Polymerizable compound, polymerizable composition and optical film
By using polymerizable compounds with specific chemical formulas, the problem of large wavelength dependence of optical films in the reverse wavelength dispersion region is solved, and excellent optical properties in a wider wavelength region and good liquid crystal phase existence at low temperatures are achieved, simplifying The preparation process of optical films.
Patent Information
- Application Number
- CN202011399845.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-12-04
AI Technical Summary
Existing optical films exhibit large wavelength dependence in the reverse wavelength dispersion region, making it difficult to exhibit excellent optical properties in a wider wavelength region. At the same time, polymeric compounds that exhibit a liquid crystal phase at low temperatures have insufficient solubility.
A polymeric compound containing a specific chemical formula is used to reduce wavelength dependence through its group structure and exhibit good solubility in organic solvents, forming an optical film with reverse wavelength dispersion and low phase transfer temperature.
It achieves excellent optical performance in a wider wavelength range and good liquid crystal phase existence at lower temperatures, simplifying the preparation process of optical films and reducing temperature requirements.
Smart Images

Figure CN112898229B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polymerizable compound, a polymerizable composition and an optical film. Background Art
[0002] Flat panel displays (FPDs) include components using optical films such as polarizing plates and phase difference plates. Examples of optical films include those obtained by applying a solution obtained by dissolving a polymerizable compound in a solvent onto a supporting substrate and then polymerizing the solution.
[0003] In addition, it is known that the phase difference (Re(λ)) of an optical film formed by light of wavelength λnm is equal to the product of the birefringence (Δn) and the film thickness (d) (Re(λ)=Δn×d). Moreover, wavelength dispersion is usually expressed as the value of the phase difference value (Re(λ)) at a certain wavelength λnm divided by the phase difference value (Re(550)) at 550nm (Re(λ) / Re(550)), and the wavelength region where the wavelength dispersion (Re(λ) / Re(550)) is close to 1 or the wavelength dispersion at 450nm [Re(450) / Re(550)] <1 and the wavelength dispersion at 650nm [Re(650) / Re(550)] >1 is called reverse wavelength dispersion. It is known that a certain polarization conversion can be achieved in the wavelength region showing reverse wavelength dispersion.
[0004] In SID Symposium Digest of Technical Papers, Vol. 37, 2006, p. 1673, a compound (LC242) represented by the following chemical formula is disclosed as a polymerizable compound.
[0005] Summary of the invention
[0006] An object of the present invention is to provide a polymerizable compound and a polymerizable composition, and an optical film using the same, which can exhibit excellent optical properties in a wider wavelength range by reducing wavelength dependence or exhibiting reverse wavelength dispersion.
[0007] Another object of the present invention is to provide a polymerizable composition comprising a polymerizable compound that can exhibit an excellent liquid crystal phase at a relatively low temperature and has good solubility in an organic solvent.
[0008] As a means to solve the above problems,
[0009] In one embodiment of the present invention, a polymerizable compound including a group represented by the following chemical formula (1-1) or the following chemical formula (1-2) and a polymerizable group is provided.
[0010] Chemical formula (1-1)
[0011]
[0012] Chemical formula (1-2)
[0013]
[0014] (In the above chemical formula (1-1) and chemical formula (1-2),
[0015] A1 and A2 each independently represent a hydrogen atom, deuterium, halogen, amino, cyano, nitro, nitroso, sulfamoyl, isothiocyanate, thiocyanate, carboxyl, or a C1-C30 alkyl group, a C1-C30 alkylsulfinyl group, a C1-C30 alkylsulfonyl group, a C1-C30 alkylsulfanyl group, a C1-C30 alkylsulfonyl group, a C1-C30 alkylsulfanyl group, a C1-C12 fluoroalkyl group, a C2-C30 alkenyl group, a C1-C30 alkoxy group, a C1-C12 N-alkylamino group, a C2-C20 N,N-dialkylamino group, a C1-C6 N-alkylsulfamoyl group, a C2-C12 N,N-dialkylsulfamoyl group, a C3-C20 cycloalkyl group, a C2-C20 heterocycloalkyl group, a C6-C50 aryl group, and a C2-C50 heteroaryl group,
[0016] D1 each independently represents -CR1R2-, -S-, -NR2-, -CO- or -O-, R1 and R2 each independently represent a hydrogen atom or a C1-C6 alkyl group,
[0017] D2 each independently represents =CR3- or =N-, R3 each independently represents a hydrogen atom or a C1-C6 alkyl group,
[0018] E1 and E2 are each independently a substituted or unsubstituted C6-C60 aryl group, a substituted or unsubstituted C2-C60 heteroaryl group, or a combination thereof; however, when D1 in the chemical formula (1-1) is -S- and D2 is =N-, the substituent of E1 includes an isothiocyanate group or a thiocyanate group,
[0019] L1 is a C2-C10 alkynylene group with a direct bond or a triple bond,
[0020] B1 and B2 each independently represent a single bond or a divalent linking group.)
[0021] Furthermore, the present invention provides a polymerizable composition comprising the above polymerizable compound.
[0022] The present invention also provides an optical film having reverse wavelength dispersion as an optical film containing a polymer of the above-mentioned polymerizable compound.
[0023] According to an embodiment of the present invention, the polymerizable compound, the polymerizable composition, and the optical film using the same can exhibit excellent optical properties in a wider wavelength range by reducing wavelength dependence or exhibiting reverse wavelength dispersion.
[0024] In addition, it can present an excellent liquid crystal phase at a relatively low temperature and has good solubility in organic solvents.
[0025] Next, the above-mentioned effects and additional effects will be described in detail. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figures 1 to 5 FIG. 4 is a graph of the refractive index of an optical film at different wavelengths according to an embodiment of the present invention. DETAILED DESCRIPTION
[0027] Before describing the present invention in detail, it should be understood that the terms used in this specification are only used to describe specific embodiments and are not intended to limit the scope of the present invention, which shall only be limited by the scope of the appended claims. Unless otherwise expressly stated, all technical terms and scientific terms used in this specification have the same meanings as those commonly understood by people with general knowledge.
