return to the antiferroelectric state. The residual polarization intensity is close to zero, so it presents the characteristics of a double hysteresis loop. In addition, the dielectric constant of antiferroelectric ceramics increases with the applied electric field within a certain range. This is because when the electric field increases to the electric field E A-F When the antiferroelectric phase transition occurs, the polarization strength of the material increases rapidly, and the dielectric constant reaches a peak value. This electric field induces the electric field E of the antiferroelectric to ferroelectric phase transition. A-F , referred to as phase transition electric field in this article. This characteristic that the capacitance value increases instead of decreases with the increase of electric field is conducive to the development trend of capacitor miniaturization, large capacitance and lightweight.
[0004] At present, the research on antiferroelectric ceramic materials focuses on how to improve the phase transition electric field, breakdown field strength and polarization strength to improve energy storage density and efficiency. However, the actual situation is limited by the safety of high voltage use. High voltage or electric field can only be used in fields such as high-power pulse power supply. The increase of phase transition electric field means that antiferroelectricity is enhanced and ferroelectricity is weakened, which is generally accompanied by a lower dielectric constant (~several hundred) at room temperature, which limits the application of antiferroelectric ceramic materials. Therefore, the research and exploration of antiferroelectric ceramic materials under low electric field is the key to further expand the application range of antiferroelectric ceramic materials. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide a lead zirconate-based antiferroelectric ceramic material and its preparation and application. The present invention uses a lead zirconate-based system as a matrix, and by doping some elements into the matrix (by component regulation), a lead zirconate-based antiferroelectric ceramic material with an ultra-low phase transition electric field and a high dielectric constant at room temperature is prepared, which exhibits good energy storage and charge-discharge performance under a low electric field, is conducive to the development of large-capacitance capacitors, and is expected to be applied to power semiconductor devices (such as electronic circuits, fast-breaking power semiconductors) and other fields, expanding the application range of antiferroelectric ceramic capacitors.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The first object of the present invention is to provide a lead zirconate-based antiferroelectric ceramic material, the chemical formula of which is (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.5-x Sn 0.4 Ti 0.1+x )O3, where the value range of x is 0.01≤x<0.03;
[0008] Preferably, x is 0.01 or 0.02.
[0009] The second object of the present invention is to provide a method for preparing a lead zirconate-based antiferroelectric ceramic material, comprising the following steps:
[0010] (S1) Pb3O4, BaCO3, La2O3, ZrO2, SnO2 and TiO2 are mixed to obtain a mixture;
[0011] (S2) subjecting the mixed material prepared in step (S1) to a first ball milling treatment, and then drying (to remove moisture), grinding, and pre-calcining in sequence to obtain a pre-calcined powder;
[0012] (S3) subjecting the pre-calcined powder prepared in step (S2) to a second ball milling treatment, and then drying (to remove moisture) and grinding in sequence to obtain a lead zirconate-based antiferroelectric ceramic material with an ultra-low phase transition electric field.
[0013] In one embodiment of the present invention, in step (S1), the purity of the metal oxide raw materials is greater than 99wt%, and in order to compensate for the volatilization of the Pb element during the sintering process, the excess of Pb3O4 is adjusted to 2% mol based on the chemical dosage ratio.
[0014] In one embodiment of the present invention, in step (S2), during the first ball milling process, the mass ratio of the mixed material, the ball milling medium, and the grinding body is 1:1.5-2:2-2.5; the ball milling speed is 360 rpm, and the ball milling time is 20-24h;
[0015] During the drying process, the temperature is 110-130°C and the time is 6-8h;
[0016] During the pre-sintering process, the temperature is 850-900°C and the time is 2-3h;
[0017] In step (S3), during the second ball milling process, the mass ratio of the mixed material, the ball milling medium, and the grinding body is 1:1.5-2:2-2.5; the ball milling speed is 360 rpm, and the ball milling time is 20-24 hours;
[0018] During the drying process, the temperature is 110-130°C and the time is 6-8 hours.
