Liquid crystal polymer film and laminate containing the same

By controlling the surface roughness of the liquid crystal polymer film, especially Sa less than 0.32 microns, the problem of large signal loss of the laminate in the high-frequency band is solved, and a laminate with low loss and high peel strength is achieved, which is suitable for high-frequency applications. electronic products.

CN113087938BActive Publication Date: 2024-10-29CHANG CHUN PLASTICS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202011494479.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-17
Publication Date
2024-10-29
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Existing liquid crystal polymer film laminates suffer significant signal loss when transmitting in high-frequency bands, making it difficult to meet the excellent transmission quality requirements of high-frequency electronic products.

Method used

By controlling the surface arithmetic average height (Sa) of the first surface and the second surface of the liquid crystal polymer film to be less than 0.32 microns, signal loss is slowed down or suppressed, and the maximum surface height (Sz) is adjusted when necessary to improve the peeling strength.

Benefits of technology

It achieves low signal loss of the laminate in the high-frequency band and is suitable for high-frequency electronic products. It also improves the peeling strength of the liquid crystal polymer film and the metal foil to avoid the problem of circuit detachment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002841351750000071
    Figure BDA0002841351750000071
  • Figure BDA0002841351750000081
    Figure BDA0002841351750000081
  • Figure BDA0002841351750000121
    Figure BDA0002841351750000121
Patent Text Reader

Abstract

The present invention provides a liquid crystal polymer film and a laminated board containing the same. The liquid crystal polymer film has a first surface and a second surface opposite to each other, and the surface arithmetic mean height Sa of the first surface is less than 0.32 microns. By controlling the Sa of the liquid crystal polymer film, the liquid crystal polymer film of the present invention can be applied to be laminated with a metal foil, so that the laminated board containing the liquid crystal polymer film has the advantage of low signal loss.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polymer film, in particular to a liquid crystal polymer film and a laminate comprising the same. Background Art

[0002] With the rapid development of mobile communication technology, the industry is actively developing the fifth generation mobile communication technology (5th generation mobile networks, referred to as 5G) to optimize the data transmission speed, response time, system capacity and other performance of 4G communication technology.

[0003] Since 5G communication technology uses high-frequency bands for signal transmission, the higher the signal frequency, the more significant the attenuation and distortion of the signal during transmission, and the greater the signal loss (insertion loss). Therefore, the existing technology selects a liquid crystal polymer film (LCP film) with low hygroscopicity and relatively low dielectric properties to replace the polyimide film (PI film) with high hygroscopicity and relatively high dielectric properties, and laminates the LCP film with metal foil to form a laminate to achieve signal transmission in the high-frequency band.

[0004] However, with the advancement of the technology industry, current products no longer meet demand. The industry is actively pursuing various electronic products to have better transmission quality. How to further slow down or suppress the signal loss of laminated boards has become a topic of active research and development in all walks of life. Summary of the invention

[0005] In view of this, the purpose of the present invention is to mitigate or suppress the signal loss generated when a laminate containing a liquid crystal polymer film transmits signals in a high-frequency band, thereby making the laminate more suitable for high-frequency electronic products.

[0006] To achieve the above object, the present invention provides a liquid crystal polymer film having a first surface and a second surface opposite to each other, wherein the arithmetic mean height of a surface (Sa) of the first surface is less than 0.32 micrometers (μm).

[0007] By controlling the Sa of the first surface of the liquid crystal polymer film, it is possible to mitigate or suppress the signal loss caused by the laminate containing the liquid crystal polymer film transmitting signals in the high-frequency band, so that the laminate can be suitable for high-frequency electronic products (for example, 5G products).

[0008] In addition to controlling the Sa of the first surface of the liquid crystal polymer film, in one embodiment of the present invention, the Sa of the second surface of the liquid crystal polymer film of the present invention can also be controlled to be less than 0.32 microns. Accordingly, the liquid crystal polymer film of the present invention can make the laminate have the advantage of low signal loss whether it is laminated with at least one metal foil through the first surface, the second surface or both of them.

[0009] Optionally, Sa of the first surface of the liquid crystal polymer film of the present invention may also be any of the following values ​​(all in micrometers): 0.31, 0.30, 0.29, 0.28, 0.27, 0.26, 0.25, 0.24, 0.23, 0.22, 0.21, 0.20, 0.19, 0.18, 0.17, 0.16, 0.15, 0.14, 0.13, 0.12, 0.11, 0.10, 0.09, 0.08, 0.07, 0.06, 0.05, 0.04, 0.039, 0.038, 0.037, 0.036, 0.035, 0.034, 0.033, 0.032, 0.031, 0.030, 0.029, 0.028. Alternatively, the Sa of the first surface of the liquid crystal polymer film is within the range formed by any two of the above values, but is not limited thereto. In one embodiment, the Sa of the first surface of the liquid crystal polymer film of the present invention may be less than or equal to 0.31 microns; in another embodiment, the Sa of the first surface of the liquid crystal polymer film of the present invention may be less than or equal to 0.30 microns; in another embodiment, the Sa of the first surface of the liquid crystal polymer film of the present invention may be less than or equal to 0.29 microns; in another embodiment, the Sa of the first surface of the liquid crystal polymer film of the present invention may be greater than or equal to 0.028 microns; in another embodiment, the Sa of the first surface of the liquid crystal polymer film of the present invention is 0.028 microns to 0.290 microns; in another embodiment, the Sa of the first surface of the liquid crystal polymer film of the present invention is 0.028 microns to 0.289 microns. In one embodiment, the Sa of the first surface and the Sa of the second surface of the liquid crystal polymer film of the present invention both fall within the aforementioned range. As required, the Sa of the first surface and the Sa of the second surface of the liquid crystal polymer film of the present invention may be the same or different. In one embodiment, Sa of the first surface and Sa of the second surface of the liquid crystal polymer film of the present invention are different.

