Mirror glass processed in a different place and preparation method thereof
By plating multiple dielectric layers and metal layers on the tin liquid surface and air surface on the glass substrate, the problem that mirror glass cannot be heat treated in the existing technology is solved, and high outdoor reflectivity and neutral color effects are achieved.
Patent Information
- Application Number
- CN202110390461.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-04-12
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-04-12
AI Technical Summary
Existing mirror glass cannot be heat treated after the functional layer is plated, resulting in oxidation of the silver layer and a decrease in reflectivity, making off-site processing impossible.
At least two dielectric layers are plated on the glass substrate with tin liquid surface, and multiple dielectric layers and metal layers are plated on the air surface. They are formed through a sputtering process to ensure that the film layer is not oxidized and the reflectivity remains high after heat treatment.
It realizes that heat treatment can be carried out after coating to maintain high outdoor visible light reflectivity, with a reflectivity of more than 72%, while maintaining a neutral color.
Smart Images

Figure CN112960913B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of glass manufacturing, relates to glass surface coating, and in particular to a mirror-coated glass processed remotely and a preparation method thereof. Background Art
[0002] Mirror glass is widely used in our daily life. There are two common ways to produce mirrors: chemical silver plating and vacuum evaporation. The former is the most widely used production process. A layer of silver film is plated on the surface of the glass using a series of chemical reactions, so that the plated glass has a high reflectivity of visible light, and the visible light reflectivity is generally over 90%.
[0003] However, if the product prepared by this method is not protected by a protective layer, the silver layer will be directly exposed to the air and oxidized within a week, resulting in the failure of the mirror effect. In addition, there are aluminum mirrors and chrome mirrors on the market. Although their visible light reflectivity is not as high as that of silver mirrors, their chemical stability is better than that of silver mirrors. However, they cannot be processed in other places, that is, they cannot be heat treated after the functional film layer (Ag, Cu, Al, Cr, etc.) is plated. High outdoor visible light reflectivity and remote processing have become a dilemma.
[0004] CN105776893A discloses a low-radiation coated glass and a manufacturing process thereof, wherein the low-radiation coated glass comprises a glass substrate and a coating disposed on the surface of the glass substrate, wherein the coating comprises a metal tungsten layer, wherein the thickness of the metal tungsten layer is 2 to 7 nm, and the thickness of the coating is 180 to 220 nm. The low-radiation coated glass is prepared by a sputtering process.
[0005] CN202242181U discloses a large-area tempered coated glass, wherein silicon nitride (SiN x ) layer, metal nickel chromium (NiCr) layer, metal silver (Ag) layer, metal nickel chromium (NiCr) layer, silicon nitride (SiN x The first silicon nitride layer on the float glass substrate has a thickness of 10 to 50 nm, the second metal nickel-chromium layer has a thickness of 3 to 11 nm, the third metal silver layer has a thickness of 3 to 10 nm, the fourth metal nickel-chromium layer has a thickness of 3 to 11 nm, and the fifth silicon nitride layer has a thickness of 30 to 55 nm.
[0006] CN208632388U discloses a tempered one-way perspective glass, comprising a glass substrate, and a first dielectric layer stacked and arranged on one surface of the glass substrate in sequence to reduce the illumination of light emitted from the glass substrate to the metal reflection layer; a metal reflection layer reflecting the light emitted from the first dielectric layer; a second dielectric layer for reducing the transmission of light to achieve a perspective effect; a dielectric protection layer for protecting the second dielectric layer; the material of the first dielectric layer is selected from Si3N4 layer, SiO x Layer, SiO x N x any one of a layer, a TiO2 layer, a ZrO2 layer, and a ZnSnO3 layer; the metal reflective layer is a NiCr layer, a NiC r O x Layer, NiCrN x Layer, C r Layer, C r N x The material of the second dielectric layer is selected from Si3N4 layer, SiO x Layer, SiO x N x any one of a layer, a TiO2 layer, a ZrO2 layer, and a ZnSnO3 layer; the dielectric protection layer is a Si3N4 layer, a SiO x Layer, SiO x N x Any one of layer, TiO2 layer, ZrO2 layer and ZnSnO3 layer.
[0007] In the above-reported glass coating, a silver layer is plated on the glass substrate to obtain a high outdoor visible light reflectivity. However, if there is no protective layer, if the silver layer is directly exposed to the air, oxidation will occur, resulting in failure of the glass mirror. In addition, in order not to damage the coating, the above patent can only perform a heating treatment before plating the functional layer, so it is impossible to realize off-site processing of the glass.
[0008] Therefore, how to improve the outdoor visible light reflectivity of glass by coating the surface of the glass substrate, while solving the problem of not being able to heat the glass after coating the functional layer, that is, to achieve remote processing and manufacturing, has become an urgent problem to be solved. Summary of the invention
[0009] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a mirror glass processed off-site and a preparation method thereof, which can meet the requirements of heat treatment after coating, and the coated film layer after heat treatment will not be oxidized and can be used normally without delamination. At the same time, it is ensured that the outdoor visible light reflectivity of the glass after heat treatment is maintained at a high level.
[0010] To achieve this object, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a mirror glass processed remotely, the mirror glass comprising a glass substrate and a tin liquid surface coating arranged on one side of the tin liquid surface of the glass substrate, the tin liquid surface coating comprising at least two tin liquid surface dielectric layers stacked sequentially from the surface of the glass substrate to the outside, and the refractive index of the tin liquid surface dielectric layer material decreases sequentially from the surface of the glass substrate to the outside.
[0012] The present invention provides a mirror glass processed off-site, in which at least two dielectric layers are plated on a glass substrate on a tin liquid surface, so that the glass can meet a high outdoor visible light reflectivity before heat treatment and can also meet a high outdoor visible light reflectivity after heat treatment. The reflectivity can reach more than 72% and can still maintain a neutral color.
[0013] It should be noted that the glass substrate in the present invention is obtained by the process of forming by the float method, in which molten glass continuously flows from a tank kiln and floats on the surface of a relatively dense tin liquid. Under the action of gravity and surface tension, the molten glass spreads and flattens on the tin liquid surface to form a flat upper and lower surface, hardens, and cools. The tin liquid surface of the glass substrate in the present invention refers to the side where the molten glass contacts and forms the tin liquid during the glass forming process.
[0014] As a preferred technical solution of the present invention, the tin liquid surface dielectric layer includes a first tin liquid surface dielectric layer and a second tin liquid surface dielectric layer stacked in sequence from the surface of the glass substrate to the outside, and the refractive index of the first tin liquid surface dielectric layer is higher than that of the second tin liquid surface dielectric layer.
[0015] Preferably, the material of the first tin liquid level dielectric layer comprises ZnSnO x 、SiN x 、TiO x or ZrO x Any one or a combination of at least two of the following.
[0016] Preferably, the material of the first tin liquid surface dielectric layer is SiN x or ZrO x .
[0017] Preferably, the material of the second tin liquid level dielectric layer comprises SiO x 、AlO x Or any one of MgAl2O4 or a combination of at least two.
[0018] Preferably, the material of the second tin liquid surface dielectric layer is SiO x .
