Solar Cells

By using transparent electrodes and non-diffusion layers in perovskite solar cells, the diffusion of anode material and the light absorption are suppressed, and the problem of reduced photoelectric conversion efficiency of perovskite solar cells is solved, achieving efficient and durable photoelectric conversion performance.

CN113261126BActive Publication Date: 2024-12-03SEKISUI CHEMICAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080007442.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-19
Filing Date
2020-03-16
Publication Date
2024-12-03
Estimated Expiration
2040-03-16

AI Technical Summary

Technical Problem

After a perovskite solar cell applies voltage for a long time, the anode material diffuses into the photoelectric conversion layer, resulting in a decrease in the photoelectric conversion efficiency, and the prior art is difficult to effectively suppress this phenomenon.

Method used

Transparent electrodes, organic inorganic perovskite compound photoelectric conversion layer and anti-diffusion layer are introduced into solar cells. The anti-diffusion layer contains metals such as molybdenum, tungsten, tantalum, niobium, and other metals or their oxides, with a thickness of 5 to 50 nm, which inhibits the diffusion of the anode and Reduce the absorption of light by the non-diffusion layer.

Benefits of technology

It effectively prevents the diffusion of the anode material, maintains high photoelectric conversion efficiency, and maintains high efficiency conversion performance even after long-term voltage application, improving the durability of solar cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113261126B_ABST
    Figure CN113261126B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a solar cell having high photoelectric conversion efficiency and which is not easily reduced in photoelectric conversion efficiency even when voltage is applied for a long time. The present invention is a solar cell characterized in that it has a cathode, a photoelectric conversion layer, a diffusion prevention layer and an anode in order, wherein the cathode is a transparent electrode, the anode contains at least one selected from aluminum, copper, antimony and molybdenum, the photoelectric conversion layer contains an organic-inorganic perovskite compound represented by the general formula AMX (wherein A is an organic alkali compound and / or an alkali metal, M is a lead or tin atom, and X is a halogen atom), the diffusion prevention layer contains molybdenum, tungsten, tantalum, niobium, zirconium, hafnium or an alloy thereof, and has a thickness of 5 to 30 nm, or the diffusion prevention layer contains an oxide containing titanium, gallium, zinc, tin, indium, antimony, molybdenum, tungsten, vanadium, chromium, nickel or lead, or the diffusion prevention layer contains a nitride containing titanium, vanadium, chromium, niobium, tantalum, molybdenum, zirconium or hafnium, and has a thickness of 5 to 50 nm, or the diffusion prevention layer contains graphite, and has a thickness of 2 nm to 50 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a solar cell having high photoelectric conversion efficiency and whose photoelectric conversion efficiency is not easily reduced even when voltage is applied for a long period of time. Background Art

[0002] Solar cells have been developed that have a stacked structure (photoelectric conversion layer) in which an N-type semiconductor layer and a P-type semiconductor layer are arranged between opposing electrodes. In such solar cells, photocarriers (electron-hole pairs) are generated by light excitation, and electrons move in the N-type semiconductor and holes move in the P-type semiconductor, thereby generating an electric field.

[0003] At present, most of the practical solar cells are inorganic solar cells made of inorganic semiconductors such as silicon. However, inorganic solar cells are not only expensive to manufacture, but also difficult to be large-scale, and their scope of use is limited. Therefore, organic solar cells made of organic semiconductors instead of inorganic semiconductors (such as patent documents 1 and 2) and organic-inorganic solar cells made by combining organic semiconductors with inorganic semiconductors have attracted much attention.

[0004] In organic solar cells and organic inorganic solar cells, fullerenes are used in most cases. It is known that fullerenes mainly function as N-type semiconductors. For example, Patent Document 3 describes a semiconductor heterojunction film formed by using an organic compound that becomes a P-type semiconductor and fullerenes. However, it is known that in organic solar cells and organic inorganic solar cells manufactured using fullerenes, the cause of their degradation is fullerenes (for example, refer to Non-Patent Document 1), and a material to replace fullerenes is sought.

[0005] Therefore, in recent years, photoelectric conversion materials having a perovskite structure using lead, tin, or the like as a central metal, which are called organic-inorganic hybrid semiconductors, have been discovered and shown to have high photoelectric conversion efficiency (for example, Non-Patent Document 2).

[0006] However, a perovskite solar cell using a photoelectric conversion material having such a perovskite structure has high photoelectric conversion efficiency immediately after manufacture. However, if voltage is applied for a long time, the anode material may diffuse into the photoelectric conversion layer containing the organic-inorganic perovskite compound, thereby reducing the photoelectric conversion efficiency.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2006-344794

[0010] Patent Document 2: Japanese Patent No. 4120362

[0011] Patent Document 3: Japanese Patent Application Publication No. 2006-344794

[0012] Non-patent literature

[0013] Non-patent document 1: Reese et al., Adv. Funct. Mater., 20, 3476-3483 (2010)

[0014] Non-patent document 2: MMLee et al., Science, 338, 643-647 (2012) Summary of the invention

[0015] Problems to be solved by the invention

[0016] In response to this problem, the inventors disclosed in Japanese Patent Application No. 2016-184375 a solar cell having a diffusion prevention layer containing a specific metal between a photoelectric conversion layer using an organic-inorganic perovskite compound and a specific anode. The solar cell of Japanese Patent Application No. 2016-184375 suppresses diffusion of the anode by providing a photoelectric conversion layer containing a specific metal, and can maintain a high photoelectric conversion efficiency even when a voltage is applied for a long time.

