Negative electrode for nonaqueous electrolyte secondary battery and nonaqueous electrolyte secondary battery

By arranging two graphite particle mixture layers with different volume change rates on the negative electrode of the non-aqueous electrolyte secondary battery, and using high-concentration inorganic fillers at the interface, the problem of interface peeling caused by repeated charging and discharging is solved and the battery cycle is improved. Characteristics and capacity maintenance.

CN113097447BActive Publication Date: 2024-10-01PANASONIC HOLDINGS CORP +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202011507442.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-23
Filing Date
2020-12-18
Publication Date
2024-10-01
Estimated Expiration
2040-12-18

AI Technical Summary

Technical Problem

The negative electrode of existing non-aqueous electrolyte secondary batteries suffers from interfacial peeling due to different volume change rates during repeated charge and discharge processes, resulting in reduced battery capacity and poor cycle characteristics.

Method used

Two layers of graphite particle mixture layers are provided on the surface of the negative electrode current collector. The volume change rates of the first layer and the second layer are different from each other, and contain a high concentration of inorganic filler at the interface. The inorganic filler content rate at the interface is higher than that of the main body. part, graphite particles are sandwiched by inorganic fillers to suppress interfacial peeling.

Benefits of technology

It effectively suppresses the interface peeling of the negative electrode mixture layer during the charge and discharge process, and improves the cycle characteristics and capacity maintenance rate of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113097447B_ABST
    Figure CN113097447B_ABST
Patent Text Reader

Abstract

The present invention provides a negative electrode for a non-aqueous electrolyte secondary battery and a non-aqueous electrolyte secondary battery. The negative electrode for a non-aqueous electrolyte secondary battery comprises a negative electrode collector, a first negative electrode mixture layer comprising first graphite particles disposed on the surface of the negative electrode collector, and a second negative electrode mixture layer comprising second graphite particles disposed on the surface of the first negative electrode mixture layer. The volume change rates of the first negative electrode mixture layer and the second negative electrode mixture layer during charge and discharge are different from each other, the first negative electrode mixture layer has an interface portion in contact with the second negative electrode mixture layer, and a main body portion present on the negative electrode collector side than the interface portion, the thickness t of the interface portion and the average particle size dg of the first graphite particles satisfy the relationship t≤dg / 2, the first negative electrode mixture layer comprises an inorganic filler, and the content of the inorganic filler in the interface portion is higher than the content of the inorganic filler contained in the main body portion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a negative electrode for a nonaqueous electrolyte secondary battery and a nonaqueous electrolyte secondary battery. Background Art

[0002] As negative electrode active materials, Sn, Si, and their oxides have attracted much attention as materials with high energy density. Patent document 1 discloses a negative electrode, which has a compound layer containing Sn, Si, and their oxides on a negative electrode collector in order to increase the capacity of a secondary battery and suppress internal short circuits, and further has a carbon material layer containing graphite on the compound layer.

[0003] However, if the negative electrode mixture layer has a two-layer structure, the upper and lower layers repeatedly expand and contract at different volume change rates due to repeated charge and discharge. Therefore, sometimes the interface between the upper and lower layers peels off, the conductive path is disconnected, and the battery capacity is reduced. From the perspective of improving the cycle characteristics, the technology of Patent Document 1 still has room for improvement.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2009-266705 Summary of the invention

[0007] Problem that the invention aims to solve

[0008] Therefore, an object of the present application is to provide a negative electrode having a two-layer structure and improved cycle characteristics.

[0009] Solutions for solving problems

[0010] A negative electrode for a non-aqueous electrolyte secondary battery as one embodiment of the present application comprises: a negative electrode collector; a first negative electrode mixture layer including first graphite particles disposed on the surface of the negative electrode collector, and a second negative electrode mixture layer including second graphite particles disposed on the surface of the first negative electrode mixture layer. The negative electrode mixture layer is characterized in that the volume change rates of the first negative electrode mixture layer and the second negative electrode mixture layer during charge and discharge are different from each other, the first negative electrode mixture layer has an interface portion in contact with the second negative electrode mixture layer, and a main body portion existing on the negative electrode collector side relative to the interface portion, the thickness t of the interface portion and the average particle size dg of the first graphite particles satisfy the relationship t≤dg / 2, the first negative electrode mixture layer contains an inorganic filler, and the content of the inorganic filler in the interface portion is higher than the content of the inorganic filler contained in the main body portion.

