Method for manufacturing a semiconductor device
By using electron beam irradiation and development techniques in high-frequency FETs to form an asymmetric gate electrode, the problem of electric field concentration caused by the reduction of gate length is solved, the manufacturing process is simplified and the high-frequency characteristics are improved.
Patent Information
- Application Number
- CN202110153382.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-02-06
- Filing Date
- 2021-02-04
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-02-04
AI Technical Summary
In high-frequency FETs, the decrease in the gate length leads to concentrated electric fields, and the existing manufacturing process is complicated and it is difficult to form a gate electrode with an asymmetric shape, affecting the high-frequency characteristics.
By forming a protective film and a resist film on the semiconductor substrate, an asymmetric gate electrode is formed using electron beam irradiation and development techniques, gate-source capacitance is reduced, and a field plate is formed through a metal film to suppress electric field concentration .
The manufacturing process is simplified, gate-source capacitance is reduced, electric field concentration is suppressed, high frequency characteristics are improved, and productivity is improved.
Smart Images

Figure CN113223935B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for manufacturing a semiconductor device, for example, a method for manufacturing a semiconductor device including the step of forming a gate electrode. Background Art
[0002] In a high-frequency FET (field effect transistor), the gate length is reduced to improve high-frequency characteristics. Due to the reduction in gate length, the transconductance of the FET increases. However, in a state where the gate length is reduced, for example, when the source electrode is grounded and a high voltage is applied to the drain electrode, the electric field is concentrated at the gate end on the drain electrode side. In order to alleviate this situation, a field plate (FP) structure is known (for example, Japanese Patent Application Publication No. 2015-220430 and Japanese Patent Application Publication No. 2016-136547). Summary of the invention
[0003] In the field plate structure, a field plate (FP) is formed on the drain electrode side of the gate electrode, and the field plate is also formed on the source electrode side. The increase in gate-source capacitance due to the field plate on the source electrode side is a factor that deteriorates the high-frequency characteristics of the transistor. Therefore, in order to reduce the gate-source capacitance, it is preferred that the length of the field plate on the source electrode side is smaller than the length of the field plate on the drain electrode side. However, if the gate length is shortened and the field plate on the source electrode side is shortened so that the shape of the gate electrode is asymmetric in the channel direction, the manufacturing process becomes complicated.
[0004] An object of the present disclosure is to provide a simplified manufacturing process capable of forming a gate electrode having an asymmetric shape even when the gate electrode is reduced in size.
[0005] According to the method for manufacturing a semiconductor device disclosed in the present invention, the semiconductor device has a source electrode, a drain electrode and a gate electrode arranged between the source electrode and the drain electrode, and the method includes the following steps: forming a protective film on a semiconductor substrate; forming a resist film on the protective film so that the resist film includes the following area: at the area, the resist film becomes thicker from the drain electrode side to the source electrode side between the source electrode and the drain electrode; forming a first opening in the resist film by irradiating the resist film in the area with an electron beam and developing the resist film; forming a second opening exposing the upper surface of the semiconductor substrate by removing the protective film using the resist film with the first opening formed thereon as a mask; forming the third opening in the resist film by further developing the resist film after forming the second opening, extending the first opening toward the drain electrode side; and forming a gate electrode in the second opening and the third opening. BRIEF DESCRIPTION OF THE DRAWINGS
[0006] Figures 1A to 1D is a cross-sectional view (Part 1) illustrating a method for forming a semiconductor device according to a first embodiment.
[0007] Figures 2A to 2D is a cross-sectional view (Part 2) illustrating the method for forming the semiconductor device according to the first embodiment.
[0008] Figure 3A and 3B is a cross-sectional view (Part 3) illustrating the method for forming the semiconductor device according to the first embodiment.
[0009] Figures 4A to 4C is a cross-sectional view (Part 1) illustrating a method for forming a semiconductor device according to a second embodiment.
[0010] Figures 5A to 5C is a cross-sectional view (Part 2) illustrating a method for forming a semiconductor device according to a second embodiment.
[0011] Figures 6A to 6D is a cross-sectional view illustrating a method for forming a semiconductor device according to a first comparative example.
[0012] Figures 7A to 7C is a cross-sectional view illustrating a method for forming a semiconductor device according to a second comparative example. DETAILED DESCRIPTION
[0013] Some embodiments will now be described.
