Pressure sensitive adhesive tape
By designing a high-density resin film and a pressure-sensitive adhesive layer with a specific composition, the problem of insufficient impact resistance and reprocessability of double-sided pressure-sensitive adhesive sheets is solved, providing a high-performance adhesive solution suitable for mobile devices.
Patent Information
- Application Number
- CN202011501763.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-20
- Filing Date
- 2020-12-18
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-12-18
AI Technical Summary
Existing double-sided pressure-sensitive adhesive sheets have shortcomings in terms of impact resistance and reprocessability. In particular, the adhesion decreases when the foam is stretched or subjected to stress, and it is easy to tear during reprocessing, making it difficult to meet the needs of mobile devices.
The substrate layer is composed of a high-density resin film, and the pressure-sensitive adhesive layer contains a specific ratio of butyl methacrylate and methacrylic acid. The combination design of the substrate layer and the pressure-sensitive adhesive layer ensures that the density of the substrate layer is above 0.8 g/cm3, the modulus of the pressure-sensitive adhesive tape is below 50 MPa, and the thickness ratio is reasonably distributed.
It achieves improved reprocessability while maintaining excellent impact resistance, avoiding problems such as foam tearing and reduced adhesion, and is suitable for fixing mobile devices.
Smart Images

Figure CN113004828B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to pressure sensitive adhesive tapes. Background Art
[0002] In recent years, with the trend of diversification of various performances of mobile devices, diversification of various performances of various constituent members used in mobile devices has been required. In mobile devices, double-sided pressure-sensitive adhesive tapes are sometimes used for joining housings, etc. In recent years, diversification of various performances of double-sided pressure-sensitive adhesive tapes has also been required.
[0003] There is a risk that the mobile device falls depending on its usage form. Therefore, a mobile device having high impact resistance has been required. A shock absorbing member is sometimes configured outside the housing of the mobile device for improving the impact resistance of the mobile device. However, in such a form, the size of the mobile device increases or its designability is impaired.
[0004] In view of the foregoing, it is desirable that excellent impact resistance be imparted to a double-sided pressure-sensitive adhesive tape that can be disposed in a mobile device.
[0005] Recently, a double-sided pressure-sensitive adhesive sheet with impact resistance has been reported (Japanese Patent Application Laid-Open No. 2015-120876). The double-sided pressure-sensitive adhesive sheet includes a substrate made of a foam as an essential component to exhibit impact resistance. However, when the foam is extended to a certain extent or a force is applied thereto, the foam tears and has a smaller area or becomes thinner. As a result, there is a problem in that the cell portion of the foam occupies the majority of the bonding portion between the sheet and the adherend, thereby reducing the adhesion therebetween.
[0006] Furthermore, double-sided pressure-sensitive adhesive sheets to be used in mobile devices are often attached to expensive components, and therefore are required to have satisfactory reworkability at the time of re-attachment, etc. However, double-sided pressure-sensitive adhesive sheets of the prior art may cause problems such as tearing during rework, and double-sided pressure-sensitive adhesive sheets to be used in mobile devices have been required to have excellent reworkability. Summary of the invention
[0007] An object of the present invention is to provide a pressure-sensitive adhesive tape which can exhibit both excellent impact resistance and excellent reworkability.
[0008] According to at least one embodiment of the present invention, there is provided a pressure-sensitive adhesive tape comprising: a substrate layer; and a pressure-sensitive adhesive layer disposed on at least one side of the substrate layer, wherein the specific gravity of the substrate layer is 0.8 g / cm 3 or above, and wherein the 100% modulus at 23° C. and 50% RH of the pressure-sensitive adhesive tape is 50 MPa or less.
[0009] In at least one embodiment of the present invention, the base material layer is formed of a resin film.
[0010] In at least one embodiment of the present invention, the resin film contains one of a polyolefin resin and a polyurethane resin as a main component.
[0011] In at least one embodiment of the present invention, the ratio of the thickness of the base material layer to the total thickness of the pressure-sensitive adhesive tape is less than 40%.
[0012] In at least one embodiment of the present invention, the pressure-sensitive adhesive layer is formed of a pressure-sensitive adhesive composition, the pressure-sensitive adhesive composition contains at least one selected from the group consisting of a monomer component (m) and a polymer component (P) obtained by polymerizing the monomer component (m), and the monomer component (m) contains 50 wt% or more of butyl (meth)acrylate.
[0013] In at least one embodiment of the present invention, the monomer component (m) contains 90 wt% to 99 wt% of butyl (meth)acrylate.
[0014] In at least one embodiment of the present invention, the monomer component (m) contains 1 wt% to 10 wt% of (meth)acrylic acid.
[0015] In at least one embodiment of the present invention, the total thickness of the pressure-sensitive adhesive tape is 100 μm or more.
[0016] In at least one embodiment of the present invention, the pressure-sensitive adhesive tape is used for fixing electronic device components. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 FIG. is a schematic cross-sectional view of a pressure-sensitive adhesive tape according to at least one embodiment of the present invention. DETAILED DESCRIPTION
[0018] As used herein, the term "(meth)acryloyl" means at least one selected from the group consisting of acryloyl and methacryloyl, and the term "(meth)acrylate" means at least one selected from the group consisting of acrylate and methacrylate.
[0019] <<A. Pressure-Sensitive Adhesive Tape>>
[0020] The pressure-sensitive adhesive tape according to at least one embodiment of the present invention includes a base material layer and a pressure-sensitive adhesive layer disposed on at least one side thereof. To such an extent that the effects of the present invention are not impaired, the pressure-sensitive adhesive tape according to at least one embodiment of the present invention may include any appropriate other layers as long as the pressure-sensitive adhesive layer is disposed on at least one side of the base material layer.
[0021] Figure 1 is a schematic cross-sectional view of a pressure-sensitive adhesive tape according to at least one embodiment of the present invention. Figure 1 In the embodiment of the present invention, the pressure-sensitive adhesive tape 100 includes a substrate layer 10, and a pressure-sensitive adhesive layer 20a and a pressure-sensitive adhesive layer 20b on both sides thereof. Different from this, the pressure-sensitive adhesive tape according to at least one other embodiment of the present invention may be a single-sided pressure-sensitive adhesive tape in which the pressure-sensitive adhesive layer is disposed only on one side of the substrate layer.
[0022] The pressure-sensitive adhesive layer may be a single layer, or may include two or more layers.
[0023] The substrate layer may be a single layer, or may include two or more layers.
[0024] The total thickness of the pressure-sensitive adhesive tape according to at least one embodiment of the present invention is preferably 50 μm or more because the effects of the present invention can be further exhibited, and is more preferably 100 to 1,000 μm, still more preferably 100 to 500 μm, particularly preferably 150 to 400 μm.
[0025] To the extent that the effect of the present invention is not impaired, any appropriate release liner may be arranged on the surface of the pressure-sensitive adhesive layer for, for example, protecting the tape until the tape is used. Examples of release liners include: a release liner obtained by subjecting the surface of a substrate (liner substrate) such as paper or a plastic film to a silicone treatment; and a release liner obtained by laminating a polyolefin-based resin on the surface of a substrate (liner substrate) such as paper or a plastic film. Examples of plastic films as liner substrates include polyethylene films, polypropylene films, polybutylene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polybutylene terephthalate films, polyurethane films, and ethylene-vinyl acetate copolymer films. The plastic film as the liner substrate is preferably a polyethylene film.
[0026] The thickness of the release liner is preferably 1 μm to 500 μm, more preferably 3 μm to 450 μm, still more preferably 5 μm to 400 μm, particularly preferably 10 μm to 300 μm.
[0027] The 100% modulus at 23°C and 50%RH of the pressure-sensitive adhesive tape according to at least one embodiment of the present invention is 50MPa or less, preferably 1MPa to 50MPa, more preferably 3MPa to 40MPa, still more preferably 5MPa to 35MPa, and particularly preferably 7MPa to 30MPa. When the 100% modulus at 23°C and 50%RH falls within the above range, a pressure-sensitive adhesive tape that can exhibit both excellent impact resistance and excellent reworkability can be provided.
[0028] The pressure-sensitive adhesive strength of the pressure-sensitive adhesive tape according to at least one embodiment of the present invention is preferably 10 N / 20 mm to 60 N / 20 mm, more preferably 12 N / 20 mm to 40 N / 20 mm, still more preferably 14 N / 20 mm to 30 N / 20 mm, and particularly preferably 14 N / 20 mm to 25 N / 20 mm. When the pressure-sensitive adhesive strength of the pressure-sensitive adhesive tape according to at least one embodiment of the present invention falls within the above range, the function as a pressure-sensitive adhesive tape can be sufficiently exhibited.
[0029] The impact resistance of the pressure-sensitive adhesive tape according to at least one embodiment of the present invention, measured for a laminate structure thereof with a SUS plate at 23 °C and 50% RH, is preferably 0.10 J or more, more preferably 0.12 J or more, still more preferably 0.14 J or more, particularly preferably 0.15 J or more, and most preferably 0.20 J or more. The laminate structure is prepared by laminating the pressure-sensitive adhesive tape with the SUS plate. When the impact resistance is too low to fall outside the above range, there is a risk that a laminate having high impact resistance cannot be provided.
[0030] <A-1. Substrate layer>
[0031] The substrate layer may be a single layer or may include two or more layers. In the case of two or more layers, all of the substrate layers may have the same composition, or at least one of the substrate layers may be different in composition from the others.