[0011] A nonaqueous electrolyte secondary battery as one embodiment of the present application is characterized by comprising the above-mentioned negative electrode for a nonaqueous electrolyte secondary battery, a positive electrode, and a nonaqueous electrolyte.

[0012] Effects of the Invention

[0013] According to one aspect of the present application, it is possible to suppress a decrease in battery capacity due to repeated charge and discharge. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 It is a longitudinal cross-sectional view of a cylindrical secondary battery as an example of an embodiment.

[0015] Figure 2 It is a cross-sectional view of a negative electrode as an example of an embodiment.

[0016] Description of Reference Numerals

[0017] 10 secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 outer packaging body, 16 sealing body, 17, 18 insulating plate, 19 positive electrode lead, 20 negative electrode lead, 21 groove part, 22 perforated metal plate, 23 lower valve plug, 24 insulating member, 25 upper valve plug, 26 cover, 26a opening part, 27 gasket, 30 negative electrode collector, 32 first negative electrode mixture layer, 32a interface part, 34 second negative electrode mixture layer DETAILED DESCRIPTION

[0018] As described above, in the prior art, it is difficult to suppress the reduction of battery capacity caused by repeated charge and discharge in secondary batteries obtained by using a two-layered negative electrode for high capacity. Therefore, the inventors of the present invention found through in-depth research that by providing an interface portion of a specified thickness containing an inorganic filler at a high concentration between two layers of negative electrode mixture layers with different volume change rates during charge and discharge, even if the negative electrode mixture layer is repeatedly expanded and compressed during charge and discharge, the interface peeling between the upper layer and the lower layer can be suppressed. It can be inferred that this is because: by clamping the inorganic filler between the graphite particles contained in the upper layer and the graphite particles contained in the lower layer, the inorganic filler functions like a wedge, and can suppress the sliding of the graphite particles along the surface direction. This conceived a non-aqueous electrolyte secondary battery of the following scheme that suppresses the reduction of charge and discharge cycle characteristics.

[0019] A negative electrode for a non-aqueous electrolyte secondary battery as one embodiment of the present application comprises: a negative electrode collector; a first negative electrode mixture layer including first graphite particles disposed on the surface of the negative electrode collector, and a second negative electrode mixture layer including second graphite particles disposed on the surface of the first negative electrode mixture layer. The negative electrode mixture layer is characterized in that the volume change rates of the first negative electrode mixture layer and the second negative electrode mixture layer during charge and discharge are different from each other, the first negative electrode mixture layer has an interface portion in contact with the second negative electrode mixture layer, and a main body portion existing on the negative electrode collector side relative to the interface portion, the thickness t of the interface portion and the average particle size dg of the first graphite particles satisfy the relationship t≤dg / 2, the first negative electrode mixture layer contains an inorganic filler, and the content of the inorganic filler in the interface portion is higher than the content of the inorganic filler contained in the main body portion.

[0020] Hereinafter, with reference to the accompanying drawings, an example of an embodiment of the cylindrical secondary battery described in the present application is described in detail. In the following description, specific shapes, materials, values, directions, etc. are examples for making the present invention easy to understand and can be appropriately changed according to the specifications of the cylindrical secondary battery. In addition, the outer packaging body is not limited to a cylindrical shape and can be, for example, a square shape. In addition, when the following description includes multiple embodiments and variations, it is assumed from the beginning that these feature parts are appropriately combined and used.

[0021] Figure 1 1 is an axial cross-sectional view of a cylindrical secondary battery 10 as an example of an embodiment. Figure 1 In the secondary battery 10 shown, an electrode body 14 and a nonaqueous electrolyte (not shown) are contained in an outer package 15. The electrode body 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. It should be noted that, for the sake of convenience, the sealing body 16 side is set as "upper" and the bottom side of the outer package 15 is set as "lower" for the purpose of explanation.