[0028] Throughout this specification and claims, unless expressly stated otherwise, terms such as comprise, comprises, and comprising merely indicate the inclusion of the stated item, step, or series of items and steps, and do not exclude any other item, step, or series of items or steps in advance.
[0029] Throughout the specification and claims, the term "aryl" refers to groups such as phenyl, benzyl, naphthyl, biphenyl, terphenyl, fluorenyl, phenanthrenyl, triphenylene, phenylene, The aromatic ring may include a C6-50 aromatic hydrocarbon ring such as a benzoyl, fluoranthenyl, benzofluorenyl, benzotriphenylene, benzo, anthracenyl, stilbene and pyrenyl.
[0030] In addition, the term "heteroaryl" may refer to a C2-50 aromatic ring including one or more hetero elements, such as a heterocyclic group including pyrrolyl, pyrazinyl, pyridyl, indolyl, isoindolyl, furanyl, benzofuranyl, isobenzofuranyl, dibenzofuranyl, benzothiophenyl, dibenzothiophenyl, quinolyl, isoquinolyl, quinoxalinyl, carbazolyl, phenanthridinyl, acridinyl, phenanthrolinyl, thienyl, and pyridine, pyrazine, pyrimidine, pyridazine, triazine, indole, quinoline, acridine, pyrrolidine, dioxane, piperidine, morpholine, piperazine, carbazole, furan, thiophene, oxazole, oxadiazole, benzoxazole, thiazole, thiadiazole, benzothiazole, benzotriazole, imidazole, benzimidazole, pyran, dibenzofuran, and the like.
[0031] In addition, L in the chemical formula x (wherein x is an integer) unless otherwise clearly defined, it represents a directly bonded, substituted or unsubstituted C6-C50 arylene group, or a substituted or unsubstituted C2-C50 heteroarylene group, R x (wherein x is an integer) unless explicitly defined otherwise, represents hydrogen, deuterium, halogen, nitro, nitrile, substituted or unsubstituted C1-C30 alkyl, substituted or unsubstituted C2-C30 alkenyl, substituted or unsubstituted C1-C30 alkoxy, substituted or unsubstituted C1-C30 mercapto, substituted or unsubstituted C6-C50 aryl, or substituted or unsubstituted C2-C50 heteroaryl.
[0032] Throughout the specification and claims, the term "substituted or unsubstituted" refers to a group consisting of deuterium, halogen, amino, cyano, nitro, nitroso, sulfamoyl, isothiocyanate, thiocyanate, carboxyl, or C1-C30 alkyl, C1-C30 alkylsulfinyl, C1-C30 alkylsulfonyl, C1-C30 alkylsulfanyl, C1-C12 fluoroalkyl, C2-C30 alkenyl, C1-C30 The alkyl radical may be substituted or unsubstituted by any one or more groups selected from the group consisting of an alkoxyl group, a C1-C12 N-alkylamino group, a C2-C20 N,N-dialkylamino group, a C1-C6 N-alkylsulfamoyl group, a C2-C12 N,N-dialkylsulfamoyl group, a C3-C30 silyl group, a C3-C20 cycloalkyl group, a C2-C20 heterocycloalkyl group, a C6-C50 aryl group, and a C2-C50 heteroaryl group. In addition, throughout the present specification, unless otherwise explicitly stated, the same symbols may have the same meaning.
[0033] In addition, when -NCS is represented in the structural formula, it means -NCS or -SCN.
[0034] In addition, unless otherwise explicitly stated to the contrary, the various embodiments of the present invention may be combined with certain other embodiments. Next, the embodiments of the present invention and their effects will be described.
[0035] The polymerizable compound according to one embodiment of the present invention may include a group or a polymerizable group represented by the following chemical formula (1-1) or the following chemical formula (1-2).
[0036] Chemical formula (1-1)
[0037]
[0038] Chemical formula (1-2)
[0039]
[0040] In the above Chemical Formula 1-1 and Chemical Formula 1-2,
[0041] A1 and A2 each independently represent a hydrogen atom, deuterium, halogen, amino, cyano, nitro, nitroso, sulfamoyl, isothiocyanate, thiocyanate, carboxyl, or a C1-C30 alkyl group, a C1-C30 alkylsulfinyl group, a C1-C30 alkylsulfonyl group, a C1-C30 alkylsulfanyl group, a C1-C30 alkylsulfonyl group, a C1-C30 alkylsulfanyl group, a C1-C12 fluoroalkyl group, a C2-C30 alkenyl group, a C1-C30 alkoxy group, a C1-C12 N-alkylamino group, a C2-C20 N,N-dialkylamino group, a C1-C6 N-alkylsulfamoyl group, a C2-C12 N,N-dialkylsulfamoyl group, a C3-C20 cycloalkyl group, a C2-C20 heterocycloalkyl group, a C6-C50 aryl group, and a C2-C50 heteroaryl group,
[0042] D1 each independently represents -CR1R2-, -S-, -NR2-, -CO- or -O-, R1 and R2 each independently represent a hydrogen atom or a C1-C6 alkyl group,
[0043] D2 each independently represents =CR3- or =N-, R3 each independently represents a hydrogen atom or a C1-C6 alkyl group,
[0044] E1 and E2 are each independently a substituted or unsubstituted C6-C60 aryl group, a substituted or unsubstituted C2-C60 heteroaryl group, or a combination thereof,
[0045] L1 is a C2-C10 alkynylene group with a direct bond or a triple bond,
[0046] B1 and B2 each independently represent a single bond or a divalent linking group. The divalent linking group is not particularly limited, but can be a substituted or unsubstituted C1-C30 alkyl group, a substituted or unsubstituted C3-C20 cycloalkyl group, a substituted or unsubstituted C2-C20 heterocycloalkyl group, a substituted or unsubstituted C6-C50 aryl group, a substituted or unsubstituted C2-C50 heteroaryl group, or a combination thereof, wherein -CH2- can be substituted by -CO-, -COO-, -OCO-, -O-, -S-, -C(=S)-, -C(=S)-O-, -OC(=S)-, or -NR-, and R can be hydrogen or a C1-C30 alkyl group.