[0032] The specific gravity of the substrate layer is 0.8 g / cm 3 or more, preferably 0.8 g / cm 3 to 2.0 g / cm 3 , more preferably 0.8 g / cm 3 to 1.4 g / cm 3 , still more preferably 0.8 g / cm 3 to 1.2 g / cm 3 , particularly preferably 0.9 g / cm 3 to 1.2 g / cm 3 . When the specific gravity of the substrate layer falls within the above range, a pressure-sensitive adhesive tape that can exhibit both excellent impact resistance and excellent reprocessability can be provided.
[0033] The thickness of the substrate layer is preferably 2 μm to 300 μm because the effects of the present invention can be further exhibited, and the thickness is more preferably 2 μm to 150 μm, still more preferably 5 μm to 100 μm, and particularly preferably 5 μm to 50 μm.
[0034] The ratio of the thickness of the substrate layer to the total thickness of the pressure-sensitive adhesive tape according to at least one embodiment of the present invention is preferably less than 40% because the effect of the present invention can be further exhibited, and the ratio is more preferably 1% to 40%, still more preferably 5% to 30%, particularly preferably 10% to 25%.
[0035] The base material layer is preferably formed of a resin film containing a resin material as a main component.
[0036] As used herein, the term "main component" means the component blended in the highest proportion, typically the component contained at more than 50 wt%.
[0037] The content of resin material in the resin film is preferably greater than 50wt% and less than 100wt%, more preferably 60wt% to 100wt%, even more preferably 70wt% to 100wt%, even more preferably 80wt% to 100wt%, particularly preferably 90wt% to 100wt%, most preferably 95wt% to 100wt%.
[0038] As used herein, the term "resin film" typically means a substantially non-foamed resin film. That is, herein, the resin film may be substantially free of the bubbles (no voids) present inside the resin film. Therefore, herein, the concept of "resin film" is distinguished from the so-called foam film. In addition, herein, the resin film is typically a substantially non-porous film, which is a concept distinguished from the so-called non-woven fabric or woven fabric. Herein, the following can be preferably used as resin film: a substrate that does not contain a porous layer such as a foam, non-woven fabric or woven fabric, i.e. a substrate formed by a non-porous layer. Compared with a foam, non-woven fabric or woven fabric, a resin film is generally inclined to be excellent in mechanical strengths such as tensile strength.
[0039] Examples of resin materials for forming the resin film include polyolefin resins (e.g., polyethylene, polypropylene, ethylene-propylene copolymers, or ethylene-vinyl acetate copolymers), polyvinyl chloride resins (typically soft polyvinyl chloride resins), polyvinyl acetate resins, polyurethane resins (e.g., ether polyurethane, ester polyurethane, or carbonate polyurethane), polyurethane (meth) acrylate resins, thermoplastic elastomers (e.g., olefin elastomers, styrene elastomers, or acrylic elastomers), polyester resins (e.g., polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, or polybutylene naphthalate), polycarbonate resins, polyamide resins, polyimide resins, fluororesins, and cellulose resins such as cellophane resins. These resin materials can be used alone or in combination. A preferred example of the resin material for forming the resin film is at least one selected from the group consisting of polyolefin resins, polyvinyl chloride resins, polyurethane resins, and polyester resins, and a more preferred example is a polyolefin resin or a polyurethane resin. That is, a preferred example of the resin film is at least one selected from the group consisting of polyolefin resin films, polyvinyl chloride resin films, polyurethane resin films, and polyester resin films, and a more preferred example is a polyolefin resin film or a polyurethane resin film. When the resin film is the above-mentioned resin film, a pressure-sensitive adhesive tape that can exhibit both better impact resistance and better reprocessability can be provided.
[0040] In at least one exemplary embodiment of the present invention, the resin film is a polyolefin resin film comprising a polyolefin resin as a main component. Specifically, the content of the polyolefin resin in the polyolefin resin film as a whole is preferably 50wt% to 100wt%, more preferably 70wt% to 100wt%, still more preferably 90wt% to 100wt%, particularly preferably 95wt% to 100wt%, and most preferably substantially 100wt%. When the resin film as a whole comprises a polyolefin resin as a main component, the effect of the present invention can be further exhibited.
[0041] Herein, the case described as “substantially 100 wt %” means that trace amounts of impurities and the like may be contained to such an extent that the effects of the present invention are not impaired, and such a case may generally be described as “100 wt %”.
[0042] The resin film as a whole may contain only one kind of polyolefin-based resin, or two or more kinds of polyolefin-based resins.
[0043] Any appropriate polyolefin resin can be used as the polyolefin resin to the extent that the effect of the present invention is not impaired. From the viewpoint that the effect of the present invention can be further exhibited, an example of such a polyolefin resin is at least one selected from the group consisting of polyethylene resins, polypropylene resins and polybutene resins, and a preferred example is at least one selected from the group consisting of polyethylene resins and polypropylene resins.
[0044] Any appropriate polyethylene resin can be used as the polyethylene resin to the extent that the effect of the present invention is not impaired. Examples of such polyethylene resins are at least one selected from the group consisting of low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ultra-low-density polyethylene, medium-density polyethylene (MDPE), high-density polyethylene (HDPE), ultra-high-density polyethylene, and copolymers of ethylene and other monomers (e.g., ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-methacrylic acid copolymers, ethylene-acrylate copolymers, ethylene-methacrylate copolymers, ethylene-butene-1 copolymers, ethylene-propylene-butene-1 copolymers, copolymers of ethylene and α-olefins having 5 to 12 carbon atoms, or ethylene-non-conjugated diene copolymers), and preferred examples are at least one selected from the group consisting of low-density polyethylene and ethylene-vinyl acetate copolymers.
[0045] The polyethylene-based resin may be a metallocene-catalyzed polyethylene-based resin obtained using a metallocene catalyst.
[0046] Any appropriate polypropylene resin may be used as the polypropylene resin to the extent that the effects of the present invention are not impaired. Examples of such polypropylene resins are at least one selected from the group consisting of random polypropylene, block polypropylene, homopolypropylene, and copolymers of propylene and other monomers.
[0047] The polypropylene-based resin may be a metallocene-catalyzed polypropylene-based resin obtained using a metallocene catalyst.
[0048] Any appropriate polybutene-based resin may be used as the polybutene-based resin to the extent that the effects of the present invention are not impaired. Examples of such a polybutene-based resin are at least one selected from the group consisting of polybutene-1 and a copolymer of butene-1 and α-olefin.
[0049] The polybutene-based resin may be a metallocene-catalyzed polybutene-based resin obtained using a metallocene catalyst.
[0050] In at least one other exemplary embodiment of the present invention, the substrate layer is a polyurethane resin film containing a polyurethane resin as a main component. The polyurethane resin film is typically formed of a material that does not substantially show a yield point. The polyurethane resin film can achieve satisfactory physical properties even without adding, for example, additive components such as plasticizers, and can therefore be used as a substrate layer that is preferred in the technology disclosed herein because it prevents the leakage of such additive components.
[0051] Specifically, the content of the polyurethane resin in the polyurethane resin film as a whole is preferably 50wt% to 100wt%, more preferably 70wt% to 100wt%, still more preferably 90wt% to 100wt%, particularly preferably 95wt% to 100wt%, and most preferably substantially 100wt%. When the resin film as a whole contains the polyurethane resin as a main component, the effect of the present invention can be further exhibited.
[0052] The polyurethane resin film may be a film formed of a polymer blend of a polyurethane resin and other resins. The other resin is preferably at least one selected from the group consisting of, for example, acrylic resins, polyolefin resins, polyester resins, and polycarbonate resins.
[0053] Polyurethane resin is a polymer compound synthesized by polyaddition reaction of polyol (e.g., diol) and polyisocyanate (e.g., diisocyanate) in a predetermined ratio. The NCO / OH ratio of polyurethane only needs to be appropriately set based on the conventional technical knowledge known to those of ordinary skill in the art in order to achieve the desired mechanical properties (e.g., breaking strength, breaking elongation, and tensile resilience).
[0054] Examples of polyols that can be used to synthesize polyurethane resins include: diols, such as ethylene glycol, propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 1,8-octanediol, polyoxytetramethylene glycol, diethylene glycol, polyethylene glycol, or polypropylene glycol; polyester polyols, which are polycondensates of diols and dicarboxylic acids (e.g., adipic acid, azelaic acid, or sebacic acid); and carbonate diols, such as polyalkylene carbonate diols. These polyols can be used alone or in combination.
[0055] Examples of polyisocyanates that can be used to synthesize polyurethane-based resins include aromatic, aliphatic, and alicyclic diisocyanates, as well as polymers of diisocyanates (e.g., dimers and trimers). Examples of diisocyanates include toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, butane-1,4-diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, dicyclohexylmethane-4,4-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, and m-tetramethylxylylene diisocyanate. These diisocyanates can be used alone or in combination. Among the diisocyanates, aromatic diisocyanates are preferred because the effects of the present invention can be further exhibited.
[0056] In addition to polyols and polyisocyanates, other copolymerization components can also be introduced into the polyurethane-based resin. Examples of other copolymerization components include monocarboxylic acids, dicarboxylic acids, polycarboxylic acids having three or more functional groups, hydroxycarboxylic acids, alkoxycarboxylic acids, and their derivatives. These other copolymerization components can be used alone or in combination.
[0057] Preferably, in the polyurethane-based resin, the proportion of other copolymerization components is set to be approximately less than 30 wt% (e.g., less than 10 wt%, typically less than 5 wt%).