[0019] Preferably, the thickness of the first tin liquid surface dielectric layer is 40-60 nm, more preferably 45-55 nm, for example, it can be 40 nm, 41 nm, 42 nm, 43 nm, 44 nm, 45 nm, 46 nm, 47 nm, 48 nm, 49 nm, 50 nm, 51 nm, 52 nm, 53 nm, 54 nm, 55 nm, 56 nm, 57 nm, 58 nm, 59 nm or 60 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0020] Preferably, the thickness of the second tin liquid surface dielectric layer is 40-60nm, more preferably 40-50nm, for example, it can be 40nm, 41nm, 42nm, 43nm, 44nm, 45nm, 46nm, 47nm, 48nm, 49nm, 50nm, 51nm, 52nm, 53nm, 54nm, 55nm, 56nm, 57nm, 58nm, 59nm or 60nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] As a preferred technical solution of the present invention, the mirror glass also includes an air surface coating arranged on one side of the air surface of the glass substrate, the air surface coating includes a first air surface dielectric layer, a second air surface dielectric layer, a metal layer and a third air surface dielectric layer stacked in sequence from the surface of the glass substrate to the outside, and the refractive index of the air surface dielectric layer material decreases in sequence from the surface of the glass substrate to the outside.
[0022] It should be noted that the glass substrate in the present invention is obtained by the process of forming the glass substrate by the float method, in which the molten glass continuously flows from the tank kiln and floats on the surface of the tin liquid with a relatively high density. Under the action of gravity and surface tension, the molten glass spreads and flattens on the tin liquid surface to form a flat upper and lower surface, hardens, and cools. The air surface of the glass substrate in the present invention refers to the side of the molten glass that is not in contact with the tin liquid and formed during the glass forming process, that is, the opposite side of the tin liquid surface.
[0023] As a preferred technical solution of the present invention, the material of the first air surface dielectric layer includes ZnSnO x 、SiN x 、TiO x or ZrO x Any one or a combination of at least two of the following.
[0024] Preferably, the material of the first air surface dielectric layer is SiN x or ZrO x .
[0025] Preferably, the material of the second air surface dielectric layer comprises SiO x、AlO x Or MgAl2O4, any one or a combination of at least two, more preferably SiO x .
[0026] Preferably, the material of the third air-plane dielectric layer comprises ZnSnO x 、SiN x 、TiO x or ZrO x Any one or a combination of at least two of the above, more preferably SiN x or ZrO x .
[0027] Preferably, the thickness of the first air surface dielectric layer is 45-75nm, and further preferably 55-65nm, for example, it can be 45nm, 46nm, 47nm, 48nm, 49nm, 50nm, 51nm, 52nm, 53nm, 54nm, 55nm, 56nm, 57nm, 58nm, 59nm, 60nm, 61nm, 62nm, 63nm, 64nm, 65nm, 66nm, 67nm, 68nm, 69nm, 70nm, 71nm, 72nm, 73nm, 74nm or 75nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0028] Preferably, the thickness of the second air surface dielectric layer is 60-80nm, further preferably 70-80nm, for example, it can be 60nm, 61nm, 62nm, 63nm, 64nm, 65nm, 66nm, 67nm, 68nm, 69nm, 70nm, 71nm, 72nm, 73nm, 74nm, 75nm, 76nm, 77nm, 78nm, 79nm or 80nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0029] Preferably, the thickness of the third air surface dielectric layer is 110-130nm, further preferably 110-120nm, for example, it can be 110nm, 111nm, 112nm, 113nm, 114nm, 115nm, 116nm, 117nm, 118nm, 119nm, 120nm, 121nm, 122nm, 123nm, 124nm, 125nm, 126nm, 127nm, 128nm, 129nm or 130nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0030] As a preferred technical solution of the present invention, the material of the metal layer includes any one of NiCr, Ti, Cr or Zr, or a combination of at least two of them.
[0031] Preferably, the material of the metal layer is NiCr.
[0032] Preferably, the thickness of the metal layer is 55-70 nm, more preferably 60-70 nm, for example, it can be 55 nm, 56 nm, 57 nm, 58 nm, 59 nm, 60 nm, 61 nm, 62 nm, 63 nm, 64 nm, 65 nm, 66 nm, 67 nm, 68 nm, 69 nm or 70 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] In a second aspect, the present invention provides a method for preparing the mirror glass processed remotely according to the first aspect, the preparation method comprising:
[0034] A sputtering process is used to sequentially sputter a first tin liquid surface dielectric layer and a second tin liquid surface dielectric layer on the tin liquid surface side of the glass substrate, and sequentially sputter a first air surface dielectric layer, a second air surface dielectric layer, a metal layer and a third air surface dielectric layer on the air surface side of the glass substrate.
[0035] The present invention provides a method for preparing mirror glass, which comprises coating at least two dielectric layers on the tin liquid surface of a glass substrate and coating multiple dielectric layers on the air surface, so that the glass can meet a relatively high outdoor visible light reflectivity before heat treatment and can also meet a relatively high outdoor visible light reflectivity after heat treatment, and its reflectivity can reach more than 72% while still maintaining a neutral color.
[0036] As a preferred technical solution of the present invention, the sputtering process of the first tin liquid surface dielectric layer includes: forming the first tin liquid surface dielectric layer by sputtering the surface of the first tin liquid surface target on one side of the tin liquid surface of the glass substrate.
[0037] Preferably, the first tin liquid level target is an AC round target.
[0038] Preferably, the sputtering process of the first tin liquid surface dielectric layer is performed in a mixed atmosphere of argon and nitrogen.
[0039] Preferably, the volume ratio of argon and nitrogen during the sputtering process of the first tin liquid surface dielectric layer is (0.7-1):1, for example, it can be 0.7:1, 0.72:1, 0.74:1, 0.76:1, 0.78:1, 0.8:1, 0.82:1, 0.85:1, 0.86:1, 0.88:1, 0.9:1, 0.92:1, 0.94:1, 0.96:1, 0.98:1 or 1:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] Preferably, the sputtering of the first tin liquid surface target is carried out at a pressure of 1.05×10 -3 ~1.25×10 -3 mbar, for example, 1.05×10 -3 mbar, 1.06×10 -3 mbar, 1.07×10 -3 mbar, 1.08×10 -3 mbar, 1.09×10 -3 mbar, 1.1×10 -3 mbar, 1.11×10 -3 mbar, 1.12×10 -3 mbar, 1.13×10 -3 mbar, 1.14×10 - 3 mbar, 1.15×10 -3 mbar, 1.16×10 -3 mbar, 1.17×10 -3 mbar, 1.18×10 -3 mbar, 1.19×10 -3 mbar, 1.2×10 -3 mbar, 1.21×10 -3 mbar, 1.22×10 -3 mbar, 1.23×10 -3 mbar, 1.24×10 -3 mbar or 1.25×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0041] Preferably, the sputtering thickness of the first tin liquid surface target is 40 to 60 nm, for example, it can be 40 nm, 41 nm, 42 nm, 43 nm, 44 nm, 45 nm, 46 nm, 47 nm, 48 nm, 49 nm, 50 nm, 51 nm, 52 nm, 53 nm, 54 nm, 55 nm, 56 nm, 57 nm, 58 nm, 59 nm or 60 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0042] Preferably, the sputtering process of the second tin liquid level dielectric layer comprises: forming the second tin liquid level dielectric layer by sputtering on the surface of the first tin liquid level dielectric layer through the second tin liquid level target and the third tin liquid level target in sequence.