[0047] However, when D1 in Chemical Formula 1-1 is -S- and D2 is =N-, the substituent of E1 may include an isothiocyanate group or a thiocyanate group.
[0048] When E1 contains an isothiocyanate group or a thiocyanate group, there are advantages of increased refractive index, excellent reverse wavelength dispersion, and reduced phase transition temperature. In addition, although not particularly limited, E2 may also contain the above-mentioned isothiocyanate group or thiocyanate group.
[0049] The above-mentioned polymerizable groups are not subject to special limitations, but can be connected to the two ends of the polymerizable compound, that is, the positions of B1 and B2 of chemical formula (1-1) and chemical formula (1-2), and can contain 2 to 4. In the case where the polymerizable groups contain only 2 at the two ends, it can show orientation during polymerization. On the contrary, when the polymerizable groups exceed 4, they will be entangled with each other and lose orientation during polymerization. The type of polymerizable group is not subject to special limitations, as long as it is a group that participates in the polymerization reaction. Specifically, it can be a vinyl group, a styryl group, an acryloyl group, a methacryloyl group, an acryloyloxy group, a methacryloyloxy group, a carboxyl group, an acetyl group, a hydroxyl group, a carbamoyl group, a C1 to C4 N-alkylamino group, an amino group, an epoxy group, an oxetanyl group, a formyl group, -N=C=O and -N=C=S, etc.
[0050] The polymerizable compound according to one embodiment of the present invention may have a liquid crystal phase, and in particular, may present a nematic phase. In addition, the phase transition temperature of the polymerizable compound according to one embodiment of the present invention is within the range of 0 to 130°C, and has the advantage of a low phase transition temperature. Specifically, the polymerizable compound according to one embodiment of the present invention may present a liquid crystal phase within the range of 20 to 130°C, specifically within the range of 70 to 120°C. The phase transition temperature of the polymerizable compound is low, which means that the temperature can be lowered during the process of polymerization and film formation by irradiating ultraviolet rays after coating a composition containing the polymerizable compound, so that an optically anisotropic film can be obtained under simpler and milder conditions, thereby preventing various problems caused by applying high temperatures.
[0051] Furthermore, E1 and E2 in the above chemical formula (1-1) or the above chemical formula (1-2) can be represented by any one of the following chemical formulas Y-1 to Y-13.
[0052]
[0053] In the above chemical formula,
[0054] Z 3 and R each independently represents deuterium, halogen, amino, cyano, nitro, nitroso, sulfamoyl, isothiocyanate, thiocyanate, carboxyl, or C1-C30 alkyl, C1-C30 alkylsulfinyl, C1-C30 alkylsulfonyl, C1-C30 alkylsulfanyl, C1-C12 fluoroalkyl, C2-C30 alkenyl, C1-C30 alkoxy, C1-C12 N-alkylamino, C2-C20 N,N-dialkylamino, C1-C6 N-alkylsulfamoyl, C2-C12 N,N-dialkylsulfamoyl, C3-C20 cycloalkyl, C2-C20 heterocycloalkyl, C6-C50 aryl, and C2-C50 heteroaryl,
[0055] V 1 and V 2 Each independently represents -CO-, -S-, -NR3-, -O-, -Se- or -SO2-, and R3 each independently represents a hydrogen atom or a C1-C4 alkyl group,
[0056] W 1 To W 5 Each independently represents -CR4= or -N=, and each R4 independently represents a hydrogen atom or a C1-C4 alkyl group. 1 、V 2 , W 1 To W 5 At least one of them contains S, N, O or Se.
[0057] When D1 in the above chemical formula 1-1 is -S- and D2 is =N-, Z in the chemical formula Y-1 3 It may contain an isothiocyanate group or a thiocyanate group, and may also contain an isothiocyanate group or a thiocyanate group in other cases.
[0058] Furthermore, the above chemical formula (1-1) can be represented by the following chemical formula (1-3).
[0059] Chemical formula (1-3)
[0060]
[0061] In the above chemical formula (1-3), the definitions of L1, A1, A2, B1 and B2 are the same as those in the above chemical formula (1-1).
[0062] R5 is each independently selected from deuterium, halogen, amino, cyano, nitro, nitroso, sulfamoyl, isothiocyanate, thiocyanate, carboxyl, or C1-C30 alkyl, C1-C30 alkylsulfinyl, C1-C30 alkylsulfonyl, C1-C30 alkylsulfanyl, C1-C12 fluoroalkyl, C2-C30 alkenyl, C1-C30 alkoxy, C1-C12 N-alkylamino, C2-C20 N,N-dialkylamino, C1-C6 N-alkylsulfamoyl, C2-C12 N,N-dialkylsulfamoyl, C3-C20 cycloalkyl, C2-C20 heterocycloalkyl, C6-C50 aryl, and C2-C50 heteroaryl.
[0063] n is an integer of 0-4.
[0064] Furthermore, the above Chemical Formula (1-2) can be represented by any one of the following Chemical Formulas (1-4) to (1-5).
[0065]
[0066] In the above chemical formula, the definitions of A1, A2, B1 and B2 are the same as those in the above chemical formula (1-2).