[0058] The substrate layer can optionally contain any suitable additives as needed. Examples of additives that can be included in the substrate layer include release agents, UV absorbers, heat stabilizers, fillers, lubricants, colorants (e.g., dyes), antioxidants, anti-build up agents, anti-blocking agents, foaming agents, and polyethyleneimine. These additives can be used alone or in combination. The content of additives in the substrate layer is preferably 10 wt% or less, more preferably 7 wt% or less, still more preferably 5 wt% or less, particularly preferably 2 wt% or less, and most preferably 1 wt% or less.
[0059] <A-2. Pressure-sensitive adhesive layer>
[0060] The pressure-sensitive adhesive layer can be a single layer, or can include two or more layers. In the case of two or more layers, all of the pressure-sensitive adhesive layers can have the same composition, or at least one of the pressure-sensitive adhesive layers can be different in composition from the others.
[0061] The pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive composition.
[0062] The pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive composition by any suitable method. Examples of such methods include: a method (direct method) involving applying a pressure-sensitive adhesive composition, which is a forming material for the pressure-sensitive adhesive layer, to any suitable substrate (e.g., a substrate film), and drying the composition as needed to form a pressure-sensitive adhesive layer on the substrate; and a method (transfer method) involving applying the pressure-sensitive adhesive composition to a surface having peelability (peel surface), drying the composition as needed to form a pressure-sensitive adhesive layer on the surface having peelability (peel surface), and transferring the pressure-sensitive adhesive layer to any suitable substrate (e.g., a substrate film). The surface having peelability (peel surface) is, for example, the surface of the release liner described above.
[0063] To the extent that the effects of the present invention are not impaired, any suitable coating method can be used as the method for applying the pressure-sensitive adhesive composition. Examples of such coating methods include roll coating, gravure coating, reverse coating, roller brushing, spraying, air knife coating method, and extrusion coating using a die coater or the like. Actinic ray irradiation such as UV irradiation can be carried out for curing the coating layer formed by the application.
[0064] From the viewpoints of, for example, promoting the crosslinking reaction of the composition and improving the production efficiency of the tape, the drying of the pressure-sensitive adhesive composition can be carried out under heating. The drying temperature can typically be set, for example, to 40°C to 150°C, and preferably 60°C to 130°C. After drying the pressure-sensitive adhesive composition, aging can be further carried out for the purpose of, for example, regulating the migration of components in the pressure-sensitive adhesive layer, promoting the crosslinking reaction, and reducing the strain that may be present in the pressure-sensitive adhesive layer.
[0065] The thickness of the pressure-sensitive adhesive layer is preferably 10 μm to 1,000 μm because the effects of the present invention can be further exhibited, and the thickness is more preferably 20 μm to 700 μm, still more preferably 30 μm to 500 μm, particularly preferably 40 μm to 300 μm, and most preferably 50 μm to 200 μm.
[0066] <A-2-1. Pressure-Sensitive Adhesive Composition>
[0067] The pressure-sensitive adhesive composition contains at least one selected from the group consisting of a monomer component (m) and a polymer component (P) obtained by polymerizing the monomer component (m). That is, typically, the pressure-sensitive adhesive composition can have any one of the following forms: a form (Form 1) containing the polymer component (P) and substantially free of the monomer component (m); a form (Form 2) containing the monomer component (m) and substantially free of the polymer component (P); and a form (Form 3) containing both the monomer component (m) and the polymer component (P).
[0068] The form (form 1) containing the polymer component (P) and substantially containing no monomer component (m) is a form in which the polymer component (P) is substantially formed by polymerization of the monomer component (m) in the stage of preparing the pressure-sensitive adhesive composition.
[0069] The form containing the monomer component (m) and substantially not containing the polymer component (P) (form 2) is a form in which substantially no polymerization of the monomer component (m) occurs in the stage of preparing the pressure-sensitive adhesive composition, and thus the polymer component (P) has not yet been formed. In this form, the polymer component (P) can be formed by, for example, curing the applied layer formed by applying the prepared pressure-sensitive adhesive composition by irradiation with active energy rays such as UV irradiation.
[0070] The form (form 3) containing both the monomer component (m) and the polymer component (P) is a form in which, in the stage of preparing the pressure-sensitive adhesive composition, part of the molecules of the monomer component (m) are polymerized to form a part of the polymer, and the molecules of the unreacted monomer component (m) remain. In this form, the polymer component (P) can be formed by, for example, curing the applied layer formed by applying the prepared pressure-sensitive adhesive composition by irradiation with active energy rays such as UV irradiation.
[0071] In the case of form 1 (a form comprising a polymer component (P) and substantially free of a monomer component (m)), the content of the polymer component (P) in the pressure-sensitive adhesive composition is as follows: When the total amount of the pressure-sensitive adhesive composition is set to 100 parts by weight, the content of the polymer component (P) is preferably 50 wt % to 100 wt %, more preferably 60 wt % to 100 wt %, still more preferably 70 wt % to 100 wt %, and particularly preferably 80 wt % to 100 wt %.
[0072] In the case of form 2 (a form containing monomer component (m) and substantially free of polymer component (P)), the content of monomer component (m) in the pressure-sensitive adhesive composition is as follows: when the total amount of the pressure-sensitive adhesive composition is set to 100 parts by weight, the content of monomer component (m) is preferably 50 wt% to 100 wt%, more preferably 60 wt% to 100 wt%, still more preferably 70 wt% to 100 wt%, and particularly preferably 80 wt% to 100 wt%.
[0073] In the case of Form 3 (a form comprising both a monomer component (m) and a polymer component (P)), the total content of the polymer component (P) and the monomer component (m) in the pressure-sensitive adhesive composition is as follows: When the total amount of the pressure-sensitive adhesive composition is set to 100 parts by weight, the total content of the polymer component (P) and the monomer component (m) is preferably 50 wt% to 100 wt%, more preferably 60 wt% to 100 wt%, still more preferably 70 wt% to 100 wt%, and particularly preferably 80 wt% to 100 wt%.
[0074] The pressure-sensitive adhesive composition may contain any appropriate colorant to such an extent that the effects of the present invention are not impaired, from the viewpoint of, for example, adjusting its light transmittance (light-shielding property). Conventionally known pigments or dyes may be used as such a colorant. Examples of the pigment include: inorganic pigments such as carbon black, zinc carbonate, zinc oxide, zinc sulfide, talc, kaolin, calcium carbonate, titanium oxide, silicon dioxide, lithium fluoride, calcium fluoride, barium sulfate, aluminum oxide, zirconium oxide, iron oxide pigments, iron hydroxide pigments, chromium oxide pigments, spinel-type calcined pigments, chromic acid pigments, chrome vermilion pigments, iron blue pigments, aluminum powder pigments, bronze powder pigments, silver powder pigments, and calcium phosphate; and organic pigments such as phthalocyanine pigments, azo pigments, condensed azo pigments, azo lake pigments, anthraquinone pigments, perylene-pyrenone pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, azomethine pigments, dioxazine pigments, quinacridone pigments, nigrosine pigments, and triphenylmethane pigments. Examples of the dye include azo dyes, anthraquinone, quinolones, styryl dyes, diphenylmethane, triphenylmethane, oxazine, triazine, xanthan gum, azomethine, acridine, and dioxazines. The colorant may be used alone or in combination thereof.
[0075] The black colorant is specifically, for example, carbon black, graphite, copper oxide, manganese dioxide, aniline black, perylene black, titanium black, cyanine black, activated carbon, ferrite (e.g., non-magnetic ferrite or magnetic ferrite), magnetite, chromium oxide, iron oxide, molybdenum disulfide, chromium complex or anthraquinone-based colorant.
[0076] The content of the colorant in the pressure-sensitive adhesive composition is preferably less than 30 wt %, more preferably less than 20 wt %, still more preferably less than 13 wt %, particularly preferably less than 10 wt %, most preferably less than 8 wt %.
[0077] To the extent that the effects of the present invention are not impaired, the pressure-sensitive adhesive composition may contain any suitable other components. Examples of such other components include resin components other than the polymer component (P), tackifiers, crosslinking agents, inorganic fillers, organic fillers, metal powders, pigments, foil-like substances, softeners, anti-aging agents, conductive agents, rust inhibitors, UV absorbers, antioxidants, light stabilizers, surface lubricants, leveling agents, corrosion inhibitors, heat stabilizers, polymerization inhibitors, lubricants, solvents, and catalysts.
[0078] <A-2-1-1. Monomer component (m)>
[0079] The monomer component (m) contains 50 wt% or more of butyl (meth)acrylate. The content of butyl (meth)acrylate in the total amount of the monomer component (m) is preferably 50 wt% to 100 wt%, more preferably 70 wt% to 99.5 wt%, still more preferably 90 wt% to 99 wt%, particularly preferably 91 wt% to 98 wt%, and most preferably 92 wt% to 97 wt%. When the content of butyl (meth)acrylate in the monomer component (m) is adjusted within the above range, a pressure-sensitive adhesive tape can be provided that can exhibit both more excellent impact resistance and more excellent reprocessability.
[0080] Butyl (meth)acrylate is preferably butyl acrylate, and more preferably n-butyl acrylate, because the effects of the present invention can be further exhibited.
[0081] The monomer component (m) preferably contains (meth)acrylic acid, and more preferably contains acrylic acid. The content of (meth)acrylic acid in the total amount of the monomer component (m) is preferably 1 wt% to 10 wt%, more preferably 1 wt% to 8 wt%, still more preferably 2 wt% to 7 wt%, particularly preferably 2 wt% to 6 wt%, and most preferably 2.5 wt% to 5.5 wt%. When the content of (meth)acrylic acid in the monomer component (m) is adjusted within the above range, a pressure-sensitive adhesive tape can be provided that can exhibit both more excellent impact resistance and more excellent reprocessability.