[0010] In one embodiment, the maximum height of a surface (Sz) of the first surface of the liquid crystal polymer film of the present invention may be greater than or equal to 0.8 micrometers. Optionally, the Sz of the first surface of the liquid crystal polymer film of the present invention may also be any of the following values ​​(all in micrometers): 0.80, 0.81, 0.82, 0.83, 0.84, 0.85, 0.86, 0.87, 0.88, 0.89, 0.90, 0.91, 0.92, 0.93, 0.94, 0.95, 0.96, 0.97, 0.98, 0.99, 1.00, 1.10, 1.20, 1.30, 1.40, 1.50, 1.60, 1.70, 1.80, 1.90, 2.00, 2.10, 2.20, 2.30, 2.40, 2.50, 2.60, 2.70, 2.80, 2.90, 3.00, 3.10, 3.20, 3.30, 3.40, 3.50, 3.60, 3.70, 3.80, 3.90, 4.00, 4.11, 4.12, 4.13, 4.14, 4.15 20, 3.30, 3.40, 3.50, 3.60, 3.70, 3.80, 3.90, 4.00, 4.10, 4.20, 4.30, 4.40, 4.50, 4.60, 4.70, 4.80, 4.90, 5.00, 5.10, 5.20, 5.30, 5.40, 5.50, 5.60, 5.7 0, 5.80, 5.90, 6.00, 6.10, 6.20, 6.30, 6.40, 6.50, 6.60, 6.70, 6.80, 6.90, 7.00, 7.10, 7.20, 7.21, 7.22, 7.23, 7.24, 7.25, 7.26, 7.27, 7.28, 7.29, 7.30. Alternatively, the Sz of the first surface of the liquid crystal polymer film may also be within the range consisting of any two of the above values, but is not limited thereto. Preferably, the Sz of the first surface of the liquid crystal polymer film of the present invention may be greater than or equal to 0.9 microns; more preferably, the Sz of the first surface of the liquid crystal polymer film of the present invention may be greater than or equal to 0.92 microns; therefore, the liquid crystal polymer film of the present invention is applied to the laminated board, in addition to having the advantage of low signal loss, and can also make the liquid crystal polymer film and the metal foil have better peel strength (peel strength), thereby avoiding the problem of the laminated board such as circuit shedding during subsequent processing. In another embodiment, the Sz of the first surface of the liquid crystal polymer film of the present invention may be less than or equal to 7.30 microns; in another embodiment, the Sz of the first surface of the liquid crystal polymer film of the present invention may be 0.92 microns to 7.30 microns. In yet another embodiment, the Sz of the first surface of the liquid crystal polymer film of the present invention may be 0.921 microns to 7.239 microns. In one embodiment of the present invention, the Sz of the first surface and the Sz of the second surface of the liquid crystal polymer film of the present invention both fall within the aforementioned range.As required, the Sz of the first surface and the Sz of the second surface of the liquid crystal polymer film of the present invention may be the same or different. In one embodiment, the Sz of the first surface and the Sz of the second surface of the liquid crystal polymer film of the present invention are different.

[0011] The liquid crystal polymer film of the present invention can be prepared using commercially available liquid crystal polymer resins, or using conventional raw materials in the art, and there is no particular limitation in the present invention. For example, aromatic or aliphatic hydroxy compounds (e.g., hydroquinone, resorcin, 2,6-naphthalenediol, ethanediol, 1,4-butanediol, 1,6-hexanediol), aromatic or aliphatic dicarboxylic acids (e.g., terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2-chloroterephthalic acid, adipic acid), aromatic hydroxycarboxylic acids (e.g., 3-hydroxybenzoic acid, 4-hydroxybenzoic acid, 6-hydroxy-2-naphthalene carboxylic ... A liquid crystal polymer resin is prepared by using 6-hydroxy-2-naphthoic acid, 4-hydroxybenzoic acid and acetyl anhydride as raw materials to prepare the liquid crystal polymer film of the present invention. In one embodiment of the present invention, 6-hydroxy-2-naphthoic acid, 4-hydroxybenzoic acid and acetyl anhydride can be used to obtain the liquid crystal polymer resin for preparing the liquid crystal polymer film of the present invention. In one embodiment, the melting point of the liquid crystal polymer resin is about 250° C. to 360° C.

