By doping the active material with alkali metal using a doping solution containing alkali metal in an atmosphere with a specific oxygen concentration in the electrode manufacturing method, the problem that the doping solution is prone to fire is solved, and safety and performance are improved.
Patent Information
- Application Number
- CN201980077550.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-11-28
- Filing Date
- 2019-09-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2039-09-19
AI Technical Summary
The doping solution used in existing electrode manufacturing methods is flammable and can easily catch fire when the electrode breaks or sparks, causing safety hazards.
The active material is doped with alkali metal using a doping solution containing alkali metal ions in an atmosphere with an oxygen concentration of 1 volume % or more and 18 volume % or less, and the atmosphere is controlled by an electrode manufacturing device to suppress ignition of the doping solution.
It effectively suppresses the risk of fire in the doping solution and improves the safety of the electrode manufacturing process and product performance.
Smart Images

Figure CN113169311B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This international application claims the benefit of Japanese Patent Application No. 2018-222469 filed in the Japan Patent Office on November 28, 2018, the entire contents of which are hereby incorporated by reference. Technical Field
[0003] The present disclosure relates to an electrode manufacturing method, a power storage device manufacturing method, and an electrode manufacturing device. Background Art
[0004] In recent years, the miniaturization and lightness of electronic devices have attracted attention. Along with the miniaturization and lightness of electronic devices, there is also an increasing demand for miniaturization and lightness of batteries used as a power source for driving the electronic devices.
[0005] In order to meet the above-mentioned needs of miniaturization and lightness, non-aqueous electrolyte secondary batteries represented by lithium ion secondary batteries have been developed. In addition, lithium ion capacitors are known as power storage devices for applications requiring high energy density characteristics and high output characteristics. In addition, sodium ion batteries or capacitors using sodium, which is less expensive than lithium and has abundant resources, are also known.
[0006] In the above-mentioned battery or capacitor, a process of pre-doping the electrode with an alkali metal (generally referred to as pre-doping) is adopted for various purposes. As a method of pre-doping the electrode with an alkali metal, there are, for example, a single-sheet method and a continuous method. The single-sheet method and the continuous method implement pre-doping outside the storage device. The single-sheet method implements pre-doping in a state where the cut electrode plate and the alkali metal plate are arranged in a doping solution with a separator between them. The continuous method implements pre-doping while transferring the strip-shaped electrode plate in the doping solution. The single-sheet method is disclosed in Patent Documents 1 and 2. The continuous method is disclosed in Patent Documents 3 to 6.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 9-293499
[0010] Patent Document 2: Japanese Patent Publication No. 2012-69894
[0011] Patent Document 3: Japanese Patent Application Laid-Open No. 10-308212
[0012] Patent Document 4: Japanese Patent Application Publication No. 2008-77963
[0013] Patent Document 5: Japanese Patent Application Publication No. 2012-49543
[0014] Patent Document 6: Japanese Patent Application Publication No. 2012-49544 Summary of the invention
[0015] Problem that the invention aims to solve
[0016] The doping solution used in the single-sheet method and the continuous method is flammable. In addition, the single-sheet method and the continuous method perform pre-doping while passing current through the electrode. If the electrode breaks or a spark is generated in the electrode conveying unit, the doping solution may catch fire.
[0017] One aspect of the present disclosure is to provide an electrode manufacturing method, a power storage device manufacturing method, and an electrode manufacturing device capable of suppressing ignition of a doping solution.
[0018] Technical solutions to the problem
[0019] One aspect of the present disclosure relates to an electrode manufacturing method for manufacturing an electrode having an active material layer, wherein the active material layer includes an active material doped with an alkali metal, the electrode manufacturing method comprising the following steps: in an atmosphere having an oxygen concentration of 1 volume % or more and 18 volume % or less, doping the active material with an alkali metal using a doping solution containing alkali metal ions. According to the electrode manufacturing method of one aspect of the present disclosure, ignition of the doping solution can be suppressed.
[0020] Another aspect of the present disclosure relates to a method for manufacturing an electric storage device, wherein the electric storage device includes an electrode battery, and the method for manufacturing the electric storage device includes the following steps: in an atmosphere with an oxygen concentration of 1 volume % or more and 18 volume % or less, using a doping solution containing alkali metal ions to dope an alkali metal into a negative electrode active material included in a negative electrode active material layer provided by a negative electrode, and after doping with the alkali metal, sequentially stacking the negative electrode, a separator, and an electrode different from the negative electrode to form the electrode battery. According to the method for manufacturing an electric storage device according to another aspect of the present disclosure, it is possible to suppress the ignition of the doping solution.
[0021] Another aspect of the present disclosure relates to an electrode manufacturing device that manufactures an electrode having an active material layer, wherein the active material layer includes an active material doped with an alkali metal, and the electrode manufacturing device includes an atmosphere setting unit, wherein the atmosphere setting unit is configured to set the atmosphere inside the electrode manufacturing device to an atmosphere having an oxygen concentration of 1 volume % or more and 18 volume % or less. According to the electrode manufacturing device of another aspect of the present disclosure, it is possible to suppress the ignition of a doping solution. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1It is an explanatory diagram showing the structure of an electrode manufacturing apparatus.
[0023] Figure 2 This is an explanatory diagram showing a state in which the electrolytic solution tank is moved downward.
[0024] Figure 3 It is an explanatory diagram showing the electrical structure of the electrode manufacturing apparatus.
[0025] Figure 4 It is a side cross-sectional view showing the structure of the counter electrode unit and the porous insulating member.
[0026] Figure 5 is a top view showing the structure of an electrode precursor.
[0027] Figure 6 It is shown Figure 5 Cross-sectional view at section VI-VI in FIG.