[0067] R5 and R6 are each independently selected from deuterium, halogen, amino, cyano, nitro, nitroso, sulfamoyl, isothiocyanate, thiocyanate, carboxyl, or C1-C30 alkyl, C1-C30 alkylsulfinyl, C1-C30 alkylsulfonyl, C1-C30 alkylsulfanyl, C1-C12 fluoroalkyl, C2-C30 alkenyl, C1-C30 alkoxy, C1-C12 N-alkylamino, C2-C20 N,N-dialkylamino, C1-C6 N-alkylsulfamoyl, C2-C12 N,N-dialkylsulfamoyl, C3-C20 cycloalkyl, C2-C20 heterocycloalkyl, C6-C50 aryl, and C2-C50 heteroaryl.
[0068] n is independently an integer of 0 to 5 (wherein n in Chemical Formula 1-4 is an integer of 0 to 4).
[0069] Specifically, the chemical formula (1-1) may include a structure represented by any of the following chemical formulas: Both ends of the following structure are connected to B1 and B2.
[0070]
[0071] Alternatively, the above chemical formula (1-2) may include a structure represented by any of the following chemical formulas.
[0072]
[0073]
[0074] Furthermore, the above Chemical Formula (1-1) or Chemical Formula (1-2) can be represented by the following Chemical Formula (1-6) or Chemical Formula (1-7).
[0075] Chemical formula (1-6)
[0076]
[0077] Chemical formula (1-7)
[0078]
[0079] In the above chemical formula (1-6) and chemical formula (1-7), the definitions of L1, A1, A2, D1, D2, E1 and E2 are the same as those in chemical formula 1-1 and chemical formula 1-2.
[0080] R7 each independently represents deuterium, halogen, amino, cyano, nitro, nitroso, sulfamoyl, isothiocyanate, thiocyanate, carboxyl, or C1-C30 alkyl, C1-C30 alkylsulfinyl, C1-C30 alkylsulfonyl, C1-C30 alkylsulfanyl, C1-C12 fluoroalkyl, C2-C30 alkenyl, C1-C30 alkoxy, C1-C12 N-alkylamino, C2-C20 N,N-dialkylamino, C1-C6 N-alkylsulfamoyl, C2-C12 N,N-dialkylsulfamoyl, C3-C20 cycloalkyl, C2-C20 heterocycloalkyl, C6-C50 aryl, and C2-C50 heteroaryl,
[0081] m is an integer of 0 to 4, and p is an integer of 0 to 10, respectively, independently of each other.
[0082] Specific examples of the polymerizable compound according to one embodiment of the present invention may include compounds with the following structures.
[0083]
[0084]
[0085] According to another embodiment of the present invention, there is provided a polymerizable composition comprising the above polymerizable compound, wherein the polymerizable compound may be contained in an amount of 0.5 to 50 parts by weight, preferably 1 to 15 parts by weight, relative to 100 parts by weight of the polymerizable composition.
[0086] In addition to the above-mentioned polymerizable compound, the above-mentioned polymerizable composition may further include polymerization initiators, other polymerizable compounds, non-polymerizable liquid crystal compounds, solvents, additives, etc. Among them, the other polymerizable compound may be a polymerizable liquid crystal compound.
[0087] In addition, specific examples of other polymerizable compounds are not particularly limited, and compounds represented by the following chemical formula M1 and chemical formula M2 can be taken as examples.
[0088]
[0089] In the above chemical formula (M1) and chemical formula (M2), A M Each is independently 1,4-phenylene, 1,4-cyclohexylene, 1,4-cyclohexenylene, pyridine-2,5-diyl, naphthalene-2,6-diyl or fluorene-2,7-diyl, wherein at least one hydrogen atom may be substituted by fluorine, chlorine, cyano, hydroxyl, formyl, trifluoroacetyl, difluoromethyl, trifluoromethyl, C1-C5 alkyl, C1-C5 alkoxy, C1-C5 alkyl ester or C1-C5 alkanoyl; Z MEach is independently a single bond, -OCH2-, -CH2O-, -COO-, -OCO-, -COS-, -SCO-, -OCOO-, -CONH-, -NHCO-, -CF2O-, -OCF2-, -CH2CH2-, -CF2CF2-, -CH=CHCOO-, -OCOCH=CH-, -CH2CH2COO-, -OCOCH2CH2-, -CH=CH-, -N=CH-, -CH=N-, -N=CCH3-, -CCH3=N-, -N=N- or -C≡C-; X M is hydrogen, fluorine, chlorine, trifluoromethyl, trifluoromethoxy, cyano, C1-C20 alkyl, C1-C20 alkenyl, C1-C20 alkoxy or C1-C20 alkyl ester; q is an integer of 1 to 4; a is an integer of 0 to 20; R M is hydrogen or methyl; Y M is a single bond, -O-, -COO-, -OCO- or -OCOO-. When q is 2 or more, the above A M and Z M It may be different in each repeating unit.
[0090] Specific examples of the non-polymerizable liquid crystal compound can be selected from compounds listed in the liquid crystal compound database LiqCryst (LCI Publisher GmbH, Hamburg, Germany) or known non-polymerizable liquid crystal compounds.
[0091] As the polymerization initiator, a photopolymerization initiator can be exemplified, and as the photopolymerization initiator, benzoin compounds, benzophenone compounds, benzyl ketal compounds, α-hydroxyketone compounds, α-aminoketone compounds, iodonium salts, sulfonium salts and the like can be exemplified. Specific examples of the photopolymerization initiator include IRGACURE 907 (manufactured by Chiba Japan Co., Ltd.), IRGACURE 184 (manufactured by Chiba Japan Co., Ltd.), IRGACURE 651 (manufactured by Chiba Japan Co., Ltd.), IRGACURE 819 (manufactured by Chiba Japan Co., Ltd.), IRGACURE 250 (manufactured by Chiba Japan Co., Ltd.), IRGACURE 369 (manufactured by Chiba Japan Co., Ltd.), SEIKUOL BZ (manufactured by Seiko Chemical Co., Ltd.), SEIKUOL Z (manufactured by Seiko Chemical Co., Ltd.), SEIKUOL BEE (manufactured by Seiko Chemical Co., Ltd.), KAYACURE BP100 (manufactured by Nippon Kayaku Co., Ltd.), KAYACURE UVI-6992 (manufactured by Dow Chemical), ADEKA OPTOMER SP-152 (manufactured by ADEKA Corporation), ADEKA OPTOMER Take SP-170 (manufactured by ADICO Co., Ltd.) as an example.
