Isomerization method

Ethylbenzene isomerization and xylene isomerization are solved by using ZSM-48 and/or EU-2 type zeolite catalyst systems, combined with extrudates of alumina binders, to form high C/A value catalyst carriers The problem of excessive by-products is eliminated, the ethylbenzene conversion rate and the xylene production volume are improved, and an efficient catalytic effect is achieved.

CN113165997BActive Publication Date: 2024-10-15SHELL INTERNATIONALE RESEARCH MAATSCHAPPIJ BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980083567.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-21
Filing Date
2019-12-19
Publication Date
2024-10-15
Estimated Expiration
2039-12-19

AI Technical Summary

Technical Problem

Existing ethylbenzene isomerization and transalkylation methods, while increasing the xylene ratio, produce undesirable by-products such as compounds with 1 to 5 carbon atoms, benzene and C9+ aromatics, and ethylbenzene There is a trade-off between conversion rate and selectivity.

Method used

Using a catalyst system containing ZSM-48 and/or EU-2 zeolites, by adding extrudates of alumina binders to the catalyst carrier, a molded catalyst carrier with a C/A value of at least 3 is formed to reduce side reactions and improve Ethylbenzene conversion rate.

Benefits of technology

Significantly improve the conversion rate of ethylbenzene and the production volume of xylene, reduce the formation of by-products, and increase the equilibrium value of para-xylene to close to or exceed 100% while maintaining a high conversion rate of ethylbenzene. pX-ATE value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113165997B_ABST
    Figure CN113165997B_ABST
Patent Text Reader

Abstract

The present invention relates to a process for carrying out a combination of ethylbenzene reforming and xylene isomerization, the process comprising contacting a hydrocarbon feedstock containing ethylbenzene and xylenes with a catalyst comprising a catalyst support and one or more metals supported on the catalyst support, wherein the catalyst support is an extrudate comprising (i) a ZSM-48 and / or EU-2 type zeolite and (ii) an alumina binder, the extrudate having a shape with a C / A value of at least 3, wherein C is the circumference of the extrudate and A is the cross-sectional area of ​​the extrudate. The metal may be platinum and the alumina may be wide pore alumina. The process exhibits high conversion while maintaining low levels of by-product formation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a process for reforming ethylbenzene and isomerizing xylenes using a zeolite-based catalyst. Background Art

[0002] After fractionation or distillation of petroleum crude oil, a straight-run naphtha fraction is obtained boiling in the range of 70° C. to 190° C. This fraction can be catalytically converted into aromatic reformates.

[0003] Upon conversion to reformate, the content of aromatic compounds increases significantly and the resulting hydrocarbon mixture becomes highly desirable as a source of valuable chemical intermediates and a component of gasoline.

[0004] The reformate generally contains aromatic hydrocarbons having 8 carbon atoms, such as ethylbenzene and xylenes. Other components may be present, such as their hydrogenated homologues, such as cycloalkanes.

[0005] Among the xylenes, para-xylene is the most useful commodity, and isomerization or transalkylation processes have been developed to increase the proportion of para-xylene ("pX"). However, isomerization or transalkylation processes may also produce undesirable by-products, such as compounds having 1 to 5 carbon atoms, benzene, toluene, and compounds having 9 or more carbon atoms.

[0006] Many catalysts have been prepared and proposed for various reactions involving aromatic compounds, but for some reactions, such as ethylbenzene isomerization or transalkylation processes, there is usually a compromise between providing the desired product and known side reactions. A common side reaction of ethylbenzene hydroisomerization is the formation of compounds with 1 to 5 carbon atoms, which is unfavorable from an environmental and economic point of view.

[0007] US 3856872 A describes a xylene isomerization process in which the conventional platinum silica-alumina catalyst is replaced by a zeolite catalyst of the ZSM-5 type, or a zeolite ZSM-12 catalyst, or a zeolite ZSM-21 catalyst. The zeolite may be incorporated into an inert alumina matrix.