[0012] In one embodiment, those skilled in the art may add additives such as lubricants, antioxidants, electrical insulators or fillers when preparing the liquid crystal polymer film of the present invention according to different needs, but are not limited thereto. For example, the optional additives are polycarbonate, polyamide, polyphenylene sulfide or polyetheretherketone, but are not limited thereto.

[0013] The thickness of the liquid crystal polymer film of the present invention is not particularly limited. For example, the thickness of the liquid crystal polymer film may be 10 microns to 500 microns; preferably, the thickness of the liquid crystal polymer film of the present invention may be 10 microns to 300 microns; more preferably, the thickness of the liquid crystal polymer film of the present invention may be 15 microns to 250 microns; even more preferably, the thickness of the liquid crystal polymer film of the present invention may be 15 microns to 200 microns; even more preferably, the thickness of the liquid crystal polymer film of the present invention may be 20 microns to 200 microns.

[0014] To achieve the aforementioned objectives, the present invention further provides a laminated board, which comprises a first metal foil and the above-mentioned liquid crystal polymer film of the present invention, wherein the first metal foil is disposed on the first surface of the liquid crystal polymer film, that is, in the laminated board of the present invention, the first metal foil is superimposed on the first surface of the liquid crystal polymer film.

[0015] As mentioned above, since the Sa of the first surface of the liquid crystal polymer film is less than 0.32 micrometers, the laminate including such a liquid crystal polymer film can have the advantage of low signal loss, making the laminate suitable for high-frequency electronic products.

[0016] In one embodiment, the laminate of the present invention contains a liquid crystal polymer film with a thickness of about 50 microns, and the signal loss generated by this laminate at a high frequency of 10 gigahertz (GHz) may not exceed -3.0 decibels (decibel, dB) / 10 cm; specifically, in one embodiment, the laminate of the present invention contains a liquid crystal polymer film with a thickness of about 50 microns, and the signal loss generated by this laminate at a high frequency of 10 GHz can be controlled within -2.8 dB / 10 cm to -3.0 dB / 10 cm.

[0017] In one embodiment, the laminate of the present invention may further include a second metal foil, and the second metal foil is disposed on the second surface of the liquid crystal polymer film, that is, in the laminate of the present invention, the first metal foil is stacked on the first surface of the liquid crystal polymer film, and the second metal foil is stacked on the second surface of the liquid crystal polymer film. In this embodiment, the Sa of the first and second surfaces of the liquid crystal polymer film can be controlled simultaneously, so that the laminate has the advantage of low signal loss. Alternatively, the Sa and Sz of the first and second surfaces of the liquid crystal polymer film can be controlled simultaneously, so that in addition to the advantage of low signal loss, the laminate can also simultaneously improve the adhesion of the liquid crystal polymer film stacked on the first and second metal foils, that is, the peel strength between the liquid crystal polymer film and the first and second metal foils is simultaneously improved.

[0018] In the present invention, "overlapping" is not limited to direct contact, but also includes indirect contact. For example, in one embodiment of the present invention, the first metal foil in the laminate is in direct contact with the first surface of the liquid crystal polymer film. In another embodiment of the present invention, the first metal foil in the laminate is in indirect contact with the first surface of the liquid crystal polymer film. Specifically, a connecting layer can be provided between the first metal foil and the first surface of the liquid crystal polymer film according to different requirements, so that the first metal foil and the first surface of the liquid crystal polymer film are in contact through the connecting layer. The material of the connecting layer can be adjusted according to different requirements; for example, the material of the connecting layer can include nickel, cobalt, chromium or its alloy to provide, for example, heat resistance, chemical resistance, or electrical resistance. Similarly, the second metal foil in the laminate and the liquid crystal polymer film can also be selected to overlap in direct contact or indirect contact. In one embodiment, the overlapping method of the liquid crystal polymer film and the first metal foil is the same as the overlapping method of the liquid crystal polymer film and the second metal foil. In one embodiment, the stacking method of the liquid crystal polymer film and the first metal foil is different from the stacking method of the liquid crystal polymer film and the second metal foil.

[0019] In the present invention, the first metal foil and / or the second metal foil may be copper foil, gold foil, silver foil, nickel foil, aluminum foil or stainless steel foil, etc., but are not limited thereto. In one embodiment, the first metal foil and the second metal foil are made of different materials. Preferably, the first metal foil and / or the second metal foil may be copper foil, and the copper foil and the liquid crystal polymer film are laminated to form a copper clad laminate (CCL). In addition, the preparation method of the first metal foil and / or the second metal foil is not particularly limited, as long as it does not violate the purpose of the present invention. For example, a rolling method or an electrolytic method may be selected for preparation, but are not limited thereto.

