Catalysts based on bimetallic nanoparticles, their use in selective hydrogenation and methods for making the catalysts

By using bimetal nanoparticle catalysts, the problems of low selectivity and short service life of existing catalysts are solved, and the selective hydrogenation effect with high selectivity and stability are achieved, especially in the effective removal of acetylene in the ethylene process stream. Extend the service life of the catalyst.

CN113365729BActive Publication Date: 2024-11-12SHELL INTERNATIONALE RESEARCH MAATSCHAPPIJ BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080011845.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-01-17
Filing Date
2020-01-15
Publication Date
2024-11-12
Estimated Expiration
2040-01-15

AI Technical Summary

Technical Problem

When existing selective hydrogenation catalysts treat high-concentration unsaturated hydrocarbon product streams, they are not selective and have a short service life, making it difficult to effectively remove contaminants such as acetylene and methylacetylene, resulting in excessive generation of side reaction products.

Method used

Using bimetallic nanoparticles (composition of silver and palladium) catalyst, an aqueous dispersion is formed by reducing mixture of surfactant, incorporated into the support and calcined at low temperature to form a catalyst with high selectivity and stability. The bimetallic nanoparticles are dispersed in inorganic The oxide carrier surface provides a high surface area volume ratio and core-shell structure.

Benefits of technology

The selectivity and stability of the catalyst are significantly improved, the cycle length is extended, and the generation of side reaction products is reduced, especially the selective hydrogenation effect of acetylene in the ethylene process stream is significant, providing a longer service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113365729B_ABST
    Figure CN113365729B_ABST
Patent Text Reader

Abstract

A selective hydrogenation catalyst and a method for making the catalyst are provided. The catalyst includes a support containing bimetallic nanoparticles. The nanoparticles contain a silver component and a palladium component. The catalyst is made by incorporating an aqueous dispersion of the bimetallic nanoparticles onto a catalyst support, followed by drying and calcining the support with the dispersion incorporated therein. The catalyst is used to selectively hydrogenate an olefin product stream containing highly unsaturated hydrocarbons.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Patent Application No. 62 / 793,561, filed on January 17, 2019, entitled BIMETALLIC NANOPARTICLE-BASED CATALYST, ITS USE IN SELECTIVE HYDROGENATION, AND A METHOD OF MAKING THE CATALYST, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to a catalyst composition comprising bimetallic nanoparticles contained on a support, and a method for preparing the catalyst composition. The catalyst composition can be used to selectively hydrogenate highly unsaturated hydrocarbons in a process stream containing lower unsaturated hydrocarbons. Background Art

[0004] Steam crackers and refinery cracking units provide production of unsaturated hydrocarbon product streams that are used as feedstocks for downstream processes and other applications. Steam crackers typically crack lower molecular weight saturated hydrocarbons, such as ethane, propane and butane, or naphtha boiling range hydrocarbons, to produce lighter olefins, such as ethylene, propylene and butenes. Refinery cracking units typically crack heavier hydrocarbon fractions to produce multiple product streams, among which are lighter gaseous hydrocarbons with a high concentration of unsaturated hydrocarbons.

[0005] One problem with the light olefin product streams produced from these cracking units is that these olefin product streams may contain unacceptable concentrations of higher unsaturated hydrocarbons. For example, an ethylene product stream may have contaminating concentrations of acetylene, or a propylene product stream may have contaminating concentrations of methylacetylene (MA) and propadiene (PD). The acetylene contained in the ethylene product stream and the methylacetylene and propadiene contained in the propylene product stream need to be removed from these products to make them usable.

[0006] Therefore, highly unsaturated hydrocarbons, such as dienes and hydrocarbons with triple bonds (alkynes), need to be removed from lower unsaturation product streams, such as ethylene product streams or propylene product streams. Selective hydrogenation processes are often used to remove unwanted highly unsaturated hydrocarbons from lower unsaturation hydrocarbon streams.