[0014] (1) An embodiment of the present disclosure is a method for manufacturing a semiconductor device having a source electrode, a drain electrode, and a gate electrode disposed between the source electrode and the drain electrode, the method comprising the following steps: forming a protective film on a semiconductor substrate; forming a resist film on the protective film so that the resist film includes a region where the resist film becomes thicker from the drain electrode side to the source electrode side between the source electrode and the drain electrode; forming a first opening in the resist film by irradiating the resist film in the region with an electron beam and developing the resist film; forming a second opening exposing the upper surface of the semiconductor substrate by removing the protective film using the resist film on which the first opening is formed as a mask; forming the third opening in the resist film by further developing the resist film after forming the second opening, extending the first opening toward the drain electrode side; and forming a gate electrode in the second opening and the third opening. Thus, the manufacturing process can be simplified.
[0015] (2) Preferably, the step of forming an anti-etching film includes: setting the thickness of the source electrode and the drain electrode to be greater than the thickness of the protective film, and forming the anti-etching film so that the anti-etching film covers the source electrode and the drain electrode, thereby forming the anti-etching film and causing the area to be formed.
[0016] (3) Preferably, the distance between the region and the source electrode is smaller than the distance between the region and the drain electrode.
[0017] (4) Preferably, in the step of forming the resist film, the thickness of the source electrode is set larger than the thickness of the drain electrode.
[0018] A specific example of a method for manufacturing a semiconductor device according to the present disclosure will be described below with reference to the accompanying drawings. It should be noted that the present disclosure is not limited to these examples, but is indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0019] (First embodiment)
[0020] Figures 1A to 3B 1 is a cross-sectional view illustrating a method for forming a semiconductor device according to a first embodiment. Figure 1A As shown in , a semiconductor substrate 10 is prepared. The semiconductor substrate 10 has a substrate 11 and a semiconductor layer 12 formed on the substrate 11. When the semiconductor device is a HEMT (high mobility electron transistor), the substrate 11 is, for example, a SiC substrate, a silicon substrate, a GaN substrate, or a sapphire substrate. The semiconductor layer 12 has, for example, an AlN layer, a GaN layer, an AlGaN electron supply layer, and a GaN cap layer from the substrate 11 side. The substrate 11 may be a GaAs substrate, and the semiconductor layer 12 may be a GaAs layer, an AlGaAs electron supply layer, and a GaAs cap layer from the substrate 11 side. The semiconductor device may be a FET (field effect transistor) other than a HEMT. The direction in which the semiconductor layer 12 is formed on the substrate 11 may be referred to as a film formation direction.
[0021] like Figure 1B As shown in FIG. 1 , a protective film 16 is formed on the semiconductor substrate 10. The protective film 16 is an insulating film such as a silicon nitride film and is formed by using a CVD (Chemical Vapor Deposition) method. The thickness of the protective film 16 is, for example, 60 nm, and can be, for example, 50 nm to 200 nm.
[0022] like Figure 1CAs shown in , an opening is formed in the protective film 16. The formation of the opening exposes the upper surface of the semiconductor layer 12 from the protective film 16. The source electrode 14 and the drain electrode 15 are formed to contact the exposed upper surface of the semiconductor layer 12. The source electrode 14 and the drain electrode 15 include, for example, a titanium film and an aluminum film from the semiconductor substrate 10 side. The thickness of each of the source electrode 14 and the drain electrode 15 in the film formation direction is, for example, 200nm, and can be, for example, 100nm to 400nm. The thicknesses of the source electrode 14 and the drain electrode 15 are substantially the same as each other. The distance L5 between the source electrode 14 and the drain electrode 15 is, for example, 2.5μm, and can be, for example, 1μm to 5μm.
[0023] like Figure 1D As shown in , a resist film 20 is formed on a semiconductor substrate 10 so as to cover the protective film 16, the source electrode 14 and the drain electrode 15. The resist film 20 is formed using a spin coating method. The thickness of the resist film 20 on the flat surface is, for example, 400nm, and can be, for example, 200nm to 800nm. For example, the flat surface corresponds to a region separated from a step formed between the protective film 16 and the source electrode 14 (or the drain electrode 15) along the film formation direction in the channel direction. The channel direction is, for example, from the source electrode 14 to the drain electrode 15. The resist is, for example, ZEP520A manufactured by ZEON Corporation. ZEP520A contains anisole.