[0020] In the present invention, the thickness of the first metal foil and / or the second metal foil is not particularly limited, and those skilled in the art may make corresponding adjustments according to different requirements. For example, in one embodiment, the thickness of the first metal foil and / or the second metal foil may be independently 1 micron to 200 microns; preferably, the thickness of the first metal foil and / or the second metal foil may be independently 1 micron to 40 microns; more preferably, the thickness of the first metal foil and / or the second metal foil may be independently 3 microns to 40 microns.

[0021] In the present invention, those skilled in the art can perform surface treatment on the first metal foil and / or the second metal foil of the present invention according to different needs. For example, roughening treatment, acid-base treatment, heating treatment, degreasing treatment, ultraviolet irradiation treatment, corona discharge treatment, plasma treatment, primer coating treatment, etc. can be selected, but are not limited to these.

[0022] In the present invention, there is no particular restriction on the roughness of the first metal foil and / or the second metal foil, and those skilled in the art can make corresponding adjustments according to different needs. In one embodiment, the ten-point mean roughness (Rz) of the first metal foil and / or the second metal foil can be independently greater than or equal to 0.1 microns and less than or equal to 2.0 microns. Preferably, the Rz of the first metal foil and / or the second metal foil can be independently greater than or equal to 0.1 microns and less than or equal to 1.5 microns. In one embodiment, the Rz of the first metal foil and the Rz of the second metal foil can both fall within the aforementioned range. In one embodiment, the Rz of the first metal foil and / or the second metal foil can be equal to 1.0 microns. As needed, the Rz of the first metal foil and the second metal foil can be the same or different. In one embodiment, the Rz of the first metal foil is not the same as the Rz of the second metal foil.

[0023] In one embodiment, a person skilled in the art may additionally provide a third metal foil according to different requirements. The third metal foil may be the same as or different from the first metal foil and / or the second metal foil as required. In one embodiment, the Rz of the third metal foil may fall within the Rz range of the first metal foil and / or the second metal foil. In one embodiment, the Rz of the first metal foil, the Rz of the second metal foil, and the Rz of the third metal foil are not the same.

[0024] Preferably, the first metal foil, the second metal foil and / or the third metal foil may be a metal foil with low roughness, such as a copper foil with low roughness. In one embodiment, the Rz of the first metal foil, the second metal foil and / or the third metal foil may be less than 1.5 microns. In another embodiment, the Rz of the first metal foil, the second metal foil and / or the third metal foil may be equal to 1.0 microns.

[0025] In one embodiment, the laminate may include multiple layers of liquid crystal polymer films. Without violating the protection scope of the present invention, those skilled in the art may laminate multiple layers of the liquid crystal polymer films of the present invention with multiple layers (two or three layers or more) of metal foils (for example, the first metal foil, the second metal foil and / or the third metal foil) according to different needs to obtain a laminate having multiple layers of liquid crystal polymer films and multiple layers of metal foils.

[0026] In this specification, "area arithmetic mean height" (Sa) and "area maximum height" (Sz) are both area roughness defined according to the standard method specified in ISO25178:2012. Those skilled in the art should understand that the area roughness describing a specific surface is different from the line roughness describing the specific surface, and the two cannot be analogized to each other. For example, the area arithmetic mean height (Sa) cannot be analogized to the arithmetic mean roughness (Ra) obtained by evaluating the roughness profile, and vice versa; in addition, the area maximum height (Sz) cannot be analogized to the ten-point mean roughness (Rz) obtained by evaluating the roughness profile, and vice versa. DETAILED DESCRIPTION

[0027] Hereinafter, several preparation examples are listed to illustrate the raw materials used to make the liquid crystal polymer film of the present invention, and several embodiments are listed to illustrate the implementation methods of the liquid crystal polymer film and laminated board of the present invention, and several comparative examples are provided as controls. Those skilled in the art can easily understand the advantages and effects that can be achieved by the present invention through the contents of the following embodiments and comparative examples. It should be understood that the embodiments of this specification are only used to illustrate the implementation methods of the present invention, and are not used to limit the scope of the present invention. Those skilled in the art can make various modifications and changes based on their common knowledge without departing from the spirit of the present invention to implement or apply the contents of the present invention.

[0028] Liquid crystal polymer resin

[0029] Preparation example: Liquid crystal polymer resin

[0030] In a 3-liter autoclave, 440 grams of 6-hydroxy-2-naphthoic acid, 1145 grams of 4-hydroxybenzoic acid, 1085 grams of acetic anhydride and 1.3 grams of sodium phosphite were mixed and subjected to an acetylation reaction for about 2 hours under a nitrogen atmosphere at 160° C. and normal pressure. Then, the temperature was raised to 320° C. at a heating rate of 30° C. per hour, and then under this temperature condition, the pressure was slowly reduced from 760 torr to below 3 torr and the temperature was raised from 320° C. to 340° C. Afterwards, the stirring power was increased, the pressure was increased, the material was discharged, the strips were drawn, and the pellets were cut to obtain a liquid crystal polymer resin with a melting point of about 305° C. and a viscosity (@320° C.) of about 40 Pa□s.