[0028] Description of Reference Numerals
[0029] 1 ... electrode manufacturing device; 10 ... chamber; 7, 203, 205, 207 ... electrolyte tank;
[0030] 9, 11, 13, 15, 17, 19, 21, 23, 25, 27, 29, 31, 305, 307, 109, 311, 313, 315, 317, 119, 321, 323, 33, 35, 37, 39, 41, 43, 45… conveyor rollers;
[0031] 47 ... supply roller; 49 ... winding roller; 51, 52, 54 ... counter electrode unit;
[0032] 53 ... porous insulating member; 55 ... supporting platform; 57 ... circulating filtration unit;
[0033] 61, 62, 64…DC power supply; 63…blower; 66…power control unit;
[0034] 67, 68, 70 ... support rods; 69 ... separator; 71 ... space; 73 ... electrode precursor;
[0035] 75 ... electrode; 77 ... conductive substrate; 79 ... plate containing alkali metal; 81 ... filter;
[0036] 83… pump; 85… pipeline; 87, 89, 91, 93, 97, 99… cables; 93… collector;
[0037] 95…active material layer; 101…CPU; 103…cleaning tank; 105…memory DETAILED DESCRIPTION
[0038] Exemplary embodiments of the present disclosure are described with reference to the accompanying drawings.
[0039] <First Embodiment>
[0040] 1. Structure of the electrode manufacturing device 1
[0041] Reference Figure 1 to Figure 4 The structure of the electrode manufacturing device 1 is described below. Figure 1 As shown, the electrode manufacturing device 1 includes a chamber 10, electrolyte tanks 203, 205, 7, 207; a cleaning tank 103; conveying rollers 9, 11, 13, 15, 17, 19, 21, 23, 25, 27, 29, 31, 305, 307, 109, 311, 313, 315, 317, 119, 321, 323, 33, 35, 37, 39, 41, 43, 45 (hereinafter collectively referred to as a conveying roller group); a supply roller 47; a winding roller 49; an electrode unit 51, 52, 54; a porous insulating component 53; a support table 55; a circulating filtration unit 57; three DC power supplies 61, 62, 64; a blower 63; and a power control unit 66.
[0042] The chamber 10 contains electrolyte tanks 203, 205, 7, 207; a cleaning tank 103; a conveying roller group; a supply roller 47; a winding roller 49; counter electrode units 51, 52, 54; a porous insulating member 53; a support table 55; a circulation filter unit 57; and a blower 63.
[0043] like Figure 1 as well as Figure 2 As shown in FIG. 2 , the electrolyte tank 205 is a square tank with an upper opening. The bottom surface of the electrolyte tank 205 has a substantially U-shaped cross-sectional shape. The electrolyte tank 205 contains a partition 69, four counter electrode units 51, four porous insulating components 53, and a conveying roller 27. Figure 2 As shown, the four porous insulating members 53 include porous insulating members 53a, 53b, 53c, and 53d.
[0044] The partition 69 is supported by a support rod 67 that passes through the upper end of the partition 69. The support rod 67 is fixed to a wall or the like that is not shown. The portion of the partition 69 other than the upper end is located in the electrolyte tank 205. The partition 69 extends in the up-down direction and divides the interior of the electrolyte tank 205 into two spaces. The conveying roller 27 is mounted on the lower end of the partition 69. The partition 69 and the conveying roller 27 are supported by a support rod 68 that passes through the partition 69 and the conveying roller 27. In addition, the vicinity of the lower end of the partition 69 is cut away so as not to contact the conveying roller 27. There is a space between the conveying roller 27 and the bottom surface of the electrolyte tank 205.
[0045] The four electrode units 51 are supported by support rods 70 that penetrate the upper ends of the four electrode units 51, and the four electrode units 51 extend in the up-down direction. The support rods 70 are fixed to a wall or the like that is not shown. The portion of the electrode unit 51 other than the upper end is in the electrolyte tank 205. Two of the four electrode units 51 are arranged to sandwich the partition 69 from both sides. The remaining two electrode units 51 are arranged along the inner side of the electrolyte tank 205.
[0046] As shown in FIG. 1 , there is a space 71 between the counter electrode unit 51 disposed on the separator 69 side and the counter electrode unit 51 disposed along the inner side surface of the electrolyte tank 205. The counter electrode unit 51 is connected to the positive electrode of the DC power supply 61. The detailed structure of the counter electrode unit 51 will be described later.
[0047] A porous insulating member 53 is attached to the surface of each counter electrode unit 51 on the side of the space 71. The detailed structure of the porous insulating member 53 will be described later.
[0048] The electrolyte tank 203 has basically the same structure as the electrolyte tank 205. However, the electrolyte tank 203 does not include the counter electrode unit 51 and the porous insulating member 53. In addition, the electrolyte tank 203 does not include the conveying roller 27 but includes the conveying roller 17. The conveying roller 17 is the same as the conveying roller 27.
[0049] The electrolyte tank 7 has basically the same structure as the electrolyte tank 205. However, the electrolyte tank 7 does not include the four counter electrode units 51 and the conveying rollers 27, but includes four counter electrode units 54 and the conveying rollers 109. The four counter electrode units 54 are the same as the four counter electrode units 51. The conveying rollers 109 are the same as the conveying rollers 27. The counter electrode units 54 are connected to the positive pole of the DC power supply 62.
[0050] The electrolyte tank 207 has the same structure as the electrolyte tank 205. However, the electrolyte tank 207 does not include four counter electrode units 51 and the conveying roller 27, but includes four counter electrode units 52 and the conveying roller 119. The four counter electrode units 52 are the same as the four counter electrode units 51. The conveying roller 119 is the same as the conveying roller 27. The counter electrode unit 52 is connected to the positive electrode of the DC power supply 64.
[0051] The cleaning tank 103 has basically the same structure as the electrolyte tank 205. However, the cleaning tank 103 does not include the counter electrode unit 51 and the porous insulating member 53. In addition, the cleaning tank 103 does not include the conveying roller 27 but includes the conveying roller 37. The conveying roller 37 is the same as the conveying roller 27.
[0052] The conveying rollers 25, 29, 307, 311, 317, and 321 are formed of a conductive material. The other conveying rollers in the conveying roller group are formed of an elastomer except for the bearing portion. The conveying roller group conveys the electrode precursor 73 described later along a predetermined path. The path along which the conveying roller group conveys the electrode precursor 73 is as follows: from the supply roller 47, it passes through the electrolyte tank 203, the electrolyte tank 205, the electrolyte tank 7, the electrolyte tank 207, and the cleaning tank 103 in sequence, and then reaches the winding roller 49.