[0017] However, in the field of solar cells in recent years, competition for photoelectric conversion efficiency has intensified, and solar cells having higher photoelectric conversion efficiency have been demanded.

[0018] An object of the present invention is to provide a solar cell having high photoelectric conversion efficiency and whose photoelectric conversion efficiency is unlikely to decrease even when a voltage is applied for a long period of time.

[0019] Means for solving problems

[0020] The present invention is a solar cell, characterized in that it has a cathode, a photoelectric conversion layer, an anti-diffusion layer and an anode in sequence, the cathode being a transparent electrode, the anode containing at least one selected from aluminum, copper, antimony and molybdenum, the photoelectric conversion layer containing an organic-inorganic perovskite compound represented by the general formula AMX (wherein A is an organic alkali compound and / or an alkali metal, M is a lead or tin atom, and X is a halogen atom), the anti-diffusion layer containing molybdenum, tungsten, tantalum, niobium, zirconium, hafnium or an alloy thereof, and having a thickness of 5 to 30 nm, or the anti-diffusion layer containing an oxide containing titanium, gallium, zinc, tin, indium, antimony, molybdenum, tungsten, vanadium, chromium, nickel or lead, or the anti-diffusion layer containing a nitride containing titanium, vanadium, chromium, niobium, tantalum, molybdenum, zirconium or hafnium, and having a thickness of 5 to 50 nm, or the anti-diffusion layer containing graphite, and having a thickness of 2 nm to 50 nm.

[0021] Hereinafter, the present invention will be described in detail.

[0022] In order to further improve the photoelectric conversion efficiency of a perovskite solar cell with an anti-diffusion layer, the inventors of the present invention have studied the use of materials that reflect light transmitted through the photoelectric conversion layer for the anode. The photoelectric conversion layer containing an organic-inorganic perovskite compound particularly absorbs light with a wavelength of 400 to 600 nm, and light with wavelengths outside the above range is mostly transmitted. Therefore, by reflecting the light that has transmitted through the photoelectric conversion layer, especially the light of 600 nm to 800 nm, at the anode and allowing it to pass through the photoelectric conversion layer again, it is possible to expect an increase in the photoelectric conversion efficiency. However, even when an anode that reflects light is used in a perovskite solar cell with an anti-diffusion layer, the photoelectric conversion efficiency is not improved to the expected level.

[0023] The present inventors have studied the reasons for this and found that the reason is that the diffusion prevention layer absorbs light. Since the diffusion prevention layer absorbs light, the amount of light that is reflected by the anode and reaches the photoelectric conversion layer again is reduced, so the improvement of the photoelectric conversion efficiency is suppressed. In addition, gold has been used as a material for reflecting light of 600nm to 800nm, but gold has the property of easily diffusing into the photoelectric conversion layer. In order to suppress diffusion, the diffusion prevention layer must be thickened, and the absorption of light in the diffusion prevention layer becomes greater. Based on the above insights, the present inventors have further studied and found that by using specific metals in the anode and the diffusion prevention layer, the diffusion of the anode can be prevented, and the absorption of light in the diffusion prevention layer can be suppressed to further improve the photoelectric conversion efficiency, thereby completing the present invention.

[0024] The solar cell of the present invention comprises a cathode, a photoelectric conversion layer, a diffusion prevention layer and an anode in sequence.

[0025] In this specification, a layer refers not only to a layer with a clear boundary, but also to a layer with a concentration gradient of the elements contained gradually changing. It should be noted that the elemental analysis of the layer can be performed, for example, by performing FE-TEM / EDS line analysis measurement of the cross section of the solar cell, confirming the elemental distribution of a specific element, etc. In addition, in this specification, a layer refers not only to a flat film-like layer, but also to a layer that can form a complex interlaced structure with other layers.

[0026] The cathode is a transparent electrode.

[0027] Examples of the cathode material include FTO (fluorine-doped tin oxide), ITO (tin-doped indium oxide), sodium, sodium-potassium alloy, lithium, magnesium, aluminum, magnesium-silver mixture, magnesium-indium mixture, aluminum-lithium alloy, Al / Al2O3 mixture, Al / LiF mixture, etc. These materials may be used alone or in combination of two or more.

[0028] The thickness of the cathode is not particularly limited, but preferably has a lower limit of 10 nm and an upper limit of 1000 nm. If the thickness is 10 nm or more, the resistance can be suppressed on the basis of making the cathode function as an electrode. If the thickness is 1000 nm or less, the light transmittance can be further improved. The thickness of the cathode is more preferably 50 nm lower limit, and more preferably 500 nm upper limit.

[0029] The photoelectric conversion layer contains an organic-inorganic perovskite compound represented by the general formula AMX (wherein A is an organic alkali compound and / or an alkali metal, M is a lead or tin atom, and X is a halogen atom). A solar cell in which the photoelectric conversion layer contains the organic-inorganic perovskite compound is also called an organic-inorganic hybrid solar cell.