[0031] Liquid crystal polymer film

[0032] Examples 1 to 12, Comparative Examples 1 to 5: Liquid crystal polymer film

[0033] The liquid crystal polymer resin of the aforementioned preparation example was selected as a raw material, and the liquid crystal polymer films of Examples 1 to 12 and Comparative Examples 1 to 5 were prepared respectively by the following method.

[0034] First, a liquid crystal polymer resin is fed into an extruder (instrument model: ZSE27, purchased from Leistritz) with a screw diameter of 27 mm and heated to 300° C. to 330° C., and then extruded from a T-die with a width of 500 mm and a temperature of 300° C. to 330° C. at a feeding rate of 5.5 kg / hr to 9.5 kg / hr. Then, the liquid crystal polymer resin is passed into a space between two casting wheels with a distance of about 5 to 40 mm from the T-die, a temperature of about 290° C. to 330° C., and a diameter of about 35 cm to 45 cm, and extruded with a force of about 20 kilonewtons (kN) to 60 kN. Afterwards, the liquid crystal polymer film with a thickness of about 50 micrometers (μm) and a melting point of about 250° C. to 360° C. is obtained.

[0035] The process parameters set in each embodiment and comparative example are listed in the following Table 1. The process differences in preparing the liquid crystal polymer films of embodiments 1 to 12 and comparative examples 1 to 5 are mainly in: the distance from the T-die to the casting wheel surface, the feeding speed and the temperature set in the extruder.

[0036] Table 1: Process parameters for preparing the liquid crystal polymer films of Examples 1 to 12 and Comparative Examples 1 to 5.

[0037]

[0038]

[0039] The above-mentioned method for preparing liquid crystal polymer film is only used to illustrate the embodiments of the present invention. Those skilled in the art may select conventional methods such as laminate extension method, inflation method, solution casting method, etc. to prepare liquid crystal polymer film.

[0040] In one embodiment, after the liquid crystal polymer resin is extruded from the T-die, a person skilled in the art may, as needed, pass the liquid crystal polymer resin and two high temperature resistant films into the space between two casting wheels to further form a three-layer laminated structure, and then peel off the high temperature resistant film and the liquid crystal polymer resin at room temperature to obtain the liquid crystal polymer film of the present invention. It is understood that there is no special restriction on the diameter of the casting wheel; the high temperature resistant film may be selected from, for example, polytetrafluoroethylene film (PTFE film), polyimide film (PI film), polyether sulfone film (PES film), but is not limited thereto.

[0041] In addition, the technicians in this field can perform post-treatments such as polishing, ultraviolet irradiation, heating, plasma, etc. on the prepared liquid crystal polymer film according to different needs, but it is not limited to this. For example, for plasma post-treatment, the technicians in this field can also perform 1 kilowatt plasma post-treatment in nitrogen, oxygen or air atmosphere, in reduced pressure or normal pressure (1 atmosphere) environment according to different needs, but it is not limited to this.

[0042] Test Example 1: Surface Roughness Analysis of Liquid Crystal Polymer Film

[0043] In this test example, the liquid crystal polymer films prepared in the above-mentioned Examples 1 to 12 and Comparative Examples 1 to 5 are used as test samples, and the surface roughness of one surface of each test sample, namely, Sa and Sz, is analyzed according to the standard method specified in ISO25178:2012.

[0044] To measure the Sa and Sz of each sample to be tested, a laser scanning conjugate microscope (model: LEXTOLS5000-SAF, purchased from Olympus Corporation, objective lens: MPLAPON-50xLEXT) was first used to observe the surface morphology of each sample to be tested and obtain its image under the conditions of a light source with a wavelength of 405 nanometers, an objective lens magnification of 50 times, and an optical zoom of 1.0 times at a temperature of 24±3°C and a relative humidity of 63±3%. After that, the above image was analyzed with the setting mode of eliminating autotilt removal and a resolution of 1024 pixels (pixels)×1024pixels to obtain the Sa and Sz of each sample to be tested.

[0045] According to the above analysis method, the measurement results of Sa and Sz of one surface of the liquid crystal polymer films of Examples 1 to 12 and Comparative Examples 1 to 5 are listed in Table 2 below.

[0046] Table 2: Sa and Sz results of the liquid crystal polymer films of Examples 1 to 12 and Comparative Examples 1 to 5.