[0053] The portion of the path that passes through the electrolyte tank 203 is the following path: first, it moves downward between the inner side surface of the electrolyte tank 203 and the partition 69, then the moving direction is changed to an upward direction by the conveying roller 17, and finally, it moves upward between the inner side surface of the electrolyte tank 203 and the partition 69 opposite to the inner side surface of the electrolyte tank 203.
[0054] In addition, the portion of the above-mentioned path that passes through the electrolyte tank 205 is the following path: first, it moves downward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 205 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53, then, the moving direction is changed to an upward direction by the conveying roller 27, and finally, it moves upward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 205 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53.
[0055] In addition, the portion of the above-mentioned path that passes through the electrolyte tank 7 is the following path: first, it moves downward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 7 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53, then, the moving direction is changed to an upward direction by the conveying roller 109, and finally, it moves upward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 7 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53.
[0056] In addition, the portion of the above-mentioned path that passes through the electrolyte tank 207 is the following path: first, it moves downward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 207 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53, then, the moving direction is changed to an upward direction by the conveying roller 119, and finally, it moves upward in the following space 71, wherein the space 71 is located between the porous insulating part 53 installed along the inner side surface of the electrolyte tank 207 and the porous insulating part 53 on the side of the partition 69 opposite to the porous insulating part 53.
[0057] In addition, the portion of the above-mentioned path that passes through the cleaning tank 103 is the following path: first, it moves downward between the inner side surface of the cleaning tank 103 and the partition 69, then the moving direction is changed to an upward direction by the conveying roller 37, and finally, it moves upward between the inner side surface of the cleaning tank 103 and the partition 69.
[0058] The electrode precursor 73 is wound around the outer periphery of the supply roller 47. That is, the supply roller 47 holds the electrode precursor 73 in a wound state. The conveying roller group pulls out the electrode precursor 73 held by the supply roller 47 and conveys it.
[0059] The winding roll 49 winds up and stores the electrode 75 conveyed by the conveying roll group. The electrode 75 is an electrode produced by pre-doping the electrode precursor 73 with an alkali metal in the electrolyte tanks 205 , 7 , and 207 .
[0060] The electrode units 51, 52, 54 have a plate-like shape. Figure 4 As shown, the electrode units 51, 52, and 54 have a structure in which a conductive substrate 77 and an alkali metal-containing plate 79 are stacked. Examples of the material of the conductive substrate 77 include copper, stainless steel, and nickel. The form of the alkali metal-containing plate 79 is not particularly limited, and examples thereof include an alkali metal plate and an alkali metal alloy plate. The thickness of the alkali metal-containing plate 79 can be, for example, 0.03 to 3 mm.
[0061] The porous insulating member 53 has a plate-like shape. Figure 4 As shown in the figure, the porous insulating member 53 is stacked on the plate 79 containing an alkali metal and is attached to the surface of the counter electrode units 51, 52, and 54. The plate-like shape of the porous insulating member 53 refers to the shape when the porous insulating member 53 is attached to the surface of the counter electrode units 51, 52, and 54. The porous insulating member 53 may be a member that maintains a predetermined shape itself, or may be a member that can be easily deformed, such as a mesh.
[0062] like Figure 4As shown, the porous insulating member 53 does not contact the electrode 73 conveyed by the conveying roller group. The shortest distance d from the surface of the porous insulating member 53 to the electrode precursor 73 is preferably in the range of 0.5 to 100 mm, and more preferably in the range of 1 to 10 mm. The shortest distance d refers to the distance between the point on the surface of the porous insulating member 53 closest to the electrode precursor 73 and the electrode precursor 73.
[0063] The porous insulating member 53 is porous. Therefore, a doping solution described later can pass through the porous insulating member 53. Thus, the counter electrode units 51, 52, and 54 can come into contact with the doping solution.
[0064] As the porous insulating component 53, for example, a screen made of resin can be listed. As the resin, for example, polyethylene, polypropylene, nylon, polyetheretherketone, polytetrafluoroethylene, etc. can be listed. The mesh size of the screen can be set appropriately, for example, it can be set to 0.1μm~10mm, preferably in the range of 0.1~5mm. The thickness of the screen can be set appropriately, for example, it can be set to 1μm~10mm, preferably in the range of 30μm~1mm. The opening rate of the screen can be set appropriately, for example, it can be set to 5~98%, preferably set to 5~95%, and more preferably in the range of 50~95%.
[0065] The porous insulating member 53 may be formed entirely of an insulating material, or may include a layer having insulating properties in part.
[0066] The support stand 55 supports the electrolyte tanks 203, 205, 7, 207 and the cleaning tank 103 from below. The height of the support stand 55 can be changed. If the support stand 55 supporting the electrolyte tank 205 is lowered while the separator 69, the counter electrode unit 51 and the porous insulating member 53 are kept in the vertical position, the support stand 55 supporting the electrolyte tank 205 is lowered. Figure 2 As shown, the electrolyte tank 205 can be moved downward relative to the partition plate 69, the counter electrode unit 51, and the porous insulating member 53. In addition, if the support table 55 is raised, the electrolyte tank 205 can be moved upward relative to the partition plate 69, the counter electrode unit 51, and the porous insulating member 53. The support table 55 supporting the electrolyte tanks 203, 7, 207 and the cleaning tank 103 also has the same function.
[0067] The circulation filtering unit 57 is respectively disposed on the electrolyte tanks 203, 205, 7, and 207. The circulation filtering unit 57 includes a filter 81, a pump 83, and a pipeline 85.
[0068] In the circulation filtration unit 57 provided in the electrolyte tank 203, the pipeline 85 is a circulation pipeline starting from the electrolyte tank 203, passing through the pump 83 and the filter 81 in sequence, and returning to the electrolyte tank 203. The driving force of the pump 83 is used to circulate the doping solution in the electrolyte tank 203 in the pipeline 85 and the filter 81 and return to the electrolyte tank 203 again. At this time, foreign matter in the doping solution is filtered by the filter 81. As foreign matter, foreign matter precipitated from the doping solution, foreign matter generated by the electrode precursor 73, etc. can be listed. The material of the filter 81 can be, for example, a resin such as polypropylene and polytetrafluoroethylene. The pore size of the filter 81 can be appropriately set, for example, it can be set to 30 to 50 μm.