[0024] Due to the corresponding thickness difference (step) between the protective film 16 and the source electrode 14 and between the protective film 16 and the drain electrode 15, the thickness of the resist film 20 changes along the channel direction. The basic central region 54 located between the source electrode 14 and the drain electrode 15 is a region (flat region) where the thickness of the resist film 20 is roughly uniform. This flat region can be considered as a part of the above-mentioned flat surface. The region 50 from the region 54 toward the source electrode 14 is a region where the thickness of the resist film 20 becomes thicker toward the source electrode 14 (first inclined region). The region 52 from the region 54 toward the drain electrode 15 is a region where the thickness of the resist film 20 becomes thicker toward the drain electrode 15 (second inclined region). Therefore, the thickness of the regions 50 and 52 of the resist film 20 is greater than the thickness of the above-mentioned flat surface.
[0025] like Figure 2AAs shown in , the resist film 20 in the region 50 is irradiated with the electron beam 22. The resist film 20 is sensitized by the electron beam 22. At this time, in the resist film 20, the region 56 closer to the source electrode 14 than the position irradiated with the electron beam 22 has a greater thickness than the region 58 closer to the drain electrode 15 than the position irradiated with the electron beam 22. Therefore, in the region near the lower surface of the resist film 20 below the region 56 where the resist film 20 is thicker, the number of irradiated electrons is relatively small. In the region near the upper surface of the resist film 20, a small amount of electrons are reflected by the semiconductor substrate 10. Therefore, fewer electrons are used to sensitize the resist film 20. Under the region 58 having the resist film 20 thinner than the region 56, a relatively large amount of electrons are irradiated even in the region near the lower surface of the resist film 20. Since many electrons are reflected by the semiconductor substrate 10, there are many electrons in the region near the upper surface of the resist film 20. Therefore, there are relatively many electrons to sensitize the resist film 20. Therefore, the resist film 20 is more sensitized in the region 58 than in the region 56.
[0026] like Figure 2B As shown in , the resist film 20 is developed, for example, by a spray developing method or an immersion developing method. The developer is, for example, ZED-N50 manufactured by ZEON Corporation. The main component in ZED-N50 is n-pentyl acetate (n-pentyl acetate), and its content is 99 weight % or more. The developing time is, for example, 120 seconds. For example, depending on the temperature, the developing time can be from 60 seconds to 240 seconds. Thus, an opening 30 is formed in the resist film 20. At this time, relative to the irradiation position of the electron beam 22, the more sensitized region 58 is opened wider than the region 56, for example, about 10nm wider than the region 56. The opening length of the opening 30 is, for example, 0.05μm to 0.2μm. Here, the opening length is, for example, the length of the upper surface of the protective film 16 exposed by the opening 30 in the channel direction. The center of the opening length is closer to the drain electrode 15 side than the irradiation position of the electron beam 22. On the source electrode 14 side of the opening 30 , the thickness T3 of the resist film 20 is, for example, 520 nm, and on the drain electrode 15 side of the opening 30 , the thickness T4 of the resist film 20 is, for example, 400 nm.
[0027] like Figure 2CAs shown in , the protective film 16 is dry-etched using the resist film 20 as a mask to form an opening 32 in the protective film 16. As a result, a portion of the upper surface of the semiconductor substrate 10 is exposed. The distance L3 between the center of the opening 32 and the end of the source electrode 14 is, for example, 0.5 μm, and the distance L4 between the center of the opening 32 and the end of the drain electrode 15 is, for example, 2.5 μm. That is, the openings 30 and 32 are arranged closer to the source electrode 14 side than the center between the source electrode 14 and the drain electrode 15 in the channel direction.