[0082] The monomer component (m) may contain any other monomers. Such other monomers can be used alone or in combination.
[0083] The content of other monomers in the total amount of the monomer component (m) is preferably 0 wt% to 10 wt%, more preferably 0 wt% to 8 wt%, still more preferably 0 wt% to 6 wt%, particularly preferably 0 wt% to 4 wt%, and most preferably 0 wt% to 2 wt%. When the content of other monomers in the monomer component (m) is adjusted within the above range, a pressure-sensitive adhesive tape can be provided that can exhibit both more excellent impact resistance and more excellent reprocessability.
[0084] Examples of other monomers include acrylic monomers containing an alicyclic structure, alkyl (meth)acrylates other than butyl (meth)acrylate, hydroxyl-containing monomers, carboxyl-containing monomers other than (meth)acrylic acid, nitrogen-containing cyclic structure monomers, cyclic ether group-containing monomers, glycol acrylate monomers, styrene-based monomers, amide group-containing monomers, amino group-containing monomers, imide group-containing monomers, vinyl ether monomers, silane-based monomers, and multifunctional monomers.
[0085] The acrylic monomer containing an alicyclic structure is preferably an acrylic monomer having a cyclic aliphatic hydrocarbon structure. The number of carbon atoms in the cyclic aliphatic hydrocarbon structure is preferably 3 or more, more preferably 6 to 24, still more preferably 6 to 18, and particularly preferably 6 to 12. Specific examples of such acrylic monomers containing an alicyclic structure include cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, cyclooctyl (meth)acrylate, isobornyl (meth)acrylate, and dicyclopentyl (meth)acrylate.
[0086] Herein, the alkyl (meth)acrylate other than butyl (meth)acrylate does not include an alkyl (meth)acrylate having an alicyclic structure. Specific examples of the alkyl (meth)acrylate other than butyl (meth)acrylate include: alkyl (meth)acrylates each having a linear alkyl group (except n-butyl) at its ester end, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, n-undecyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, n-pentadecyl (meth)acrylate, n-hexadecyl (meth)acrylate, n-heptadecyl (meth)acrylate, and n-octadecyl (meth)acrylate; and alkyl (meth)acrylate each having a linear alkyl group (except n-butyl) at its ester end, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptadecyl (meth)acrylate, and n-octadecyl (meth)acrylate; Alkyl (meth)acrylates having a branched alkyl group having 4 to 18 carbon atoms (excluding isobutyl), for example, isopropyl (meth)acrylate, tert-butyl (meth)acrylate, isopentyl (meth)acrylate, tert-amyl (meth)acrylate, neopentyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, 2-propylheptyl (meth)acrylate, isoundecyl (meth)acrylate, isododecyl (meth)acrylate, isotridecyl (meth)acrylate, isomyristyl (meth)acrylate, isopentadecyl (meth)acrylate, isohexadecyl (meth)acrylate, isoheptadecyl (meth)acrylate and isostearyl (meth)acrylate.
[0087] Specific examples of hydroxyl-containing monomers include: hydroxyalkyl (meth)acrylates, such as 2-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; hydroxyalkylcycloalkyl (meth)acrylates, such as (4-hydroxymethylcyclohexyl)methyl (meth)acrylate; and other hydroxyl-containing monomers, such as hydroxyethyl (meth)acrylamide, allyl alcohol, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, and diethylene glycol monovinyl ether. Among those hydroxyl-containing monomers, hydroxyalkyl (meth)acrylates are preferred because more excellent impact resistance can be exhibited, and hydroxyalkyl (meth)acrylates having a hydroxyalkyl group having 2 to 6 carbon atoms are more preferred, and 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate is even more preferred.
[0088] Specific examples of the carboxyl group-containing monomer other than (meth)acrylic acid include carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.
[0089] Specific examples of monomers with nitrogen-containing cyclic structures include: lactam-based vinyl monomers, such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam and methylvinylpyrrolidone; vinyl-based monomers each having a nitrogen-containing heterocyclic ring, such as vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole and vinylmorpholine; and (meth)acrylic monomers each containing a heterocyclic ring such as a morpholine ring, a piperidine ring, a pyrrolidine ring or a piperazine ring (e.g., N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine and N-acryloylpyrrolidine).
[0090] Specific examples of the cyclic ether group-containing monomer include: epoxy group-containing monomers such as glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, methyl glycidyl (meth)acrylate and allyl glycidyl ether; oxetane group-containing monomers such as 3-oxetane methyl (meth)acrylate, 3-methyl-oxetane methyl (meth)acrylate, 3-ethyl-oxetane methyl (meth)acrylate, 3-butyl-oxetane methyl (meth)acrylate and 3-hexyl-oxetane methyl (meth)acrylate.
[0091] Specific examples of the diol-based acrylate monomer include polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate.
[0092] Specific examples of the styrene-based monomers include styrene and α-methylstyrene.
[0093] Specific examples of the amide group-containing monomer include acrylamide, methacrylamide, diethylacrylamide, N-vinylpyrrolidone, N,N-dimethylacrylamide, N,N-(dimethyl)methacrylamide, N,N-diethylacrylamide, N,N-diethylmethacrylamide, N,N′-methylenebisacrylamide, N,N-dimethylaminopropylacrylamide, N,N-dimethylaminopropylmethacrylamide, diacetoneacrylamide and N,N-hydroxyethylacrylamide.
[0094] Specific examples of the amino group-containing monomer include aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate.
[0095] Specific examples of the imide group-containing monomers include cyclohexyl maleimide, isopropyl maleimide, N-cyclohexyl maleimide, and itaconic imide.
[0096] Specific examples of the silane-based monomers include 3-acryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloxydecyltrimethoxysilane, 10-acryloxydecyltrimethoxysilane, 10-methacryloxydecyltriethoxysilane, and 10-acryloxydecyltriethoxysilane.
[0097] Specific examples of the polyfunctional monomers include ester compounds of polyhydric alcohols and (meth)acrylic acid, such as (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate; vinyl (meth)acrylate; divinylbenzene; epoxy acrylate; polyester acrylate; polyurethane acrylate; dibutyl (meth)acrylate; and dihexyl (meth)acrylate.
[0098] <A-2-1-2. Polymer Component (P)>
[0099] The polymer component (P) is obtained by polymerizing the monomer component (m). The polymer component (P) is typically an acrylic polymer. The polymer component (P) can be used alone or in combination.
[0100] To the extent that the effects of the present invention are not impaired, any suitable production method can be used as the production method of the polymer component (P). Examples of such production methods include various types of radical polymerization, which include: solution polymerization; active energy ray polymerization, such as UV polymerization; bulk polymerization; and emulsion polymerization. To the extent that the effects of the present invention are not impaired, any suitable polymerization conditions can be used as the polymerization conditions.
[0101] To the extent that the effects of the present invention are not impaired, any suitable polymerization structure can be used as the polymerization structure of the polymer component (P) to be obtained. Examples of such polymerization structures include random copolymers, block copolymers, and graft copolymers.
[0102] Any appropriate additive may be used as the additive to be used in the radical polymerization, such as a polymerization initiator, a chain transfer agent, or an emulsifier, to such an extent that the effects of the present invention are not impaired.
[0103] The polymerization solvent which can be used in solution polymerization etc. is, for example, ethyl acetate or toluene. The polymerization solvent can be used alone or in combination thereof.
[0104] Typically, solution polymerization is carried out under reaction conditions of a temperature of about 50° C. to about 70° C. and a time of about 5 hours to about 30 hours, after adding a polymerization initiator, in a stream of an inert gas such as nitrogen.
[0105] Any appropriate thermal polymerization initiator may be used as the polymerization initiator that can be used in solution polymerization, etc., to such an extent that the effects of the present invention are not impaired. The polymerization initiator may be used alone or in combination thereof. Examples of such polymerization initiators include azo-based initiators such as 2,2′-azobisisobutyronitrile, 2,2′-azobis-2-methylbutyronitrile, 2,2′-azobis(2-methylpropionic acid) dimethyl ester, 4,4′-azobis-4-cyanovaleric acid, azobisisovaleronitrile, 2,2′-azobis(2-amidinopropane) dihydrochloride, 2,2′-azobis[2-(5-methyl-2-imidazolin-2-yl)propane] dihydrochloride, 2,2′-azobis(2-methylpropionamidine) disulfate, 2,2′-azobis(N,N′-dimethyleneisobutyramidine) and 2,2′-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] hydrate (VA-057, manufactured by Wako Pure Chemical Industries, Ltd.); peroxide-based initiators, including persulfates such as potassium persulfate and ammonium persulfate, di(2-ethylhexyl) peroxydicarbonate, di(4-tert-butylcyclohexyl) peroxydicarbonate, di-sec-butyl peroxydicarbonate, tert-butyl peroxyneodecanoate, tert-hexyl peroxypivalate, tert-butyl peroxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, di(4-methylbenzoyl) peroxide, dibenzoyl peroxide, tert-butyl peroxyisobutyrate, 1,1-di(tert-hexylperoxy)cyclohexane, tert-butyl hydroperoxide and hydrogen peroxide; and redox-based initiators each obtained by combining a peroxide and a reducing agent, such as a combination of a persulfate and sodium bisulfite, and a combination of a peroxide and sodium ascorbate.