[0008] The article "Dealuminated zeolite-based composite catalysts for reforming of an industrial naphthene-rich feedstock" (Applied Catalysis, Vol. 168, No. 1, March 1998, pp. 113-130) describes catalysts for reforming naphthene feedstocks. The preferred ZSM-12 zeolite has a Si / Al ratio of 54. It is taught that ZSM-12 with a higher silica to alumina ratio should not be used for such catalysts because this would produce a large amount of CH4 and less aromatic compounds.

[0009] Other catalysts known for C8 aromatic isomerization processes include catalysts based on mordenite (MOR) and EU1 (EUO) zeolites, as defined in Atlas of Zeolite Framework Types, Olson et al., 5th Revised Edition, 2001, published by Elsevier on behalf of the Structure Commission of the International Zeolite Association. EU1-based catalysts can achieve high selectivity, but this is usually accompanied by lower ethylbenzene conversion, thus limiting production. MOR and ZSM-12-based catalysts tend to achieve higher ethylbenzene conversion, but they also produce more byproducts in the form of toluene and C9+ aromatic compounds.

[0010] It is known from US 4741891 A and US 5075269 that ZSM-48 and / or EU-2 zeolites are suitable for hydrocarbon conversion catalysts. As described in "Catalog of Disorder in Zeolite Frameworks" published in 2000, both ZSM-48 and EU-2 zeolites belong to the MRE type zeolite family.

[0011] WO 2012 / 055755 A1 describes dealuminated ZSM-48 and / or EU-2 zeolites having a refractory oxide which is substantially free of alumina for use as hydrocarbon conversion catalysts.

[0012] It is an object of the present invention to provide an improved process for reforming alkylaromatic compounds, especially C8 alkylaromatic compounds (such as ethylbenzene) and isomerizing the xylenes. Summary of the invention

[0013] It has surprisingly been found that this object can be achieved when using a catalyst system comprising ZSM-48 and / or EU-2 zeolite, in particular a shaped catalyst system of ZSM-48 and / or EU-2 zeolite wherein the shaped catalyst has an increased circumference relative to its cross-sectional area.

[0014] Thus, the present invention provides a process for carrying out a combination of ethylbenzene reforming and xylene isomerization, the process comprising contacting a hydrocarbon feedstock containing ethylbenzene and xylenes with a catalyst comprising a catalyst support and one or more metals supported on the catalyst support, wherein the catalyst support is an extrudate comprising (i) a ZSM-48 and / or EU-2 type zeolite and (ii) an alumina binder, the extrudate having a shape with a C / A value of at least 3, wherein C is the circumference of the extrudate and A is the cross-sectional area of ​​the extrudate. DETAILED DESCRIPTION

[0015] In the present invention, it has been found that the use of the above-described shaped catalyst support extrudates is unexpectedly beneficial in providing a catalyst for isomerizing alkyl aromatic compounds containing 8 carbon atoms. In addition, the shaped catalyst used in the process of the present invention can: reduce side reactions, such as the formation of compounds containing 1 to 5 carbon atoms; and / or reduce the formation of benzene; and / or increase the conversion of ethylbenzene; and / or increase the production of other desired products (such as para-xylene).

[0016] One or more of the above provisions result in increased final yields of one or more of the desired products and, unexpectedly, result in higher pX-approach to equilibrium ("pX-ATE") values ​​while maintaining excellent ethylbenzene conversion.

[0017] In the present invention, the reference to ZSM-48 and EU-2 is used to indicate that all zeolites belonging to the MRE family with a disordered structure as described in the "Catalog of Disorder in Zeolite Frameworks" published on behalf of the International Zeolite Association Structure Committee in 2000 can be used. Zeolites ZBM-30 and EU-11 are very similar to ZSM-48 and are also considered to be members of the zeolite family whose structure belongs to the MRE family. Therefore, in this application, any reference to ZSM-48 zeolite is also a reference to EU-2, ZBM-30 and EU-11 zeolites.