[0047] Sa(micrometer) Sz(micrometer) Example 1 0.098 4.856 Example 2 0.058 2.347 Example 3 0.043 1.602 Example 4 0.289 7.239 Example 5 0.195 5.609 Example 6 0.187 2.591 Example 7 0.179 1.806 Example 8 0.164 1.334 Example 9 0.051 4.386 Example 10 0.028 1.402 Embodiment 11 0.036 0.921 Example 12 0.037 0.864 Comparative Example 1 0.441 5.826 Comparative Example 2 0.437 3.186 Comparative Example 3 0.426 2.394 Comparative Example 4 0.396 1.535 Comparative Example 5 0.320 0.893

[0048] As shown in Table 2 above, the Sa of one of the surfaces of the liquid crystal polymer films of Examples 1 to 12 is less than 0.32 micrometers, but the Sa of one of the surfaces of the liquid crystal polymer films of Comparative Examples 1 to 5 is greater than or equal to 0.32 micrometers. For the liquid crystal polymer films of Examples 1 to 12, in addition to the Sa less than 0.32 micrometers, the Sz of one of the surfaces of the liquid crystal polymer films of Examples 1 to 12 can be greater than or equal to 0.8 micrometers, that is, one of the surfaces of the liquid crystal polymer films of Examples 1 to 12 has the characteristics of (1) Sa less than 0.32 micrometers and (2) Sz greater than or equal to 0.8 micrometers.

[0049] Test Example 2: Comparison of Ra and Sa of Liquid Crystal Polymer Film

[0050] In order to explore the difference between line roughness (e.g., Ra) and surface roughness (e.g., Sa), this test example takes the liquid crystal polymer films of Examples 5, 6 and Comparative Example 5 as examples from the aforementioned multiple embodiments and comparative examples, and analyzes the line roughness of one surface of the liquid crystal polymer film according to the standard method specified in JISB 0601:1994, and analyzes the surface roughness of one surface of the liquid crystal polymer film according to the standard method specified in ISO25178:2012.

[0051] When measuring the Ra of one surface of the liquid crystal polymer film of Examples 5, 6 and Comparative Example 5, a laser scanning conjugate focus microscope (model: LEXT OLS5000-SAF, purchased from Olympus Corporation, objective lens: MPLAPON-50xLEXT) was first used to observe the surface morphology of each sample under the conditions of a light source with a wavelength of 405 nanometers, an objective lens magnification of 50 times, and an optical zoom of 1.0 times at a temperature of 24±3°C and a relative humidity of 63±3%, and to obtain its image. Afterwards, the aforementioned image was analyzed with an evaluation length of 4 mm and a cutoff value of 0.8 mm to obtain the Ra of each liquid crystal polymer film, and the results are listed in Table 3.

[0052] In this test example, the method for measuring the surface roughness is the same as the method described in the above test example 1, and the measurement results are the same as those shown in Table 2. In order to facilitate the confirmation of the difference between Ra and Sa, in addition to the Ra of the liquid crystal polymer film, the Sa of the liquid crystal polymer films of Examples 5, 6 and Comparative Example 5 in Table 2 are also listed in Table 3 below.

[0053] Table 3: Ra and Sa results of the liquid crystal polymer films of Examples 5, 6 and Comparative Example 5.

[0054] Ra(μm) Sa(micrometer) Example 5 0.086 0.195 Example 6 0.089 0.187 Comparative Example 5 0.096 0.320

[0055] As shown in Table 3 above, the Ra ranking and Sa ranking of the three liquid crystal polymer films are as follows:

[0056] Ra ranking: Example 5 < Example 6 < Comparative Example 5;

[0057] Sa ranking: Example 6 < Example 5 < Comparative Example 5.

[0058] It can be seen that the relative increasing relationship of Ra of multiple liquid crystal polymer films is obviously different from the relative increasing relationship of Sa of multiple liquid crystal polymer films, and it can be seen that Ra and Sa cannot be directly inferred from each other. The difference in Ra or Sa is discussed from the relative magnification of the maximum and minimum values ​​in these three liquid crystal polymer films. The Ra of the liquid crystal polymer film of Comparative Example 5 (the maximum value among the three Ra) is close to the Ra of the liquid crystal polymer film of Example 5 (the minimum value among the three Ra), but the Sa of the liquid crystal polymer film of Comparative Example 5 (the maximum value among the three Sa) and the Sa of the liquid crystal polymer film of Example 6 (the minimum value among the three Sa) differ by about 1.7 times; the experimental results show that even if the liquid crystal polymer films of Example 5 and Comparative Example 5 have similar Ra, the two can still have Sa with relatively different differences. This result once again shows that Ra and Sa cannot be directly inferred from each other.

[0059] Test Example 3: Comparison of Rz and Sz of Liquid Crystal Polymer Films

[0060] In order to explore the difference between line roughness (e.g., Rz) and surface roughness (e.g., Sz), this test example takes the liquid crystal polymer films of Example 1 and Example 12 as examples, and analyzes the line roughness of one surface of the liquid crystal polymer film according to the standard method specified in JISB 0601:1994, and analyzes the surface roughness of one surface of the liquid crystal polymer film according to the standard method specified in ISO25178:2012.

[0061] When measuring the Rz of one surface of the liquid crystal polymer film of Example 1 and Example 12, a laser scanning conjugate focus microscope (model: LEXT OLS5000-SAF, purchased from Olympus Corporation, objective lens: MPLAPON-50xLEXT) was first used to observe the surface morphology of each sample under the conditions of a light source with a wavelength of 405 nanometers, an objective lens magnification of 50 times, and an optical zoom of 1.0 times at a temperature of 24±3°C and a relative humidity of 63±3%, and to obtain its image. Afterwards, the aforementioned image was analyzed with an evaluation length of 4 mm and a cutoff value of 0.8 mm to obtain the Rz of each liquid crystal polymer film, and the results are listed in the following Table 4.