[0106] The amount of the polymerization initiator used is preferably 1 part by weight or less, more preferably 0.005 to 1 part by weight, still more preferably 0.01 to 0.7 parts by weight, and particularly preferably 0.02 to 0.5 parts by weight, relative to 100 parts by weight of the total amount of the monomer component (m), for example, because the polymerization reaction can be effectively promoted.
[0107] Any suitable chain transfer agent may be used as the chain transfer agent to the extent that the effect of the present invention is not impaired. The chain transfer agent may be used alone or in combination. Examples of such chain transfer agents include lauryl mercaptan, glycidyl mercaptan, mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, and 2,3-dimercapto-1-propanol.
[0108] The chain transfer agent is preferably used in an amount of 0.1 parts by weight or less relative to 100 parts by weight of the total amount of the monomer component (m) because, for example, the polymerization reaction can be efficiently advanced.
[0109] Any appropriate emulsifier may be used as the emulsifier to the extent that the effect of the present invention is not impaired. The emulsifier may be used alone or in combination. Examples of such emulsifiers include anionic emulsifiers such as sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, ammonium polyoxyethylene alkyl ether sulfate, and sodium polyoxyethylene alkylphenyl ether sulfate; and nonionic emulsifiers such as polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene fatty acid esters, and polyoxyethylene-polyoxypropylene block polymers.
[0110] From the viewpoint of polymerization stability and mechanical stability, the amount of the emulsifier used is preferably 5 parts by weight or less, more preferably 0.3 to 5 parts by weight, still more preferably 0.4 to 3 parts by weight, particularly preferably 0.5 to 1 part by weight, relative to 100 parts by weight of the total amount of the monomer component (m).
[0111] When UV polymerization is performed, it is preferred to use a photopolymerization initiator.
[0112] Any suitable photopolymerization initiator may be used as the photopolymerization initiator to the extent that the effect of the present invention is not impaired. The photopolymerization initiator may be used alone or in combination. Examples of such photopolymerization initiators include benzoin ether photopolymerization initiators, acetophenone photopolymerization initiators, α-ketol photopolymerization initiators, aromatic sulfonyl chloride photopolymerization initiators, photoactive oxime photopolymerization initiators, benzoin photopolymerization initiators, benzyl photopolymerization initiators, benzophenone photopolymerization initiators, ketal photopolymerization initiators, thioxanthone photopolymerization initiators, and acylphosphine oxide photopolymerization initiators.
[0113] Specific examples of the benzoin ether-based photopolymerization initiator include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethane-1-one (for example, a commercially available product under the trade name "Irgacure 651" from BASF), and anisole methyl ether.
[0114] Specific examples of the acetophenone-based photopolymerization initiator include 1-hydroxycyclohexyl phenyl ketone (e.g., a commercial product available under the trade name "Irgacure 184" from BASF), 4-phenoxydichloroacetophenone, 4-tert-butyl-dichloroacetophenone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one (e.g., a commercial product available under the trade name "Irgacure 2959" from BASF), 2-hydroxy-2-methyl-1-phenyl-propane-1-one (e.g., a commercial product available under the trade name "DAROCUR 1173" from BASF), and methoxyacetophenone.
[0115] Specific examples of the α-ketol-based photopolymerization initiator include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)-phenyl]-2-hydroxy-2-methylpropane-1-one.
[0116] A specific example of the aromatic sulfonyl chloride-based photopolymerization initiator is 2-naphthalenesulfonyl chloride.
[0117] A specific example of the photoactive oxime-based photopolymerization initiator is 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime.
[0118] A specific example of the benzoin-based photopolymerization initiator is benzoin.
[0119] A specific example of the benzil-based photopolymerization initiator is benzil.
[0120] Specific examples of the benzophenone-based photopolymerization initiator include benzophenone, benzoylbenzoic acid, 3,3′-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, and α-hydroxycyclohexylphenylketone.
[0121] A specific example of the ketal-based photopolymerization initiator is benzyl dimethyl ketal.
[0122] Specific examples of the thioxanthone-based photopolymerization initiator include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.
[0123] Specific examples of the acylphosphine oxide-based photopolymerization initiator include bis(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis(2,6-dimethoxybenzoyl)(2,4,4-trimethylpentyl)phosphine oxide, bis(2,6-dimethoxybenzoyl)-n-butylphosphine oxide, bis(2,6-dimethoxybenzoyl)-(2-methylpropane-1-yl)phosphine oxide, bis(2,6-dimethoxybenzoyl)-(1-methylpropane-1-yl)phosphine oxide, bis(2,6-dimethoxybenzoyl)-tert-butylphosphine oxide, bis(2,6-dimethoxybenzoyl)cyclohexylphosphine oxide, bis(2,6-dimethoxybenzoyl)octylphosphine oxide, bis(2-methoxybenzoyl)(2-methylpropane-1-yl)phosphine oxide, -1-yl) phosphine oxide, bis(2-methoxybenzoyl)(1-methylpropane-1-yl) phosphine oxide, bis(2,6-diethoxybenzoyl)(2-methylpropane-1-yl) phosphine oxide, bis(2,6-diethoxybenzoyl)(1-methylpropane-1-yl) phosphine oxide, bis(2,6-dibutoxybenzoyl)(2-methylpropane-1-yl) phosphine oxide, bis(2,4-dimethoxybenzoyl)(2-methylpropane-1-yl) phosphine oxide, bis(2,4,6-trimethylbenzoyl)(2,4-dipentyloxyphenyl) phosphine oxide, bis(2,6-dimethoxybenzoyl)benzyl phosphine oxide, bis(2,6-dimethoxybenzoyl)-2-phenylpropyl phosphine oxide, bis(2,6 bis(2,6-dimethoxybenzoyl)-2-phenylethylphosphine oxide, bis(2,6-dimethoxybenzoyl)benzylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2-phenylpropylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2-phenylethylphosphine oxide, 2,6-dimethoxybenzoylbenzylbutylphosphine oxide, 2,6-dimethoxybenzoylbenzyloctylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,5-diisopropylphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2-methylphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-4-methylphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,5-diethylphenylphosphine oxide phosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,3,5,6-tetramethylphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-n-butoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis(2,4,6-trimethylbenzoyl)isobutylphosphine oxide, 2,6-dimethoxybenzoyl-2,4,6-trimethylbenzoyl-n-butylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-butoxyphenylphosphine oxide, 1,10-bis[bis(2,4,6-trimethylbenzoyl)phosphine oxide] decane, and tri(2-methylbenzoyl)phosphine oxide.
[0124] From the viewpoint of, for example, the expression of satisfactory polymerizability, the amount of the photopolymerization initiator used is preferably 5 parts by weight or less, more preferably 0.01 to 5 parts by weight, still more preferably 0.05 to 3 parts by weight, particularly preferably 0.05 to 1.5 parts by weight, most preferably 0.1 to 1 part by weight, relative to 100 parts by weight of the total amount of the monomer component (m).
[0125] When UV polymerization is performed, polyfunctional (meth)acrylates are preferably used.
[0126] Any appropriate polyfunctional (meth)acrylate may be used as the polyfunctional (meth)acrylate to such an extent that the effects of the present invention are not impaired. The polyfunctional (meth)acrylate may be used alone or in combination. Specific examples of such multifunctional (meth)acrylates include: ester compounds of polyols and (meth)acrylic acid, such as (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,2-ethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate; vinyl (meth)acrylate; divinylbenzene; epoxy acrylate; polyester acrylate; polyurethane acrylate; butyl di(meth)acrylate; and hexyl di(meth)acrylate.
[0127] From the viewpoint of, for example, the expression of satisfactory crosslinking properties, the amount of the multifunctional (meth)acrylate used is preferably 5 parts by weight or less, more preferably 0.01 to 5 parts by weight, still more preferably 0.05 to 3 parts by weight, particularly preferably 0.05 to 1.5 parts by weight, most preferably 0.1 to 1 part by weight, relative to 100 parts by weight of the total amount of the monomer component (m).
[0128] Any appropriate UV polymerization method can be used as a method for UV polymerization to the extent that the effects of the present invention are not impaired. Such a UV polymerization method is, for example, as follows: the monomer component (m) is blended with a photopolymerization initiator and, if necessary, a multifunctional (meth)acrylate, and the resultant is irradiated with UV light.
[0129] The weight-average molecular weight of the polymer component (P) is preferably from 100,000 to 3,000,000, more preferably from 300,000 to 2,000,000, still more preferably from 500,000 to 1,500,000, and particularly preferably from 500,000 to 1,000,000, because the pressure-sensitive adhesive tape according to at least one embodiment of the present invention can exhibit more excellent impact resistance. The weight-average molecular weight is a value measured by gel permeation chromatography (GPC) and converted to polystyrene. It may be difficult to measure the weight-average molecular weight of the polymer component (P) obtained by living energy ray polymerization.
[0130] <A-2-1-3. Tackifying resin>
[0131] The pressure-sensitive adhesive composition may contain a tackifying resin. The tackifying resin may be used alone or in combination thereof.
[0132] To the extent that the effects of the present invention are not impaired, any suitable tackifying resin can be used as the tackifying resin. Examples of such tackifying resins include phenolic tackifying resins, terpene tackifying resins, modified terpene tackifying resins, rosin tackifying resins, hydrocarbon tackifying resins, epoxy tackifying resins, polyamide tackifying resins, elastomeric tackifying resins, and ketone tackifying resins.