[0019] In one embodiment of the present invention, the ball milling medium is anhydrous ethanol, and the grinding body is a zirconia ball.
[0020] The third object of the present invention is to provide an application of a lead zirconate-based antiferroelectric ceramic material in the preparation of a lead zirconate-based antiferroelectric ceramic sheet.
[0021] A fourth object of the present invention is to provide a method for preparing a lead zirconate-based antiferroelectric ceramic sheet, comprising the following steps:
[0022] (A1) mixing a lead zirconate-based antiferroelectric ceramic material and a binder, granulating the mixture, and pressing the mixture to obtain a ceramic green sheet;
[0023] (A2) Debinding and sintering the ceramic green sheet prepared in step (A1) in sequence, and cooling in a furnace to obtain a lead zirconate-based antiferroelectric ceramic sheet.
[0024] In one embodiment of the present invention, in step (A1), the amount of the binder added is 15-25% of the mass of the lead zirconate-based antiferroelectric ceramic material;
[0025] During the pressing process, the forming method is dry pressing (compared with the wet forming method, its preparation method is simple, the operation is convenient, and the subsequent ceramic forming has good mechanical strength and excellent electrical properties). A mold with a diameter of 10 mm is selected, the pressure is 6-8 MPa, and the holding time is 1 min.
[0026] In step (A2), during the debinding process, the temperature is raised to 500-600° C. at a heating rate of 1° C. / min and maintained at a constant temperature for 6-10 hours;
[0027] During the sintering process, the temperature is increased to 1200-1300°C at a heating rate of 2°C / min and maintained at a constant temperature for 3-4 hours.
[0028] In one embodiment of the present invention, the binder is 8 wt % polyvinyl alcohol, which is added in multiple portions during the granulation process and is covered with a lead zirconate-based antiferroelectric ceramic material.
[0029] The fifth object of the present invention is to provide a lead zirconate-based antiferroelectric ceramic sheet prepared by the above method.
[0030] A sixth object of the present invention is to provide an application of a lead zirconate-based antiferroelectric ceramic sheet in the preparation of a power semiconductor device.
[0031] In the present invention, lead zirconate-based ceramic materials are prepared using a traditional solid-state reaction method based on the calculation formula of the tolerance factor t of the perovskite structure (Formula 1.1). When t<1, it is an antiferroelectric phase, and the smaller t is, the more stable the antiferroelectric phase is, and the higher the phase transition electric field is.
[0032]
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention stably synthesizes an antiferroelectric phase by doping elements and regulating the proportion at the A and B positions of lead zirconate-based antiferroelectric ceramics. The antiferroelectric phase has a high dielectric constant at room temperature and can undergo an antiferroelectric-ferroelectric phase transition under an ultra-low electric field. The polarization intensity increases rapidly and is expected to be applied to the manufacture of multilayer ceramic capacitors, thereby expanding the application range of antiferroelectric ceramic capacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is the PE hysteresis loop spectrum of the lead zirconate-based antiferroelectric ceramic sheet prepared in Comparative Example 1 at room temperature;
[0036] Figure 2 PE hysteresis loop spectra of the lead zirconate-based antiferroelectric ceramic sheets prepared in Comparative Example 1, Comparative Example 2, Example 1 and Example 2 under the same electric field;
[0037] Figure 3 XRD patterns of the lead zirconate-based antiferroelectric ceramic sheets prepared in Example 1 and Example 2 at room temperature;
[0038] Figure 4 The dielectric temperature spectra of the lead zirconate-based antiferroelectric ceramic sheets prepared in Examples 1 and 2 of the present invention. DETAILED DESCRIPTION
[0039] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0040] In the following comparative examples and embodiments, unless otherwise specified, all reagents used are commercially available reagents, and all detection means and methods used are conventional detection means and methods in the art.