[0062] In this test example, the method for measuring the surface roughness is the same as the method described in the above test example 1, and the measurement results are the same as those shown in Table 2. In order to facilitate the confirmation of the difference between Rz and Sz, in addition to listing the Rz of the liquid crystal polymer film in Table 4 below, the Sz of the liquid crystal polymer films of Example 1 and Example 12 measured in the above test example 1 are also listed in Table 4.

[0063] Table 4: Rz and Sz results of liquid crystal polymer films of Examples 1 and 12.

[0064] Rz(micrometer) Sz(micrometer) Example 1 1.406 4.856 Example 12 1.804 0.864

[0065] As shown in Table 4 above, the Rz of the liquid crystal polymer film of Example 1 is lower than the Rz of the liquid crystal polymer film of Example 12, but the Sz of the liquid crystal polymer film of Example 1 is higher than the Sz of the liquid crystal polymer film of Example 12; it can be seen that Rz and Sz cannot be directly analogized to each other. Then, the difference in Rz or Sz is discussed from the relative magnification of the two. The Rz of the liquid crystal polymer film of Example 12 is only about 1.3 times higher than the Rz of the liquid crystal polymer film of Example 1, but the Sz of the liquid crystal polymer film of Example 1 is about 5.6 times higher than the Sz of the liquid crystal polymer film of Example 12; the experimental results show that even if the liquid crystal polymer films of Example 1 and Example 12 have similar Rz, the two can still have Sz that is quite different. This result once again shows that Rz and Sz cannot be directly analogized to each other.

[0066] The results of the above-mentioned Test Examples 2 and 3 confirm that there is indeed a significant difference between the line roughness and the surface roughness, and it is difficult or even impossible for a person skilled in the art to predict or infer the surface roughness of the liquid crystal polymer film from the line roughness of the liquid crystal polymer film. Specifically, a person skilled in the art cannot predict or infer the Sa of the liquid crystal polymer film from the Ra of the liquid crystal polymer film, nor can he predict or infer the Sz of the liquid crystal polymer film from the Rz of the liquid crystal polymer film, and vice versa.

[0067] Laminated board

[0068] Examples 1A to 12A, Comparative Examples 1A to 5A: Laminated Boards

[0069] Here, the liquid crystal polymer films of the aforementioned embodiments 1 to 12 and comparative examples 1 to 5 are laminated with the same commercially available copper foil to prepare laminates of embodiments 1A to 12A and comparative examples 1A to 5A, respectively.

[0070] Specifically, the aforementioned liquid crystal polymer film with a thickness of about 50 microns and two commercially available copper foils with a thickness of about 12 microns (product model CF-H9A-HD2, purchased from Fukuda Metal Foil Powder Industry Co., Ltd., with an Rz of about 1.0 microns) were selected, and the aforementioned liquid crystal polymer film and the two commercially available copper foils were cut into a size of 20 cm × 20 cm, and the liquid crystal polymer film was stacked between the two commercially available copper foils; first, the temperature was 180°C, 5kg / cm 2 The pressure was continued for 60 seconds, and then the temperature was 300℃ and 20kg / cm 2 The pressure was continuously pressed for 25 minutes, and then cooled to room temperature to obtain a laminate. The sample numbers of the liquid crystal polymer films contained in each laminate are shown in Table 5 below.

[0071] There is no particular limitation on the lamination method of the laminate, and those skilled in the art may choose conventional methods such as line lamination or surface lamination to complete the lamination step; the present invention may be applied to lamination machines such as intermittent hot presses, roll-to-roll roller presses, double-belt presses, etc., but is not limited thereto. According to different requirements, those skilled in the art may also directly align the liquid crystal polymer film and the copper foil and then perform heating and pressurization steps to complete the surface lamination step.

[0072] In other embodiments, those skilled in the art may select, according to different needs, methods such as sputtering, electroplating, chemical plating, or evaporation to form a metal foil (e.g., copper foil) on the liquid crystal polymer film or a connecting layer (e.g., glue, nickel layer, cobalt layer, chromium layer, or alloy layer thereof) between the liquid crystal polymer film and the metal foil.

[0073] Test Example 4: Signal Loss Analysis of Laminated Board

[0074] In this test example, the laminates of the aforementioned embodiments 1A to 12A and comparative examples 1A to 5A were made into strip line specimens with a length of about 10 cm, a width of about 140 μm, and an impedance of about 50 ohms. A microwave network analyzer (instrument model: 8722ES, purchased from Agilent Technology) and a probe (model: ACP40-250, purchased from Cascade Microtech) were used to measure the signal loss of each specimen at 10 GHz. The results are listed in the following Table 5.