[0043] Preferably, the second tin liquid level target position and the third tin liquid level target position are both AC round targets.
[0044] Preferably, the sputtering process of the second tin liquid surface dielectric layer is carried out in a mixed atmosphere of argon and oxygen.
[0045] Preferably, the volume ratio of argon and oxygen during the sputtering process of the second tin liquid surface dielectric layer is (3-5):3, for example, it can be 3:3, 3.1:3, 3.2:3, 3.3.:3, 3.4:3, 3.5:3, 3.6:3, 3.7:3, 3.8:3, 3.9:3, 4:3, 4.1:3, 4.2:3, 4.3:3, 4.4:3, 4.5:3, 4.6:3, 4.7:3, 4.8:3, 4.9:3 or 5:3, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0046] Preferably, the sputtering of the second tin liquid surface target is carried out at a pressure of 1.4×10 -3 ~1.5×10 -3 mbar, for example, 1.4×10 -3 mbar, 1.41×10 -3 mbar, 1.42×10 -3 mbar, 1.43×10 -3 mbar, 1.44×10 -3 mbar, 1.45×10 -3 mbar, 1.46×10 -3 mbar, 1.47×10 -3 mbar, 1.48×10 -3 mbar, 1.49×10 - 3 mbar or 1.5×10 -3mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0047] Preferably, the sputtering of the third tin liquid level target is carried out at a pressure of 2.5×10 -3 ~2.7×10 -3 mbar. For example, it can be 2.5×10 -3 mbar, 2.51×10 -3 mbar, 2.52×10 -3 mbar, 2.53×10 -3 mbar, 2.54×10 -3 mbar, 2.55×10 -3 mbar, 2.56×10 -3 mbar, 2.57×10 -3 mbar, 2.58×10 -3 mbar, 2.59×10 - 3 mbar, 2.6×10 -3 mbar, 2.61×10 -3 mbar, 2.62×10 -3 mbar, 2.63×10 -3 mbar, 2.64×10 -3 mbar, 2.65×10 -3 mbar, 2.66×10 -3 mbar, 2.67×10 -3 mbar, 2.68×10 -3 mbar, 2.69×10 -3 mbar or 2.7×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0048] Preferably, the sputtering thickness of the second tin liquid level target and the third tin liquid level target are independently selected from 20 to 30 nm, for example, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm or 30 nm, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] It should be noted that the sputtering thicknesses of the second tin liquid level target position and the third tin liquid level target position in the sputtering of the second tin liquid level dielectric layer in the method for preparing mirror glass processed off-site provided by the present invention can be the same or different.
[0050] As a preferred technical solution of the present invention, the sputtering process of the first air surface dielectric layer includes: sputtering on the air surface side of the glass substrate through the first air surface target position and the second air surface target position in sequence to form the first air surface dielectric layer.
[0051] Preferably, the first air surface target position and the second air surface target position are both AC round targets.
[0052] Preferably, the sputtering process of the first air-side dielectric layer is carried out in a mixed atmosphere of argon and nitrogen.
[0053] Preferably, the volume ratio of argon and nitrogen during the sputtering process of the first air surface dielectric layer is (0.7-1):1, for example, it can be 0.7:1, 0.72:1, 0.74:1, 0.76:1, 0.78:1, 0.8:1, 0.82:1, 0.84:1, 0.86:1, 0.88:1, 0.9:1, 0.92:1, 0.94:1, 0.96:1, 0.98:1 or 1:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] Preferably, the sputtering of the first air surface target is carried out at a pressure of 1.05×10 -3 ~1.25×10 -3 mbar, for example, 1.05×10 -3 mbar, 1.06×10 -3 mbar, 1.07×10 -3 mbar, 1.08×10 -3 mbar, 1.09×10 -3 mbar, 1.1×10 -3 mbar, 1.11×10 -3 mbar, 1.12×10 -3 mbar, 1.13×10 -3 mbar, 1.14×10 - 3 mbar, 1.15×10 -3 mbar, 1.16×10 -3 mbar, 1.17×10 -3 mbar, 1.18×10 -3 mbar, 1.19×10 -3 mbar, 1.2×10 -3 mbar, 1.21×10 -3 mbar, 1.22×10 -3 mbar, 1.23×10 -3 mbar, 1.24×10-3 mbar or 1.25×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0055] Preferably, the sputtering of the second air surface target is carried out at a pressure of 3.5×10 -3 ~4×10 -3 mbar, for example, 3.5×10 -3 mbar, 3.52×10 -3 mbar, 3.56×10 -3 mbar, 3.6×10 -3 mbar, 3.62×10 - 3 mbar, 3.67×10 -3 mbar, 3.7×10 -3 mbar, 3.72×10 -3 mbar, 3.76×10 -3 mbar, 3.8×10 -3 mbar, 3.82×10 -3 mbar, 3.86×10 -3 mbar, 3.9×10 -3 mbar, 3.92×10 -3 mbar, 3.94×10 -3 mbar, 3.98×10 -3 mbar or 4×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0056] Preferably, the sputtering thickness of the first air surface target and the second air surface target are both 20 to 40 nm, for example, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, 31 nm, 32 nm, 33 nm, 34 nm, 35 nm, 36 nm, 37 nm, 38 nm, 39 nm or 40 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0057] It should be noted that in the method for preparing mirror glass processed off-site provided by the present invention, the sputtering thicknesses of the first air surface target position and the second air surface target position in the sputtering of the first air surface dielectric layer can be the same or different.
[0058] Preferably, the sputtering process of the second air surface dielectric layer comprises: sputtering on the surface of the first air surface dielectric layer through a third air surface target position, a fourth air surface target position and a fifth air surface target position in sequence to form the second air surface dielectric layer.
[0059] Preferably, the third air surface target position, the fourth air surface target position and the fifth air surface target position are AC round targets.
[0060] Preferably, the sputtering process of the second air-side dielectric layer is carried out in a mixed atmosphere of argon and oxygen.