[0092] The amount of the polymerization initiator used can be 0.1 to 30 parts by weight, specifically 0.5 to 10 parts by weight, relative to 100 parts by weight of the total of the polymerizable compound and other liquid crystal compounds. Within the above range, polymerization can be performed while ensuring excellent liquid crystal alignment.
[0093] According to the polymerizable composition of the present invention, the polymerizable composition may be diluted with a solvent for convenient coating, or the polymerizable composition may be coated with a solution of the polymerizable composition composed of the polymerizable composition and the solvent after the components of the polymerizable composition are added to the solvent. As the solvent, ester solvents, amide solvents, alcohol solvents, ether solvents, glycol monoalkyl ether solvents, aromatic hydrocarbon solvents, halogenated aromatic hydrocarbon solvents, aliphatic hydrocarbon solvents, halogenated aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, ketone solvents, acetate solvents, etc. may be used.
[0094] Examples of additives include photosensitizers, chain transfer agents, antioxidants, ultraviolet absorbers, radical scavengers, light stabilizers, optically active compounds, silane coupling agents, solvents, and other additives, which may be included within a range that does not impair the effects of the present invention.
[0095] According to another embodiment of the present invention, an optical film comprising a polymer of the polymerizable compound is provided.
[0096] The optical film may include a polymer obtained by applying a polymerizable composition containing a polymerizable compound onto a substrate and then polymerizing the polymerized composition. It has been confirmed from the examples described below that the reverse wavelength dispersion property thereof is very excellent.
[0097] Specifically, the optical film may satisfy the following <Formula 1> and <Formula 2> under the condition of a thickness of 0.1 to 10 μm, thereby having excellent reverse wavelength dispersion.
[0098] <Formula 1>
[0099] Re(450) / Re(550)≤0.970
[0100] <Formula 2>
[0101] 1.020≤Re(650) / Re(550)
[0102] In the above-mentioned Formula 1 and Formula 2, Re(450) is the phase difference value at a wavelength of 450 nm, Re(550) is the phase difference value at a wavelength of 550 nm, and Re(650) is the phase difference value at a wavelength of 650 nm.
[0103] Because of the above-mentioned characteristics, the above-mentioned optical film is also very suitable for use as a reverse wavelength dispersion phase difference film.
[0104] The above-mentioned substrate is not subject to special limitations and is not limited to materials or forms such as glass, plastic, film, sheet, plate, etc. The above-mentioned substrate can be a photo-alignment layer, a polarizing layer, a protective layer, a phase difference layer, etc., but is not limited thereto.
[0105] The optical film according to one embodiment of the present invention can be used as a reverse wavelength dispersion phase difference film, or as a broadband λ / 4 plate or λ / 2 plate. In addition, it can also be used as an optical film for vertical alignment (VA) mode, or as a reflection prevention film such as an anti-reflection (AR) film, a polarizing film, an elliptically polarizing film, a viewing angle magnification film, or an optical compensation film for viewing angle compensation of a transmissive liquid crystal display.
[0106] Next, the polymerizable compound and the optical film according to one embodiment of the present invention will be described in detail with reference to the manufacturing examples and embodiments. The following manufacturing examples and embodiments are only used to illustrate the present invention, and the scope of the present invention is not limited to the following manufacturing examples and embodiments.
[0107] <Production Example 1-1> Synthesis of Compound 7
[0108] Using compound 1 as the starting material, compound 7 was synthesized by the following reaction formula.
[0109]
[0110] (1) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, 2,5-dimethoxyaniline compound 1 (25 g, 0.163 mol) and 4-nitrobenzyl chloride 36.34 g (0.195 mol) and triethylamine 45.5 ml (0.326 mol) were dissolved in chloroform (700 ml), and then heated at 90°C for 18 hours under a nitrogen environment. After cooling to room temperature, the reaction solution was diluted with water and dichloromethane and phase separated. The organic layer was then extracted and dried over magnesium sulfate. The obtained solid was washed with hexane to obtain compound 2 (48.7 g). GC-MS (EI): m / z 302 [M+H+]
[0111] (2) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, the obtained compound 2 (48.7 g, 0.161 mol) and Lawesson reagent 42.8 g (0.105 mol) were dissolved in toluene (1 L), and then heated and refluxed for 24 hours under a nitrogen environment. The reaction solution was cooled at room temperature and then concentrated. Ethanol was added to the concentrated residue, and then the generated precipitate was filtered to obtain compound 3 (39.5 g). The yield was 77%, GC-MS (EI): m / z 318 [M+H+]
[0112] (3) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, the obtained compound 3 (39.5 g, 0.124 mol), 54.45 g (0.165 mol) of potassium ferrocyanide and 10 ml of methanol were mixed in water (160 ml). After heating the obtained mixture to 90°C, a 30% aqueous solution of NaOH (132 ml) was added dropwise for about 30 minutes, followed by a 2-hour heating reaction at 90°C. After cooling to room temperature, the precipitated solid was washed with water and hexane and filtered to obtain compound 4 (18.3 g). The yield was 47%, GC-MS (EI): m / z 316 [M+H+]