[0075] Table 5: Sa of the liquid crystal polymer films of Examples 1 to 12 and Comparative Examples 1 to 5 and the signal loss test results (@10 GHz) of the laminates of Examples 1A to 12A and Comparative Examples 1A to 5A.

[0076]

[0077]

[0078] As shown in Table 5, since the Sa of one of the surfaces of the liquid crystal polymer films of Examples 1 to 12 is less than 0.32 micrometers, the signal loss of the laminated boards (Examples 1A to 12A) formed by such liquid crystal polymer films and commercially available copper foil can be controlled below -3.0 dB / 10cm, that is, -2.8 dB / 10cm to -3.0 dB / 10cm. On the contrary, the Sa of one of the surfaces of the liquid crystal polymer films of Comparative Examples 1 to 5 is as high as 0.32 micrometers or more, so the signal loss of the laminated boards of Comparative Examples 1A to 5A has reached more than -3.1 dB / 10cm; in particular, the Sa of one of the surfaces of the liquid crystal polymer film of Comparative Example 1 is as high as 0.441 micrometers, resulting in the signal loss of the laminated board of Comparative Example 1A reaching as high as -3.2 dB / 10cm, which is difficult to meet the current industry's demand for actively improving the transmission quality of electronic products.

[0079] Experimental results show that controlling the Sa of one surface of the liquid crystal polymer film to less than 0.32 microns can help reduce the signal loss of the laminate, thereby improving the performance of the laminate in electronic products.

[0080] Test Example 5: Peel Strength Analysis of Laminated Boards

[0081] In this test example, according to the test method of IPC-TM-650 No.: 2.4.9, the laminates of the above-mentioned embodiments 1A to 12A and comparative examples 1A to 5A were made into etched specimens with a length of about 228.6 mm and a width of about 3.2 mm, and then each etched specimen was placed at a temperature of 23±2°C and a relative humidity of 50±5% for 24 hours to stabilize it; then, each etched specimen was adhered to the fixture of the test machine (instrument model: HT-9102, purchased from Hung Ta Instrument Co., Ltd.) with double-sided tape, and then the etched specimen on the fixture was peeled off at a peeling speed of 50.8 mm / min, and the peeling tension during the peeling process was continuously recorded. The peeling tension should be controlled within 15% to 85% of the test machine's tolerance, the peeling length should be at least more than 57.2 mm, and the initial peeling tension of 6.4 mm was ignored, and the results are shown in Table 6 below.

[0082] Table 6: Sa, Sz of the liquid crystal polymer films of Examples 1 to 12 and Comparative Examples 1 to 5, and the signal loss and peel strength test results of the laminates of Examples 1A to 12A and Comparative Examples 1A to 5A.

[0083]

[0084] As shown in Table 6 above, the surface roughness of the liquid crystal polymer films of Examples 1 to 11 compared with Example 12 and Comparative Examples 1 to 5 and the performance of the corresponding laminates can be seen that one of the surfaces of the liquid crystal polymer films of Examples 1 to 11 has both the surface characteristics of (1) Sa less than 0.32 microns and (2) Sz greater than or equal to 0.9 microns. Therefore, when the liquid crystal polymer films of Examples 1 to 11 are pressed with copper foil, not only can the laminates of Examples 1A to 11A have the advantage of low signal loss (less than -3.0 dB / 10 cm), but the peel strength between the liquid crystal polymer film and the copper foil can be further increased to more than 1.0 kN / m. Accordingly, in addition to adjusting the Sa of the liquid crystal polymer film, simultaneously controlling the Sz of the liquid crystal polymer film can further help optimize the performance of the liquid crystal polymer film and the copper foil pressing, thereby providing a laminate that exhibits both high peel strength and low signal loss.

[0085] In summary, the present invention can specifically slow down or suppress the signal loss of the laminated board including the liquid crystal polymer film by controlling the Sa of the first surface of the liquid crystal polymer film to be less than 0.32 microns, thereby making the laminated board including the liquid crystal polymer film suitable for high-end high-frequency products.

Claims

1. A liquid crystal polymer film having a first surface and a second surface opposite to each other, wherein the surface arithmetic mean height Sa of the first surface is 0.028 micrometers to 0.289 micrometers, and the surface maximum height Sz of the first surface is 0.921 micrometers to 7.239 micrometers.

2. The liquid crystal polymer film according to claim 1, wherein The Sa of the second surface is less than 0.32 micrometers.

3. The liquid crystal polymer film according to claim 2, wherein: The Sz of the second surface is greater than or equal to 0.8 micrometers.

4. A laminated plate comprising a first metal foil and the liquid crystal polymer film according to any one of claims 1 to 3, wherein: The first metal foil is disposed on the first surface of the liquid crystal polymer film.

5. The laminate according to claim 4, wherein: The laminate further includes a second metal foil, and the second metal foil is disposed on the second surface of the liquid crystal polymer film.

Citation Information

Patent Citations

  • Substrate for printed circuit board and printed circuit board

    US20180147815A1