[0028] like Figure 2D As shown in FIG. 1 , the resist film 20 is additionally developed with a developer. The developer may be a Figure 2B The developer of the same composition as the developer or the developer having a different composition. The more sensitized region 58 opens wider toward the drain electrode 15 than the region 56. An opening 34 having a longer opening length than the opening 30 is formed. The distance L1 between the side surface of the opening 32 disposed on the source electrode 14 side (the side surface of the protective film 16 disposed on the source electrode 14 side) and the side surface of the opening 34 disposed on the source electrode 14 side (the side surface of the resist film 20 disposed on the source electrode 14 side) is smaller than the distance L2 between the side surface of the opening 32 disposed on the drain electrode 15 side (the side surface of the protective film 16 disposed on the drain electrode 15 side) and the side surface of the opening 34 disposed on the drain electrode 15 side (the side surface of the resist film 20 disposed on the drain electrode 15 side). For example, when the developer is ZED-N50 and the additional development time is 90 seconds, the distance L1 is 20 nm, and the distance L2 is 70 nm. In order to increase the distance L2, Figure 2B The difference between the thickness T3 and T4 of the resist film 20 in the embodiment is preferably, for example, 50 nm or more. In order to suppress the opening defect caused by the large inclination of the resist film 20 in the channel direction at the irradiation position of the electron beam 22, the difference between T3 and T4 is preferably, for example, 200 nm or less. Therefore, the thickness difference between the protective film 16 and the source electrode 14 is preferably, for example, 50 nm or more and 200 nm or less.
[0029] like Figure 3A As shown in FIG. 1 , the metal film 17 is formed in the openings 34 and 32 and on the resist film 20 by using a vacuum deposition method. The metal film 17 includes, for example, a nickel film, a palladium film, and a gold film in order from the semiconductor layer 12 in the film formation direction.
[0030] like Figure 3BAs shown in , the metal film 17 on the resist film 20 is peeled off by removing the resist film 20. Thus, the gate electrode 18 is formed on the semiconductor substrate 10 in the opening 32. The length of the field plate 19a provided on the source electrode 14 side of the gate electrode 18 in the channel direction is L1, and the length of the field plate 19b provided on the drain electrode 15 side in the channel direction is a distance L2. In this way, the length of the field plate 19a provided on the source electrode 14 side in the channel direction can be made smaller than the length of the field plate 19b provided on the drain electrode 15 side in the channel direction. Therefore, the gate-source capacitance can be reduced, and the electric field concentration on the drain electrode 15 side of the gate electrode 18 can be suppressed. Since the opening 30 is formed by using an electron beam stretching method, the opening length of the opening 32 can be reduced to reduce the gate length.
[0031] When the resist film 20 is formed, in a state where the protective film 16 is sandwiched between the source electrode 14 and the drain electrode 15, the thickness of the resist film 20 on the source electrode 14 side and the drain electrode 15 side is substantially the same. Therefore, the regions 50 and 52 of the resist film 20 are formed symmetrically with respect to the centers of the source electrode 14 and the drain electrode 15. Therefore, the region 50 is formed on the source electrode 14 side with respect to the centers of the source electrode 14 and the drain electrode 15. As described above, the opening 32 is provided in the region 50, and the distance L3 between the center of the opening 32 and the end of the source electrode 14 is set to be smaller than the distance L4 between the center of the opening 32 and the end of the drain electrode 15. As the distance L3 increases or decreases, the gate-source resistance also increases or decreases, and as the distance L4 increases or decreases, the gate-drain resistance also increases or decreases. Therefore, the gate-source resistance can be reduced.
[0032] (experiment)
[0033] An experiment was conducted to examine how much the difference between the distances L1 and L2 is caused by the difference in thickness T3 and T4 of the resist film 20. In this experiment, ZEP520A was used as a resist and ZED-N50 was used as a developer. In order to facilitate observation by SEM (Scanning Electron Microscope), Figure 2B The opening length of the opening 30 in the resist film 20 is set to about 0.6 μm. The thicknesses T3 and T4 of the resist film 20 are about 520 nm and about 400 nm, respectively. Figure 2D , when additional development was performed for 90 seconds, the distances L1 and L2 became approximately 20 nm and 70 nm, respectively. It was thus found that the distance L2 can be made larger than the distance L1 by making the thickness T3 of the resist film 20 larger than the thickness T4.