[0018] The molar ratio of silica to alumina of ZSM-48 and / or EU-2 zeolite can affect the properties of the catalyst derived from the zeolite. The molar ratio of silica to alumina ("SAR") is determined by the volume ratio. This ratio is also called the total ratio. Such a ratio is different from the SAR of the crystalline framework. The volume ratio or total ratio can be determined by any of a variety of chemical analysis techniques. Such techniques include X-ray fluorescence, atomic adsorption, and inductively coupled plasma-atomic emission spectroscopy (ICP-AES). All will provide substantially the same volume ratio value. The molar ratio of silica to alumina used in the present invention is determined by X-ray fluorescence.

[0019] The SAR of the ZSM-48 and / or EU-2 zeolite is preferably at least 50, more specifically at least 70, more specifically at least 100, most preferably at least 110. The SAR of the ZSM-48 and / or EU-2 zeolite is preferably at most 300, more specifically at most 250, more specifically at most 200, most specifically at most 160.

[0020] The ZSM-48 and / or EU-2 zeolites may be prepared in any manner known to those skilled in the art. Suitable methods for making such zeolites having a SAR of 100 to 250 are described in US-A-5075269 and US-A-4741891.

[0021] The ZSM-48 and / or EU-2 zeolite may be dealuminated. Dealumination may be achieved by methods known in the art, such as acid leaching or by steam treatment. Steam treatment is carried out by contacting the zeolite, preferably as part of a catalyst composition, with steam at an elevated temperature in the range of about 250°C to 650°C, preferably about 400°C to 550°C. The treatment may be accomplished in an atmosphere of 100% steam or in an atmosphere consisting of steam or some other gas that is substantially inert to the zeolite. Similar treatments may be accomplished at lower temperatures and elevated pressures, such as at 180°C to 370°C at 10 to 200 atmospheres.

[0022] The expression "dealumination" is used to indicate the removal of aluminum and / or aluminum-containing compounds (eg, alumina) from the bulk of the zeolite. The aluminum and aluminum-containing compounds may, but need not, become part of the zeolite framework.

[0023] The ZSM-48 and / or EU-2 zeolite is combined with an alumina binder in the catalyst support of the present invention. In one embodiment, the alumina binder preferably comprises "wide pore alumina", sometimes alternatively referred to as "high pore" alumina. "Wide pore alumina" refers to an alumina having an average pore size of about or greater, preferably greater than about In another embodiment, the surface area of ​​the wide pore alumina may be greater than about 200 m 2 / g, and about 25% or more of the pores of the wide-pore alumina have a diameter greater than about

[0024] The pore volume of the wide pore alumina may be at least about 0.5 cm 3 / g, preferably at least 0.6 cm 3 / g, and more preferably at least 1.2 cm 3 / g. The pore volume can be as high as about 2.0cm 3 / g, preferably up to 1.6 cm 3 / g.

[0025] It is believed that the more open structure of wide pore alumina provides for better diffusion of reactants to the catalytic material in the catalyst, and better diffusion of products away from the catalytic material, based on one or more parameters such as pore volume, pore diameter, and packing density.

[0026] Examples of wide pore aluminas suitable for use in the catalyst of the present invention include grades from the Pural range from Sasol, such as "Pural KR II" (average bulk density 0.315 g / cm 3 , pore volume is 1.4 cm 3 / g, and the average surface area is 290m 2 / g), and other wide pore aluminas, such as WPA available from Criterion (average bulk density 0.2 g / cm 3 , pore volume is 1cm 3 / g, and the average surface area is 345m 2 / g). The pore size and pore volume can be measured by mercury intrusion porosimetry testing (MIP).

[0027] When the content of binder and zeolite is described in the context of the present invention, it refers to the content on a dry basis. The catalyst composition used in the method of the present invention preferably comprises up to 80% by weight (% wt), more particularly up to 70% by weight, more particularly up to 65% by weight, most preferably up to 55% by weight of zeolite. These amounts are preferably applicable to ZSM-48 and / or EU-2 zeolite. In addition, it is preferred that the amount of ZSM-48 and / or EU-2 zeolite is at least 30% by weight, more particularly at least 35% by weight, more particularly at least 40% by weight, most particularly at least 45% by weight.