[0061] Preferably, the volume ratio of argon and oxygen during the sputtering process of the second air surface dielectric layer is (3-5):3, for example, it can be 3:3, 3.1:3, 3.2:3, 3.3.:3, 3.4:3, 3.5:3, 3.6:3, 3.7:3, 3.8:3, 3.9:3, 4:3, 4.1:3, 4.2:3, 4.3:3, 4.4:3, 4.5:3, 4.6:3, 4.7:3, 4.8:3, 4.9:3 or 5:3, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0062] Preferably, the sputtering of the third air surface target is carried out at a pressure of 2.5×10 -3 ~3×10 -3 mbar, for example, it can be 2.5×10 -3 mbar, 2.53×10 -3 mbar, 2.57×10 -3 mbar, 2.6×10 -3 mbar, 2.63×10 - 3 mbar, 2.67×10 -3 mbar, 2.7×10 -3 mbar, 2.73×10 -3 mbar, 2.75×10 -3 mbar, 2.78×10 -3 mbar, 2.8×10 -3 mbar, 2.84×10 -3 mbar, 2.88×10 -3 mbar, 2.9×10 -3 mbar, 2.94×10 -3 mbar, 2.97×10 -3 mbar or 3×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0063] Preferably, the sputtering of the fourth air surface target is carried out at a pressure of 4×10 -3 ~4.5×10 -3 mbar, for example, it can be 4.04×10 -3 mbar, 4.08×10 -3 mbar, 4.1×10 -3 mbar, 4.13×10 -3 mbar, 4.17×10 - 3 mbar, 4.2×10 -3 mbar, 4.22×10 -3 mbar, 4.26×10 -3 mbar, 4.28×10 -3 mbar, 4.3×10 -3 mbar, 4.33×10 -3 mbar, 4.37×10 -3 mbar, 4.4×10 -3 mbar, 4.42×10 -3 mbar, 4.44×10 -3 mbar, 4.48×10 -3 mbar or 4.5×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0064] Preferably, the sputtering of the fifth air surface target is carried out at a pressure of 2.5×10 -3 ~3×10 -3 mbar, for example, it can be 2.5×10 -3 mbar, 2.53×10 -3 mbar, 2.57×10 -3 mbar, 2.6×10 -3 mbar, 2.63×10 - 3 mbar, 2.67×10 -3 mbar, 2.7×10 -3 mbar, 2.73×10 -3 mbar, 2.75×10 -3 mbar, 2.78×10 -3 mbar, 2.8×10 -3 mbar, 2.84×10 -3 mbar, 2.88×10 -3 mbar, 2.9×10 -3mbar, 2.94×10 -3 mbar, 2.97×10 -3 mbar or 3×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0065] Preferably, the sputtering thickness of the third air surface target, the fourth air surface target and the fifth air surface target are all 20 to 40 nm, for example, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, 31 nm, 32 nm, 33 nm, 34 nm, 35 nm, 36 nm, 37 nm, 38 nm, 39 nm or 40 nm, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0066] It should be noted that the sputtering thicknesses of the third air surface target position, the fourth air surface target position and the fifth air surface target position in the sputtering of the second air surface dielectric layer in the method for preparing mirror glass processed off-site provided by the present invention can be the same or different.
[0067] As a preferred technical solution of the present invention, the sputtering process of the metal layer includes: forming the metal layer by sputtering on the surface of the second air surface dielectric layer through the first metal target, the second metal target and the third metal target in sequence.
[0068] Preferably, the first metal target, the second metal target and the third metal target are all DC flat targets.
[0069] Preferably, the sputtering process of the metal layer is carried out under pure argon gas.
[0070] Preferably, the sputtering of the first metal target is carried out at a pressure of 1.5×10 -3 ~2×10 -3 mbar, for example, 1.5×10 -3 mbar, 1.52×10 -3 mbar, 1.57×10 -3 mbar, 1.6×10 -3 mbar, 1.63×10 - 3 mbar, 1.67×10 -3 mbar, 1.7×10 -3 mbar, 1.73×10 -3 mbar, 1.75×10 -3 mbar, 1.78×10 -3 mbar, 1.8×10-3 mbar, 1.84×10 -3 mbar, 1.88×10 -3 mbar, 1.9×10 -3 mbar, 1.94×10 -3 mbar, 1.97×10 -3 mbar or 2×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0071] Preferably, the sputtering of the second metal target is carried out at a pressure of 2.5×10 -3 ~3×10 -3 mbar, for example, it can be 2.5×10 -3 mbar, 2.53×10 -3 mbar, 2.57×10 -3 mbar, 2.6×10 -3 mbar, 2.63×10 - 3 mbar, 2.67×10 -3 mbar, 2.7×10 -3 mbar, 2.73×10 -3 mbar, 2.75×10 -3 mbar, 2.78×10 -3 mbar, 2.8×10 -3 mbar, 2.83×10 -3 mbar, 2.88×10 -3 mbar, 2.9×10 -3 mbar, 2.94×10 -3 mbar, 2.97×10 -3 mbar or 3×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0072] Preferably, the sputtering of the third metal target is carried out at a pressure of 4.5×10 -3 ~5×10 -3 mbar, for example, 4.5×10 -3 mbar, 4.53×10 -3 mbar, 4.57×10 -3 mbar, 4.6×10 -3 mbar, 4.63×10 - 3 mbar, 4.66×10-3 mbar, 4.68×10 -3 mbar, 4.7×10 -3 mbar, 4.73×10 -3 mbar, 4.77×10 -3 mbar, 4.8×10 -3 mbar, 4.84×10 -3 mbar, 4.88×10 -3 mbar, 4.9×10 -3 mbar, 4.94×10 -3 mbar, 4.98×10 -3 mbar or 5×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0073] Preferably, the sputtering thickness of the first metal target, the second metal target and the third metal target are all 18 to 24 nm, for example, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm or 24 nm, but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0074] It should be noted that in the method for preparing mirror glass processed off-site provided by the present invention, the sputtering thicknesses of the first metal target, the second metal target and the third metal target in the metal layer sputtering can be the same or different.
[0075] As a preferred technical solution of the present invention, the sputtering process of the third air surface dielectric layer includes: sputtering on the surface of the metal layer through the sixth air surface target position, the seventh air surface target position and the eighth air surface target position in sequence to form the third air surface dielectric layer.
[0076] Preferably, the sixth air surface target position, the seventh air surface target position and the eighth air surface target position are all AC round targets.
[0077] Preferably, the sputtering process of the third air-plane dielectric layer is carried out in a mixed atmosphere of argon and nitrogen.