[0069] The circulating filter unit 57 disposed in the electrolyte tanks 205, 7, and 207 also has the same structure and achieves the same effect. Figure 1 , Figure 2 The doping solution is omitted in the figure.
[0070] like Figure 3 As shown, the negative terminal of the DC power supply 61 is connected to the conveying rollers 25 and 29 via cables 87, respectively. In addition, the positive terminal of the DC power supply 61 is connected to a total of four counter electrode units 51 via cables 89, respectively. The electrode precursor 73 is in contact with the conductive conveying rollers 25 and 29. The electrode precursor 73 and the counter electrode unit 51 are in a doping solution as an electrolyte. Therefore, the electrode precursor 73 and the counter electrode unit 51 are electrically connected.
[0071] The DC power source 61 allows current to flow to the counter electrode unit 51 via the cables 87 , 89 and the conveying rollers 25 , 29 .
[0072] like Figure 3 As shown, the negative terminal of the DC power supply 62 is connected to the conveying rollers 307 and 311 via cables 91, respectively. In addition, the positive terminal of the DC power supply 62 is connected to a total of four counter electrode units 54 via cables 93, respectively. The electrode precursor 73 is in contact with the conductive conveying rollers 307 and 311. The electrode precursor 73 and the counter electrode unit 54 are in a doping solution as an electrolyte. Therefore, the electrode precursor 73 and the counter electrode unit 54 are electrically connected.
[0073] The DC power source 62 allows an electric current to flow to the counter electrode unit 54 via the cables 91 , 93 and the conveying rollers 307 , 311 .
[0074] like Figure 3As shown, the negative terminal of the DC power supply 64 is connected to the conveying rollers 317 and 321 via cables 97, respectively. In addition, the positive terminal of the DC power supply 64 is connected to a total of four counter electrode units 52 via cables 99, respectively. The electrode precursor 73 is in contact with the conductive conveying rollers 317 and 321. The electrode precursor 73 and the counter electrode unit 52 are in a doping solution as an electrolyte. Therefore, the electrode precursor 73 and the counter electrode unit 52 are electrically connected.
[0075] The DC power source 64 allows an electric current to flow to the counter electrode unit 52 via the cables 97 , 99 and the conveying rollers 317 , 321 .
[0076] The blower 63 blows gas toward the electrode 75 coming out of the cleaning tank 103 to vaporize the cleaning liquid, thereby drying the electrode 75. The gas used is preferably a gas that is inert to the active material doped with the alkali metal. Examples of such gases include helium, neon, argon, and dehumidified air from which water has been removed.
[0077] like Figure 3 As shown, the power control unit 66 is electrically connected to the DC power supplies 61, 62, and 64. The power control unit 66 is a microcomputer having a CPU 101 and a semiconductor memory such as a RAM or a ROM (hereinafter referred to as a memory 105).
[0078] 2. Structure of the electrode precursor 73
[0079] Reference Figure 5 as well as Figure 6 The structure of the electrode precursor 73 will be described. Figure 5 As shown, the electrode precursor 73 has a ribbon shape. Figure 6 As shown, the electrode precursor 73 includes a strip-shaped negative electrode current collector 93 and negative electrode active material layers 95 formed on both sides of the negative electrode current collector 93 .
[0080] The collector 93 is preferably made of a metal foil such as copper, nickel, or stainless steel. Alternatively, the collector 93 may be a metal foil on which a conductive layer mainly composed of a carbon material is formed. The thickness of the collector 93 may be, for example, 5 to 50 μm.
[0081] Active material layer 95 can be produced by preparing a slurry containing, for example, an active material before being doped with an alkali metal and a binder, applying the slurry onto current collector 93 , and drying the slurry.
[0082] Examples of the adhesive include rubber adhesives such as styrene-butadiene rubber (SBR) and NBR; fluorine-based resins such as polytetrafluoroethylene and polyvinylidene fluoride; polypropylene; polyethylene; and fluorine-modified (meth) acrylic adhesives such as those disclosed in Japanese Patent Application Publication No. 2009-246137.
[0083] The slurry may contain other ingredients in addition to the active material and the binder. Examples of other ingredients include conductive agents such as carbon black, graphite, vapor-grown carbon fiber, and metal powder; and thickeners such as carboxymethyl cellulose, sodium salt or ammonium salt of carboxymethyl cellulose, methyl cellulose, hydroxymethyl cellulose, ethyl cellulose, hydroxypropyl cellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, and casein.
[0084] The thickness of active material layer 95 is not particularly limited, and may be, for example, 5 to 500 μm, preferably 10 to 200 μm, and particularly preferably 10 to 100 μm.
[0085] The active material contained in active material layer 95 is not particularly limited as long as it can be an electrode active material applicable to a battery or capacitor utilizing insertion / extraction of alkali metal ions, and may be a negative electrode active material or a positive electrode active material.
[0086] The negative electrode active material is not particularly limited, and examples thereof include carbon materials such as graphite, graphitizable carbon, non-graphitizable carbon, and composite carbon materials formed by covering graphite particles with carbides of asphalt or resin; materials containing metals or semimetals such as Si and Sn that can be alloyed with lithium, or oxides of the metals or semimetals, etc. As specific examples of carbon materials, carbon materials described in Japanese Patent Publication No. 2013-258392 can be cited. As specific examples of materials containing metals or semimetals that can be alloyed with lithium, or oxides of the metals or semimetals, materials described in Japanese Patent Publication No. 2005-123175 and Japanese Patent Publication No. 2006-107795 can be cited.
[0087] Examples of the positive electrode active material include activated carbon, transition metal oxides such as cobalt oxide, nickel oxide, manganese oxide, and vanadium oxide; and sulfur-based active materials such as simple sulfur and metal sulfides.