[0022] The interior of the secondary battery 10 is sealed by blocking the open end of the outer package 15 with the sealing body 16. Insulating plates 17 and 18 are provided above and below the electrode body 14, respectively. The positive lead 19 extends upward through the through hole of the insulating plate 17 and is welded to the bottom plate of the sealing body 16, that is, the lower surface of the perforated metal plate 22. In the secondary battery 10, the top plate of the sealing body 16, that is, the lid 26, which is electrically connected to the perforated metal plate 22, becomes the positive terminal. On the other hand, the negative lead 20 extends to the bottom side of the outer package 15 through the through hole of the insulating plate 18 and is welded to the bottom inner surface of the outer package 15. In the secondary battery 10, the outer package 15 becomes the negative terminal. It should be noted that when the negative lead 20 is provided at the terminal, the negative lead 20 extends to the bottom side of the outer package 15 through the outside of the insulating plate 18 and is welded to the bottom inner surface of the outer package 15.

[0023] The outer package 15 is, for example, a metal outer package can in a bottomed cylindrical shape. A gasket 27 is provided between the outer package 15 and the sealing body 16, so that the airtightness of the interior of the secondary battery 10 is ensured. The outer package 15 has a groove portion 21 for supporting the sealing body 16, which is formed by, for example, pressing the side portion from the outside. The groove portion 21 is preferably formed in an annular shape along the circumferential direction of the outer package 15, and supports the sealing body 16 on its upper surface via the gasket 27.

[0024] The sealing body 16 has a perforated metal plate 22, a lower valve plug 23, an insulating component 24, an upper valve plug 25 and a cover 26 stacked in sequence from the electrode body 14 side. The components constituting the sealing body 16 have, for example, a disc shape or a ring shape, and the components except the insulating component 24 are electrically connected to each other. The lower valve plug 23 and the upper valve plug 25 are connected to each other at their respective central portions, and the insulating component 24 is sandwiched between their respective edge portions. If the internal pressure of the battery rises due to abnormal heat, for example, the lower valve plug 23 breaks, whereby the upper valve plug 25 expands toward the cover 26 side and away from the lower valve plug 23, resulting in the electrical connection between the two being blocked. Furthermore, if the internal pressure rises, the upper valve plug 25 breaks, and the gas is discharged from the opening 26a of the cover 26.

[0025] Hereinafter, the positive electrode 11 , the negative electrode 12 , the separator 13 , and the non-aqueous electrolyte constituting the secondary battery 10 , particularly the negative electrode mixture layer constituting the negative electrode 12 , will be described in detail.

[0026] [negative electrode]

[0027] Figure 2 1 is a cross-sectional view of a negative electrode 12 as an example of an embodiment. The negative electrode 12 includes: a negative electrode current collector 30, a first negative electrode mixture layer 32 provided on the surface of the negative electrode current collector 30, and a second negative electrode mixture layer 34 provided on the surface of the first negative electrode mixture layer 32. The thickness of the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 may be the same or different. The thickness ratio of the first negative electrode mixture layer 32 to the second negative electrode mixture layer 34 is, for example, 3:7 to 7:3, preferably 4:6 to 6:4.

[0028] The negative electrode current collector 30 may be made of a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a thin film having the metal disposed on the surface. The thickness of the negative electrode current collector 30 is, for example, 5 μm to 30 μm.

[0029] The first negative electrode mixture layer 32 includes first graphite particles, and the second negative electrode mixture layer 34 includes second graphite particles. In other words, the first negative electrode mixture layer 32 includes at least first graphite particles as a negative electrode active material, and the second negative electrode mixture layer 34 includes at least second graphite particles as a negative electrode active material. Examples of the first graphite particles and the second graphite particles include natural graphite, artificial graphite, and the like. The average particle size (volume-converted median particle size D50, the same below) of the first graphite particles and the second graphite particles is preferably 5 μm to 30 μm, and more preferably 8 μm to 20 μm. The plane spacing (d ) of the (002) plane of the first graphite particles and the second graphite particles based on the wide-angle X-ray diffraction method is 002 ) are preferably 0.3354 nm or more, more preferably 0.3357 nm or more, and are preferably less than 0.340 nm, and are more preferably 0.338 nm or less. In addition, the crystallite size (Lc(002)) of the first graphite particle and the second graphite particle determined by X-ray diffraction is preferably 5 nm or more, more preferably 10 nm or more, and is preferably 300 nm or less, and is more preferably 200 nm or less. The interplanar spacing (d 002 When the crystallite size (Lc(002)) and the crystallite size (Lc(002)) satisfy the above ranges, the battery capacity of the secondary battery 10 tends to be larger than when the above ranges are not satisfied.