[0041] Comparative Example 1
[0042] This comparative example provides a (Pb 0.96 Sr 0.01 La 0.02 )(Zr 0.6 Sn 0.4 )O3 antiferroelectric ceramic material and preparation method thereof. Among them, (Pb 0.96 Sr 0.01 La 0.02 )(Zr 0.6 Sn 0.4 ) The preparation method of O3 antiferroelectric ceramic material comprises the following steps:
[0043] (S1) Pb3O4, SrCO3, La2O3, ZrO2 and SnO2 with a purity greater than 99 wt% are selected as initial raw materials, and the materials are mixed according to the stoichiometric ratio in the above chemical formula, and an excess of 2% mol of Pb3O4 is weighed to obtain a mixed material;
[0044] (S2) The mixture in step (S1) is subjected to a first ball milling for 24 hours (the mass ratio of the mixture, the ball milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:2:2.5, and the rotation speed is 360 rpm). After the mixture is discharged, it is dried at 110°C for 6 hours, and then ground into powder with a mortar. After pre-calcining at 900°C for 3 hours, a pre-calcined powder is obtained.
[0045] (S3) The pre-calcined powder in step (S2) is ball-milled for the second time (the mass ratio of the pre-calcined powder, the ball-milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:2:2.5, and the rotation speed is 360 rpm). After the material is discharged, it is dried at 110° C. for 6 h, and then crushed in a mortar to obtain a lead zirconate-based antiferroelectric ceramic material with uniform particles.
[0046] The lead zirconate-based antiferroelectric ceramic material obtained above is further used to prepare a lead zirconate-based antiferroelectric ceramic sheet, which specifically includes the following steps:
[0047] (A1) adding a binder (8 wt % polyvinyl alcohol) to a lead zirconate-based antiferroelectric ceramic material and granulating the material, wherein the amount of the binder added is 20 wt % of the mass of the lead zirconate-based antiferroelectric ceramic material (the binder needs to be added in multiple times during the granulation process and covered with the antiferroelectric ceramic powder), and after the granulation, placing the antiferroelectric ceramic powder with uniform particles and good fluidity in a mold with a diameter of 10 mm through a dry pressing process, maintaining the pressure at a pressure of 6 MPa for 1 min, and then taking it out to obtain a cylindrical ceramic green sheet with a smooth surface, a diameter of 10 mm, and a thickness of 0.7 mm;
[0048] (A2) The cylindrical ceramic green sheet obtained in step (A1) is heated at 600°C for 8 hours at a heating rate of 1°C / min for debinding, and then sintered at 1300°C for 3 hours at a heating rate of 2°C / min, and then cooled in the furnace to obtain a lead zirconate-based antiferroelectric ceramic sheet.
[0049] Comparative Example 2
[0050] This comparative example provides a (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.47 Sn 0.4 Ti 0.13 )O3 antiferroelectric ceramic material and preparation method thereof.
[0051] Among them, (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.47 Sn 0.4 Ti 0.13 ) The preparation method of O3 antiferroelectric ceramic material comprises the following steps:
[0052] (S1) Pb3O4, BaCO3, La2O3, ZrO2, SnO2 and TiO2 with a purity greater than 99 wt% are selected as initial raw materials, and the materials are prepared according to the stoichiometric ratio in the above chemical formula, and an excess of 2% mol of Pb3O4 is weighed to obtain a mixed material;
[0053] (S2) The mixture in step (S1) is subjected to a first ball milling for 24 hours (the mass ratio of the mixture, the ball milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:2:2.5, and the rotation speed is 360 rpm). After the mixture is discharged, it is dried at 110°C for 6 hours, and then ground into powder with a mortar. After pre-calcining at 900°C for 3 hours, a pre-calcined powder is obtained.