[0007] The selective hydrogenation process is a catalytic process. The process includes contacting an olefin stream of a hydrocarbon with a certain concentration of higher unsaturation with a selective hydrogenation catalyst under suitable reaction conditions. These higher unsaturation hydrocarbons are selectively hydrogenated to olefins, wherein only a minimum amount of hydrogenation occurs to the desired olefins in the olefin stream. The desired properties of the selective hydrogenation catalyst are that it has a high activity for providing the selective hydrogenation and exhibits a long service life.

[0008] PCT publication WO 2013 / 186789 describes one of these selective hydrogenation catalysts. The catalyst comprises an inorganic oxide support, and so-called fine alloy particles having an active metal component and a promoter component. The active metal is selected from palladium, platinum and nickel, and the promoter is selected from silver, gold and copper. The fine alloy particles are dispersed onto the surface of the inorganic oxide support by a simultaneous dispersion process that employs equilibrium absorption impregnation of the inorganic oxide support by contacting the inorganic oxide support with a solution containing the fine alloy particles.

[0009] Fine alloy particles are prepared by dissolving an active metal precursor (e.g., palladium salt) and a promoter metal precursor (e.g., silver salt) in an acidic aqueous solution. These precursors are dissolved in water, and the pH is controlled in the range of from 1.2 to 1.4. The acidic aqueous solution is heated and maintained at a temperature of about 70°C for a period of time.

[0010] No surfactant is used in the preparation of the acidic aqueous solution. There is no indication or suggestion that the fine alloy particles are bimetallic core-shell nanoparticles, especially because no surfactant is used in the preparation of the acidic aqueous solution. The disclosure also does not provide any information about the form or other properties of the fine alloy particles. The specification does not mention other components of the acidic aqueous solution other than water, metal precursors and hydrochloric acid. Therefore, no typical known reducing agent is used in the preparation of the acidic aqueous solution.

[0011] The catalyst of WO 2013 / 186789 is prepared by impregnating an inorganic oxide support with an acidic aqueous solution of fine alloy particles, then drying and calcining the impregnated support to provide the final catalyst. The desired property of the catalyst is that the palladium is dispersed over at least 30% of the surface area of ​​the inorganic oxide support, such as by H 2 Measured by chemical adsorption method.

[0012] US 6,572,673 is a relevant publication because it discloses a method for preparing noble metal nanoparticles. The '673 publication mentions that its noble metal nanoparticles can be used for electroless plating of electronic circuits and as catalysts to catalyze the reaction of unsaturated hydrocarbons. These nanoparticles are prepared by reacting a noble metal salt and an anionic surfactant without adding a reducing agent and at a temperature ranging from 50°C to 140°C.

[0013] However, the '673 patent does not mention bi-metallic nanoparticles, and in particular, it does not teach anything about bi-metallic nanoparticles having a core-shell structure. Nor does it teach a catalyst composition prepared by impregnating an inorganic oxide support with a dispersion of precious metal nanoparticles or a dispersion of any type of supported catalyst composition. Summary of the invention

[0014] It is an object of the present invention to provide improved selective hydrogenation catalysts.

[0015] Therefore, a composition useful as a selective hydrogenation catalyst or a selective hydrogenation catalyst precursor is provided. The composition comprises a support comprising bimetallic nanoparticles. The bimetallic nanoparticles of the composition comprise a silver component and a palladium component.

[0016] The selective hydrogenation catalyst of the present invention is prepared by providing an aqueous dispersion of bimetallic nanoparticles formed by reducing a palladium salt and a silver salt in a mixture using a surfactant, incorporating the aqueous dispersion into a support to provide an impregnated support, drying it, and then calcining it at a low calcination temperature to provide a catalyst composition. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The following drawings are provided to aid in describing and explaining the present invention.

[0018] Figure 1 Plots of catalyst selectivity versus time on stream (TOS) are presented for inventive and comparative catalysts.

[0019] Figure 2 is a transmission electron microscopy (TEM) image of the catalyst of the present invention, showing palladium / silver nanoparticles on an alumina support.