[0030] As the negative electrode active material contained in the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34, in addition to the above-mentioned graphite particles, metals such as Si and Sn that alloy with lithium, or alloys and oxides containing metal elements such as Si and Sn that reversibly absorb and release lithium ions can be listed. In the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34, the content of the graphite particles can be set to, for example, 90 mass% to 100 mass% relative to the total amount of the negative electrode active material.

[0031] The first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 may further include a binder, a thickener, etc., respectively. As a binder, for example, fluorine resin, PAN, polyimide resin, acrylic resin, polyolefin resin, styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), etc. can be listed. As a thickener, carboxymethyl cellulose (CMC) or its salt, polyacrylic acid (PAA) or its salt (PAA-Na, PAA-K, etc., or it can be a partially neutralized salt), polyvinyl alcohol (PVA), etc. can be listed. They can be used alone or in combination of two or more.

[0032] The volume change rates of the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 during charge and discharge (during charge and discharge) are different. The volume change rate of the first negative electrode mixture layer 32 may be greater than or less than the volume change rate of the second negative electrode mixture layer 34. In any case, stress is applied to the interface between the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 during charge and discharge, and peeling is likely to occur. For example, when at least one of the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 contains Si-based materials, and the content of Si-based materials in the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 are different, the volume change rates of the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 are different. Si-based materials are materials that can reversibly absorb and release lithium ions, and function as negative electrode active materials. Examples of Si-based materials include Si, alloys containing Si, and SiO x (x is 0.8 to 1.6) and other silicon oxides. Si-based materials are negative electrode materials that can improve battery capacity more than graphite particles. From the viewpoint of improving battery capacity and suppressing the reduction of fast charging cycle characteristics, the content of Si-based materials is preferably 1% to 10% by mass, and more preferably 3% to 7% by mass, relative to the total amount of negative electrode active materials. In addition, as another example, when the degree of graphitization of the first graphite particles and the second graphite particles is different, the volume change rate of the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 is different. As a material with a high degree of graphitization, natural graphite can be exemplified. On the other hand, as a material with a low degree of graphitization, artificial graphite such as hard carbon can be exemplified. It should be noted that the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 can each contain one or more negative electrode active materials, and their combination is not particularly limited as long as the volume change rates during charge and discharge are different from each other.

[0033] Artificial graphite can be made, for example, by the following operation. The coke (precursor) to be the main raw material is crushed into a specified size, and after aggregating them with an aggregating agent, they are further pressurized into a block shape. In this state, they are calcined at a temperature of 2600°C or above to graphitize them. The block-shaped body after graphitization is crushed and sieved to obtain graphite particles of the desired size. Here, the internal porosity of the graphite particles can be adjusted according to the particle size of the precursor after crushing, the particle size of the precursor in the aggregated state, etc. For example, the average particle size of the precursor after crushing is preferably in the range of 12μm to 20μm. In addition, the internal porosity of the graphite particles can also be adjusted according to the amount of volatile components added to the block-shaped body. When a part of the aggregating agent added to the coke (precursor) is volatilized during roasting, the aggregating agent can be used as a volatile component. As such an aggregating agent, asphalt can be exemplified.