[0054] (S3) The pre-calcined powder in step (S2) is ball-milled for the second time (the mass ratio of the pre-calcined powder, the ball-milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:2:2.5, and the rotation speed is 360 rpm). After the material is discharged, it is dried at 110° C. for 6 h, and then crushed in a mortar to obtain a lead zirconate-based antiferroelectric ceramic material with uniform particles.
[0055] The lead zirconate-based antiferroelectric ceramic material obtained above is further used to prepare a lead zirconate-based antiferroelectric ceramic sheet, which specifically includes the following steps:
[0056] (A1) adding a binder (8 wt % polyvinyl alcohol) to a lead zirconate-based antiferroelectric ceramic material and granulating the material, wherein the amount of the binder added is 20 wt % of the mass of the lead zirconate-based antiferroelectric ceramic material (the binder needs to be added in multiple times during the granulation process and covered with the antiferroelectric ceramic powder), and after the granulation, placing the antiferroelectric ceramic powder with uniform particles and good fluidity in a mold with a diameter of 10 mm through a dry pressing process, maintaining the pressure at a pressure of 6 MPa for 1 min, and then taking it out to obtain a cylindrical ceramic green sheet with a smooth surface, a diameter of 10 mm, and a thickness of 0.7 mm;
[0057] (A2) The cylindrical ceramic green sheet obtained in step (A1) is heated at 600°C for 8 hours at a heating rate of 1°C / min for debinding, and then sintered at 1300°C for 3 hours at a heating rate of 2°C / min, and then cooled in the furnace to obtain a lead zirconate-based antiferroelectric ceramic sheet.
[0058] Example 1
[0059] This embodiment provides a (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.49 Sn 0.4 Ti 0.11 )O3 antiferroelectric ceramic material and preparation method thereof.
[0060] Among them, (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.49 Sn 0.4 Ti 0.11 ) The preparation method of O3 antiferroelectric ceramic material comprises the following steps:
[0061] (S1) Pb3O4, BaCO3, La2O3, ZrO2, SnO2 and TiO2 with a purity greater than 99 wt% are selected as initial raw materials, and the materials are prepared according to the stoichiometric ratio in the above chemical formula, and an excess of 2% mol of Pb3O4 is weighed to obtain a mixed material;
[0062] (S2) The mixture in step (S1) is subjected to a first ball milling for 24 hours (the mass ratio of the mixture, the ball milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:2:2.5, and the rotation speed is 360 rpm). After the mixture is discharged, it is dried at 110°C for 6 hours, and then ground into powder with a mortar. After pre-calcining at 900°C for 3 hours, a pre-calcined powder is obtained.
[0063] (S3) The pre-calcined powder in step (S2) is ball-milled for the second time (the mass ratio of the pre-calcined powder, the ball-milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:2:2.5, and the rotation speed is 360 rpm). After the material is discharged, it is dried at 110° C. for 6 h, and then crushed in a mortar to obtain a lead zirconate-based antiferroelectric ceramic material with uniform particles.
[0064] The lead zirconate-based antiferroelectric ceramic material obtained above is further used to prepare a lead zirconate-based antiferroelectric ceramic sheet, which specifically includes the following steps:
[0065] (A1) adding a binder (8 wt % polyvinyl alcohol) to a lead zirconate-based antiferroelectric ceramic material and granulating the material, wherein the amount of the binder added is 20 wt % of the mass of the lead zirconate-based antiferroelectric ceramic material (the binder needs to be added in multiple times during the granulation process and covered with the antiferroelectric ceramic powder), and after the granulation, placing the antiferroelectric ceramic powder with uniform particles and good fluidity in a mold with a diameter of 10 mm through a dry pressing process, maintaining the pressure at a pressure of 6 MPa for 1 min, and then taking it out to obtain a cylindrical ceramic green sheet with a smooth surface, a diameter of 10 mm, and a thickness of 0.7 mm;
[0066] (A2) The cylindrical ceramic green sheet obtained in step (A1) is heated at 600°C for 8 hours at a heating rate of 1°C / min for debinding, and then sintered at 1300°C for 3 hours at a heating rate of 2°C / min, and then cooled in the furnace to obtain a lead zirconate-based antiferroelectric ceramic sheet.