[0028] Optionally, in addition to ZSM-48 and / or EU-2 zeolites, further zeolites may be present in the catalyst composition, in particular if it is desired to modify its catalytic properties. If further zeolites are present in addition to ZSM-48 and / or EU-2 zeolites, such zeolites are preferably present in an amount of up to 50% by weight, based on the amount of ZSM-48 and EU-2 zeolites present.

[0029] The combined alkylaromatic reforming and xylene isomerization catalyst for use in the process of the present invention may be prepared by extruding a mixture comprising ZSM-48 and / or EU-2 type zeolite and alumina to form a catalyst support having a C / A value of at least 3, and impregnating the extruded catalyst support with a metal.

[0030] The catalyst support may be extruded prior to metal loading. Preferably, the catalyst support is calcined prior to metal loading. Calcination may occur in an inert atmosphere or in an oxygen-containing gas at from 350-850°C, more preferably 400-750°C.

[0031] The catalyst support is formed or formed by extrusion, for example, by preparing an extrudable mass comprising an alumina binder and ZSM-48 and / or EU-2 zeolite. The extrudable mass may have a viscosity that allows extrusion, preferably such that the extruded shape is maintained during subsequent calcination. Those skilled in the art will know how to realize an extrudable mixture, such as a pasty mixture, which is easy to carry out such extrusion and subsequently maintains the extruded shape while calcining. For example, the extrudable mass preferably has a water content that is sufficient to provide for extrusion, while maintaining the extruded shape during subsequent calcination. Preferably, the water content is no more than 65 wt %, and is preferably at least 35 wt %.

[0032] The zeolite and alumina mixture may further comprise a debonding agent to sufficiently change the pH of the mixture to induce deagglomeration of the solid particles. Debonding agents are well known and encompass inorganic acids such as sulfuric acid or nitric acid as well as organic acids such as formic acid and acetic acid. Such debonding agents are removed upon calcination.

[0033] Plasticizer can be added to the catalyst support composition, preferably before extrusion, introduce plasticizer.Plasticizer can be used to increase the viscosity of the mixture, to obtain extrudable agglomerates.Suitable plasticizer is for example dextrose, gelatin, glucose, glue, gum, salt, wax, starch and cellulose ether.In the practice of the present invention, methylcellulose and / or methylcellulose derivatives are particularly suitable as organic binders, wherein methylcellulose, hydroxypropyl methylcellulose or these combinations are preferred.The preferred source of cellulose ether is " Methocel " A4M, F4M, F240 and K75M from Dow Chemical Co.

[0034] The extrusion of the catalyst support composition can be performed by any of the well-known extrusion methods. Examples of such methods are extrusion performed by a screw extruder or a plate or ram extruder.

[0035] Extrudate can have various forms and sizes, and its C / A value is at least 3, wherein C is the girth of extrudate, and A is the cross-sectional area of ​​extrudate.It should be noted that the cross-sectional area (A) of extrudate is measured at right angles (vertical) to the extrusion axis, and its girth (C) is the length of the extrudate girth around the cross section.The extrudate with a C / A value of at least 3 can be easily formed into cylindrical or multi-lobed extrudate, for example, has a trilobal, four-lobal or expanded trilobal shape.That is to say, in the present invention, in cross section, catalyst carrier preferably has a trilobal, four-lobal or expanded trilobal shape.More preferably, in cross section, catalyst carrier has a trilobal, four-lobal or expanded trilobal shape.

[0036] An extrudable composition comprising ZSM-48 and / or EU-2 zeolite and an alumina binder may be extruded using an extruder die having slots that can produce an extrudate having a desired cross-section to achieve a C / A value of at least 3.

[0037] After extrusion, the extrudate obtained is preferably dried before calcination. Drying is preferably carried out at a temperature of 60° C. to 250° C. for a time sufficient to dry the extrudate, for example at least 1 hour. Calcination is preferably carried out at a temperature in the range of 250° C. to 850° C. in an oxygen-containing gas (including in air or in an inert gas) for a period of time ranging, for example, from 1 to 48 hours or more.