[0034] like Figure 2As shown, the first negative electrode mixture layer 32 has an interface portion 32a in contact with the second negative electrode mixture layer 34, and a main body portion 32b that exists on the negative electrode collector 30 side more than the interface portion 32a. The thickness t of the interface portion 32a and the average particle size dg of the first graphite particles satisfy the relationship of t≤dg / 2. The first negative electrode mixture layer 32 contains an inorganic filler, and the content of the inorganic filler in the interface portion 32a is higher than the content of the inorganic filler in the main body portion 32b. As a result, the first graphite particles and the second graphite particles are fixed by the inorganic filler, so that the peeling at the interface between the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 can be suppressed. The content of the inorganic filler in the interface portion 32a is, for example, 1% by mass to 10% by mass, and the content of the inorganic filler in the main body portion 32b is, for example, 0% by mass to 5% by mass. When the thickness t of the interface portion 32a exceeds dg / 2, the conduction between the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 is hindered, the battery resistance of the secondary battery 10 becomes larger, and the output power of the secondary battery is reduced. In addition, the lower limit value of t can be set to, for example, dg / 10. It should be noted that the thickness t of the interface portion 32a can be measured by observing the cross section of the negative electrode using a scanning electron microscope (SEM). When the thickness of the interface portion 32a is not fixed, 10 points can be measured and the average value thereof is taken as t.

[0035] The inorganic filler may be ceramic particles. Examples of ceramic particles include alumina, boehmite, and silica. In addition, the average particle size dc of the ceramic particles and the average particle size dg of the first graphite particles preferably satisfy the relationship of dc≤dg / 10. As a result, the bonding force between the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 can be improved, and the occurrence of peeling can be more reliably suppressed. The average particle size dc of the ceramic particles is preferably dc≥dg / 30. When dc is less than dg / 30, the bonding force that fixes the first graphite particles and the second graphite particles becomes smaller, and the peeling of the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 cannot be suppressed. The average particle size dc of the ceramic particles is preferably 0.5μm to 3μm, and more preferably 0.8μm to 2μm.

[0036] The content of the inorganic filler in the interface portion 32a can be set to 1 mass % to 10 mass % relative to the content of the first graphite particles in the first negative electrode mixture layer 32. If the content of the inorganic filler is less than 1 mass %, sufficient bonding strength cannot be obtained, and if it exceeds 10 mass %, the battery resistance increases and the output power of the secondary battery decreases.

[0037] Next, an example of a specific method for forming the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 is described. For example, first, a graphite layer containing first graphite particles and SiO xAfter mixing the negative electrode active material (x is 0.8 to 1.6), thickener, binder and solvent such as water, add inorganic filler and stir until the inorganic filler is not dispersed to prepare the first negative electrode mixture slurry. Separately, mix the negative electrode active material containing the second graphite particles, thickener, binder and solvent such as water to prepare the second negative electrode mixture slurry. Furthermore, after applying the first negative electrode mixture slurry on both sides of the negative electrode collector and drying it, apply the second negative electrode mixture slurry on both sides of the coating based on the first negative electrode mixture slurry and dry it. Furthermore, the negative electrode can be formed by rolling the first negative electrode mixture layer 32 and the second negative electrode mixture layer 34 using a calendering roller. As described above, for the first negative electrode mixture slurry, by making the inorganic filler in a state where it is not fully dispersed, when the first negative electrode mixture slurry is applied to the negative electrode collector 30, the inorganic filler moves to the vicinity of the surface, and the first negative electrode mixture layer 32 forms a main body 32b and an interface portion 32a in which the inorganic filler concentration is higher than that of the main body 32b. It should be noted that in the above method, after the first negative electrode mixture slurry is applied and dried, the second negative electrode mixture slurry is applied, or the second negative electrode mixture slurry can be applied after the first negative electrode mixture slurry is applied and before drying. In addition, the second negative electrode mixture slurry can be applied on the first negative electrode mixture layer 32 after the first negative electrode mixture slurry is applied, dried and rolled.

[0038] [positive electrode]

[0039] The positive electrode 11 is composed of a positive electrode current collector such as a metal foil and a positive electrode mixture layer formed on the positive electrode current collector. The positive electrode current collector can be a foil of a metal such as aluminum that is stable in the potential range of the positive electrode, a thin film having the metal on the surface, etc. The positive electrode mixture layer contains, for example, a positive electrode active material, a binder, a conductive agent, etc.