[0113] (4) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, the obtained compound 4 (3.2 g, 0.010 mol) and 6.8 g (0.030 mol) of tin (II) chloride were dissolved in ethanol (60 ml), and then heated to reflux for 6 hours under a nitrogen environment. After cooling at room temperature, the reaction solution was diluted with 10% sodium hydroxide and dichloromethane and phase separated. Then, the organic layer was extracted and dried over magnesium sulfate. The obtained solid was washed with methanol to obtain compound 5 (2.3 g). The yield was 76%, GC-MS (EI): m / z 286 [M+H+]
[0114] (5) In a reaction vessel equipped with a stirring device and a thermometer, the obtained compound 5 (6.0 g, 0.021 mol) and 6.45 ml (0.046 mol) of triethylamine were dissolved in anhydrous tetrahydrofuran (THF) (150 ml), and then ice-cooled to 0°C. Thiophosgene 3.2 ml (0.042 mol) was dripped into the cooled reaction vessel, and then the temperature was raised to room temperature and the reaction was carried out for 2 hours. After the reaction was completed, the reaction mixture was filtered. After the filtrate was concentrated, it was eluted on a silica gel column using a solution of n-heptane: ethyl acetate = 2:1 to obtain compound 6 (2.2 g). The yield was 33%, GC-MS (EI): m / z 328 [M+H+]
[0115] (6) In a reaction vessel equipped with a stirring device and a thermometer, the obtained compound 6 (1.1 g, 0.003 mol) was dissolved in chloroform (60 ml), and then ice-cooled to -60°C under a nitrogen environment. 10 ml of chloroform containing 2.3 ml (0.021 mol) of tribromoboric acid was added dropwise. The temperature was raised to room temperature and the reaction was carried out for 12 hours. The reaction solution was diluted with water and ethyl acetate and phase separated. The organic layer was then extracted and dried over magnesium sulfate. After the organic layer was concentrated, it was eluted on a silica gel column using a tetrahydrofuran (THF) solution to obtain compound 7 (0.93 g). The yield was 93%, GC-MS (EI): m / z 300 [M+H+]
[0116] <Production Example 1-2> Synthesis of Compound 10
[0117] Using compound 8 as the starting material, compound 10 was synthesized through the following reaction formula.
[0118]
[0119] In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, cyclohexyl dicarboxylic acid compound 8 (60.0 g, 0.348 mol) and compound 9 (18.4 g, 0.069 mol), 3,5-dibutyl-4-hydroxytoluene 1.0 g (0.024 mol), 4-dimethylaminopyridine 0.1 g (0.003 mol) were dissolved in N-methyl-2-pyrrolidone (120 ml), and then the reaction solution was heated to 45 ° C under a nitrogen atmosphere, and then 14.1 g (0.452 mol) of diisopropylcarbodiimide was dripped for 1 hour. Then, the reaction was carried out at 45 ° C for 20 hours. After cooling at room temperature, 3.5 g (0.087 mol) of sodium hydroxide aqueous solution (240 ml) was dripped and stirred for 2 hours. The obtained suspension was washed with a methanol:water=1:1 solution to obtain Compound 10 (28.5 g) (yield: 97%).
[0120] 1 H-NMR: δ(ppm)1.44~1.62(m,8H),1.72(m,2H),1.80(m,2H),2.16(m,2H),2.22(m,2H),2.41(m,1H),2. 53(m,1H),3.94(t,2H),4.18(t,2H),5.82(d,1H),6.13(m,1H),6.40(d,1H),6.88(d,2H),6.97(d,2H).
[0121] <Production Example 1-3> Synthesis of Compound 11
[0122] Compound 10 produced in the above-mentioned Production Example 1-2 and Compound 7 produced in Production Example 1-1 were reacted to synthesize Compound 11 according to the following reaction formula.
[0123]
[0124] In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, compound 10 (4.18 g, 0.010 mol) and compound 7 (1.5 g, 0.005 mol) and 0.12 g (0.001 mol) of 4-dimethylaminopyridine were dissolved in tetrahydrofuran (THF) (16 ml), and then cooled to 0 ° C under a nitrogen environment, and then 2.47 g (0.012 mol) of dicyclohexylcarbodiimide was dripped for 15 minutes. Next, the reaction was carried out at room temperature for 24 hours. After cooling at room temperature, the reaction mixture was filtered. After the filtrate was dried, it was concentrated under reduced pressure. A small amount of ethyl acetate was added to the concentrated residue, and then methanol (200 ml) was added. After filtering the precipitated material, it was washed with methanol, and then vacuum dried to obtain compound 11 (2.5 g) (yield 45%).
[0125] 1 H-NMR: δ(ppm)1.48~1.74(m,16H),1.76(m,4H),1.81(m,4H),2.36(m,4H),2.45(m,4H),2.71(m,2H),2.85(m,2H),3.97(t, 4H),4.20(t,4H),5.84(d,2H),6.16(m,2H),6.42(d,2H),6.91(d,4H),7.01(d,4H),7.25(s,2H),7.35(d,2H),8.05(d,2H).
[0126] <Production Example 1-4> Synthesis of Compound 12
[0127] Compound 12 was synthesized by the same method except that Compound 9-2 was used instead of Compound 9 in the above Preparation Example 1-2 and the reaction was carried out according to the following reaction formula.
[0128]
[0129] <Production Example 1-5> Synthesis of Compound 13
[0130] Compound 13 was synthesized by the same method except that Compound 12 was used instead of Compound 10 in the above Preparation Example 1-3 and the reaction was carried out according to the following reaction formula.
[0131]
[0132] 1H-NMR: δ(ppm)1.76(m,4H),1.81(m,4H),2.38(m,4H),2.45(m,2H),2.70(m,2H),2.82(m,2H),4.08(t,4H),4.39( t,4H),5.86(d,2H),6.15(m,2H),6.45(d,2H),7.01(d,4H),7.03(d,4H),7.25(s,2H),7.36(d,2H),8.05(d,2H).
[0133] <Production Example 1-6> Synthesis of Compound 14
[0134] Compound 14 was synthesized by the same method except that Compound 9-3 was used instead of Compound 9 in the above Preparation Example 1-2 and the reaction was carried out according to the following reaction formula.