[0133] Examples of phenolic tackifying resins include terpene-phenol resins, hydrogenated terpene-phenol resins, alkylphenol resins, and rosin-phenol resins. A terpene-phenol resin refers to a polymer containing terpene residues and phenol residues, and is a concept including both a copolymer of terpenes and phenol compounds (terpene-phenol copolymer resin) and a phenol-modified product of a homopolymer or copolymer of terpenes (phenol-modified terpene resin). Examples of terpenes forming such a terpene-phenol resin include monoterpenes such as α-pinene, β-pinene, and limonene (including d-type, l-type, and d / l-type (dipentene)). A hydrogenated terpene-phenol resin refers to a hydrogenated terpene-phenol resin having a structure obtained by hydrogenating such a terpene-phenol resin, and is sometimes referred to as a hydrogenated terpene-phenol resin. An alkylphenol resin is a resin obtained from an alkylphenol and formaldehyde (oil-soluble phenolic resin). Examples of alkylphenol resins include novolak-type resins and resol-type resins. Examples of rosin-phenol resins include phenol-modified products of rosins or various rosin derivatives (including rosin esters, unsaturated fatty acid-modified rosins, and unsaturated fatty acid-modified rosin esters). A rosin-phenol resin is, for example, a rosin-phenol resin obtained by the following method: the method involves adding phenol to a rosin or various rosin derivatives with an acid catalyst and subjecting the resulting product to thermal polymerization.
[0134] Examples of terpene-based tackifying resins include polymers of terpenes (typically monoterpenes) such as α-pinene, β-pinene, d-limonene, l-limonene and dipentene. A terpene homopolymer is, for example, an α-pinene polymer, a β-pinene polymer or a dipentene polymer.
[0135] Examples of the modified terpene resin include styrene-modified terpene resins and hydrogenated terpene resins.
[0136] The concept of rosin-based tackifying resins includes both rosins and rosin derivative resins. Examples of rosins include: unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin; and modified rosins obtained by modifying these unmodified rosins by hydrogenation, disproportionation, or polymerization (e.g., hydrogenated rosin, disproportionated rosin, polymerized rosin, and any other chemically modified rosin).
[0137] Examples of rosin derivative resins include: rosin esters such as unmodified rosin esters as esters of unmodified rosin and alcohols, and modified rosin esters as esters of modified rosin and alcohols; unsaturated fatty acid-modified rosins obtained by modifying rosins with unsaturated fatty acids; unsaturated fatty acid-modified rosin esters obtained by modifying rosin esters with unsaturated fatty acids; rosin alcohols obtained by subjecting rosins or rosin derivative resins (e.g., rosin esters, unsaturated fatty acid-modified rosins, and unsaturated fatty acid-modified rosin esters) to reduction treatment; and metal salts thereof. Examples of rosin esters include methyl esters, triethylene glycol esters, glycerol esters, and pentaerythritol esters of unmodified rosins or modified rosins (e.g., hydrogenated rosin, disproportionated rosin, and polymerized rosin).
[0138] Examples of hydrocarbon-based tackifying resins include aliphatic hydrocarbon resins, aromatic hydrocarbon resins, aliphatic cyclic hydrocarbon resins, aliphatic-aromatic petroleum resins (e.g., styrene-olefin copolymers), aliphatic-alicyclic petroleum resins, hydrogenated hydrocarbon resins, coumarone-based resins, and coumarone-indene-based resins.
[0139] In the case of Form 1, the content of the tackifier resin in the pressure-sensitive adhesive composition is preferably 1 to 50 parts by weight, more preferably 5 to 30 parts by weight, still more preferably 8 to 25 parts by weight, particularly preferably 10 to 20 parts by weight, relative to 100 parts by weight of the polymer component (P).
[0140] In the case of form 2, the content of the tackifier resin in the pressure-sensitive adhesive composition is preferably 1 to 50 parts by weight, more preferably 5 to 30 parts by weight, still more preferably 8 to 25 parts by weight, and particularly preferably 10 to 20 parts by weight, relative to 100 parts by weight of the total amount of the monomer component (m).
[0141] In the case of Form 3, the content of the tackifying resin in the pressure-sensitive adhesive composition is preferably 1 part by weight to 50 parts by weight, more preferably 5 parts by weight to 30 parts by weight, still more preferably 8 parts by weight to 25 parts by weight, and particularly preferably 10 parts by weight to 20 parts by weight, based on 100 parts by weight of the total amount of the polymer component (P) and the monomer component (m).
[0142] <A-2-1-4. Crosslinking agent>
[0143] The pressure-sensitive adhesive composition may contain a crosslinking agent. The crosslinking agent can be used alone or in combination.
[0144] To the extent that the effects of the present invention are not impaired, any suitable crosslinking agent can be used as the crosslinking agent. Examples of such crosslinking agents include isocyanate-based crosslinking agents and non-isocyanate-based crosslinking agents.
[0145] To the extent that the effects of the present invention are not impaired, any suitable isocyanate-based crosslinking agent can be used as the isocyanate-based crosslinking agent. Examples of such isocyanate-based crosslinking agents include aromatic diisocyanates, aliphatic diisocyanates, and alicyclic diisocyanates, as well as dimers and trimers of those diisocyanates. Specific examples thereof include toluene diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, hydrogenated xylylene diisocyanate, isophorone diisocyanate, hydrogenated diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, butane-1,4-diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, dicyclohexylmethane-4,4-diisocyanate, 1,3-bis(isocyanatomethyl)cyclohexane, methylcyclohexane diisocyanate, and m-tetramethylxylylene diisocyanate, as well as their dimers and trimers, and polyphenylmethane polyisocyanate. In addition, the trimer can be, for example, of the isocyanurate type, biuret type, or urethane type.
[0146] Commercially available products can be used as isocyanate-based crosslinking agents. Examples of commercially available products of polyisocyanates include products available under the trade name "TAKENATE 600" from Mitsui Chemicals, Inc., products available under the trade name "DURANATE TPA100" from Asahi Kasei Chemicals Corporation, and products available under the trade names "CORONATE L", "CORONATE HL", "CORONATE HK", "CORONATE HX" and "CORONATE 2096" from Nippon Polyurethane Industry Co., Ltd.
[0147] Examples of non-isocyanate crosslinking agents include epoxy crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, melamine crosslinking agents, carbodiimide crosslinking agents, hydrazine crosslinking agents, amine crosslinking agents, peroxide crosslinking agents, metal chelate crosslinking agents, metal alkoxide crosslinking agents, metal salt crosslinking agents, and silane coupling agents.
[0148] In at least one exemplary embodiment of the present invention, an epoxy crosslinking agent can be used as a non-isocyanate crosslinking agent. The epoxy crosslinking agent is preferably a compound having two or more epoxy groups in its molecule, and more preferably an epoxy crosslinking agent having 3 to 5 epoxy groups in its molecule.
[0149] Specific examples of epoxy crosslinking agents include N, N, N', N'-tetraglycidyl-m-xylenediamine, 1,3-bis(N, N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, polyethylene glycol diglycidyl ether, and polyglycerol polyglycidyl ether. Examples of commercially available epoxy crosslinking agents include products available under the trade names "TETRAD-C" and "TETRAD-X" from Mitsubishi Gas Chemical Company, products available under the trade name "EPICLON CR-5L" from DIC Corporation, products available under the trade name "DENACOL EX-512" from Nagase ChemteX Corporation, and products available under the trade name "TEPIC-G" from Nissan Chemical Industries, Ltd.
[0150] In the case of Form 1, the content of the crosslinking agent in the pressure-sensitive adhesive composition is preferably 0.01 parts by weight to 10 parts by weight, more preferably 0.1 parts by weight to 8 parts by weight, still more preferably 0.5 parts by weight to 7 parts by weight, and particularly preferably 1.5 parts by weight to 5 parts by weight, based on 100 parts by weight of the polymer component (P). When the content of the crosslinking agent in the pressure-sensitive adhesive composition falls within the above range, a pressure-sensitive adhesive tape can be provided that can exhibit both more excellent impact resistance and more excellent reprocessability.
[0151] In the case of Form 2, the content of the crosslinking agent in the pressure-sensitive adhesive composition is preferably 0.01 parts by weight to 10 parts by weight, more preferably 0.1 parts by weight to 8 parts by weight, still more preferably 0.5 parts by weight to 7 parts by weight, and particularly preferably 1.5 parts by weight to 3 parts by weight, based on the total amount of 100 parts by weight of the monomer component (m). When the content of the crosslinking agent in the pressure-sensitive adhesive composition falls within the above range, a pressure-sensitive adhesive tape can be provided that can exhibit both more excellent impact resistance and more excellent reprocessability.
[0152] In the case of Form 3, the content of the crosslinking agent in the pressure-sensitive adhesive composition is preferably 0.01 parts by weight to 10 parts by weight, more preferably 0.1 parts by weight to 8 parts by weight, still more preferably 0.5 parts by weight to 7 parts by weight, and particularly preferably 1.5 parts by weight to 3 parts by weight, based on 100 parts by weight of the total of the polymer component (P) and the monomer component (m). When the content of the crosslinking agent in the pressure-sensitive adhesive composition falls within the above range, a pressure-sensitive adhesive tape can be provided that can exhibit both more excellent impact resistance and more excellent reprocessability.