[0040] The positive electrode 11 can be produced by, for example, applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive agent, etc., on a positive electrode current collector, drying the slurry to form a positive electrode mixture layer, and then rolling the positive electrode mixture layer.

[0041] Examples of the positive electrode active material include lithium transition metal oxides containing transition metal elements such as Co, Mn, and Ni. Lithium transition metal oxides are, for example, Li x CoO 2 , Li x NiO 2 , Li x MnO 2 , Li x Co y Ni 1-y O 2 , Li x Co y M 1-y O z, Li x Ni 1- y M y O z , Li x Mn 2 O 4 , Li x Mn 2-y M y O 4 , LiMPO 4 , Li 2 MPO 4 F (M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B; 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3). They can be used alone or in combination of multiple kinds. From the viewpoint of enabling high capacity of the non-aqueous electrolyte secondary battery, the positive electrode active material preferably contains Li x NiO 2 , Li x Co y Ni 1-y O 2 , Li x Ni 1-y M y O z (M is at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B; 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3) and other lithium nickel composite oxides.

[0042] Examples of the conductive agent include carbon-based particles such as carbon black (CB), acetylene black (AB), Ketjen black, and graphite. They can be used alone or in combination of two or more.

[0043] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF); polyacrylonitrile (PAN), polyimide-based resins, acrylic-based resins, polyolefin-based resins, etc. They can be used alone or in combination of two or more.

[0044] [Separator]

[0045] The separator 13 may be made of, for example, a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, and the like. Suitable materials for the separator include olefin resins such as polyethylene (PE) and polypropylene (PP), cellulose, and the like. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. In addition, it may be a multilayer separator including a polyethylene layer and a polypropylene layer, or a separator having an aramid resin, ceramic, or the like coated on the surface of the separator 13.

[0046] [Non-aqueous electrolyte]

[0047] The non-aqueous electrolyte comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous electrolyte is not limited to a liquid electrolyte (electrolyte) and can be a solid electrolyte using a gel-like polymer or the like. The non-aqueous solvent can use, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these. The non-aqueous solvent can contain a halogen substituted product obtained by replacing at least a portion of the hydrogen in these solvents with a halogen atom such as fluorine.

[0048] Examples of the above-mentioned esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylates such as γ-butyrolactone and γ-valerolactone; chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), ethyl propionate, and γ-butyrolactone, etc.

[0049] Examples of the ethers include cyclic ethers such as 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, and crown ethers; 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, and ethylethylene. Chain ethers such as 1,2-dimethoxyethane, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0050] As the above-mentioned halogenated compound, fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated linear carbonates, fluorinated linear carboxylates such as methyl fluoropropionate (FMP), etc. are preferably used.

[0051] The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiBF 4 , LiClO 4 , LiPF 6 , LiAsF 6 , LiSbF 6 , LiAlCl 4 , LiSCN, LiCF 3 SO 3 , LiCF 3 CO 2 , Li(P(C 2 O 4 )F 4 ), LiPF 6-x (C n F 2n+1 ) x (1 < x < 6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, Li 2 B 4 O 7 , Li(B(C 2 O 4 )F 2 ) and other borate salts; LiN(SO 2 CF 3 ) 2 , LiN(C 1 F 2l+1 SO 2 )(C m F 2m+1 SO 2 ) {l, m are integers of 1 or more} and other imide salts, etc. The lithium salts can be used alone or in combination of multiple kinds. Among these, from the viewpoints of ionic conductivity, electrochemical stability, etc., LiPF 6 is preferably used. The concentration of the lithium salt is preferably set to 0.8 to 1.8 mol with respect to 1 L of the solvent.

[0052] Examples

[0053] Hereinafter, the present application will be further described by way of examples, but the present application is not limited to these examples.