[0030] By using the organic-inorganic perovskite compound in the photoelectric conversion layer, the photoelectric conversion efficiency of the solar cell can be improved.

[0031] The above-mentioned A is an organic base compound and / or an alkali metal.

[0032] Specific examples of the organic base compounds include methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, dimethylamine, diethylamine, dipropylamine, dibutylamine, dipentylamine, dihexylamine, trimethylamine, triethylamine, tripropylamine, tributylamine, tripentylamine, trihexylamine, ethylmethylamine, methylpropylamine, butylmethylamine, methylpentylamine, hexylmethylamine, ethylpropylamine, ethylbutylamine, formamidine, acetamidine, guanidine, imidazole, oxazole, pyrrole, aziridine, azirine, azetidine, azete, oxazole, imidazoline, carbazole and ions thereof (e.g., methylammonium (CH3NH3)), phenethylammonium, and the like. Among them, methylamine, ethylamine, propylamine, butylamine, pentylamine, hexylamine, formamidine, acetamidine and ions thereof, and phenethylammonium are preferred, and methylamine, ethylamine, propylamine, formamidine and ions thereof are more preferred.

[0033] Examples of the alkali metal include lithium, sodium, potassium, rubidium, and cesium.

[0034] The above-mentioned M is a metal atom, which is lead or tin. These metal atoms may be used alone or in combination of two or more.

[0035] Above-mentioned X is a halogen atom, for example, chlorine, bromine, iodine, sulfur, selenium etc. can be mentioned. These halogen atoms can be used alone, and two or more kinds can also be used in combination. By containing halogen in the structure, the above-mentioned organic-inorganic perovskite compound is soluble in an organic solvent and can be applied to a cheap printing method etc. Among them, from the aspect that the energy band gap of the above-mentioned organic-inorganic perovskite compound narrows, X is preferably iodine.

[0036] The organic-inorganic perovskite compound preferably has a cubic crystal structure in which a metal atom M is arranged at the body center, an organic alkali compound or an alkali metal A is arranged at each vertex, and a halogen atom X is arranged at the face center.

[0037] Figure 1 It is a schematic diagram showing an example of a crystal structure of an organic-inorganic perovskite compound, which is a cubic crystal structure in which a metal atom M is arranged at the body center, an organic alkali compound or an alkali metal A is arranged at each vertex, and a halogen atom X is arranged at the face center. Although the details are not clear, it is inferred that by having the above structure, the direction of the octahedron in the lattice can be easily changed, so the mobility of electrons in the above organic-inorganic perovskite compound becomes higher, and the photoelectric conversion efficiency of the solar cell is improved.

[0038] The organic-inorganic perovskite compound is preferably a crystalline semiconductor. A crystalline semiconductor refers to a semiconductor whose scattering peak can be detected by measuring the X-ray scattering intensity distribution. By making the organic-inorganic perovskite compound a crystalline semiconductor, the mobility of electrons in the organic-inorganic perovskite compound becomes higher, and the photoelectric conversion efficiency of the solar cell is improved.

[0039] In addition, the crystallinity can also be evaluated as an index of crystallization. The crystallinity can be obtained by separating the scattering peak from the crystalline and the halo from the amorphous part detected by X-ray scattering intensity distribution measurement by fitting, obtaining the respective intensity integrals, and calculating the proportion of the crystalline part in the whole.

[0040] The preferred lower limit of the crystallinity of the organic-inorganic perovskite compound is 30%. If the crystallinity is 30% or more, the mobility of electrons in the organic-inorganic perovskite compound increases, and the photoelectric conversion efficiency of the solar cell improves. The more preferred lower limit of the crystallinity is 50%, and the further preferred lower limit is 70%.

[0041] Examples of methods for increasing the crystallinity of the organic-inorganic perovskite compound include thermal annealing, irradiation with strong light such as laser light, and plasma irradiation.

[0042] As long as the effects of the present invention are not impaired, the photoelectric conversion layer may further include an organic semiconductor or an inorganic semiconductor in addition to the organic-inorganic perovskite compound. It should be noted that the organic semiconductor or inorganic semiconductor mentioned here may function as a hole transport layer or an electron transport layer.

[0043] As the above-mentioned organic semiconductor, for example, compounds having a thiophene skeleton such as poly(3-alkylthiophene) can be cited. In addition, for example, conductive polymers such as poly(p-phenylene vinylene) skeleton, polyvinyl carbazole skeleton, polyaniline skeleton, polyacetylene skeleton can be cited. In addition, for example, compounds having a porphyrin skeleton such as a phthalocyanine skeleton, a naphthalocyanine skeleton, a pentacene skeleton, a benzoporphyrin skeleton, a spirobifluorene skeleton, etc. can be cited.

[0044] Examples of the inorganic semiconductors include titanium oxide, zinc oxide, indium oxide, tin oxide, gallium oxide, tin sulfide, indium sulfide, zinc sulfide, CuSCN, Cu2O, CuI, MoO3, V2O5, WO3, MoS2, MoSe2, and Cu2S.