[0088] The positive electrode active material and the negative electrode active material may be composed of a single substance or a mixture of two or more substances. The electrode manufacturing device 1 disclosed in the present invention is suitable for pre-doping the negative electrode active material with an alkali metal, and it is particularly preferred that the negative electrode active material is a carbon material or a material containing Si or its oxide.
[0089] As the alkali metal predoped in the active material, lithium or sodium is preferred, and lithium is particularly preferred. When the electrode precursor 73 is used to manufacture an electrode of a lithium ion secondary battery, the density of the active material layer 95 is preferably 1.50 to 2.00 g / cc, and particularly preferably 1.60 to 1.90 g / cc.
[0090] 3. Composition and temperature of doping solution
[0091] When the electrode manufacturing apparatus 1 is used, a solution containing alkali metal ions (hereinafter referred to as a doping solution) is contained in the electrolyte tanks 203 , 205 , 7 , and 207 .
[0092] The doping solution contains alkali metal ions and a solvent. As the solvent, for example, an organic solvent can be mentioned. As the organic solvent, a non-protonic organic solvent is preferred. As the non-protonic organic solvent, for example, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, 1-fluoroethylene carbonate, γ-butyrolactone, acetonitrile, dimethoxyethane, tetrahydrofuran, dioxolane, methylene chloride, sulfolane, diethylene glycol dimethyl ether (diglyme), diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether (triglyme), triethylene glycol methyl butyl ether, tetraethylene glycol dimethyl ether (tetraglyme), etc. can be mentioned.
[0093] In addition, as the above-mentioned organic solvent, ionic liquids such as quaternized imidazolium salts, quaternized pyridinium salts, quaternized pyrrolidinium salts, and quaternized piperidinium salts can also be used. The above-mentioned organic solvent can be composed of a single component or a mixed solvent of two or more components. The organic solvent can be composed of a single component or a mixed solvent of two or more components.
[0094] The alkali metal ions contained in the above-mentioned doping solution are ions constituting alkali metal salts. The alkali metal salt is preferably a lithium salt or a sodium salt. Examples of the anion part constituting the alkali metal salt include PF6 - PF3(C2F5)3 - PF3(CF3)3 - Phosphorus anions with fluorine groups, such as BF4 - 、BF2(CF)2 - 、BF3(CF3) - 、B(CN)4 - Boron anions with fluorine or cyanide groups, such as N(FSO2)2 - 、N(CF3SO2)2 - 、N(C2F5SO2)2 - Sulfonyl imide anions with fluorine groups, such as CF3SO3 - Such as organic sulfonic acid anions having a fluorine group.
[0095] The concentration of the alkali metal salt in the doping solution is preferably 0.1 mol / L or more, and more preferably in the range of 0.5 to 1.5 mol / L. When it is in this range, pre-doping with the alkali metal can be performed efficiently.
[0096] The doping solution may further contain additives such as vinylene carbonate, vinyl ethylene carbonate, 1-fluoroethylene carbonate, 1-(trifluoromethyl)ethylene carbonate, anhydrous succinic acid, anhydrous maleic acid, propane sultone, diethyl sulfone, and the like.
[0097] The above-mentioned doping solution may also contain flame retardants such as phosphazene compounds. As in the electrode manufacturing method disclosed in the present invention, when an alkali metal is doped into the active material in a specific oxygen concentration atmosphere, the amount of flame retardant added can be made less than the previous amount. In the case of adding a flame retardant, the lower limit of the amount of the flame retardant added is not particularly limited. From the viewpoint of effectively controlling the thermal runaway reaction when doping with alkali metals, the amount of the flame retardant added is preferably 0.01 parts by mass or more relative to 100 parts by mass of the doping solution, more preferably 0.03 parts by mass or more, and more preferably 0.05 parts by mass or more. In addition, from the viewpoint of obtaining a high-quality doped electrode, the amount of the flame retardant added is preferably 1 part by mass or less relative to 100 parts by mass of the doping solution, more preferably 0.8 parts by mass or less, and more preferably 0.5 parts by mass or less. When pre-doping is performed, the temperature of the doping solution is preferably above 25°C and below 50°C.
[0098] 4. Method for manufacturing electrode 75 using electrode manufacturing apparatus 1
[0099] First, as a preparation for manufacturing the electrode 75, the following operations are performed. The electrode precursor 73 is wound on the supply roll 47. Then, the electrode precursor 73 is pulled out from the supply roll 47 by the conveying roller group and conveyed to the winding roll 49 along the above-mentioned path. Then, the electrolyte tanks 203, 205, 7, 207, and the cleaning tank 103 are raised and placed on the Figure 1 The fixed position shown. The doping solution is contained in the electrolyte tanks 203, 205, 7, and 207. The doping solution is the doping solution described in "3. Components of the doping solution". The cleaning solution is contained in the cleaning tank 103. The cleaning solution is an organic solvent. As a result, the space 71 of the electrolyte tanks 203, 205, 7, and 207 is filled with the electrolyte. The space 71 of the cleaning tank 103 is filled with the cleaning solution.
[0100] Next, the electrode precursor 73 fed from the supply roller 47 to the winding roller 49 is pulled out from the supply roller 47 toward the winding roller 49 by the conveying roller group and conveyed along the above-mentioned path. When the electrode precursor 73 passes through the electrolyte tanks 205, 7, and 207, the active material contained in the active material layer 95 is pre-doped with alkali metal.
[0101] When pre-doping is performed, the oxygen concentration in the atmosphere in the chamber 10 is greater than 1 volume % and less than 18 volume %. That is, the chamber 10 is set to make the atmosphere in the chamber 10 an atmosphere with an oxygen concentration of greater than 1 volume % and less than 18 volume %. The atmosphere in the chamber 10 is the atmosphere of the electrolyte tanks 205, 7, and 207. The inside of the chamber 10 corresponds to the inside of the electrode manufacturing device 1. The chamber 10 corresponds to the atmosphere setting unit.