[0038] The extruded catalyst supports may be separated (e.g., cut or broken), preferably after an initial calcination step, to reduce their aspect ratio and thereby help reduce cracking of the catalyst, for example when subjected to crushing forces in a catalyst bed in a reactor. The aspect ratio may optionally be in the range of 1:1 to 20:1, preferably 2:1 to 9:1, most preferably 4:1 to 8:1. For example, the diameter of the extruded catalyst may be in the range of 0.5 mm to 5 mm, preferably 1 mm to 2 mm, and the average length of the catalyst shape may be in the range of 2 mm to 10 mm, preferably 4 mm to 9 mm, more preferably about 8 mm.

[0039] The catalyst also comprises one or more metals, which are preferably incorporated into the catalyst support. The metal can be incorporated by means of impregnated zeolite, by impregnating an alumina support or by impregnating a composite of a zeolite and a support. Preferably, the metal is incorporated into the catalyst support. The incorporation of the metal can be performed using ion exchange techniques, such as involving contacting the catalyst support composition with a salt of the desired metal ion. This can be accomplished by, for example, pore volume impregnation or continuous solution impregnation. Representative ion exchange techniques are disclosed in various patent specifications including US 3140249 A, US 3140251 A and US 3140253 A.

[0040] The catalytic metal is preferably incorporated by pore volume impregnation. More preferably, the metal is incorporated into the extruded catalyst support by impregnation, for example after calcining the support. Most preferably, the impregnation is performed after calcining and dividing the extruded support into the desired length.

[0041] The catalytic metal is selected from the group consisting of metals of Group VIII of the Periodic Table of the Elements, as shown in the 63rd edition of Handbook of Chemistry and Physics, 1983, more specifically selected from one or more of platinum, palladium, cobalt, iron and nickel. Preferably, one or more catalytic metals are selected from the group consisting of platinum, palladium and nickel, with platinum being particularly preferred. Combinations of two or more catalytically active metals are also possible, preferably platinum metal combinations. The catalytically active metals can be provided in the form of compounds, which optionally require activation before use.

[0042] The catalytic metal may be included in the final catalyst composition in an amount of up to about 3% by weight, based on the total dry weight of the catalyst, the metal content being determined as an element, regardless of its actual form. Preferably, the metal component is present in the catalyst composition in an amount of 0.1% to 3% by weight. More preferably, the metal is present in the composition in an amount of 0.2% to 2% by weight, and most preferably, the amount is in the range of 0.3% to 1% by weight. More preferably, the catalyst composition comprises about 0.3% by weight of platinum.

[0043] The catalysts are useful in isomerization and reforming processes, particularly ethylbenzene conversion and xylene isomerization as described herein.

[0044] Advantageously, the catalyst prepared as described above may be used in the isomerization of alkyl aromatic compounds to produce a product having an increased xylene content.

[0045] The catalyst described herein is particularly suitable for increasing the xylene content, more particularly the p-xylene content, of a hydrocarbon fraction containing aromatic hydrocarbons having 8 carbon atoms. The hydrocarbon stream preferably contains up to 60% by weight, more particularly up to 50% by weight of ethylbenzene. Preferably, the hydrocarbon stream comprises at least 8% by weight, more particularly at least 10% by weight, most preferably at least 15% by weight of ethylbenzene. The hydrocarbon stream is preferably contacted with the catalyst at a temperature in the range of 300° C. to 450° C., preferably at least 340° C., preferably up to 400° C.

[0046] In the process of the present invention, it has surprisingly been found that in addition to successful ethylbenzene conversion, further improvements in isomerization to high-p-xylene reformate can be achieved, as evidenced by the pX-ate value. Two Toluene Balancing Act (para- X ylene- a pproach- t o- e quilibrium)) provides a measure of the effectiveness of a catalyst in increasing the concentration of para-xylene relative to the maximum achievable para-xylene concentration of a thermodynamic equilibrium mixture based on xylenes, as defined by the following equation:

[0047]

[0048] wherein pX represents para-xylene, Xyl generally represents xylene, f. represents feed, and pr. represents product.