[0135]
[0136] <Production Example 1-7> Synthesis of Compound 15
[0137] Compound 15 was synthesized by the same method except that Compound 14 was used instead of Compound 10 in the above Preparation Example 1-3 and the reaction was carried out according to the following reaction formula.
[0138]
[0139] 1 H-NMR: δ(ppm)1.48~1.74(m,10H),1.76(m,8H),1.81(m,8H),2.36(m,4H),2.45(m,4H),2.71(m,2H),2.85(m,2H),3.96(t, 4H),4.18(t,4H),5.84(d,2H),6.15(m,2H),6.42(d,2H),6.91(d,4H),7.01(d,4H),7.25(s,2H),7.36(d,2H),8.05(d,2H).
[0140] <Production Example 2-1> Synthesis of Compound 22
[0141] Using compound 16 as the starting material, compound 22 was synthesized by the following reaction formula.
[0142]
[0143] (1) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, compound 16 (10.0 g, 0.058 mol) and 16.3 g (0.176 mol) of chloroacetone, 10.7 g (0.087 mol) of NaCO3 / SiO2, and 20.5 g (10 wt%) of polyphthalamide (PPA) / SiO2 were dissolved in 90 ml of chlorobenzene, and then heated and refluxed for 6 hours under a nitrogen environment. After cooling at room temperature, the reaction mixture was filtered with ethyl acetate. After concentrating the filtrate, it was eluted on a silica gel column with a solution of n-heptane:ethyl acetate = 2:1 to obtain compound 17 (2.2 g). The yield was 81%, GC-MS (EI): m / z 208 [M+H+]
[0144] (2) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, compound 17 (9.9 g, 0.047 mol) was dissolved in 60 ml of acetonitrile, and then ice-cooled to 0°C under a nitrogen environment. 8.9 g (0.049 mol) of N-bromosuccinimide was added to the cooled reaction solution. Then the temperature was raised to room temperature and the reaction was carried out for 30 minutes. After 60 ml of distilled water was slowly added to the reaction mixture, it was stirred. After filtering the generated solid, it was washed with distilled water: acetonitrile = 1:1 20 ml to obtain compound 18 (12.4 g). The yield was 98%, GC-MS (EI): m / z 249 [M+H+]
[0145] (3) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube, and a temperature control device, compound 18 (8.7 g, 0.034 mol), 4,4,5,5-tetramethyl-2-(4-nitrobenzene)-1,3,2-dioxaborolane 9.5 g (0.033 mol), and tetrakis(triphenylphosphine)palladium(0) 1.9 g (0.001 mol) were dissolved in 195 ml of dioxane, and then 65 ml of a 2M aqueous solution of NaCO3 was added. Next, heating and reflux were performed for 6 hours. After cooling to room temperature, the reaction solution was diluted with a saturated aqueous solution of aluminum chloride and dichloromethane and phase separated. Next, the organic layer was extracted and dried over magnesium sulfate. The concentrated residue was eluted on a silica gel column with a solution of n-heptane:ethyl acetate = 2:1 to obtain compound 19 (9.9 g). The yield was 91%, GC-MS (EI): m / z 329 [M+H+]
[0146] (4) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, compound 19 (9.9 g, 0.030 mol) and 20.5 g (0.090 mol) of tin chloride were dissolved in 200 ml of ethanol, and then heated to reflux for 2 hours under a nitrogen environment. After cooling at room temperature, the reaction solution was diluted with a 2N potassium hydroxide aqueous solution and ethyl acetate and phase separated. The organic layer was then extracted and dried over magnesium sulfate. The concentrated residue was eluted on a silica gel column with a solution of dichloromethane:tetrahydrofuran (THF) = 10:1 to obtain compound 20 (9.9 g). The yield was 74%, GC-MS (EI): m / z 299 [M+H+]
[0147] (5) In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, compound 20 (6.8 g, 0.030 mol) and triethylamine 7.0 ml (0.069 mol) were dissolved in anhydrous tetrahydrofuran (THF) (100 ml), and then ice-cooled to 0°C. Thiophosgene 3.5 ml (0.045 mol) was added dropwise to the cooled reaction solution. Next, the temperature was raised to room temperature and the reaction was carried out for 2 hours. After the reaction was completed, the reaction mixture was filtered. After the filtrate was concentrated, eluted on a silica gel column using a chloroform solution to obtain compound 21 (4.5 g). The yield was 58%, GC-MS (EI): m / z 341 [M+H+]
[0148] (6) In a reaction vessel equipped with a thermometer, the obtained compound 21 (4.5 g, 0.013 mol) was dissolved in chloroform (250 ml), and then ice-cooled to -60°C under a nitrogen atmosphere. After 20 ml of chloroform containing 8.9 ml (0.035 mol) of tribromoboric acid was dripped into the cooled reaction solution, the temperature was raised to room temperature and the reaction was carried out for 12 hours. The reaction solution was diluted with water and ethyl acetate and phase separated. Then, the organic layer was extracted and dried over magnesium sulfate. After the organic layer was concentrated, it was eluted on a silica gel column using a tetrahydrofuran (THF) solution to obtain compound 22 (3.7 g). The yield was 90%, GC-MS (EI): m / z 313 [M+H+].
[0149] <Production Example 2-2> Synthesis of Compound 23
[0150] Compound 23 was synthesized according to the following reaction formula by reacting Compound 10 produced in the above Production Example 1-2 and Compound 22 produced in the above Production Example 2-1.
[0151]
[0152] In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, compound 10 (9.9 g, 0.024 mol) and compound 22 (3.7 g, 0.012 mol) and 0.28 g (0.002 mol) of 4-dimethylaminopyridine were dissolved in tetrahydrofuran (THF) (200 ml), and then the reaction solution was cooled to 0 ° C under a nitrogen environment, and then 5.85 g (0.028 mol) of dicyclohexylcarbodiimide was dripped for 15 minutes. Next, the reaction was carried out at room temperature for 24 hours. After cooling at room temperature, the reaction mixture was filtered. After the filtrate was dried, it was concentrated under reduced pressure. A small amount of ethyl acetate was added to the concentrated residue, and then methanol (200 ml) was added. After filtering the precipitated material, it was washed with methanol, and then vacuum dried to obtain compound 23 (5.26 g) (yield 40%).