[0067] Example 2
[0068] This embodiment provides a (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.48 Sn 0.4 Ti 0.12 )O3 antiferroelectric ceramic material and preparation method thereof.
[0069] Among them, (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.48 Sn 0.4 Ti 0.12 ) The preparation method of O3 antiferroelectric ceramic material comprises the following steps:
[0070] (S1) Pb3O4, BaCO3, La2O3, ZrO2, SnO2 and TiO2 with a purity greater than 99 wt% are selected as initial raw materials, and the materials are prepared according to the stoichiometric ratio in the above chemical formula, and an excess of 2% mol of Pb3O4 is weighed to obtain a mixed material;
[0071] (S2) The mixture in step (S1) is subjected to a first ball milling for 24 hours (the mass ratio of the mixture, the ball milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:2:2.5, and the rotation speed is 360 rpm). After the mixture is discharged, it is dried at 110°C for 6 hours, and then ground into powder with a mortar. After pre-calcining at 900°C for 3 hours, a pre-calcined powder is obtained.
[0072] (S3) The pre-calcined powder in step (S2) is ball-milled for the second time (the mass ratio of the pre-calcined powder, the ball-milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:2:2.5, and the rotation speed is 360 rpm). After the material is discharged, it is dried at 110° C. for 6 h, and then crushed in a mortar to obtain a lead zirconate-based antiferroelectric ceramic material with uniform particles.
[0073] The lead zirconate-based antiferroelectric ceramic material obtained above is further used to prepare a lead zirconate-based antiferroelectric ceramic sheet, which specifically includes the following steps:
[0074] (A1) adding a binder (8 wt % polyvinyl alcohol) to a lead zirconate-based antiferroelectric ceramic material and granulating the material, wherein the amount of the binder added is 20 wt % of the mass of the lead zirconate-based antiferroelectric ceramic material (the binder needs to be added in multiple times during the granulation process and covered with the antiferroelectric ceramic powder), and after the granulation, placing the antiferroelectric ceramic powder with uniform particles and good fluidity in a mold with a diameter of 10 mm through a dry pressing process, maintaining the pressure at a pressure of 6 MPa for 1 min, and then taking it out to obtain a cylindrical ceramic green sheet with a smooth surface, a diameter of 10 mm, and a thickness of 0.7 mm;
[0075] (A2) The cylindrical ceramic green sheet obtained in step (A1) is heated at 600°C for 8 hours at a heating rate of 1°C / min for debinding, and then sintered at 1300°C for 3 hours at a heating rate of 2°C / min, and then cooled in the furnace to obtain a lead zirconate-based antiferroelectric ceramic sheet.
[0076] Performance Analysis:
[0077] Figure 1The PE hysteresis loop of the lead zirconate-based antiferroelectric ceramic sheet prepared in Comparative Example 1 under an applied electric field of 25 kV / mm. It can be seen from the figure that the lead zirconate-based antiferroelectric ceramic sheet prepared in Comparative Example 1 exhibits antiferroelectric behavior, and its phase transition electric field is 19.39 kV / mm, and the saturation polarization intensity is 10.34 μC / cm 2 .