[0045] The above-mentioned photoelectric conversion layer, when comprising the above-mentioned organic-inorganic perovskite compound and the above-mentioned organic semiconductor or the above-mentioned inorganic semiconductor, may be a laminated body formed by laminating a thin film organic semiconductor or inorganic semiconductor part with a thin film organic-inorganic perovskite compound part, or may be a composite film formed by compounding an organic semiconductor or inorganic semiconductor part with an organic-inorganic perovskite compound part. From the aspect of simplicity of preparation, a laminated body is preferred, and from the aspect of being able to improve the charge separation efficiency in the above-mentioned organic semiconductor or the above-mentioned inorganic semiconductor, a composite film is preferred.

[0046] The preferred lower limit of the thickness of the above-mentioned film-like organic-inorganic perovskite compound part is 5nm, and the preferred upper limit is 5000nm. If the above-mentioned thickness is more than 5nm, light can be fully absorbed, and the photoelectric conversion efficiency becomes high. If the above-mentioned thickness is below 5000nm, it is possible to suppress the generation of the region where charge separation cannot be achieved, thus contributing to the improvement of the photoelectric conversion efficiency. The more preferred lower limit of the above-mentioned thickness is 10nm, and the more preferred upper limit is 1000nm, and the further preferred lower limit is 20nm, and the further preferred upper limit is 500nm.

[0047] When the above-mentioned photoelectric conversion layer is a composite film formed by the composite of an organic semiconductor or an inorganic semiconductor part and an organic inorganic perovskite compound part, the preferred lower limit of the thickness of the above-mentioned composite film is 30nm, and the preferred upper limit is 3000nm. If the above-mentioned thickness is more than 30nm, light can be fully absorbed, and the photoelectric conversion efficiency upturns. If the above-mentioned thickness is below 3000nm, the charge easily reaches the electrode, so the photoelectric conversion efficiency upturns. The more preferred lower limit of the above-mentioned thickness is 40nm, and the more preferred upper limit is 2000nm, and the further preferred lower limit is 50nm, and the further preferred upper limit is 1000nm.

[0048] The method for forming the above-mentioned photoelectric conversion layer is not particularly limited, and vacuum evaporation, sputtering, gas phase reaction (CVD), electrochemical deposition, printing, etc. can be cited. Among them, by adopting the printing method, a solar cell capable of exerting high photoelectric conversion efficiency can be formed in a large area and simply. As a printing method, for example, a spin coating method, a casting method, etc. can be cited, and as a method using the printing method, a roll-to-roll method, etc. can be cited.

[0049] The solar cell of the present invention may include an electron transport layer between the cathode and the photoelectric conversion layer.

[0050] The material of the electron transport layer is not particularly limited, and examples thereof include N-type conductive polymers, N-type low molecular weight organic semiconductors, N-type metal oxides, N-type metal sulfides, alkali metal halides, alkali metals, surfactants, and the like. Specifically, examples thereof include cyano-containing poly(p-phenylene vinylene), boron-containing polymers, bathocuproin, bathophenanthroline, hydroxyquinoline aluminum, oxadiazole compounds, benzimidazole compounds, naphthalenetetracarboxylic acid compounds, perylene derivatives, phosphine oxide compounds, phosphine sulfide compounds, fluorine-containing phthalocyanines, titanium oxide, zinc oxide, indium oxide, tin oxide, gallium oxide, tin sulfide, indium sulfide, zinc sulfide, and the like.

[0051] The electron transport layer may be composed of only a thin film electron transport layer, but preferably includes a porous electron transport layer. In particular, when the photoelectric conversion layer is a composite film formed by compounding an organic semiconductor or inorganic semiconductor portion with an organic-inorganic perovskite compound portion, a more complex composite film (a more complex interlaced structure) can be obtained, and the photoelectric conversion efficiency becomes higher. Therefore, it is preferred to form a composite film on a porous electron transport layer.

[0052] The preferred lower limit of the thickness of the electron transport layer is 1nm, and the preferred upper limit is 2000nm. If the thickness is 1nm or more, holes can be fully blocked. If the thickness is 2000nm or less, it is not easy to become a resistance during electron transport, and the photoelectric conversion efficiency becomes high. The more preferred lower limit of the thickness of the electron transport layer is 3nm, the more preferred upper limit is 1000nm, the further preferred lower limit is 5nm, and the further preferred upper limit is 500nm.

[0053] The anode contains at least one selected from the group consisting of aluminum, copper, antimony and molybdenum.

[0054] For aluminum, copper, antimony and molybdenum, organic-inorganic perovskite compounds have sufficient reflective performance for light of 600nm to 800nm ​​for power generation, and have the property of being difficult to diffuse compared to gold used as an anode for reflecting light in the past. Therefore, by including at least any one of aluminum, copper, antimony or molybdenum in the anode, it is possible to reflect light that passes through the photoelectric conversion layer while suppressing the diffusion of the anode. In addition, by using an anode containing any one of aluminum, copper, antimony or molybdenum, the above-mentioned photoelectric conversion layer and the anti-diffusion layer described later, the amount of light absorbed by the anti-diffusion layer can be reduced, and the photoelectric conversion efficiency can be further improved.