[0054] <Example 1>

[0055] [Fabrication of positive electrode]

[0056] As the positive electrode active material, lithium nickel cobalt manganese composite oxide (LiNi 0.88 Co 0.09 Mn 0.03 O 2 ). The positive electrode active material is mixed in an amount of 100 parts by mass, acetylene black as a conductive agent is mixed in an amount of 1 part by mass, and polyvinylidene fluoride powder as a binder is mixed in an amount of 0.9 parts by mass, and N-methyl-2-pyrrolidone (NMP) is further added in an appropriate amount to prepare a positive electrode mixture slurry. The slurry is applied to both sides of a positive electrode collector composed of aluminum foil (thickness of 15 μm) by a doctor blade method, and after the coating is dried, the coating is rolled by a calendering roller to produce a positive electrode having a positive electrode mixture layer formed on both sides of the positive electrode collector.

[0057] [Production of negative electrode]

[0058] As the first graphite particles and the second graphite particles, the same natural graphite with an average particle size of 12 μm is used. In addition, as an inorganic filler, boehmite with an average particle size of 1 μm is used. They are mixed in a manner such that the mass ratio of natural graphite: SiO: carboxymethyl cellulose (CMC): styrene-butadiene copolymer rubber (SBR) reaches 95:5:1:1, and kneaded in water. 5 parts by mass of boehmite are added to the mixture, and the boehmite is stirred to such an extent that the boehmite is not dispersed, thereby preparing a first negative electrode mixture slurry. In addition, they are mixed in a manner such that the mass ratio of natural graphite: carboxymethyl cellulose (CMC): styrene-butadiene copolymer rubber (SBR) reaches 98:1:1, and the mixture is kneaded in water to prepare a second negative electrode mixture slurry.

[0059] The first negative electrode mixture slurry is applied to both sides of the negative electrode collector composed of copper foil by a scraper method, and dried to form a first negative electrode mixture layer. Furthermore, the second negative electrode mixture slurry is applied on the first negative electrode mixture layer, and dried to form a second negative electrode mixture layer. At this time, the coating mass ratio per unit area of ​​the first negative electrode mixture slurry and the second negative electrode mixture slurry is set to 5:5. The first negative electrode mixture layer and the second negative electrode mixture layer are rolled by a calendering roller to produce a negative electrode. Based on the results of cross-sectional observation by SEM, the thickness of the interface portion is 3μm.

[0060] [Preparation of non-aqueous electrolyte]

[0061] Ethylene carbonate (EC), ethyl methyl carbonate (MEC) and dimethyl carbonate (DMC) were mixed at a volume ratio of 20:40:40. Lithium hexafluorophosphate (LiPF 6 ) is dissolved in a concentration of 1 mol / L to prepare a non-aqueous electrolyte.

[0062] [Production of test battery cells]

[0063] An aluminum lead was installed on the positive electrode, and a nickel lead was installed on the negative electrode, and the positive electrode and the negative electrode were stacked with a PP / PE / PP three-layer separator to prepare a stacked electrode body. The electrode body was housed in an outer package composed of an aluminum laminate sheet, and after the non-aqueous electrolyte was injected, the opening of the outer package was sealed to obtain a test battery cell.

[0064] [Evaluation of battery resistance]

[0065] The test battery cell was charged at a constant current of 0.3C at 25°C until the depth of charge (SOC) reached 50%. After the SOC reached 50%, constant voltage charging was performed until the current value reached 0.02C. After that, after being stored at 25°C for 1 hour, constant current discharge was performed at a constant current of 1C for 10 seconds. The DC resistance was calculated as follows by dividing the difference between the open circuit voltage (OCV) and the cut-off voltage (CCV) 10 seconds after self-discharge by the discharge current 10 seconds after self-discharge.

[0066] DC resistance = [OCV-CCV (after 10 seconds of discharge)] / discharge current (after 10 seconds of discharge)

[0067] [Determination of capacity maintenance rate]

[0068] Under the condition of an ambient temperature of 25°C, the non-aqueous electrolyte secondary battery of each embodiment and each comparative example was charged to 4.2V at a constant current of 0.5C, and then charged to 0.02C at a constant voltage of 4.2V. Thereafter, it was discharged to 2.5V at a constant current of 0.5C. This charge and discharge was regarded as one cycle, and 200 cycles were performed. The capacity retention rate in the charge and discharge cycle was calculated by the following formula.