[0078] Figure 2 PE hysteresis loops of the lead zirconate-based antiferroelectric ceramic sheets prepared in Comparative Example 1, Comparative Example 2, Example 1 and Example 2 under an applied electric field of 5 kV / mm. It can be observed that the lead zirconate-based antiferroelectric ceramic sheet prepared in Comparative Example 1 did not undergo phase change, and the saturation polarization intensity was only 1.31 μC / cm 2 The lead zirconate-based antiferroelectric ceramic sheet prepared in Comparative Example 2 exhibits ferroelectric behavior, with a saturation polarization intensity of 32.71 μC / cm 2 The phase transition electric field of the lead zirconate-based antiferroelectric ceramic sheet prepared in Example 1 is 1.15 kV / mm, and the maximum polarization intensity is 35.17 μC / cm 2 The phase transition electric field of the lead zirconate-based antiferroelectric ceramic sheet prepared in Example 2 is 0.72 kV / mm, and the maximum polarization intensity is 40.04 μC / cm 2 The lead zirconate-based antiferroelectric ceramic sheet prepared in comparative example 1 has a large phase transition electric field and a low saturation polarization intensity, and the lead zirconate-based antiferroelectric ceramic sheet prepared in comparative example 2 loses the antiferroelectric characteristics, while the lead zirconate-based antiferroelectric ceramic sheets prepared in examples 1 and 2 can stably synthesize the antiferroelectric phase while also having an ultra-low phase transition electric field and a high saturation polarization intensity, which is because the Ti at the B position 4+ Ionic radius Less than Zr 4+ Ionic radius Use Ti 4+ Replace Zr 4+ This increases the tolerance factor t, enhances the ferroelectricity, and makes the antiferroelectric-ferroelectric phase transition easier to occur, as shown by E A-F of decline.
[0079] Figure 3 The XRD spectra of the lead zirconate-based antiferroelectric ceramic sheets prepared in Example 1 and Example 2 show that the prepared lead zirconate-based antiferroelectric ceramic sheets have a pure tetragonal perovskite structure without any secondary impurities and have good crystallinity.
[0080] Figure 4The dielectric temperature spectra of the lead zirconate-based antiferroelectric ceramic sheets prepared in Example 1 and Example 2 show that the dielectric constant of the lead zirconate-based antiferroelectric ceramic sheet prepared in Example 1 is higher than 3000 at room temperature, and the maximum relative dielectric constant is as high as 6197.33 at the Curie temperature (61.9°C); the dielectric constant of the lead zirconate-based antiferroelectric ceramic sheet prepared in Example 2 is higher than 4000 at room temperature, and the maximum relative dielectric constant is as high as 7328.57 at the Curie temperature (56.2°C). The large dielectric constant is beneficial to improving the charge and discharge performance of the material.
[0081] Example 3
[0082] This embodiment provides a (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.49 Sn 0.4 Ti 0.11 )O3 antiferroelectric ceramic material and preparation method thereof.
[0083] Among them, (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.49 Sn 0.4 Ti 0.11 ) The preparation method of O3 antiferroelectric ceramic material comprises the following steps:
[0084] (S1) Pb3O4, BaCO3, La2O3, ZrO2, SnO2 and TiO2 with a purity greater than 99 wt% are selected as initial raw materials, and the materials are prepared according to the stoichiometric ratio in the above chemical formula, and an excess of 2% mol of Pb3O4 is weighed to obtain a mixed material;
[0085] (S2) The mixture in step (S1) is subjected to a first ball milling for 20 hours (the mass ratio of the mixture, ball milling medium (anhydrous ethanol) and grinding body (zirconia ball) is 1:1.5:2, and the rotation speed is 360 rpm). After the mixture is discharged, it is dried at 130°C for 8 hours, and then ground into powder with a mortar. After pre-calcining at 850°C for 2.5 hours, a pre-calcined powder is obtained.
[0086] (S3) The pre-calcined powder in step (S2) is ball-milled for the second time (the mass ratio of the pre-calcined powder, the ball-milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:1.5:2, and the rotation speed is 360 rpm). After the material is discharged, it is dried at 130°C for 8h, and then crushed in a mortar to obtain a lead zirconate-based antiferroelectric ceramic material with uniform particles.