[0049] In particular, it is surprising that by means of the present invention, pX-ate values ​​approaching or exceeding 100% can be achieved while maintaining low levels of by-product formation.

[0050] For comparison purposes, examples of catalyst shapes having a C / A value of at least 3 are given as Figure 1 (b) Figure 1 (c) and Figure 1 (d) is shown in cross section, and the cylindrical shape is Figure 1 (a) is shown. It has been found that the catalysts of the present invention comprising extrudates having a trilobe (TL), quadralobe (QLSA) or trilobe extra (TX) cross section show improved performance, for example compared to conventional cylindrical (CYL) extrudates having a circular cross section and a C / A value of less than 3. Similar improvements were observed for cylinders with smaller diameters, also having a C / A value of greater than 3. On the other hand, large TX-shaped extrudates with C / A values ​​below 3 did not show the advantages.

[0051] For example, by extruding the catalyst through a die having holes with undulating perimeters, C / A values ​​of 3 or greater can be achieved. In a preferred embodiment, the shaped catalyst of the present invention has a solid structure, such as formed by extrusion through a solid die rather than through a hollow die that produces a hollow or semi-hollow shape.

[0052] Figure 1 The C / A ratio of the various catalyst shapes (a) to (d) can be determined by measuring the radius r as shown in the cross-sectional diagram and the perimeter (C) represented by the bold line in said figures, as calculated according to the following formula:

[0053]

[0054] Preferably, the catalyst is formed, for example by extrusion, into a shape having an aspect ratio of 1:1 to 20:1, preferably 2:1 to 9:1, most preferably 4:1 to 8:1. Preferably, the diameter (d) is in the range of about 0.5 mm to about 5 mm, more preferably 1 mm to 2 mm. The shape preferably has an average length (measured along the extrusion axis) of about 2 mm to about 10 mm, more preferably about 4 mm to about 9 mm, most preferably about 8 mm.

[0055] The catalyst as described above can be used in a combination of ethylbenzene reforming and xylene isomerization reactions, the reactions being performed in the gas phase. Thus, the present invention provides a process for the combined reforming of ethylbenzene and xylene isomerization, the process comprising contacting a hydrocarbon feedstock containing ethylbenzene and xylenes with a catalyst as described above at an elevated temperature of preferably 340-450°C and a pressure of from 4-12 barg. Preferably, the reforming and isomerization reactions are carried out using a reaction mixture in about 1 hour. -1 Until 20h -1, more preferably about 3h -1 Until 10h -1 The feed weight hourly space velocity (WHSV) (weight of feed per hour / weight of catalyst) within the range of 1:1 to 2:1 was performed. The WHSV was based on the weight of the catalyst composition, i.e., the total weight of the active catalyst and the binder.

[0056] Preferably, the isomerization reaction is carried out in the presence of hydrogen. More preferably, hydrogen may be present in the isomerization reaction zone in an amount of between about 0 and about 10 moles, particularly between about 1 and about 5 moles, per mole of hydrocarbon feedstock. The reaction may be carried out in a vapor, liquid phase or mixed phase.

[0057] An advantage of the process of the invention is the fact that a high hourly weight space velocity can be applied in the process, resulting in a higher throughput in the reactor and thus a higher productivity. The hourly weight space velocity applied in the process is suitably in the range of 3 to 12 hours. -1 within the range.

[0058] The invention will now be illustrated by the following non-limiting examples.

[0059] Example

[0060] Example 1

[0061] The catalyst was prepared by the following steps: catalyst support extrusion, support calcination, platinum impregnation and final calcination.

[0062] In particular, an extrudable mixture of 78 g of EU-2 zeolite having a silica to alumina ratio of 110 (prepared as described in US 4741891 A), 64 g of wide pore alumina from Criterion, 86 g of water and 2.77 g of 65% HNO3 was freshly prepared and extruded using an extruder die having holes of different shapes and sizes as described in Table 1.