[0078] Preferably, the volume ratio of argon and nitrogen during the sputtering process of the third air surface dielectric layer is (0.7-1):1, for example, it can be 0.7:1, 0.72:1, 0.74:1, 0.76:1, 0.78:1, 0.8:1, 0.82:1, 0.85:1, 0.86:1, 0.88:1, 0.9:1, 0.92:1, 0.94:1, 0.96:1, 0.98:1 or 1:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0079] Preferably, the sputtering of the sixth air surface target is carried out at a pressure of 3.5×10 -3 ~4×10 -3 mbar, for example, 3.5×10 -3 mbar, 3.52×10 -3 mbar, 3.56×10 -3 mbar, 3.6×10 -3 mbar, 3.62×10 - 3 mbar, 3.67×10 -3 mbar, 3.7×10 -3 mbar, 3.72×10 -3 mbar, 3.76×10 -3 mbar, 3.8×10 -3 mbar, 3.82×10 -3 mbar, 3.86×10 -3 mbar, 3.9×10 -3 mbar, 3.92×10 -3 mbar, 3.94×10 -3 mbar, 3.98×10 -3 mbar or 4×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0080] Preferably, the sputtering of the seventh air surface target is carried out at a pressure of 1.5×10 -3 ~2×10 -3 mbar, for example, 1.5×10 -3 mbar, 1.52×10 -3 mbar, 1.57×10 -3 mbar, 1.6×10 -3 mbar, 1.63×10 - 3 mbar, 1.67×10 -3 mbar, 1.7×10 -3 mbar, 1.73×10 -3 mbar, 1.75×10 -3 mbar, 1.78×10 -3 mbar, 1.8×10 -3 mbar, 1.84×10 -3 mbar, 1.88×10 -3 mbar, 1.9×10-3 mbar, 1.94×10 -3 mbar, 1.97×10 -3 mbar or 2×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0081] Preferably, the sputtering of the eighth air surface target is carried out at a pressure of 3.5×10 -3 ~4×10 -3 mbar, for example, 3.5×10 -3 mbar, 3.52×10 -3 mbar, 3.56×10 -3 mbar, 3.6×10 -3 mbar, 3.62×10 - 3 mbar, 3.67×10 -3 mbar, 3.7×10 -3 mbar, 3.72×10 -3 mbar, 3.76×10 -3 mbar, 3.8×10 -3 mbar, 3.82×10 -3 mbar, 3.86×10 -3 mbar, 3.9×10 -3 mbar, 3.92×10 -3 mbar, 3.94×10 -3 mbar, 3.98×10 -3 mbar or 4×10 -3 mbar, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0082] Preferably, the sputtering thickness of the sixth air surface target, the seventh air surface target and the eighth air surface target are all 36 to 47 nm, for example, 36 nm, 37 nm, 38 nm, 39 nm, 40 nm, 41 nm, 42 nm, 43 nm, 44 nm, 45 nm, 46 nm or 47 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0083] It should be noted that the sputtering thicknesses of the sixth air surface target position, the seventh air surface target position and the eighth air surface target position in the sputtering of the third air surface dielectric layer in the method for preparing mirror glass processed off-site provided by the present invention can be the same or different.
[0084] Compared with the prior art, the present invention has the following beneficial effects:
[0085] The present invention provides a mirror glass processed off-site and a preparation method thereof. At least two dielectric layers are plated on a glass substrate on a tin liquid surface, so that the glass can meet a high outdoor visible light reflectivity before heat treatment and can also meet a high outdoor visible light reflectivity after heat treatment. The reflectivity can reach more than 72%, and at the same time, a neutral color can still be maintained. BRIEF DESCRIPTION OF THE DRAWINGS
[0086] Figure 1 A structural diagram of a mirror glass dielectric layer provided for a specific embodiment of the present invention.
[0087] Among them, 1 is a glass substrate; 2 is a first tin liquid surface dielectric layer; 3 is a second tin liquid surface dielectric layer; 4 is a first air surface dielectric layer; 5 is a second air surface dielectric layer; 6 is a metal layer; and 7 is a third air surface dielectric layer. DETAILED DESCRIPTION
[0088] It should be understood that, in the description of the present invention, the terms "upper", "lower", "front", "back", "bottom", "inside", "outside", etc. indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", etc. are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, features defined as "first", "second", etc. may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0089] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0090] In a specific embodiment, the present invention provides a mirror glass processed in a different place, such as Figure 1 As shown, the mirror glass includes a glass substrate 1 and a first tin liquid surface dielectric layer 2 and a second tin liquid surface dielectric layer 3 arranged on the tin liquid surface side of the glass substrate 1, and a first air surface dielectric layer 4, a second air surface dielectric layer 5, a metal layer 6 and a third air surface dielectric layer 7 arranged on the air surface side of the glass substrate 1 and stacked in sequence from the surface of the glass substrate 1 to the outside.
[0091] The material of the first tin liquid surface dielectric layer 2 is ZnSnO x 、SiN x 、TiO x or ZrO xAny one or a combination of at least two of the above, with a thickness of 40 to 60 nm, and the material of the second tin liquid surface dielectric layer 3 is SiO x 、AlO x or MgAl2O4, any one or a combination of at least two thereof, with a thickness of 40 to 60 nm, and the material of the first air surface dielectric layer 4 is ZnSnO x 、SiN x 、TiO x or ZrO x Any one or a combination of at least two of the above, with a thickness of 45 to 75 nm, and the material of the second air surface dielectric layer 5 is SiO x 、AlO x or MgAl2O4, any one or a combination of at least two thereof, with a thickness of 60 to 80 nm; the material of the metal layer 6 is any one or a combination of at least two thereof, with a thickness of 55 to 70 nm; the material of the third air surface dielectric layer 7 is ZnSnO x 、SiN x 、TiO x or ZrO x Any one or a combination of at least two of the following or ZrO x , thickness is 110~130nm.
[0092] In another specific embodiment, the present invention provides a method for preparing the mirror glass provided in a specific embodiment, the preparation method comprising:
[0093] A sputtering process is used to sequentially sputter a first tin liquid surface dielectric layer 2 and a second tin liquid surface dielectric layer 3 on the tin liquid surface side of the glass substrate 1, and sequentially sputter a first air surface dielectric layer 4, a second air surface dielectric layer 5, a metal layer 6 and a third air surface dielectric layer 7 on the air surface side of the glass substrate 1. The preparation method specifically comprises the following steps:
[0094] (1) A first tin liquid surface target is sputtered on a surface of a glass substrate 1 on one side of the tin liquid surface to form a first tin liquid surface dielectric layer 2, wherein the first tin liquid surface target is an AC round target in a mixed atmosphere of argon and nitrogen with a volume ratio of (0.7 to 1):1 and a gas pressure range of 1.05×10 -3 ~1.25×10 -3 mbar conditions, the sputtering thickness of the first tin liquid surface target position is 40-60nm;
[0095] (2) The second tin liquid level target position and the third tin liquid level target position are sequentially sputtered on the surface of the first tin liquid level dielectric layer 2 to form a second tin liquid level dielectric layer 3, wherein the second tin liquid level target position and the third tin liquid level target position are AC round targets, and in a mixed atmosphere of argon and oxygen with a volume ratio of (3 to 5):3, the sputtering of the second tin liquid level target position is carried out at a pressure of 1.4×10 -3 ~1.5×10 -3 The sputtering of the third tin liquid surface target was carried out at a pressure of 2.5×10 -3 ~2.7×10 -3 mbar, the sputtering thickness of the second tin liquid level target and the third tin liquid level target is 20-30nm;
[0096] (3) The first air surface target and the second air surface target are sequentially sputtered on the air surface side of the glass substrate 1 to form a first air surface dielectric layer, wherein the first air surface target and the second air surface target are AC round targets, and the sputtering of the first air surface target is carried out in a mixed atmosphere of argon and nitrogen with a volume ratio of (0.7 to 1):1 at a pressure of 1.05×10 -3 ~1.25×10 -3 The sputtering of the second air surface target was carried out at a pressure of 3.5×10 -3 ~4×10 -3 mbar, the sputtering thickness of the first air surface target and the second air surface target is 20-40nm;
[0097] (4) The second air surface dielectric layer is formed by sputtering on the surface of the first air surface dielectric layer 4 in sequence through the third air surface target position, the fourth air surface target position and the fifth air surface target position, wherein the third air surface target position, the fourth air surface target position and the fifth air surface target position are AC round targets, in a mixed atmosphere of argon and oxygen with a volume ratio of (3 to 5):3, wherein the sputtering of the third air surface target position is at a pressure of 2.5×10 -3 ×10 -3 The sputtering was carried out at a pressure of 4×10 -3 ~4.5×10 -3 The sputtering was carried out at a pressure of 2.5×10 -3 ~3×10 -3 The sputtering was performed at 20 mbar, and the sputtering thicknesses of the third air surface target position, the fourth air surface target position and the fifth air surface target position were all 20-40 nm.