[0153] In the pressure-sensitive adhesive composition, an isocyanate-based crosslinking agent and a non-isocyanate-based crosslinking agent (for example, an epoxy-based crosslinking agent) can be used in combination. In this case, the ratio of the content of the non-isocyanate-based crosslinking agent in the pressure-sensitive adhesive composition to the content of the isocyanate-based crosslinking agent in the pressure-sensitive adhesive composition is preferably 1 / 50 or less, more preferably 1 / 75 or less, still more preferably 1 / 100 or less, and particularly preferably 1 / 150 or less, because the pressure-sensitive adhesive tape according to at least one embodiment of the present invention can exhibit more excellent oil resistance. In addition, the ratio of the content of the non-isocyanate-based crosslinking agent in the pressure-sensitive adhesive composition to the content of the isocyanate-based crosslinking agent in the pressure-sensitive adhesive composition is preferably 1 / 1,000 or more, more preferably 1 / 500 or more, because the pressure-sensitive adhesive tape according to at least one embodiment of the present invention can exhibit more excellent oil resistance.
[0154] <<B. Method for manufacturing a pressure-sensitive adhesive tape>>
[0155] The pressure-sensitive adhesive tape according to at least one embodiment of the present invention can be manufactured by any appropriate method to the extent that the effects of the present invention are not impaired. The following method is given as an example of such a method: a pressure-sensitive adhesive layer is prepared separately and attached to a substrate layer by any appropriate method. When the pressure-sensitive adhesive tape according to at least one embodiment of the present invention is as follows Figure 1 When the case where the pressure-sensitive adhesive layer is included on both sides of the substrate layer is taken as an example, one example of the method is a method involving laminating two pressure-sensitive adhesive layers to the two surfaces of the substrate layer, respectively. For example, a laminator can be used for lamination. In addition, after lamination, aging can be performed at any appropriate temperature for any appropriate time as needed.
[0156] Example
[0157] Now, the present invention is specifically described by examples. However, the present invention is by no means limited to examples. The test and evaluation methods in the examples, etc. are as follows. Unless otherwise specified, the term "part" in the following description means "part by weight", and unless otherwise specified, the term "%" in the following description means "wt%".
[0158] <Weight Average Molecular Weight>
[0159] The weight average molecular weight is determined from a value converted into standard polystyrene obtained by gel permeation chromatography (GPC). An apparatus available under the model "HLC-8320GPC" (column: TSKgel GMH-H(S), manufactured by Tosoh Corporation) is used as a GPC apparatus.
[0160] <100% modulus of pressure-sensitive adhesive tape>
[0161] The double-sided pressure-sensitive adhesive tape obtained in each of the examples and comparative examples was cut into a size of 10 mm wide × 50 mm long to produce a test piece. The test piece was pulled up and down in each vertical direction at a chuck-to-chuck distance of 20 mm and a speed of 50 mm / min, and the force was measured and converted into stress.
[0162] <Impact Resistance>
[0163] The double-sided pressure-sensitive adhesive tape obtained in each of the embodiments and comparative examples sandwiched between the release liners was punched into a frame shape of 2 mm in width and 24.5 mm in profile to provide an evaluation sample. The evaluation sample was set between a square stainless steel plate (the plate had a hole of 20 mm long × 20 mm wide in its central portion) with a thickness of 2 mm and a profile of 50 mm × 50 mm and a square stainless steel plate (25 mm square in profile, 3 mm in thickness), and was pressed onto the plate (62 N × 10 seconds) in such a way that the force was uniformly applied to the sample in the direction of gravity. Afterwards, the resultant was left to stand at 80 ° C for 30 minutes and taken out. Afterwards, the resultant was returned to an environment of 23 ° C to provide a test piece. A cylindrical measuring table with a length of 50 mm, an outer diameter of 49 mm and an inner diameter of 43 mm was set on the base of a Du Pont type impact tester (manufactured by Toyo Seiki Seisaku-sho, Ltd.), and the test piece was mounted thereon in such a way that the square stainless steel plate was located on the lower side. A stainless steel impact shaft with a tip radius of 3.1 mm is mounted on the test piece, and the weight of the drop weight and its drop height are changed as follows to increase the energy until the stripping of the tape occurs: when the weight is 100 g, the height is changed from 50 mm to 500 mm in increments of 50 mm; when the weight is 150 g, the height is changed from 350 mm to 500 mm in increments of 50 mm; when the weight is 200 g, the height is changed from 400 mm to 500 mm in increments of 50 mm; and when the weight is 300 g, the height is changed from 350 mm to 500 mm in increments of 50 mm. At this time, for the energy that has been evaluated, no test is performed, and the load and height are set in such a way that the amount of energy does not overlap each other. Afterwards, the energy immediately before stripping is calculated by the expression "load × height" and used as the result. In actual use, the energy until stripping is required to be 0.3 J or more.
[0164] <Reprocessability (vertical direction)>
[0165] The double-sided pressure-sensitive adhesive tape obtained in each of Examples and Comparative Examples sandwiched between release liners on both sides was cut into a size of 10 mm wide×50 mm long, thereby producing a test piece.
[0166] One release liner of the test piece is peeled off, and by passing through once with a 2kg roller back and forth, the pressure-sensitive adhesive layer surface of the test piece is crimped to a stainless steel plate (SUS304BA plate) washed with toluene (manufactured by Nippon Kinzoku Co., Ltd.). The resulting product is stored for 24 hours under heating at 50°C. Afterwards, another release liner is peeled off, and the short side end of the test piece is peeled off from the stainless steel plate, and the test piece is continuously pulled in a direction perpendicular to the adherend to determine whether the test piece is peelable without being torn. The test piece is more capable of being peeled off but not torn, and is judged as "◎", the test piece is capable of being peeled off but not torn, and the test piece is judged as "×".
[0167] <Reprocessability (Horizontal Direction)>
[0168] The double-sided pressure-sensitive adhesive tape obtained in each of Examples and Comparative Examples having release liners arranged on both sides was cut into a size of 10 mm wide×50 mm long, thereby producing a test piece.
[0169] One release liner of the test piece is peeled off, and the pressure-sensitive adhesive layer surface of the test piece is pressed to a stainless steel plate (SUS304BA plate) (manufactured by Nippon Kinzoku Co., Ltd.) washed with toluene by a 2kg roller. The resulting product is stored for 24 hours under heating at 50°C. Afterwards, another release liner is peeled off, and the short side end of the test piece is peeled off from the stainless steel plate, and the test piece is continuously pulled at an angle of 30° relative to the adherend to determine whether the test piece is peelable without being torn. The situation where the test piece can be peeled off but not torn is judged as "○", and the situation where the test piece cannot be peeled off is judged as "×".
[0170] <Pressure-Sensitive Adhesive Strength relative to SUS>
[0171] The pressure-sensitive adhesive tape is cut into a size of 20mm wide × 150mm long, thereby manufactured a measurement sample. Under the environment of 23 ℃ and 50%RH, the pressure-sensitive adhesive layer surface of the measurement sample is exposed, and by passing through once with a 2kg rubber roller back and forth, the pressure-sensitive adhesive layer surface is crimped to the stainless steel plate (SUS304BA plate) as adherend. Under the environment of 23 ℃ and 50%RH, the peel strength (relative to the pressure-sensitive adhesive strength of SUS) (N / 20mm) of the measurement sample is measured with a tensile tester according to JIS Z0237:2000 under the condition that the peel angle is 180 ° and the peeling speed is 300mm / min. Universal stretching and compression testing machine (equipment name: "Tensile and Compression Testing Machine, TCM-1kNB", manufactured by Minebea Co., Ltd.) is used as a tensile tester. In the measurement, as required (for example, when substrate is easily deformed), the pressure-sensitive adhesive tape as the measurement object can be enhanced by fitting a suitable backing material to it. For example, a PET film having a thickness of about 50 μm may be used as a backing material, and the backing material is used in each of the Examples and Comparative Examples described herein.
[0172] [Manufacturing Example 1]: Manufacture of pressure-sensitive adhesive layer (1)
[0173] 95 parts of butyl acrylate (BA) and 5 parts of acrylic acid (AA) as monomer components and 233 parts of ethyl acetate as a polymerization solvent were charged into a reaction vessel including a stirrer, a thermometer, a nitrogen introduction tube, a reflux condenser, and a dropping funnel, and stirred for 2 hours while introducing nitrogen into the vessel. After oxygen in the polymerization system had been removed as described above, 0.2 parts of 2,2′-azobisisobutyronitrile was added to the mixture as a polymerization initiator, and the whole was subjected to solution polymerization at 60° C. for 8 hours, thereby providing a solution of an acrylic polymer. The weight average molecular weight of the acrylic polymer was 700,000.
[0174] With respect to 100 parts of the acrylic polymer in the obtained acrylic polymer solution, 20 parts of a terpene-phenol resin (trade name: "YS POLYSTER T-115", softening point: about 115° C., hydroxyl value: 30 mgKOH / g to 60 mgKOH / g, manufactured by Yasuhara Chemical Co., Ltd.) as a tackifier resin, 3 parts of an isocyanate crosslinking agent (trade name: "CORONATE L", a 75% ethyl acetate solution of a trimethylolpropane / toluene diisocyanate trimer adduct, manufactured by Tosoh Corporation) and 0.02 parts of an epoxy crosslinking agent (trade name: "TETRAD-C", 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, manufactured by Mitsubishi Gas Chemical Company, Inc.) as a crosslinking agent, and 6 parts of a product available under the trade name "AT-DN101 BLACK" (manufactured by Dainichiseika Color & Chemicals) as a black pigment were added. Mfg. Co., Ltd.) was added to the solution, and the contents were stirred and mixed to prepare a pressure-sensitive adhesive composition (1).
[0175] The pressure-sensitive adhesive composition (1) was applied to the release surface of a 38 μm thick polyester release liner (trade name: "DIAFOILMRF", manufactured by Mitsubishi Polyester Film, Inc.) and dried at 100° C. for 2 minutes to form a pressure-sensitive adhesive layer (1) having a thickness of 85.0 μm.