[0063] The resulting extruded catalyst supports were each calcined in a static oven at 600° C. for 2 hours and then broken into pieces with an average length of 6 mm. The calcined supports were then impregnated with platinum by pore volume impregnation using a mixture of chloroplatinic acid in a 0.5 M HNO3 aqueous solution, dried at 120° C. for 2 hours, and then calcined at 550° C. for 2 hours to produce a final catalyst containing 0.3 wt% platinum.

[0064] Example 2

[0065] The catalyst prepared by the method of Example 1 was then used in an ethylbenzene reforming process.

[0066] In particular, the catalysts were evaluated for a combination of ethylbenzene reforming and xylene isomerization reactions in a pilot plant using on-line GC analysis.

[0067] Throughout the reaction, a hydrogen: hydrocarbon molar ratio of 4 was maintained. Prior to the reforming process, the catalyst was dried in a hydrogen stream at room temperature and atmospheric pressure for 1 hour, then heated to 400°C for 4 hours, pressurized to 12 barg, and maintained under these conditions for another hour.

[0068] 5h -1 A first hydrocarbon feed consisting of 20 wt% ethylbenzene and 80 wt% meta-xylene was introduced at a WHSV of 4.0 h and the temperature was raised to 420°C. These conditions were maintained for 24 h and then the temperature was lowered to 375°C. At this temperature, the hydrocarbon feed was switched to a WHSV of 4.0 h. -1 A mixture of 20% ethylbenzene, 23% o-xylene and 57% m-xylene was prepared. These conditions were maintained for 6 hours.

[0069] Subsequently, the reactor temperature was increased to 387 °C and the hydrocarbon feed was switched to a WHSV of 3.5 h -1 The final mixture was 19% ethylbenzene, 15.5% o-xylene, 59% m-xylene and 6.5% ethylcyclohexane (representing the C8 cycloalkanes that mediate the ethylbenzene reforming reaction).

[0070] The pressure was adjusted so that the level of C8-cycloalkanes in the product stream was equal to the level of ethylcyclohexane in the feed. The product stream was passed through an online GC at 3.5 h -1 The WHSV analysis was performed for 10 hours and then at 6.0 hours. -1 The WHSV was analyzed for 4 hours. Based on these data, the parameters in Table 1 were determined.

[0071] Table 1:

[0072]

[0073] a Circumference (C) / cross-sectional area (A) of the extrudate.

[0074] The results shown in Table 1 unexpectedly demonstrate that the pX-ATE values ​​at both WHSVs tested increase significantly when the C / A ratio of the catalyst extrudates is increased from 2.86 (comparing cylinders) or 2.72 (comparing TX-shaped extrudates) to above 3. At the same time, the conversion of ethylbenzene (EB) remains at an extremely high level.

[0075] A person skilled in the art will appreciate that the present invention can be implemented in many ways without departing from the scope of the claims.

Claims

1. A process for carrying out a combination of ethylbenzene reforming and xylene isomerization, the process comprising contacting a hydrocarbon feedstock containing ethylbenzene and xylenes with a catalyst comprising a catalyst support and one or more metals supported on the catalyst support, wherein the catalyst support is an extrudate comprising (i) a ZSM-48 and / or EU-2 type zeolite and (ii) an alumina binder, the extrudate having a shape with a C / A value of at least 3, wherein C is the circumference of the extrudate and A is the cross-sectional area of ​​the extrudate. 2 . The method according to claim 1 , wherein in cross section the catalyst support has a round, trilobal, quadrilobal or extended trilobal shape. 3 . The method according to claim 1 , wherein in cross section the catalyst support has a trilobal, quadrilobal or extended trilobal shape.

4. The method according to claim 1 or 2, wherein the alumina binder has an average pore diameter of or larger wide pore alumina.

5. The method according to claim 1 or 2, wherein the zeolite is present in an amount of 30 wt% to 70 wt% based on the total weight of the catalyst.

6. The method according to claim 1 or 2, wherein the metal supported on the catalyst support is a Group VIII metal.

7. The method according to claim 1 or 2, wherein the metal supported on the catalyst support is platinum.

8. The method of claim 6, wherein the Group VIII metal is present in an amount of 0.1 wt% to 3 wt%, based on the total weight of the catalyst.