[0034] (Second embodiment)
[0035] The second embodiment describes an example in which the thickness of the source electrode is different from the thickness of the drain electrode when the resist film 20 is formed. Figures 4A to 5C 1 is a cross-sectional view illustrating a method for forming a semiconductor device according to the second embodiment. Since the steps until the protective film 16 is formed on the surface of the semiconductor substrate 10 are the same as those of the first embodiment, the first embodiment is performed. Figure 1A and 1B Next, Figure 4A As shown in , the source electrode 14 and the drain electrode 15 are formed so that the thickness T1 of the source electrode 14 is greater than the thickness T2 of the drain electrode 15. For example, the source electrode 14 and the drain electrode 15 are formed in different steps. For example, an opening for exposing the semiconductor layer 12 is provided in the protective film 16, in the step of forming the drain electrode 15, the opening for forming the source electrode 14 is covered with a resist film, and in another step of forming the source electrode 14, the pre-formed drain electrode 15 is covered with a resist film. The source electrode 14 may be formed first, and then the drain electrode 15 may be formed. The thicknesses T1 and T2 are, for example, 300 nm and 200 nm, respectively.
[0036] like Figure 4B As shown in Figure 1D The resist film 20 is formed in the same manner as in the first embodiment. Figure 1D In contrast, regions 52, 54 and 50 are located near drain electrode 15. Figure 4C As shown in Figure 2A and 2B The opening 30 is formed in the resist film 20 in the same manner. That is, a region 50 of the resist film 20 is irradiated with the electron beam 22 to form the opening 30. In the region 50, the thickness of the resist film 20 increases from the drain electrode 15 side to the source electrode 14 side. Figure 1D In contrast, the opening 30 is located near the drain electrode 15 .
[0037] like Figure 5A As shown in Figure 2C In the same manner, an opening 32 is formed in the protective film 16. Figure 5B As shown in FIG. , the opening 30 is Figure 2D In the same manner, the opening 34 is expanded toward the drain electrode 15 side by additional development, thereby forming an opening 34. Since the opening 34 is formed to be wider than the opening 30 by additional development, the opening 34 includes the opening 30 as the shape of the hole. In terms of the opening of the resist film 20, the opening 30 and the opening 34 are basically the same. However, in order to distinguish the shape and size of the opening before and after additional development, for convenience, the opening before additional development is referred to as the opening 30, and the opening after additional development is referred to as the opening 34. Figure 5CAs shown in Figure 3A and 3B The same manner is formed on the entire surface, and the metal film formed on the upper surface of the resist film 20 is removed by a lift-off method, thereby forming the gate electrode 18 .
[0038] In the first embodiment, the gate-source resistance can be reduced. However, the distance between the gate electrode 18 and the source electrode 14 becomes too small, so the parasitic capacitance between the gate electrode 18 and the source electrode 14 may be a problem. In addition, the gate electrode 18 may be preferably formed near the center between the source electrode 14 and the drain electrode 15. In the second embodiment, the gate electrode 18 is formed in a relatively wide range between the source electrode 14 and the drain electrode 15 by making the thickness T1 of the source electrode 14 and the thickness T2 of the drain electrode 15 different from each other. When the region 50 of the resist film 20 is irradiated with the electron beam 22, the gate electrode 18 is formed near the center between the source electrode 14 and the drain electrode 15 by making the source electrode 14 thicker than the drain electrode 15. The difference between the thickness T1 of the source electrode 14 and the thickness T2 of the drain electrode 15 is, for example, 50nm or more and 200nm or less.
[0039] A comparative example will be described to explain the effects of the first embodiment and the second embodiment.
[0040] (First Comparative Example)
[0041] Figures 6A to 6D 1 is a cross-sectional view illustrating a method for forming a semiconductor device according to a first comparative example. Fig. 6A As shown in FIG. 1 , in the first embodiment Figure 1D After the step of , the region 54 is irradiated by the electron beam 22. Figure 6B As shown in Figure 2B and 2C In the same manner, the opening 30 is formed in the resist film 20, and the opening 32 is formed in the protective film 16. The openings 30 and 32 are formed in the region 54.
[0042] like Figure 6C As shown in Figure 2D The other development steps are performed in the same manner. The distance L2′ between the side surface of the opening 34 formed in the resist film 20, which is disposed on the source electrode 14 side, and the side surface of the opening 32, which is disposed on the source electrode 14 side, is substantially the same as the distance L2 between the side surface of the opening 34, which is disposed on the drain electrode 15 side, and the side surface of the opening 32, which is disposed on the drain electrode 15 side. This is because the region 54 where the thickness of the resist film 20 is substantially uniform is irradiated with the electron beam 22, as shown in FIG. Fig. 6A as shown in .