[0176] [Manufacturing Example 2]: Manufacture of pressure-sensitive adhesive layer (2)
[0177] A pressure-sensitive adhesive layer (2) having a thickness of 80.0 μm was formed in the same manner as in Production Example 1 except that the thickness of the final pressure-sensitive adhesive layer was set to 80.0 μm.
[0178] [Manufacturing Example 3]: Manufacture of pressure-sensitive adhesive layer (3)
[0179] A pressure-sensitive adhesive layer (3) having a thickness of 100.0 μm was formed in the same manner as in Production Example 1, except that the thickness of the final pressure-sensitive adhesive layer was set to 100.0 μm.
[0180] [Manufacturing Example 4]: Manufacture of pressure-sensitive adhesive layer (4)
[0181] A pressure-sensitive adhesive layer (4) having a thickness of 25.0 μm was formed in the same manner as in Production Example 1 except that the thickness of the final pressure-sensitive adhesive layer was set to 25.0 μm.
[0182] [Manufacturing Example 5]: Manufacture of pressure-sensitive adhesive layer (5)
[0183] A pressure-sensitive adhesive layer (5) having a thickness of 87.5 μm was formed in the same manner as in Production Example 1 except that the thickness of the final pressure-sensitive adhesive layer was set to 87.5 μm.
[0184] [Example 1]
[0185] The side of the pressure-sensitive adhesive layer (1) obtained in Production Example 1 on which the release liner was not provided was bonded to a polyethylene resin film (thickness = 30 μm, specific gravity = 0.94 g / cm 3 , MD direction breaking elongation = 660%, TD direction breaking elongation = 827%) on each of the two surfaces. The resulting structure was passed through a laminator (0.3 MPa, speed: 0.5 m / min) once at room temperature and then aged in an oven at 50°C for 1 day. Thereafter, the release liner was peeled off. Thus, as shown in Table 1, a double-sided pressure-sensitive adhesive tape (1) (construction: pressure-sensitive adhesive layer (1) / substrate layer (1) / pressure-sensitive adhesive layer (1)) having a total thickness of 200 μm was obtained.
[0186] The evaluation results are shown in Table 1.
[0187] [Example 2]
[0188] The side of the pressure-sensitive adhesive layer (1) obtained in Production Example 1 on which the release liner was not provided was bonded to a polypropylene resin film (manufactured by Toray Advanced Film Co., Ltd., trade name: "TORAYFAN3701J", thickness = 30 μm, specific gravity = 0.9 g / cm 3 ) on each of the two surfaces. The resulting structure was passed through a laminator (0.3 MPa, speed: 0.5 m / min) once at room temperature and then aged in an oven at 50° C. for 1 day. Thereafter, the release liner was peeled off. Thus, as shown in Table 1, a double-sided pressure-sensitive adhesive tape (2) having a total thickness of 200 μm (construction: pressure-sensitive adhesive layer (1) / substrate layer (2) / pressure-sensitive adhesive layer (1)) was obtained.
[0189] The evaluation results are shown in Table 1.
[0190] [Example 3]
[0191] The side of the pressure-sensitive adhesive layer (2) obtained in Production Example 2 on which the release liner was not provided was bonded to a polypropylene resin film (manufactured by Toray Advanced Film Co., Ltd., trade name: "TORAYFAN3701J", thickness = 40 μm, specific gravity = 0.9 g / cm3 ) on each of the two surfaces. The resulting structure was passed through a laminator (0.3 MPa, speed: 0.5 m / min) once at room temperature and then aged in an oven at 50° C. for 1 day. Thereafter, the release liner was peeled off. Thus, as shown in Table 1, a double-sided pressure-sensitive adhesive tape (3) (construction: pressure-sensitive adhesive layer (2) / base material layer (3) / pressure-sensitive adhesive layer (2)) having a total thickness of 200 μm was obtained.
[0192] The evaluation results are shown in Table 1.
[0193] [Example 4]
[0194] The side of the pressure-sensitive adhesive layer (1) obtained in Production Example 1 on which the release liner was not provided was bonded to a polyurethane resin film (manufactured by Okura Industrial Co., Ltd., trade name: "SILKLONNES85", thickness = 25 μm, specific gravity = 1.2 g / cm 3 ) on each of the two surfaces. The resulting structure was passed through a laminator (0.3 MPa, speed: 0.5 m / min) once at room temperature and then aged in an oven at 50° C. for 1 day. Thereafter, the release liner was peeled off. Thus, as shown in Table 1, a double-sided pressure-sensitive adhesive tape (4) having a total thickness of 200 μm (construction: pressure-sensitive adhesive layer (1) / substrate layer (4) / pressure-sensitive adhesive layer (1)) was obtained.
[0195] The evaluation results are shown in Table 1.
[0196] [Comparative Example 1]
[0197] The two pressure-sensitive adhesive layer surfaces on which the release liner was not provided of the pressure-sensitive adhesive layer (3) obtained in Production Example 3 were bonded to each other. The resulting structure was passed through a laminator (0.3 MPa, speed: 0.5 m / min) once at room temperature and then aged in an oven at 50° C. for 1 day. Thereafter, the release liner was peeled off. Thus, as shown in Table 1, a double-sided pressure-sensitive adhesive tape (C1) having a total thickness of 200 μm (construction: pressure-sensitive adhesive layer (3) / pressure-sensitive adhesive layer (3)) was obtained.
[0198] The evaluation results are shown in Table 1.
[0199] [Comparative Example 2]
[0200] The side of the pressure-sensitive adhesive layer (4) obtained in Production Example 4 on which the release liner was not provided was bonded to a polyethylene resin film (foam) (thickness = 150 μm, specific gravity = 0.30 g / cm 3, 25% compressive strength = 75KPa) on each of the two surfaces. The resulting structure was passed through a laminator (0.3MPa, speed: 0.5m / min) once at room temperature and then aged in an oven at 50°C for 1 day. Thereafter, the release liner was peeled off. Thus, as shown in Table 1, a double-sided pressure-sensitive adhesive tape (C2) (construction: pressure-sensitive adhesive layer (4) / base material layer (C2) / pressure-sensitive adhesive layer (4)) having a total thickness of 200μm was obtained.
[0201] The evaluation results are shown in Table 1.
[0202] [Comparative Example 3]
[0203] The side of the pressure-sensitive adhesive layer (5) obtained in Production Example 5 on which the release liner was not provided was bonded to a polyethylene terephthalate (PET) resin film (manufactured by Toray Industries, Inc., trade name: "Lumirror", thickness = 25 μm, specific gravity = 1.4 g / cm 3 ) on each of the two surfaces. The resulting structure was passed through a laminator (0.3 MPa, speed: 0.5 m / min) once at room temperature and then aged in an oven at 50° C. for 1 day. Thereafter, the release liner was peeled off. Thus, as shown in Table 1, a double-sided pressure-sensitive adhesive tape (C3) (construction: pressure-sensitive adhesive layer (5) / base material layer (C3) / pressure-sensitive adhesive layer (5)) having a total thickness of 200 μm was obtained.
[0204] The evaluation results are shown in Table 1.
[0205] Table 1
[0206]
[0207] The pressure-sensitive adhesive tape according to at least one embodiment of the present invention may be suitably used for the interior of a mobile device, etc. The pressure-sensitive adhesive tape according to at least one embodiment of the present invention is typically used for fixing electronic device members.
[0208] According to at least one embodiment of the present invention, a pressure-sensitive adhesive tape that can exhibit both excellent impact resistance and excellent reworkability can be provided.
Claims
1. A pressure-sensitive adhesive tape comprising: substrate layer; and a pressure-sensitive adhesive layer disposed on at least one side of the substrate layer, The specific gravity of the substrate layer is 0.8 g / cm 3 above, The base material layer is formed of a resin film, The resin film contains one of a polyolefin-based resin and a polyurethane-based resin as a main component, The thickness of the substrate layer is 5 μm to 50 μm, The ratio of the thickness of the substrate layer to the total thickness of the pressure-sensitive adhesive tape is less than 40%, and wherein the 100% modulus of the pressure-sensitive adhesive tape at 23° C. and 50% RH is 50 MPa or less.
2. The pressure-sensitive adhesive tape according to claim 1, wherein the pressure-sensitive adhesive layer is formed from a pressure-sensitive adhesive composition, wherein the pressure-sensitive adhesive composition comprises at least one selected from the group consisting of a monomer component (m) and a polymer component (P) obtained by polymerizing the monomer component (m), and The monomer component (m) contains 50 wt % or more of butyl (meth)acrylate. 3 . The pressure-sensitive adhesive tape according to claim 2 , wherein the monomer component (m) comprises 90 wt % to 99 wt % of butyl (meth)acrylate. 4 . The pressure-sensitive adhesive tape according to claim 2 , wherein the monomer component (m) comprises 1 wt % to 10 wt % of (meth)acrylic acid. 5 . The pressure-sensitive adhesive tape according to claim 1 , wherein the total thickness of the pressure-sensitive adhesive tape is 100 μm or more. The pressure-sensitive adhesive tape according to claim 1 , wherein the pressure-sensitive adhesive tape is used for fixing electronic device members.
Citation Information
Patent Citations
Protecting film for blade of wind power generator
CN101993666A
Adhesive sheet
CN107739578A
Steam-permeable film of thermoplastic elastomer of polyether-ester-amide base, preparation of said film, and article made of said film
JP1990199131A
Double-side tacky tape
JP1994346032A
Plaster for external use
JP1998279472A