[0102] The oxygen concentration in the atmosphere in the chamber 10 is preferably 3% by volume or more, more preferably 5% by volume or more. The oxygen concentration in the atmosphere in the chamber 10 is preferably 15% by volume or less, more preferably less than 12% by volume, and particularly preferably 11.5% by volume or less. By setting the oxygen concentration in the atmosphere in the chamber 10 to be within the above range, the ignition property of the doping solution can be reduced, and the performance of the electrode doped with the alkali metal can be improved.
[0103] In addition, the nitrogen concentration in the atmosphere in the chamber 10 is preferably 30% by volume or more, more preferably 40% by volume or more, and more preferably 50% by volume or more. The nitrogen concentration in the atmosphere in the chamber 10 is preferably 97% by volume or less, more preferably 95% by volume or less, and more preferably 88% by volume or less. By setting the nitrogen concentration in the atmosphere in the chamber 10 to be within the above range, the performance of the electrode doped with the alkali metal can be improved.
[0104] In addition, the atmosphere in the chamber 10 may further include a rare gas such as helium or argon. When the atmosphere in the chamber 10 includes a rare gas, the rare gas concentration is preferably 10% by volume or more, more preferably 20% by volume or more, and more preferably 30% by volume or more. The rare gas concentration in the atmosphere in the chamber 10 is preferably 80% by volume or less, more preferably 75% by volume or less, and more preferably 70% by volume or less. By making the rare gas concentration in the atmosphere in the chamber 10 within the above range, the performance of the electrode doped with the alkali metal can be improved.
[0105] In addition, the pressure of the atmosphere in the chamber 10 is preferably 0.1×10 5 N / m 2 Above and 5×10 5 N / m 2 By setting the pressure of the atmosphere in the chamber 10 to be within the above range, the ignition property of the doping solution can be reduced, and the performance of the electrode doped with the alkali metal can be improved.
[0106] During pre-doping, the temperature of the doping solution contained in the electrolyte tanks 205 , 7 , and 207 is preferably 25° C. or higher and 50° C. or lower.
[0107] By pre-doping the active material with an alkali metal, the electrode precursor 73 becomes the electrode 75. The electrode 75 is transported by the transport roller group and simultaneously cleaned in the cleaning tank 103. Finally, the electrode 75 is wound around the winding roller 49.
[0108] The electrode 75 manufactured by the electrode manufacturing apparatus may be a positive electrode or a negative electrode. When manufacturing a positive electrode, the electrode manufacturing apparatus 1 dopes an alkali metal into a positive electrode active material, and when manufacturing a negative electrode, the electrode manufacturing apparatus 1 dopes an alkali metal into a negative electrode active material.
[0109] When lithium is absorbed in the negative electrode active material of a lithium ion capacitor, the doping amount of the alkali metal is preferably 70 to 95% relative to the theoretical capacity of the negative electrode active material. When lithium is absorbed in the negative electrode active material of a lithium ion secondary battery, the doping amount of the alkali metal is preferably 10 to 30% relative to the theoretical capacity of the negative electrode active material.
[0110] 5. Method for manufacturing power storage device
[0111] The power storage device includes an electrode battery. Examples of the power storage device include capacitors and batteries. The capacitor is not particularly limited as long as it is a capacitor that utilizes the insertion / extraction of alkali metal ions, and examples thereof include lithium ion capacitors and sodium ion capacitors. Among them, lithium ion capacitors are preferred.
[0112] The basic structure of the positive electrode constituting the capacitor may be a common structure. As the positive electrode active material, activated carbon is preferably used.
[0113] The electrolyte constituting the capacitor is usually in the form of a liquid electrolyte. The basic composition of the electrolyte is the same as that of the above-mentioned doping solution. In addition, the concentration of alkali metal ions (alkali metal salts) in the electrolyte is preferably 0.1 mol / L or more, more preferably in the range of 0.5 to 1.5 mol / L. The electrolyte can have a gel or solid form to prevent leakage.
[0114] The capacitor may include a separator between the positive electrode and the negative electrode to prevent the positive electrode and the negative electrode from physically contacting each other. Examples of the separator include nonwoven fabrics or porous films made of cellulose rayon, polyethylene, polypropylene, polyamide, polyester, polyimide, and the like.
[0115] As the structure of the capacitor, for example, the following stacked unit can be listed, which is formed by stacking more than three plate-shaped constituent units to form a stacked body and sealing the stacked body in an outer film, wherein the constituent unit includes a positive electrode and a negative electrode, and a separator between the positive electrode and the negative electrode.
[0116] In addition, as the structure of the capacitor, for example, the following wound unit can also be listed, which is formed by winding a strip-shaped constituent unit to form a stack, and storing the stack in a square or cylindrical container, wherein the constituent unit includes a positive electrode and a negative electrode, and a separator between the positive electrode and the negative electrode.
[0117] The capacitor can be manufactured, for example, by forming a basic structure including at least a negative electrode and a positive electrode, and injecting an electrolyte into the basic structure.
[0118] In the case of a lithium ion capacitor, the density of the active material layer of the lithium ion capacitor is preferably 0.50 to 1.50 g / cc, and particularly preferably 0.70 to 1.20 g / cc.
[0119] As a battery, there is no particular limitation as long as it is a battery that utilizes the insertion / extraction of alkali metal ions. The battery may be a primary battery or a secondary battery. As a battery, for example, a lithium ion secondary battery, a sodium ion secondary battery, an air battery, etc. may be cited. Among them, a lithium ion secondary battery is preferred.
[0120] The basic structure of the positive electrode constituting the battery may be a common structure. As the positive electrode active material, in addition to the positive electrode active materials already exemplified, organic active materials such as nitroxide radical compounds or oxygen may be used.
[0121] The composition of the electrolyte constituting the battery and the composition of the battery itself are the same as those of the capacitor. The battery can be manufactured, for example, by forming a basic structure including at least a negative electrode and a positive electrode and injecting an electrolyte into the basic structure.
[0122] The method for manufacturing a power storage device disclosed herein first manufactures a negative electrode using the method described in "4. Method for manufacturing electrode 75 using electrode manufacturing apparatus 1" above, and then sequentially stacks the negative electrode, a separator, and an electrode other than the negative electrode to form an electrode battery.