[0043] like Fig.6D As shown in Figure 3A and 3B The gate electrode 18 is formed in the same manner in the openings 32 and 34. The lengths of the field plates 19a and 19b are substantially the same distances L2' and L2.
[0044] In the first comparative example, the length of the field plate 19a on the source electrode 14 side and the length of the field plate 19b on the drain electrode 15 side are approximately the same. In order to suppress the electric field concentration on the drain electrode 15 side, the field plate 19b on the drain electrode 15 side preferably has a specific length. For example, when the source electrode 14 is grounded, it is not necessary to suppress the electric field concentration in the field plate 19a on the source electrode 14 side. On the other hand, when the field plate 19a becomes longer, the gate-source capacitance increases, and the high-frequency characteristics of the transistor may deteriorate. In the following second comparative example, the field plate 19a is made shorter than the field plate 19b.
[0045] (Second Comparative Example)
[0046] Figures 7A to 7C 2 is a cross-sectional view illustrating a method for forming a semiconductor device according to a second comparative example. Fig. 7A As shown in FIG. 1 , in the first comparative example Figure 6B Thereafter, the resist film 20 disposed closer to the drain electrode 15 than the opening 30 is irradiated with the electron beam 24. Figure 7B As shown in , the resist film 20 is developed. Thus, the opening 34 expands toward the drain electrode 15 side compared to the expansion of the source electrode 14 side of the opening 30. Therefore, the distance L2 is greater than the distance L1.
[0047] like Figure 7C As shown in the first comparative example, Fig.6D The gate electrode 18 is formed in the same manner. The length of the field plate 19a on the source electrode 14 side is smaller than the length of the field plate 19b on the drain electrode 15 side. Thus, the gate-source capacitance can be suppressed, and the degradation of the transistor characteristics can be suppressed. However, since the electron beam drawing is performed twice, the time required for drawing is doubled, and the productivity for forming the gate electrode 18 is reduced. In addition, it is difficult to accurately align the first irradiation position of the electron beam 22 with the second irradiation position of the electron beam 24, so a length deviation of the field plate 19b occurs. From the point of view of suppressing the electric field concentration on the drain electrode 15 side of the gate electrode 18, the field plate 19b is preferably long. However, when the field plate 19b is too long, the gate-gate capacitance becomes large, which causes the high-frequency characteristics of the transistor to deteriorate. Therefore, it is preferable to reduce the manufacturing deviation of the length of the field plate 19b.
[0048] According to the first embodiment, the protective film 16 is formed on the semiconductor substrate 10, such as Figure 1BAs shown in Figure 1D and 4B As shown in , the resist film 20 is formed on the protective film 16 so that the resist film 20 has a region 50 where the resist film 20 becomes thicker from the drain electrode 15 side to the source electrode 14 side, and the region 50 is provided between the source electrode 14 and the drain electrode 15. Figure 2A , 2B As described in FIGS. 4A and 4C, the opening 30 (ie, the first opening) is formed in the resist film 20 by irradiating the resist film 20 in the region 50 with the electron beam 22 and developing the resist film 20. Figure 2C and 5A As shown in FIG. 1 , a portion of the protective film 16 is removed by using the resist film 20 on which the opening 30 is formed as a mask, thereby forming an opening 32 (ie, a second opening) in the protective film 16. The semiconductor layer 12 is exposed by the opening 32. Figure 2D and 5B As shown in , an opening 34 (i.e., a third opening) is formed in the resist film 20 by further developing the resist film 20, the opening 34 making the side surface on the drain electrode 15 side of the opening 30 closer to the drain electrode 15 and exposing the upper surface of the semiconductor substrate 10. The opening length of the opening 34 in the resist film 20 is greater than the opening length of the opening 30, and the difference in the opening length is mainly located at a position closer to the drain electrode 15 than the opening 32 of the protective film 16. As shown in FIG. Figure 3B and 5C As shown in , gate electrode 18 is formed in openings 32 and 34 .