[0098] (5) Under the condition of pure argon gas, the metal layer 6 is formed by sputtering the surface of the second air surface dielectric layer 5 through the first metal target, the second metal target and the third metal target in sequence, wherein the first metal target, the second metal target and the third metal target are DC flat targets, and the sputtering of the first metal target is carried out at a pressure of 1.5×10 -3 ~2×10 -3 The sputtering of the second metal target was carried out at a pressure of 2.5×10 -3 ~3×10 -3 The sputtering of the third metal target was carried out at a pressure of 4.5×10 -3 ~5×10 -3 Sputtering was performed at 100 mbar, and the sputtering thickness of the first metal target, the second metal target, and the third metal target were all 18 to 24 nm;
[0099] (6) A third air surface dielectric layer is formed on the surface of the metal layer 6 by sputtering at the sixth air surface target position, the seventh air surface target position and the eighth air surface target position in sequence, wherein the sixth air surface target position, the seventh air surface target position and the eighth air surface target position are AC round targets, and a mixed gas of argon and nitrogen with a volume ratio of (0.7-1):1 is introduced, wherein the sputtering at the sixth air surface target position is at a pressure of 3.5×10 -3 ~4×10 -3 The sputtering of the seventh air surface target was carried out at a pressure of 1.5×10 -3 ~2×10 -3 The sputtering of the eighth air surface target was carried out at a pressure of 3.5×10 -3 ~4×10 -3 The process was carried out at 100 mbar, and the sputtering thicknesses of the sixth air surface target position, the seventh air surface target position and the eighth air surface target position were all 36-47 nm.
[0100] Example 1
[0101] In this embodiment, a mirror glass processed remotely is provided, wherein the mirror glass comprises a glass substrate 1 and a first tin liquid surface dielectric layer 2 and a second tin liquid surface dielectric layer 3 arranged on the tin liquid surface side of the glass substrate, and a first air surface dielectric layer 4, a second air surface dielectric layer 5, a metal layer 6 and a third air surface dielectric layer 7 arranged on the air surface side of the glass substrate and stacked in sequence from the surface of the glass substrate to the outside.
[0102] The material of the first tin liquid level dielectric layer 2 is SiN x , with a thickness of 40nm, and the material of the second tin liquid surface dielectric layer 3 is SiO x , with a thickness of 40nm, the material of the first air surface dielectric layer 4 is SiN x, with a thickness of 45 nm, and the material of the second air surface dielectric layer 5 is SiO x , thickness is 60nm, the material of the metal layer 6 is NiCr, thickness is 55nm, the material of the third air surface dielectric layer 7 is SiN x , with a thickness of 110nm.
[0103] This embodiment also provides a method for preparing the mirror glass. The mirror glass is prepared by the preparation method provided in the specific implementation manner. The process parameters used for each target position are shown in Table 1:
[0104] Table 1
[0105]
[0106] Example 2
[0107] The present embodiment provides a mirror glass processed remotely, the mirror glass comprising a glass substrate 1 and a first tin liquid surface dielectric layer 2 and a second tin liquid surface dielectric layer 3 arranged on the tin liquid surface side of the glass substrate, and a first air surface dielectric layer 4, a second air surface dielectric layer 5, a metal layer 6 and a third air surface dielectric layer 7 arranged on the air surface side of the glass substrate and stacked in sequence from the surface of the glass substrate to the outside.
[0108] The material of the first tin liquid surface dielectric layer 2 is ZnSnO x , with a thickness of 45nm, and the material of the second tin liquid surface dielectric layer 3 is AlO x , with a thickness of 46nm, and the material of the first air surface dielectric layer 4 is ZnSnO x , with a thickness of 55nm, and the material of the second air surface dielectric layer 5 is AlO x , thickness is 65nm, the material of the metal layer 6 is Ti, thickness is 60nm, the material of the third air surface dielectric layer 7 is ZnSnO x , thickness is 116nm.
[0109] This embodiment also provides a method for preparing the mirror glass. The mirror glass is prepared by the preparation method provided in the specific implementation manner. The process parameters used for each target position are shown in Table 2:
[0110] Table 2
[0111]
[0112] Example 3
[0113] In this embodiment, a mirror glass processed remotely is provided, wherein the mirror glass comprises a glass substrate 1 and a first tin liquid surface dielectric layer 2 and a second tin liquid surface dielectric layer 3 arranged on the tin liquid surface side of the glass substrate, and a first air surface dielectric layer 4, a second air surface dielectric layer 5, a metal layer 6 and a third air surface dielectric layer 7 arranged on the air surface side of the glass substrate and stacked in sequence from the surface of the glass substrate to the outside.
[0114] The material of the first tin liquid surface dielectric layer 2 is TiO x , with a thickness of 50nm, the material of the second tin liquid surface dielectric layer 3 is MgAl2O4, with a thickness of 50nm, and the material of the first air surface dielectric layer 4 is TiO x , thickness is 60nm, the material of the second air surface dielectric layer 5 is MgAl2O4, thickness is 70nm, the material of the metal layer 6 is Cr, thickness is 64nm, the material of the third air surface dielectric layer 7 is TiO x , thickness is 120nm.
[0115] This embodiment also provides a method for preparing the mirror glass. The mirror glass is prepared by the preparation method provided in the specific implementation manner. The process parameters used for each target position are shown in Table 3:
[0116] Table 3
[0117]
[0118]
[0119] Example 4
[0120] In this embodiment, a mirror glass processed remotely is provided, wherein the mirror glass comprises a glass substrate 1 and a first tin liquid surface dielectric layer 2 and a second tin liquid surface dielectric layer 3 arranged on the tin liquid surface side of the glass substrate, and a first air surface dielectric layer 4, a second air surface dielectric layer 5, a metal layer 6 and a third air surface dielectric layer 7 arranged on the air surface side of the glass substrate and stacked in sequence from the surface of the glass substrate to the outside.
[0121] The material of the first tin liquid surface medium 2 layer is ZrO x , with a thickness of 60nm, and the material of the second tin liquid surface dielectric layer 3 is SiO x , with a thickness of 60nm, and the material of the first air surface dielectric layer 4 is ZrO x , with a thickness of 75nm, and the material of the second air surface dielectric layer 5 is SiO x , with a thickness of 80nm, the material of the metal layer 6 is Zr, with a thickness of 70nm, and the material of the third air surface dielectric layer 7 is ZrO x , thickness is 130nm.