[0055] The thickness of the above-mentioned anode is not particularly limited, and the preferred lower limit is 10nm, and the preferred upper limit is 1000nm. If the above-mentioned thickness is more than 10nm, it is possible to suppress the resistance on the basis of making the above-mentioned anode function as an electrode. If the above-mentioned thickness is below 1000nm, it is possible to further improve the transmittance of light. The more preferred lower limit of the thickness of the above-mentioned anode is 50nm, and the more preferred upper limit is 500nm.

[0056] The above-mentioned diffusion prevention layer has the following functions: preventing the material of the above-mentioned anode from diffusing into the photoelectric conversion layer containing the above-mentioned organic-inorganic perovskite compound, and maintaining a high photoelectric conversion efficiency even if a voltage is applied to the solar cell for a long time. In addition, by using the diffusion prevention layer described later as the above-mentioned diffusion prevention layer, the light transmitted through the photoelectric conversion layer is not easily absorbed by the diffusion prevention layer, and more light can be sent to the photoelectric conversion layer again. It should be noted that the degree of absorption of light in the above-mentioned diffusion prevention layer is greatly affected by the materials of the photoelectric conversion layer and the anode adjacent to the diffusion prevention layer. Therefore, in order to effectively suppress the absorption of light in the above-mentioned diffusion prevention layer, it is necessary to also consider the materials of the anode and the photoelectric conversion layer to select the material of the diffusion prevention layer.

[0057] The above-mentioned diffusion prevention layer preferably has a transmittance of 50% or more for light with a wavelength of 600 to 800 nm. By setting the transmittance of the above-mentioned light to the above-mentioned range, the absorption of light in the diffusion prevention layer can be reduced, that is, the amount of light reflected by the anode and passing through the photoelectric conversion layer again can be increased, thereby further improving the photoelectric conversion efficiency of the obtained solar cell. As mentioned above, the amount of light absorbed by the above-mentioned diffusion prevention layer is greatly affected by the materials of the adjacent anode and the photoelectric conversion layer, especially the refractive index of the material, so the transmittance of light cannot be measured using the diffusion prevention layer alone. Therefore, the transmittance of the above-mentioned light can be obtained by simulation using the Fresnel formula.

[0058] The diffusion prevention layer preferably contains a metal or a metal compound having a binding energy of 300 kJ / mol or more.

[0059] By using a metal or metal compound having the above-mentioned binding energy as the material of the diffusion prevention layer, the diffusion of the metal constituting the anode can be suppressed, and the photoelectric conversion efficiency of the obtained solar cell can be further improved. The above-mentioned binding energy is more preferably 350 kJ / mol or more. It should be noted that the above-mentioned binding energy can be obtained by the difference in formation enthalpy between the binding state and the monomer.

[0060] The above-mentioned diffusion prevention layer is preferably a dense film. More specifically, for example, it is preferably a dense film of such a density that no contact between the upper and lower layers sandwiching the above-mentioned diffusion prevention layer can be observed in a transmission electron microscope photograph of any 10 points of the cut surface when the solar cell is cut using FIB (focused ion beam). In other words, the above-mentioned diffusion prevention layer is preferably dense to such an extent that the upper and lower layers sandwiching the above-mentioned diffusion prevention layer are cut by the above-mentioned diffusion prevention layer. By making the above-mentioned diffusion prevention layer a dense film, the reduction in the photoelectric conversion efficiency of the solar cell can be further suppressed, and the reduction in the photoelectric conversion efficiency when a voltage is applied to the solar cell for a long time can be further suppressed.

[0061] As the transmission electron microscope, for example, JEM-2010-FEF (manufactured by JEOL Ltd.) or the like can be used.

[0062] The above-mentioned diffusion prevention layer contains molybdenum, tungsten, tantalum, niobium, zirconium, hafnium or their alloys, with a thickness of 5 to 30 nm, or contains oxides containing titanium, gallium, zinc, tin, indium, antimony, molybdenum, tungsten, vanadium, chromium, nickel or lead, or contains nitrides containing titanium, vanadium, chromium, niobium, tantalum, molybdenum, zirconium or hafnium, with a thickness of 5 to 50 nm, or contains graphite, with a thickness of 2 nm to 50 nm.

[0063] By forming the diffusion prevention layer from the above-mentioned metal, metal compound or graphite and setting the thickness in the above-mentioned range, the diffusion of the metal constituting the anode to the photoelectric conversion layer can be suppressed. In addition, by using the above-mentioned anode and the above-mentioned photoelectric conversion layer in combination, the absorption of light transmitted through the photoelectric conversion layer can be suppressed so that more light reaches the anode, and more light reflected from the anode can reach the photoelectric conversion layer. As a result, the amount of power generated in the photoelectric conversion layer increases, so the photoelectric conversion efficiency can be improved. Hereinafter, a diffusion prevention layer containing molybdenum, tungsten, tantalum, niobium, zirconium, hafnium or their alloys and having a thickness of 5 to 30 nm is referred to as a diffusion prevention layer 1. In addition, a diffusion prevention layer containing an oxide of titanium, gallium, zinc, tin, indium, antimony, molybdenum, tungsten, vanadium, chromium, nickel or lead is referred to as a diffusion prevention layer 2. In addition, a diffusion prevention layer containing a nitride of titanium, vanadium, chromium, niobium, tantalum, molybdenum, zirconium or hafnium and having a thickness of 5 to 50 nm is referred to as a diffusion prevention layer 3. In addition, a diffusion prevention layer containing graphite and having a thickness of 2 nm to 50 nm is referred to as a diffusion prevention layer 4.