[0049] Thus, the field plate 19a of the gate electrode 18 can be made shorter than the field plate 19b. Therefore, the increase in gate-source capacitance can be suppressed as in the first comparative example, and the degradation of the high-frequency characteristics of the transistor can be suppressed. In addition, the irradiation of the electron beam 22 is required only once. Thus, compared with the two drawing of the electron beams 22 and 24 described in the second comparative example, the productivity can be improved. In addition, the characteristic deviation caused by the alignment deviation in the channel direction between the irradiation position of the electron beam 22 and the irradiation position of the electron beam 24 can be suppressed. When reducing the gate length, if there is a large deviation in this alignment, it is difficult to reduce the gate length to the desired length.
[0050] like Figure 1D and 4B As shown in FIG. 1 , when forming the resist film 20, the thickness of the source electrode 14 and the drain electrode 15 is set to be greater than the thickness of the protective film 16, and the resist film 20 is formed so that the resist film 20 covers the source electrode 14 and the drain electrode 50 to form the region 50. Figure 2A and 4BAs shown in FIG. 5 , in the irradiation of the electron beam 22, a region closer to the source electrode 14 than the region 54 is irradiated with the electron beam 22. Thus, the opening 30 can be formed in the region 50 where the resist film 20 becomes thicker toward the source electrode 14. The region 50 can be formed by other methods, such as forming a dummy layer corresponding to the source electrode 14, for example.
[0051] In the first embodiment, the thicknesses of the source electrode 14 and the drain electrode 15 are substantially the same. In this case, in the resist film 20, the distance between the region 50 and the source electrode 14 is smaller than the distance between the region 50 and the drain electrode 15. Thus, the gate-source resistance can be reduced.
[0052] In the second embodiment, the thickness of the source electrode 14 is set to be larger than the thickness of the drain electrode 15. Thus, the distance between the region 50 and the source electrode 14 can be made larger than that in the first embodiment. Thus, in the channel direction, the gate electrode 18 can be provided from the vicinity of the center of the source electrode 14 and the drain electrode 15 to a position closer to the source electrode 14 than the vicinity of the center.
[0053] If the reason why the resist film 20 is dissolved on the drain electrode 15 side by additional development is that the number of electrons irradiated on the resist film 20 is different depending on the thickness of the resist film 20, it is considered that this is a phenomenon that occurs universally regardless of the types of the resist film 20 and the developer. Therefore, a resist and a developer other than the above-mentioned resist film 20 and the above-mentioned developer may be used.
[0054] Note that the embodiments disclosed herein are only illustrative in all aspects and should not be understood as limiting. The scope of the present invention is defined by the scope of the claims, rather than in the meanings mentioned above, and is intended to include the meanings equivalent to the scope of the claims and all modifications within the scope.
Claims
1. A method for manufacturing a semiconductor device, the semiconductor device having a source electrode, a drain electrode, and a gate electrode disposed between the source electrode and the drain electrode, the method comprising the following steps: forming a protective film on a semiconductor substrate; forming a resist film on the protective film so that the resist film includes a region where the resist film becomes thicker from the drain electrode side to the source electrode side between the source electrode and the drain electrode; forming a first opening in the resist film by irradiating the resist film in the region with an electron beam and developing the resist film; forming a second opening exposing the upper surface of the semiconductor substrate by removing the protective film using the resist film having the first opening formed thereon as a mask; forming a third opening in the resist film by further developing the resist film after forming the second opening, thereby expanding the first opening toward the drain electrode side; and The gate electrode is formed in the second opening and the third opening.
2. The method for manufacturing a semiconductor device according to claim 1, wherein: The step of forming the resist film includes setting the thickness of the source electrode and the drain electrode to be greater than the thickness of the protective film, and forming the resist film so that the resist film covers the source electrode and the drain electrode, thereby forming the resist film and causing the region to be formed.
3. The method for manufacturing a semiconductor device according to claim 2, wherein: A distance between the region and the source electrode is smaller than a distance between the region and the drain electrode.
4. The method for manufacturing a semiconductor device according to claim 2 or 3, wherein: In the step of forming the resist film, the thickness of the source electrode is set to be larger than the thickness of the drain electrode.
Citation Information
Patent Citations
Field effect transistor
JP2015220430A
Gate electrode and manufacturing method thereof
CN1679173A
Semiconductor device
JP1993326563A
Field effect transistor
JP2012004573A
Compound semiconductor device and method for manufacturing the same
JP2012023214A