[0153] 1 H-NMR: δ(ppm)1.48~1.74(m,16H),1.76(m,4H),1.81(m,4H),2.32(S,3H),2.38(m,8H),2.46(m,2H),2.65(m,2H),3.97(t, 4H),4.20(t,4H),5.84(d,2H),6.17(m,2H),6.42(d,2H),6.89(d,4H),6.99(d,4H),7.18(m,2H),7.27(d,2H),7.38(d,2H).
[0154] <Production Example 3-1> Synthesis of Compound 25
[0155]
[0156] In a reaction vessel equipped with a stirring device, a thermometer, a cooling tube and a temperature control device, compound 7 (1.1 g, 0.003 mol) and compound 24 (3.1 g, 0.007 mol) and 0.1 g (0.0006 mol) of 4-dimethylaminopyridine were dissolved in dichloromethane (Dichloromethane) (50 ml), and then the reaction solution was cooled to 0 ° C under a nitrogen environment, and then 1.12 g (0.008 mol) of diisopropylcarbodiimide was dripped for 10 minutes. Next, the reaction was carried out at room temperature for 24 hours. After cooling at room temperature, the reaction mixture was filtered. After the filtrate was dried, it was concentrated under reduced pressure. A small amount of ethyl acetate was added to the concentrated residue, and then methanol (200 ml) was added. After filtering the precipitated material, it was washed with methanol, and then vacuum dried to obtain compound 25 (1.60 g) (yield 40%).
[0157] 1 H-NMR: δ(ppm)1.48~1.74(m,16H),1.76(m,4H),1.81(m,4H),2.30(m,4H),2.39(m,4H),2.68(m,2H),2.77(m,2H),3.80(t,4H),3. 94(t,4H),4.19(t,4H),5.84(d,2H),6.14(m,2H),6.42(d,2H),6.84(d,4H),6.88(d,4H),7.23(s,2H),7.35(d,2H),8.05(d,2H).
[0158] <Examples and Comparative Examples> Production of Optical Films
[0159] A 2% aqueous solution of polyvinyl alcohol (polyvinyl alcohol Mw 31000-50000, Aldrich) was applied to a glass substrate and then heated and dried to obtain a film with a thickness of 100 nm. After the surface of the obtained film was polished, the solutions of Examples 1 to 5 and Comparative Example 1 having the compositions described in Table 1 below were applied to the polished surface by a slit coating method. Next, the film was dried on a hot plate for 3 minutes and then irradiated with 1200 mJ / cm 2 of ultraviolet light, thereby obtaining an optical film having a thickness as described in Table 2 below.
[0160] In the following Table 1, "%" indicates the content (by weight) in the entire solution. "Irg 819" indicates a photoinitiator, namely, IRGACURE 819, and "BYK-361N" indicates a leveler that functions to level the surface.
[0161] In addition, LC242 in Comparative Example 1 represents a compound having the following structure.
[0162]
[0163]
Table 1
[0164]
[0165] <Test Example 1> Optical Property Measurement
[0166] The refractive index and phase difference of the manufactured optical film were measured by a measuring instrument (RETS-100, Otsuka Corporation) in the wavelength range of 380nm to 780nm, and the phase difference value Re(450) at a wavelength of 450nm, the phase difference value Re(550) at a wavelength of 550nm, and the phase difference value Re(650) at a wavelength of 650nm were calculated. The results are shown in the following Table 2 and Figures 1 to 5 As shown, the phase difference ratios of different wavelengths are shown in Table 2.
[0167]
Table 2
[0168]
[0169] It can be confirmed from the above Table 2 and the accompanying drawings that by combining the polymerizable compound according to an embodiment of the present invention alone or with other known polymerizable liquid crystal compounds and other components and uniformly aligning them in any form, the wavelength dependence of the refractive index anisotropy of the material can be reduced, or excellent inverse wavelength dispersion can be exhibited.
[0170] On the contrary, it can be confirmed that Comparative Example 1 exhibits positive wavelength dispersion characteristics. That is, the characteristics of the reverse wavelength dispersion material show that the value of re(450 / 550) is less than 1 and the value of re(650 / 550) is greater than 1 in the phase difference ratio, and the value of re(450 / 550) in Comparative Example 1 is 1.075 and the value of re(650 / 550) is 0.978. Therefore, it can be confirmed from the results in the above Table 2 that the polymerizable compound according to the present invention exhibits reverse wavelength dispersion characteristics compared with Comparative Example 1.
Claims
1. A polymerizable compound represented by any one of the following chemical formulas, in, NCS in the above chemical formula represents an isothiocyanate group.
2. A polymerizable composition, characterized in that: Contains the polymerizable compound according to claim 1.
3. An optical film, characterized in that: A polymer comprising the polymerizable compound according to claim 1 has reverse wavelength dispersibility.
4. The optical film according to claim 3, characterized in that: Under the condition of thickness of 0.1 to 10 μm, the following equations 1 and 2 are satisfied: Formula 1 Re(450) / Re(550)≤0.970 Formula 2 1.020≤Re(650) / Re(550) In the above-mentioned Formula 1 and Formula 2, Re(450) is the phase difference value at a wavelength of 450 nm, Re(550) is the phase difference value at a wavelength of 550 nm, and Re(650) is the phase difference value at a wavelength of 650 nm.
Citation Information
Patent Citations
Polymerizable compound, polymerizable composition, polymer, and optically anisotropic material
CN104470957A
Composition for making optical film and optical film
CN107488249A