[0064] The material of the diffusion prevention layer 1 is not particularly limited as long as it is composed of the metal or alloy, but molybdenum and tungsten are preferred because the absorption of light in the diffusion prevention layer is further suppressed. In addition, when the anode is molybdenum, the material of the diffusion prevention layer 1 is preferably tungsten, tantalum, niobium, zirconium, hafnium or an alloy thereof. From the viewpoint of more reliably suppressing the diffusion of the metal constituting the anode and further suppressing the absorption of light in the diffusion prevention layer, the thickness of the diffusion prevention layer 1 is preferably 10 nm or more, more preferably 15 nm or more, preferably 25 nm or less, and more preferably 20 nm or less.

[0065] The material of the diffusion prevention layer 2 is not particularly limited as long as it is an oxide containing the metal, and examples thereof include niobium-doped titanium oxide, tin-doped indium oxide (ITO), gallium-doped zinc oxide (GZO), nickel oxide, molybdenum oxide, tungsten oxide, antimony-doped tin oxide (ATO), vanadium oxide, chromium oxide, lead oxide, etc. Among them, from the perspective of further suppressing the absorption of light in the diffusion prevention layer, tin-doped indium oxide (ITO), gallium-doped zinc oxide (GZO), nickel oxide, molybdenum oxide, tungsten oxide, and antimony-doped tin oxide (ATO) are preferred. In addition, in order to further suppress the absorption of light in the diffusion prevention layer, the material of the diffusion prevention layer 2 is preferably colorless. In addition, in the case of using a colored oxide containing the metal, in order to further suppress the absorption of light in the diffusion prevention layer, it is preferred to reduce the thickness of the diffusion prevention layer 2 as much as possible. In addition, even if the oxide containing the metal is transparent, it will absorb light in small amounts, so the thickness of the diffusion prevention layer 2 is preferably as thin as possible within the range of suppressing the diffusion of the anode. From the above viewpoints, the thickness of the diffusion prevention layer 2 is preferably 10 nm or more, more preferably 20 nm or more, and is preferably 50 nm or less, more preferably 40 nm or less.

[0066] The material of the diffusion prevention layer 3 is not particularly limited as long as it is a nitride containing the metal, and examples thereof include titanium nitride, chromium nitride, vanadium nitride, molybdenum nitride, niobium nitride, tantalum nitride, zirconium nitride, hafnium nitride, etc. Among them, titanium nitride, chromium nitride, and vanadium nitride are preferred from the perspective of further suppressing the absorption of light in the diffusion prevention layer. In addition, the material of the diffusion prevention layer 3 is mostly a light-colored but colored material, so in order to further suppress the absorption of light in the diffusion prevention layer, it is preferred to reduce the thickness of the diffusion prevention layer 3 as much as possible. From the above viewpoint, the thickness of the diffusion prevention layer 3 is preferably 10 nm or more, more preferably 15 nm or more, preferably 40 nm or less, and more preferably 30 nm or less.

[0067] The material of the above-mentioned diffusion prevention layer 4 is a film with graphite as the main component. As long as the main component of the above-mentioned graphite is sp2 bond, even if a small amount of sp3 bond, hydrogen atom is mixed, it also functions as a diffusion prevention layer. In addition, the above-mentioned graphite needs to be dense and functions as a diffusion prevention layer, so even if the nano carbon materials such as carbon nanotubes, fullerenes, graphene as the same carbon-based materials are used, it is also impossible to function fully as a diffusion prevention layer. In addition, the material of the above-mentioned diffusion prevention layer 4 is mostly a light-toned but colored material, so in order to further suppress the absorption of the light in the diffusion prevention layer, it is preferred to thin the thickness of the diffusion prevention layer 4 as much as possible. From the above-mentioned viewpoint, the thickness of the above-mentioned diffusion prevention layer 4 is preferably more than 2nm, more preferably more than 5nm, preferably below 50nm, more preferably below 30nm.

[0068] The diffusion prevention layer may contain other additives and the like as long as the effects of the present invention are not impaired.

[0069] The method for forming the diffusion prevention layer is not particularly limited, and preferably, dry film forming methods such as vapor deposition, sputtering, and CVD, and wet coating such as spray coating and spin coating are used. By using these methods, the diffusion prevention layer can be made into a dense film.

[0070] The solar cell of the present invention may include a hole transport layer between the photoelectric conversion layer and the diffusion prevention layer.