[0069] Capacity retention rate = (discharge capacity at the 200th cycle / discharge capacity at the 1st cycle) × 100

[0070] <Example 2>

[0071] Test cells were prepared and evaluated in the same manner as in Example 1 except that SiO was not added to the first negative electrode mixture slurry and SiO was added to the second negative electrode mixture slurry so that the graphite:SiO ratio was 98:5.

[0072] <Comparative Example 1>

[0073] Test cells were prepared and evaluated in the same manner as in Example 1 except that boehmite was not added to the first negative electrode mixture slurry.

[0074] <Comparative Example 2>

[0075] Test cells were prepared and evaluated in the same manner as in Example 1 except that boehmite was not added to the first negative electrode mixture slurry and a second negative electrode mixture slurry in which boehmite was dispersed was prepared by mixing natural graphite, boehmite, CMC and SBR and kneading them in water.

[0076] <Comparative Example 3>

[0077] Test cells were prepared and evaluated in the same manner as in Example 1 except that natural graphite, SiO, boehmite, CMC, and SBR were mixed and kneaded in water to prepare a first negative electrode mixture slurry in which boehmite was dispersed.

[0078] <Comparative Example 4>

[0079] Test cells were prepared and evaluated in the same manner as in Example 1 except that the first negative electrode mixture slurry and the second negative electrode mixture slurry prepared in Example 1 were mixed to form a layer and applied to a negative electrode collector made of copper foil.

[0080] The evaluation results of the test cells of Examples and Comparative Examples are summarized in Table 1. Table 1 also shows the composition (components and ratios) of the first and second negative electrode mixture layers other than CMC and SBR, and the thickness of the interface.

[0081] [Table 1]

[0082]

[0083] In the example having the interface portion containing boehmite, the charge-discharge cycle characteristics were improved. It should be noted that the battery resistance was not changed even when the interface portion was formed.

Claims

1. A negative electrode for a non-aqueous electrolyte secondary battery, comprising: A negative electrode current collector; a first negative electrode mixture layer including first graphite particles disposed on the surface of the negative electrode current collector; and a second negative electrode mixture layer including second graphite particles provided on the surface of the first negative electrode mixture layer; The first negative electrode mixture layer and the second negative electrode mixture layer have different volume change rates during charge and discharge. The first negative electrode mixture layer has an interface portion in contact with the second negative electrode mixture layer, and a main body portion that exists on the negative electrode current collector side relative to the interface portion. The thickness t of the interface portion and the average particle size dg of the first graphite particles satisfy the relationship t≤dg / 2, The first negative electrode mixture layer includes an inorganic filler, wherein the content of the inorganic filler in the interface portion is higher than the content of the inorganic filler in the main portion. The inorganic filler is ceramic particles, and the ceramic particles are selected from at least one of alumina and boehmite. The content of the inorganic filler in the interface portion is 1% by mass to 10% by mass based on the content of the first graphite particles in the first negative electrode mixture layer.

2. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1, wherein The inorganic filler is ceramic particles, and the average particle size dc of the ceramic particles and the average particle size dg of the first graphite particles satisfy the relationship of dc≤dg / 10.

3. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein: At least one of the first negative electrode mixture layer and the second negative electrode mixture layer contains a Si-based material, and the content rates of the Si-based material in the first negative electrode mixture layer and the second negative electrode mixture layer are different from each other.

4. The negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 or 2, wherein The first graphite particles and the second graphite particles have different degrees of graphitization. 5 . A non-aqueous electrolyte secondary battery comprising the negative electrode for a non-aqueous electrolyte secondary battery according to claim 1 , a positive electrode, and a non-aqueous electrolyte.

Citation Information

Patent Citations

  • Lithium secondary battery

    JP2009266705A

  • Negative electrode for nonaqueous electrolyte secondary battery, method for producing same, and nonaqueous electrolyte secondary battery

    CN102484244A

  • Negative electrode for non-aqueous electrolyte secondary battery

    CN105849945A

  • Nonaqueous-electrolyte secondary-battery negative electrode

    CN105940529A

  • Negative electrode for nonaqueous electrolyte secondary batteries, and nonaqueous electrolyte secondary battery

    CN106797020A