[0123] 6. Effects achieved by electrode manufacturing methods
[0124] (1A) The electrode manufacturing method disclosed herein uses a doping solution containing alkali metal ions to dope an active material with an alkali metal in an atmosphere having an oxygen concentration of 1% by volume or more and 18% by volume or less. Therefore, it is not easy to ignite the doping solution. In addition, the modification of the alkali metal doped into the active material can be suppressed. As the modification, for example, the doped lithium is modified into lithium nitride.
[0125] (1B) The electrode manufacturing method disclosed herein can use a doping solution containing alkali metal ions to dope the active material with alkali metal in an atmosphere with an oxygen concentration of 3% by volume or more and 15% by volume or less. In this case, it is less likely that the doping solution will ignite. In addition, the modification of the alkali metal doped into the active material can be further suppressed.
[0126] (1C) The electrode manufacturing method disclosed herein can use a doping solution containing alkali metal ions to dope the active material with alkali metal in an atmosphere with a nitrogen concentration of 30% by volume or more and 97% by volume or less. In this case, it is more difficult for the doping solution to ignite. In addition, the modification of the alkali metal doped into the active material can be further suppressed.
[0127] (1D) When doping the active material with an alkali metal, the electrode manufacturing method disclosed herein can set the temperature of the doping solution to 25° C. or higher and 50° C. or lower. In this case, the doping solution is less likely to ignite, and the modification of the alkali metal doped into the active material can be further suppressed.
[0128] (1E) When the electrode manufacturing method disclosed in the present invention dopes the active material with an alkali metal, the pressure of the atmosphere can be set to 0.1×10 5 N / m 2 Above 5×10 5 N / m 2 In this case, the doping solution is less likely to ignite. And the modification of the alkali metal doped into the active material can be further suppressed.
[0129] (1F) In the method for manufacturing a storage battery device disclosed herein, when manufacturing a negative electrode, a doping solution containing alkali metal ions is used to dope an alkali metal into a negative electrode active material in an atmosphere having an oxygen concentration of 1% by volume or more and 18% by volume or less. Therefore, it is not easy to cause the doping solution to ignite. Furthermore, the modification of the alkali metal doped into the active material can be suppressed.
[0130] 7. Examples
[0131] The present disclosure will be described in further detail using the following Examples and Comparative Examples.
[0132] (Example 1-1)
[0133] (1-1A) Manufacturing of Electrode 75
[0134] Prepare a long strip-shaped negative electrode collector. The dimensions of the negative electrode collector are: width 150 mm, length 100 m, thickness 8 μm. The surface roughness Ra of the negative electrode collector is 0.1 μm. The negative electrode collector is made of copper foil. Figure 6As shown, negative electrode active material layers 95 are formed on both surfaces of the negative electrode collector 93 to obtain an electrode precursor 73. The thickness of the negative electrode active material layer 95 is 80 μm. The negative electrode active material layer 95 is formed along the length direction of the negative electrode collector 93. The negative electrode active material layer 95 is formed at the center of the negative electrode collector 93 in the width direction, and the width of the negative electrode active material layer 95 is 120 mm. The negative electrode active material layer unformed portions at both ends of the negative electrode collector 93 in the width direction are 15 mm each. The negative electrode active material layer unformed portion is a portion where the negative electrode active material layer 95 is not formed.
[0135] Negative electrode active material layer 95 contains graphite, carboxymethyl cellulose, acetylene black, a binder, and a dispersant at a mass ratio of 88:3:5:3:1. Graphite corresponds to the negative electrode active material and to the carbon-based material. Acetylene black corresponds to the conductive agent.
[0136] Next, the counter electrode unit 51 was manufactured in the following manner. First, a long copper plate with a thickness of 2 mm was prepared. A lithium metal plate was pasted onto the copper plate. The dimensions of the lithium metal plate were: width 120 mm × length 800 mm, and thickness 1 mm. The lithium metal plate was pasted along the length direction of the copper plate. The copper plate with the lithium metal plate pasted as above was used as the counter electrode unit 51. Eight identical counter electrode units 51 were manufactured. The counter electrode unit 51 corresponds to the lithium electrode.
[0137] Prepare Figure 1 The electrode manufacturing apparatus 1 shown in the figure is provided, and the electrode precursor 73 and the counter electrode unit 51 are accommodated in the chamber 10. Then, the electrolyte is supplied to the electrolyte tanks 203, 205, 7, and 207 of the electrode manufacturing apparatus 1. The electrolyte is a solution containing 1.2M LiPF6. The solvent of the electrolyte is a mixed solvent containing ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a volume ratio of 3:4:3.
[0138] Next, the electrode precursor 73 and the electrode unit 51 set on the electrode manufacturing device 1 are connected to a DC power supply with a current and voltage monitor, and the electrode precursor 73 is transported at a speed of 0.16 m / min and a current of 40 A is simultaneously passed. The atmosphere in the chamber 10 during power-on is set to an oxygen concentration of 10% by volume and a nitrogen concentration of 90% by volume, the atmosphere temperature in the chamber 10 is adjusted to 25° C., and the temperature of the electrolyte is set to 40° C. Taking into account the irreversible capacity, the power-on time is set to the time when the lithium doping ratio in the negative electrode active material layer 95 reaches 70% of the discharge capacity C2 of the negative electrode. In addition, the irreversible capacity is estimated in advance by measuring the discharge capacity of the negative electrode after lithium doping. Through this process, lithium is doped into the negative electrode active material in the negative electrode active material layer 95, so that the electrode precursor 73 becomes the electrode 75. In addition, the electrode 75 in this embodiment, the embodiments described below, and the comparative examples is a negative electrode for a lithium ion capacitor.
[0139] The electrode 75 was passed through the cleaning tank 103 containing EMC (ethyl methyl carbonate) at 25° C. Thereafter, the electrode 75 was wound around the winding roll 49 and stored for 7 hours. In this way, the electrode 75 was manufactured.