[0122] This embodiment also provides a method for preparing the mirror glass. The mirror glass is prepared by the preparation method provided in the specific implementation manner. The process parameters used for each target position are shown in Table 4:
[0123] Table 4
[0124]
[0125]
[0126] Comparative Example 1
[0127] This comparative example provides a mirror-coated glass, which is different from Example 1 in that the first tin liquid surface dielectric layer 2 and the second tin liquid surface dielectric layer 3 are not provided on the tin liquid surface side of the glass substrate 1, and the rest of the structure is the same as that of Example 1.
[0128] Comparative Example 2
[0129] This comparative example provides a mirror-coated glass, which is different from Example 1 in that: the first tin liquid surface dielectric layer 2 is not provided on the tin liquid surface side of the glass substrate 1, and the rest of the structure is the same as that of Example 1.
[0130] Performance Test:
[0131] Under the same conditions, the optical properties of the mirror-coated glass described in Example 1, Comparative Example 1 and Comparative Example 2 before and after the heating treatment were tested. The results are shown in Table 5:
[0132] Table 5
[0133]
[0134]
[0135] Wherein, T (%) represents the transmittance of the composite glass (%), a * Indicates the red and green values of outdoor reflection of composite glass, b * Indicates the yellow-blue value of outdoor reflection of composite glass, R g Indicates the outdoor visible light reflectance of composite glass (%), R f Indicates the indoor visible light reflectance of composite glass (%).
[0136] From the results provided in Table 5, it can be seen that the outdoor visible light reflectance of the mirror glass plated on the tin liquid surface and the air surface of the glass substrate in Examples 1 to 4 reaches 72%, while the reflectance of the mirror glass currently used in the market is less than 70%, and after the mirror glass provided in the examples is heated, it also meets the high outdoor visible light reflectance and still maintains a neutral color. Under the same conditions, the outdoor reflectance of the mirror glass in Example 1 is greatly improved, and the difference in reflectance and light transmission color before and after heating the glass is very small, and the neutral color can still be maintained, which can be recognized by the market.
[0137] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A mirror glass processed in a different place, characterized in that: The mirror glass comprises a glass substrate and a tin liquid surface coating disposed on one side of the tin liquid surface of the glass substrate, wherein the tin liquid surface coating comprises at least two tin liquid surface dielectric layers sequentially stacked from the surface of the glass substrate outward, and the refractive index of the tin liquid surface dielectric layer material decreases sequentially from the surface of the glass substrate outward; The tin liquid surface dielectric layer comprises a first tin liquid surface dielectric layer and a second tin liquid surface dielectric layer sequentially stacked from the surface of the glass substrate outward, and the refractive index of the first tin liquid surface dielectric layer is higher than that of the second tin liquid surface dielectric layer; The material of the first tin liquid surface dielectric layer includes ZnSnO x 、SiN x 、TiO x or ZrO x Any one or a combination of at least two of the following: The material of the second tin liquid surface dielectric layer includes SiO x 、AlO x or MgAl2O4, any one or a combination of at least two; The mirror glass also includes an air surface coating arranged on one side of the air surface of the glass substrate, and the air surface coating includes a first air surface dielectric layer, a second air surface dielectric layer, a metal layer and a third air surface dielectric layer stacked in sequence from the surface of the glass substrate to the outside.
2. The mirror glass according to claim 1, characterized in that: The material of the first tin liquid surface dielectric layer is SiN x or ZrO x .
3. The mirror glass according to claim 1, characterized in that: The material of the second tin liquid surface dielectric layer is SiO x .
4. The mirror glass according to claim 1, characterized in that: The thickness of the first tin liquid surface dielectric layer is 40-60 nm.
5. The mirror glass according to claim 4, characterized in that: The thickness of the first tin liquid surface dielectric layer is 45-55 nm.
6. The mirror glass according to claim 1, characterized in that: The thickness of the second tin liquid surface dielectric layer is 40-60 nm.
7. The mirror glass according to claim 6, characterized in that: The thickness of the second tin liquid surface dielectric layer is 40-50 nm.
8. The mirror glass according to claim 1, characterized in that: The material of the first air surface dielectric layer includes ZnSnO x 、SiN x 、TiO x or ZrO x Any one or a combination of at least two of the following.
9. The mirror glass according to claim 8, characterized in that: The material of the first air surface dielectric layer is SiN x or ZrO x .
10. The mirror glass according to claim 1, characterized in that: The material of the second air surface dielectric layer includes SiO x 、AlO x Or any one of MgAl2O4 or a combination of at least two.
11. The mirror glass according to claim 10, characterized in that: The material of the second air surface dielectric layer is SiO x .
12. The mirror glass according to claim 1, characterized in that: The material of the third air surface dielectric layer includes ZnSnO x 、SiN x 、TiO x or ZrO x Any one or a combination of at least two of the following.
13. The mirror glass according to claim 12, characterized in that: The material of the third air surface dielectric layer is SiN x or ZrO x .
14. The mirror glass according to claim 1, characterized in that: The thickness of the first air-side dielectric layer is 45-75 nm.
15. The mirror glass according to claim 14, characterized in that: The thickness of the first air-side dielectric layer is 55-65 nm.
16. The mirror glass according to claim 1, characterized in that: The thickness of the second air-side dielectric layer is 60-80 nm.
17. The mirror glass according to claim 16, characterized in that: The thickness of the second air-side dielectric layer is 70-80 nm.
18. The mirror glass according to claim 1, characterized in that: The thickness of the third air-plane dielectric layer is 110-130 nm.
19. The mirror glass according to claim 18, characterized in that: The thickness of the third air-plane dielectric layer is 110-120 nm.
20. The mirror glass according to claim 1, characterized in that: The material of the metal layer includes any one of NiCr, Ti, Cr or Zr, or a combination of at least two of them.
21. The mirror glass according to claim 20, characterized in that: The material of the metal layer is NiCr.
22. The mirror glass according to claim 1, characterized in that: The thickness of the metal layer is 55-70 nm.
23. The mirror glass according to claim 22, characterized in that: The thickness of the metal layer is 60-70 nm.
24. A method for preparing the mirror glass according to any one of claims 1 to 23, characterized in that: The preparation method comprises: A sputtering process is used to sequentially sputter a first tin liquid surface dielectric layer and a second tin liquid surface dielectric layer on the tin liquid surface side of the glass substrate, and sequentially sputter a first air surface dielectric layer, a second air surface dielectric layer, a metal layer and a third air surface dielectric layer on the air surface side of the glass substrate.
25. The method for preparing mirror glass according to claim 24, characterized in that: The sputtering process of the first tin liquid surface dielectric layer includes: using a first tin liquid surface target to sputter on the surface of a glass substrate on one side of the tin liquid surface to form the first tin liquid surface dielectric layer.
26. The method for preparing mirror glass according to claim 25, characterized in that: The first tin liquid level target position is an AC round target.
27. The method for preparing mirror glass according to claim 25, characterized in that: The sputtering process of the first tin liquid surface dielectric layer is carried out in a mixed atmosphere of argon and nitrogen.
28. The method for preparing mirror glass according to claim 27, characterized in that: During the sputtering process of the first tin liquid surface dielectric layer, the volume ratio of argon gas to nitrogen gas is (0.7-1):
1.