[0087] The lead zirconate-based antiferroelectric ceramic material obtained above is further used to prepare a lead zirconate-based antiferroelectric ceramic sheet, which specifically includes the following steps:
[0088] (A1) adding a binder (8 wt% polyvinyl alcohol) to a lead zirconate-based antiferroelectric ceramic material and granulating the material, wherein the amount of the binder added is 15 wt% of the mass of the lead zirconate-based antiferroelectric ceramic material (the binder needs to be added in multiple times during the granulation process and covered with the antiferroelectric ceramic powder), and after the granulation, placing the antiferroelectric ceramic powder with uniform particles and good fluidity in a mold with a diameter of 10 mm through a dry pressing process, maintaining the pressure at a pressure of 8 MPa for 1 min, and then taking it out to obtain a cylindrical ceramic green sheet with a smooth surface, a diameter of 10 mm, and a thickness of 0.7 mm;
[0089] (A2) The cylindrical ceramic green sheet obtained in step (A1) is heated at 500°C for 10 hours at a heating rate of 1°C / min for debinding, and then sintered at 1200°C for 4 hours at a heating rate of 2°C / min, and then cooled in the furnace to obtain a lead zirconate-based antiferroelectric ceramic sheet.
[0090] Example 4
[0091] This embodiment provides a (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.49 Sn 0.4 Ti 0.11 )O3 antiferroelectric ceramic material and preparation method thereof.
[0092] Among them, (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.49 Sn 0.4 Ti 0.11 ) The preparation method of O3 antiferroelectric ceramic material comprises the following steps:
[0093] (S1) Pb3O4, BaCO3, La2O3, ZrO2, SnO2 and TiO2 with a purity greater than 99 wt% are selected as initial raw materials, and the materials are prepared according to the stoichiometric ratio in the above chemical formula, and an excess of 2% mol of Pb3O4 is weighed to obtain a mixed material;
[0094] (S2) The mixture in step (S1) is subjected to a first ball milling for 22 hours (the mass ratio of the mixture, the ball milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:1.8:2.2, and the rotation speed is 360 rpm). After the mixture is discharged, it is dried at 120°C for 7 hours, and then ground into powder with a mortar. After pre-calcining at 880°C for 2 hours, a pre-calcined powder is obtained.
[0095] (S3) The pre-calcined powder in step (S2) is subjected to a second ball milling for 22 hours (the mass ratio of the pre-calcined powder, the ball milling medium (anhydrous ethanol) and the grinding body (zirconia ball) is 1:1.8:2.2, and the rotation speed is 360 rpm). After the material is discharged, it is dried at 120°C for 7 hours, and then crushed in a mortar to obtain a lead zirconate-based antiferroelectric ceramic material with uniform particles.
[0096] The lead zirconate-based antiferroelectric ceramic material obtained above is further used to prepare a lead zirconate-based antiferroelectric ceramic sheet, which specifically includes the following steps:
[0097] (A1) adding a binder (8 wt% polyvinyl alcohol) to a lead zirconate-based antiferroelectric ceramic material and granulating the material, wherein the amount of the binder added is 15 wt% of the mass of the lead zirconate-based antiferroelectric ceramic material (the binder needs to be added in multiple times during the granulation process and covered with the antiferroelectric ceramic powder), and after the granulation, placing the antiferroelectric ceramic powder with uniform particles and good fluidity in a mold with a diameter of 10 mm through a dry pressing process, maintaining the pressure at a pressure of 7 MPa for 1 min, and then taking it out to obtain a cylindrical ceramic green sheet with a smooth surface, a diameter of 10 mm, and a thickness of 0.7 mm;
[0098] (A2) The cylindrical ceramic green sheet obtained in step (A1) is kept at 550°C for 6 hours at a heating rate of 1°C / min for debinding, and then sintered at 1250°C for 3.5 hours at a heating rate of 2°C / min, and the lead zirconate-based antiferroelectric ceramic sheet is obtained after cooling in the furnace.
[0099] The performance of the lead zirconate-based antiferroelectric ceramic sheets prepared in Examples 3 and 4 is substantially the same as that in Example 1.