[0071] The material of the hole transport layer is not particularly limited, and the hole transport layer may include an organic material. As the material of the hole transport layer, for example, P-type conductive polymers, P-type low molecular weight organic semiconductors, P-type metal oxides, P-type metal sulfides, surfactants, etc. can be cited. Specifically, for example, compounds with thiophene skeletons such as poly (3-alkylthiophene) can be cited. In addition, for example, conductive polymers with triphenylamine skeletons, polyphenylene vinylene skeletons, polyvinyl carbazole skeletons, polyaniline skeletons, polyacetylene skeletons, etc. can also be cited. In addition, for example, compounds with porphyrin skeletons such as phthalocyanine skeletons, naphthalocyanine skeletons, pentacene skeletons, benzoporphyrin skeletons, spirobifluorene skeletons, etc., molybdenum sulfide, tungsten sulfide, copper sulfide, tin sulfide, etc., fluorine-containing phosphonic acids, carbonyl-containing phosphonic acids, CuSCN, CuI, etc. can be cited.

[0072] The hole transport layer may be partially immersed in the photoelectric conversion layer, or may be configured as a thin film on the photoelectric conversion layer. The preferred lower limit of the thickness of the hole transport layer when it exists in a thin film is 1nm, and the preferred upper limit is 2000nm. If the thickness is 1nm or more, it is possible to fully block electrons. If the thickness is less than 2000nm, it is not easy to become a resistance during hole transport, and the photoelectric conversion efficiency becomes high. The more preferred lower limit of the thickness is 3nm, the more preferred upper limit is 1000nm, the further preferred lower limit is 5nm, and the further preferred upper limit is 500nm.

[0073] The solar cell of the present invention may further include a substrate, etc. The substrate is not particularly limited, and examples thereof include transparent glass substrates such as soda-lime glass and alkali-free glass, ceramic substrates, and transparent plastic substrates.

[0074] The method for manufacturing the solar cell of the present invention is not particularly limited, and examples thereof include a method of sequentially forming the cathode, the electron transport layer, the photoelectric conversion layer, the hole transport layer, the diffusion prevention layer, and the anode on the substrate.

[0075] Effects of the Invention

[0076] According to the present invention, it is possible to provide a solar cell having high photoelectric conversion efficiency and in which the photoelectric conversion efficiency is unlikely to decrease even when a voltage is applied for a long period of time. BRIEF DESCRIPTION OF THE DRAWINGS

[0077] Figure 1 This is a schematic diagram showing an example of the crystal structure of an organic-inorganic perovskite compound. DETAILED DESCRIPTION

[0078] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0079] (Example 1)

[0080] An ITO film with a thickness of 300 nm was formed on a glass substrate as a cathode, and ultrasonic cleaning was performed using pure water, acetone, and methanol for 10 minutes each in sequence, and then dried.

[0081] On the surface of the ITO film, a thin film electron transport layer containing titanium oxide with a thickness of 20 nm was formed by sputtering. In addition, a titanium oxide paste containing titanium oxide (a mixture of average particle sizes of 10 nm and 30 nm) was applied on the thin film electron transport layer by spin coating to form a porous electron transport layer with a thickness of 100 nm.

[0082] Next, 550 mg of lead iodide as a metal halide was added to a mixed solvent of 1 ml of N,N-dimethylformamide (DMF) and 80 μl of dimethyl sulfoxide and dissolved to prepare a solution. The first film was formed by spin coating on the porous electron transport layer. In addition, methylammonium iodide as an amine compound was dissolved in 2-propanol to prepare a 6 wt % solution. The solution was formed on the first film by spin coating, and then heated at 150°C for 5 minutes, thereby forming a photoelectric conversion layer with a thickness of 400 nm containing CH3NH3Pb3 as a perovskite compound.

[0083] Next, a 2 wt % chlorobenzene solution of Spiro-OMETAD (manufactured by Merck) was spin-coated on the photoelectric conversion layer to form a hole transport layer having a thickness of 100 nm.

[0084] Next, a diffusion prevention layer containing molybdenum was formed on the hole transport layer to a thickness of 10 nm by electron beam evaporation.

[0085] On the obtained diffusion prevention layer, a 100 nm thick aluminum film was formed as an anode by sputtering to obtain a solar cell having cathode / electron transport layer / photoelectric conversion layer / hole transport layer / diffusion prevention layer / anode stacked in this order.

[0086] The obtained solar cell was cut by FIB (focused ion beam), and the cut surface was observed by transmission electron microscope (JEM-2010-FEF, manufactured by JEOL Ltd.). In the transmission electron microscope photographs at any 10 points, no contact between the upper and lower layers sandwiching the diffusion prevention layer was observed, and it was confirmed that the diffusion prevention layer was a dense film.

[0087] (Examples 2 to 48, Comparative Examples 6 to 22)

[0088] A solar cell having cathode / electron transport layer / photoelectric conversion layer / hole transport layer / diffusion prevention layer / anode stacked in this order was obtained in the same manner as in Example 1 except that the type and thickness of the diffusion prevention layer and the anode were changed as shown in Tables 1 to 3.

[0089] (Comparative Examples 1 to 5)

[0090] A solar cell having cathode / electron transport layer / photoelectric conversion layer / hole transport layer / anode stacked in this order was obtained in the same manner as in Example 1 except that the antidiffusion layer was not formed and the anode shown in Table 3 was formed on the hole transport layer by electron beam evaporation.