[0140] (1-1B) Evaluation Method and Evaluation Results of Appearance Evaluation of Electrode 75
[0141] The appearance of the electrode 75 obtained in (1-1A) was observed. The case where no black change was observed in the electrode 75 was evaluated as "A", the case where black change was observed in a local area of the electrode 75 was evaluated as "B", and the case where the entire electrode 75 was observed to be black was evaluated as "C". The evaluation results are shown in Table 1.
[0142]
Table 1
[0143]
[0144] (1-1C) Evaluation method and results of negative electrode discharge capacity
[0145] Prepare a negative electrode of 4.0 cm × 2.6 cm (excluding the terminal welding portion) from the electrode 75 obtained in (1-1A) above by punching. Next, assemble a three-electrode battery using the negative electrode manufactured above as the working electrode and lithium metal as the counter electrode and reference electrode. Inject an electrolyte into the three-electrode battery. The electrolyte is a solution containing 1.2M LiPF6. The solvent of the electrolyte is a mixed solvent containing ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a volume ratio of 3:4:3. Through the above steps, a battery for evaluation is made.
[0146] The prepared evaluation cell was charged at a current density of 0.1 mA / cm 2The battery was discharged at a constant current of 1.50 V until the negative electrode potential reached 3.0 V vs. Li / Li+, and the discharge capacity was measured. The evaluation results are shown in Table 1.
[0147] (Examples 1-2 to 1-6, Comparative Examples 1-1, 1-2)
[0148] The electrodes of Examples 1-2 to 1-6 and Comparative Examples 1-1 and 1-2 were manufactured and evaluated in the same manner as in Example 1-1, except that the oxygen concentration, nitrogen concentration, and temperature of the atmosphere in the chamber 10 when the power was applied, and the temperature of the electrolyte shown in Table 1 were different. The evaluation results are shown in Table 1.
[0149] (Example 2-1)
[0150] The ignition property was evaluated in the following manner. An electrolyte was supplied into the container. The electrolyte was a solution containing 1.2M LiPF6. The solvent of the electrolyte was a mixed solvent containing ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate in a volume ratio of 3:4:3. The temperature of the electrolyte was adjusted to 40°C after the electrolyte was added. The atmosphere in the container was set to an oxygen concentration of 10% by volume and a nitrogen concentration of 90% by volume. The temperature in the container was 25°C. Then, the container was opened and immediately ignited. The situation where no combustion was observed was evaluated as "A", the situation where combustion was observed for a short time was evaluated as "B", and the situation where combustion was observed was evaluated as "C". The evaluation results are shown in Table 2.
[0151]
Table 2
[0152]
[0153] (Examples 2-2 to 2-6, Comparative Example 2-1)
[0154] The ignitability of Examples 2-2 to 2-6 and Comparative Example 2-1 was evaluated in the same manner as in Example 2-1, except that the oxygen concentration, nitrogen concentration, and temperature of the atmosphere in the container and the temperature of the electrolyte shown in Table 2 were different. The evaluation results are shown in Table 2.
[0155] <Other Implementation Methods>
[0156] As mentioned above, although embodiment of this disclosure was described, this disclosure is not limited to the said embodiment, Various deformation|transformation can be carried out.
[0157] (1) In the first embodiment, pre-doping may be performed by a single-sheet method. The single-sheet method is a method in which pre-doping is performed in a state where the cut electrode plate and the alkali metal plate are placed in a doping solution with a separator interposed therebetween.
[0158] (2) The functions of one constituent element in each of the above-mentioned embodiments may be shared by multiple constituent elements, or the functions of multiple constituent elements may be performed by one constituent element. In addition, a part of the configuration of each of the above-mentioned embodiments may be omitted. In addition, at least a part of the configuration of each of the above-mentioned embodiments may be added to the configuration of the other embodiments, or at least a part of the configuration of each of the above-mentioned embodiments may be replaced with the configuration of the other embodiments, etc. In addition, all the modes included in the technical ideas determined by the statements recorded in the claims are embodiments of the present disclosure.
[0159] (3) In addition to the above-mentioned electrode manufacturing method, the present disclosure can be implemented in various forms such as an electrode manufacturing device, a system using the electrode manufacturing device as a constituent element, and a pre-doping method.
Claims
1. A method for manufacturing an electrode, comprising manufacturing an electrode having an active material layer using an electrode manufacturing apparatus, in, The active material layer contains an active material doped with an alkali metal, and the electrode manufacturing method is characterized by comprising the following steps: The electrode manufacturing device comprises a chamber, an electrolyte tank and a counter electrode unit. An electrode precursor and a counter electrode unit having an active material layer are housed in a chamber. Next, a doping solution containing alkali metal ions is supplied to an electrolyte tank. Next, the electrode precursor and the counter electrode unit of the electrode manufacturing device are connected to a DC power supply and energized. In an atmosphere where an oxygen concentration is greater than 5 volume % and less than 15 volume % and a nitrogen concentration is greater than 85 volume % and less than 95 volume %, alkali metals are doped into the active material.
2. The electrode manufacturing method according to claim 1, It is characterized in that When the active material is doped with an alkali metal, the temperature of the doping solution is 25° C. or higher and 50° C. or lower.
3. The electrode manufacturing method according to claim 1, It is characterized in that The pressure of the atmosphere is 0.1×10 5 N / m 2 Above and 5×10 5 N / m 2 the following.
4. A method for manufacturing an electric storage device, in, The power storage device includes an electrode battery, and the method for manufacturing the power storage device is characterized by comprising the following steps: A negative electrode having an active material layer is manufactured by the electrode manufacturing method according to any one of claims 1 to 3, wherein the active material layer includes an active material doped with an alkali metal; and The negative electrode, a separator, and an electrode different from the negative electrode are sequentially stacked to form the electrode battery.
5. An electrode manufacturing device for manufacturing an electrode having an active material layer, in, The active material layer contains an active material doped with an alkali metal, and the electrode manufacturing device is characterized in that: The apparatus is provided with a chamber, an electrolyte tank and a counter electrode unit, wherein the chamber is configured to set the atmosphere inside the electrode manufacturing apparatus to an atmosphere having an oxygen concentration of 5% by volume to 15% by volume and a nitrogen concentration of 85% by volume to 95% by volume.