[0100] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A lead zirconate-based antiferroelectric ceramic material, characterized in that: Its chemical formula is (Pb 0.88 Ba 0.09 La 0.02 )(Zr 0.5-x Sn 0.4 Ti 0.1+x )O3, where the value range of x is 0.01≤x<0.
03.
2. A lead zirconate-based antiferroelectric ceramic material according to claim 1, characterized in that: x is 0.01 or 0.
02.
3. A method for preparing the lead zirconate-based antiferroelectric ceramic material according to any one of claims 1 or 2, characterized in that: The following steps are involved: (S1) Pb3O4, BaCO3, La2O3, ZrO2, SnO2 and TiO2 are mixed to obtain a mixture; (S2) subjecting the mixed material prepared in step (S1) to a first ball milling treatment, and then drying, grinding, and pre-calcining in sequence to obtain a pre-calcined powder; (S3) subjecting the pre-sintered powder prepared in step (S2) to a second ball milling treatment, and then drying and grinding in sequence to obtain a lead zirconate-based antiferroelectric ceramic material.
4. The method for preparing a lead zirconate-based antiferroelectric ceramic material according to claim 3, characterized in that: In step (S1), the purity of Pb3O4, BaCO3, La2O3, ZrO2, SnO2 and TiO2 is greater than 99wt%, and based on the chemical dosage ratio, the excess of Pb3O4 is adjusted to 2% mol to 3% mol.
5. The method for preparing a lead zirconate-based antiferroelectric ceramic material according to claim 3, characterized in that: In step (S2), during the first ball milling process, the mass ratio of the mixed material, the ball milling medium, and the grinding body is 1:1.5-2:2-2.5; the ball milling time is 20-24 hours; During the drying process, the temperature is 110-130°C and the time is 6-8h; During the pre-sintering process, the temperature is 850-900°C and the time is 2-3h; In step (S3), during the second ball milling process, the mass ratio of the mixed material, the ball milling medium, and the grinding body is 1:1.5-2:2-2.5; the ball milling time is 20-24 hours; During the drying process, the temperature is 110-130°C and the time is 6-8 hours.
6. Use of the lead zirconate-based antiferroelectric ceramic material as claimed in any one of claims 1 or 2 in the preparation of a lead zirconate-based antiferroelectric ceramic sheet.
7. A method for preparing a lead zirconate-based antiferroelectric ceramic sheet, characterized in that: The following steps are involved: (A1) mixing the lead zirconate-based antiferroelectric ceramic material according to any one of claims 1 and 2 with a binder, granulating the mixture, and pressing the mixture to obtain a ceramic green sheet; (A2) Debinding and sintering the ceramic green sheet prepared in step (A1) in sequence, and cooling in a furnace to obtain a lead zirconate-based antiferroelectric ceramic sheet.
8. The method for preparing a lead zirconate-based antiferroelectric ceramic sheet according to claim 7, characterized in that: In step (A1), the amount of the binder added is 15-25% of the mass of the lead zirconate-based antiferroelectric ceramic material; During the pressing process, the pressure is 6-8 MPa and the holding time is 1 min; In step (A2), during the debinding process, the temperature is raised to 500-600° C. at a heating rate of 1° C. / min and maintained at a constant temperature for 6-10 hours; During the sintering process, the temperature is raised to 1200-1300°C at a heating rate of 2°C / min and maintained at a constant temperature for 3-4 hours.
9. A lead zirconate-based antiferroelectric ceramic sheet prepared by the method according to claim 7.
10. Use of the lead zirconate-based antiferroelectric ceramic sheet as claimed in claim 9 in the preparation of power semiconductor devices.
Citation Information
Cited By
Lead zirconate-based antiferroelectric ceramic as well as preparation method and application thereof
CN120965320A
A lead zirconate-based antiferroelectric ceramic, a preparation method and applications thereof
CN120965320B