[0091] (Comparative Example 23)

[0092] An ITO film with a thickness of 300 nm was formed on a glass substrate as a cathode, and pure water, acetone, and methanol were used in sequence for ultrasonic cleaning for 10 minutes each, and then dried. Next, a thin film electron transport layer containing titanium oxide with a thickness of 20 nm was formed on the surface of the ITO film by sputtering. Next, a solution obtained by dissolving PTB7 (manufactured by Aldrich) and PCBM (manufactured by Aldrich) in chlorobenzene at a ratio of 1: 1 was formed on the electron transport layer by spin coating, thereby forming a photoelectric conversion layer containing an organic semiconductor with a thickness of 100 nm. Then, PEDOT:PSS (manufactured by Aldrich) was filmed on the photoelectric conversion layer by spin coating, thereby forming a hole transport layer with a thickness of 50 nm. Then, the diffusion prevention layer and the electrode described in Table 3 were formed into films by the same method as in Example 1, thereby obtaining a solar cell stacked with a cathode / electron transport layer / photoelectric conversion layer / hole transport layer / diffusion prevention layer / anode.

[0093] (Comparative Examples 24 and 25)

[0094] A solar cell having cathode / electron transport layer / photoelectric conversion layer / hole transport layer / anode stacked in this order was obtained in the same manner as in Comparative Example 23 except that the diffusion prevention layer was not formed and the anode shown in Table 3 was formed by electron beam deposition.

[0095] <Evaluation>

[0096] The solar cells obtained in Examples and Comparative Examples were evaluated as follows.

[0097] (1) Evaluation of photoelectric conversion efficiency

[0098] Immediately after the solar cell was manufactured, a power source (KEITHLEY, Model 236) was connected between the electrodes of the solar cell at an intensity of 100 mW / cm 2 The photoelectric conversion efficiency was measured using a sunlight simulation lamp (manufactured by Yamashita Denso Co., Ltd.), and the obtained photoelectric conversion efficiency was defined as the initial conversion efficiency. The initial conversion efficiency of the solar cell obtained in Comparative Example 11 was used as a reference for standardization.

[0099] 6: The standardized initial conversion efficiency is 1.8 or above

[0100] 5: The value of the normalized initial conversion efficiency is greater than 1.5 and less than 1.8

[0101] 4: The value of the normalized initial conversion efficiency is greater than 1.3 and less than 1.5

[0102] 3: The value of the normalized initial conversion efficiency is greater than 1.2 and less than 1.3

[0103] 2: The value of the normalized initial conversion efficiency is greater than 1.0 and less than 1.2

[0104] 1: The normalized initial conversion efficiency value is less than 1.0

[0105] (2) Evaluation of durability (light resistance) when voltage is applied for a long time

[0106] A power source (KEITHLEY, Model 236) was connected between the electrodes of the solar cell at an intensity of 100 mW / cm 2 A solar energy simulator (manufactured by Yamashita Denso Co., Ltd.) was used, voltage was applied at 25°C, and the photoelectric conversion efficiency after 24 hours was measured.

[0107] 5: After 24 hours, the photoelectric conversion efficiency remains above 95% relative to the initial conversion efficiency

[0108] 4: After 24 hours, the photoelectric conversion efficiency remains above 90% and less than 95% of the initial conversion efficiency

[0109] 3: After 24 hours, the photoelectric conversion efficiency remains at least 80% and less than 90% of the initial conversion efficiency

[0110] 2: After 24 hours, the photoelectric conversion efficiency remains at least 60% and less than 80% of the initial conversion efficiency

[0111] 1: After 24 hours, the photoelectric conversion efficiency decreases to less than 60% of the initial conversion efficiency

[0112] [Table 1]

[0113]

[0114] [Table 2]

[0115]

[0116] [Table 3]

[0117]

[0118] Industrial Applicability

[0119] According to the present invention, it is possible to provide a solar cell having high photoelectric conversion efficiency and whose photoelectric conversion efficiency is unlikely to decrease even when a voltage is applied for a long period of time.

Claims

1. A solar cell comprising, in sequence, a cathode, a photoelectric conversion layer, an anti-diffusion layer and an anode, The cathode is a transparent electrode, The anode contains at least one selected from the group consisting of aluminum, copper, antimony and molybdenum, The photoelectric conversion layer contains an organic-inorganic perovskite compound represented by the general formula AMX, wherein A is an organic alkali compound and / or an alkali metal, M is a lead or tin atom, and X is a halogen atom. The diffusion prevention layer comprises molybdenum, tungsten, tantalum, niobium, zirconium, hafnium or alloys thereof, and has a thickness of 5 nm to 30 nm. Alternatively, the diffusion prevention layer comprises an oxide containing titanium, gallium, zinc, tin, indium, antimony, molybdenum, tungsten, vanadium, chromium, nickel or lead, Alternatively, the diffusion prevention layer comprises a nitride containing titanium, vanadium, niobium, tantalum, zirconium or hafnium, and has a thickness of 5 nm to 50 nm. Alternatively, the diffusion prevention layer comprises graphite and has a thickness of 2 nm to 50 nm. When the diffusion prevention layer comprises an oxide containing titanium, gallium, zinc, tin, indium, antimony, molybdenum, tungsten, vanadium, chromium, nickel or lead, the anode contains antimony or molybdenum.