29. The method for preparing mirror glass according to claim 25, characterized in that: The sputtering of the first tin liquid surface target position is carried out at a pressure of 1.05×10 -3 ~1.25×10 -3 mbar.
30. The method for preparing mirror glass according to claim 25, characterized in that: The sputtering thickness of the first tin liquid surface target is 40-60 nm.
31. The method for preparing mirror glass according to claim 24, characterized in that: The sputtering process of the second tin liquid level dielectric layer includes: sputtering on the surface of the first tin liquid level dielectric layer through the second tin liquid level target position and the third tin liquid level target position in sequence to form the second tin liquid level dielectric layer.
32. The method for preparing mirror glass according to claim 31, characterized in that: The second tin liquid level target position and the third tin liquid level target position are both AC round targets.
33. The method for preparing mirror glass according to claim 31, characterized in that: The sputtering process of the second tin liquid surface dielectric layer is carried out in a mixed atmosphere of argon and oxygen.
34. The method for preparing mirror glass according to claim 33, characterized in that: The volume ratio of argon gas to oxygen gas during the sputtering process of the second tin liquid surface dielectric layer is (3-5):
3.
35. The method for preparing mirror glass according to claim 31, characterized in that: The sputtering of the second tin liquid surface target position is carried out at a pressure of 1.4×10 -3 ~1.5×10 -3 mbar.
36. The method for preparing mirror glass according to claim 31, characterized in that: The sputtering of the third tin liquid surface target position is carried out at a pressure of 2.5×10 -3 ~2.7×10 -3 mbar.
37. The method for preparing mirror glass according to claim 31, characterized in that: The sputtering thickness of the second tin liquid level target position and the third tin liquid level target position are independently selected from 20 to 30 nm.
38. The method for preparing mirror glass according to claim 24, characterized in that: The sputtering process of the first air surface dielectric layer includes: forming the first air surface dielectric layer by sputtering on the air surface side of the glass substrate through the first air surface target position and the second air surface target position in sequence.
39. The method for preparing mirror glass according to claim 38, characterized in that: The first air surface target position and the second air surface target position are AC round targets.
40. The method for preparing mirror glass according to claim 38, characterized in that: The sputtering process of the first air-side dielectric layer is carried out in a mixed atmosphere of argon and nitrogen.
41. The method for preparing mirror glass according to claim 40, characterized in that: During the sputtering process of the first air surface dielectric layer, the volume ratio of argon gas to nitrogen gas is (0.7-1):
1.
42. The method for preparing mirror glass according to claim 38, characterized in that: The sputtering of the first air surface target position is carried out at a pressure of 1.05×10 -3 ~1.25×10 -3 mbar.
43. The method for preparing mirror glass according to claim 38, characterized in that: The sputtering of the second air surface target position is carried out at a pressure of 3.5×10 -3 ~4×10 -3 mbar.
44. The method for preparing mirror glass according to claim 38, characterized in that: The sputtering thickness of the first air surface target and the second air surface target are independently selected from 20 to 40 nm.
45. The method for preparing mirror glass according to claim 24, characterized in that: The sputtering process of the second air surface dielectric layer includes: sputtering on the surface of the first air surface dielectric layer through the third air surface target position, the fourth air surface target position and the fifth air surface target position in sequence to form the second air surface dielectric layer.
46. The method for preparing mirror glass according to claim 45, characterized in that: The third air surface target position, the fourth air surface target position and the fifth air surface target position are AC round targets.
47. The method for preparing mirror glass according to claim 45, characterized in that: The sputtering process of the second air-side dielectric layer is carried out in a mixed atmosphere of argon and oxygen.
48. The method for preparing mirror glass according to claim 47, characterized in that: The volume ratio of argon to oxygen during the sputtering process of the second air surface dielectric layer is (3-5):
3.
49. The method for preparing mirror glass according to claim 45, characterized in that: The sputtering of the third air surface target position is carried out at a pressure of 2.5×10 -3 ~3×10 -3 mbar.
50. The method for preparing mirror glass according to claim 45, characterized in that: The sputtering of the fourth air surface target position is carried out at a pressure of 4×10 -3 ~4.5×10 -3 mbar.
51. The method for preparing mirror glass according to claim 45, characterized in that: The sputtering of the fifth air surface target position is carried out at a pressure of 2.5×10 -3 ~3×10 -3 mbar.
52. The method for preparing mirror glass according to claim 45, characterized in that: The sputtering thicknesses of the third air surface target position, the fourth air surface target position and the fifth air surface target position are independently selected from 20 to 40 nm.
53. The method for preparing mirror glass according to claim 24, characterized in that: The sputtering process of the metal layer includes: forming the metal layer by sputtering on the surface of the second air surface dielectric layer through the first metal target, the second metal target and the third metal target in sequence.
54. The method for preparing mirror glass according to claim 53, characterized in that: The first metal target, the second metal target and the third metal target are all DC flat targets.
55. The method for preparing mirror glass according to claim 53, characterized in that: The sputtering process of the metal layer is carried out under pure argon gas.
56. The method for preparing mirror glass according to claim 53, characterized in that: The first metal target is sputtered at a pressure of 1.5×10 -3 ~2×10 -3 mbar.
57. The method for preparing mirror glass according to claim 53, characterized in that: The second metal target is sputtered at a pressure of 2.5×10 -3 ~3×10 -3 mbar.
58. The method for preparing mirror glass according to claim 53, characterized in that: The sputtering of the third metal target is carried out at a pressure of 4.5×10 -3 ~5×10 -3 mbar.
59. The method for preparing mirror glass according to claim 53, characterized in that: The sputtering thicknesses of the first metal target, the second metal target and the third metal target are independently selected from 18 to 24 nm.
60. The method for preparing mirror glass according to claim 24, characterized in that: The sputtering process of the third air surface dielectric layer includes: sputtering on the surface of the metal layer through the sixth air surface target position, the seventh air surface target position and the eighth air surface target position in sequence to form the third air surface dielectric layer.
61. The method for preparing mirror glass according to claim 60, characterized in that: The sixth air surface target position, the seventh air surface target position and the eighth air surface target position are all AC round targets.
62. The method for preparing mirror glass according to claim 60, characterized in that: The sputtering process of the third air-side dielectric layer is carried out in a mixed atmosphere of argon and nitrogen.
63. The method for preparing mirror glass according to claim 62, characterized in that: The volume ratio of argon to nitrogen during the sputtering process of the third air surface dielectric layer is (0.7-1):
1.
64. The method for preparing mirror glass according to claim 60, characterized in that: The sixth air surface target position is sputtered at a pressure of 3.5×10 -3 ~4×10 -3 mbar.
65. The method for preparing mirror glass according to claim 60, characterized in that: The seventh air surface target position sputtering is carried out at a pressure of 1.5×10 -3 ~2×10 -3 mbar.
66. The method for preparing mirror glass according to claim 60, characterized in that: The eighth air surface target position sputtering is performed at a pressure of 3.5×10 -3 ~4×10 -3 mbar.
67. The method for preparing mirror glass according to claim 60, characterized in that: The sputtering thicknesses of the sixth air surface target position, the seventh air surface target position and the eighth air surface target position are independently selected from 36 to 47 nm.