[0020] Figure 3 is a transmission electron microscopy (TEM) image of isolated and dried palladium / silver nanoparticles of the present invention prepared in the micellar solution of the present invention.

[0021] Figure 4 A graph showing the size distribution of palladium / silver nanoparticles of the present invention in aqueous dispersion is presented. DETAILED DESCRIPTION

[0022] Provided herein are novel catalyst compositions that are useful for the selective catalytic hydrogenation of highly unsaturated hydrocarbons contained at contaminant levels in olefin process streams comprising olefins.

[0023] The application of the catalyst composition of the present invention includes contacting an olefin process stream with a catalyst under suitable reaction conditions, and the olefin process stream may have a certain concentration of highly unsaturated hydrocarbons. The catalyst selectively hydrogenates highly unsaturated hydrocarbons to hydrocarbons (i.e., olefins) of lower unsaturation, but only a minimum amount of undesired hydrogenation of the olefins in the olefin process stream occurs. In fact, when the selective hydrogenation catalyst of the present invention is mentioned in this specification, it is meant that the catalyst provides hydrogenation of highly unsaturated hydrocarbons (such as alkynes and dienes) contained in the olefin stream, without hydrogenating a large amount of olefins in the olefin stream to saturated hydrocarbons.

[0024] The catalyst of the present invention has high selectivity, especially when used for the selective hydrogenation of acetylene contained in ethylene process streams. The catalyst is also very stable, because its selectivity and activity decrease at a much lower rate with time on stream (TOS) than other comparative catalysts. This means that the cycle length of the catalyst in use is much longer than that of other comparative catalysts. In fact, the catalyst of the present invention can provide a cycle length that is twice that of other catalysts.

[0025] When the catalyst of the present invention is used in a selective hydrogenation process, the unexpectedly high selectivity characteristics of the catalyst provide a much lower yield of an undesirable green oil byproduct. "Green oil" refers to a mixture of compounds produced by side reactions during the selective hydrogenation of alkynes and diolefins contained in an olefin process stream. These side reactions form dimers, trimers and other oligomers of alkynes and diolefins. Each molecule of the green oil oligomer compound can have up to 16 or more carbon atoms.

[0026] The composition of the present invention is a selective hydrogenation catalyst or selective hydrogenation catalyst precursor that can provide many of the benefits discussed in this specification. The composition comprises a support containing bimetallic nanoparticles. These bimetallic nanoparticles comprise a silver component and a palladium component.

[0027] It is believed that the morphology and other characteristics of the bi-metallic nanoparticles used to prepare the catalyst compositions of the present invention contribute significantly to the special properties of the catalyst compositions. One such characteristic of the bi-metallic nanoparticles is the high surface area to volume ratio of the particles. Smaller nanoparticles have higher surface area to volume ratios than larger particles. These higher surface area to volume ratios contribute to the improved catalytic properties of the selective hydrogenation catalysts of the present invention. Therefore, it is desirable that the bi-metallic nanoparticles of the catalysts of the present invention have the highest surface area to volume ratios practicable.

[0028] The nanoparticles are dispersed on the surface of the catalyst support and typically have a size distribution such that at least 80%, but more preferably at least 90%, of the bimetallic nanoparticles have a size in the range of from 1 nanometer (nm) to 10 nm. The size distribution of the bimetallic nanoparticles may also approximate a Gaussian distribution with an average particle size in the range of from 1 nm to 10 nm and a standard deviation (σ) in the range of from 0.1 to 2.5. The bimetallic nanoparticles may be characterized using transmission electron microscopy (TEM) or dynamic light scattering methods.

[0029] In addition to the size of the bi-metallic nanoparticles, there are other properties of these nanoparticles that, in combination with the particle size, contribute to the unexpected properties of the catalyst compositions of the present invention. Among these is the relative amounts of silver metal and palladium metal contained in these nanoparticles. This ratio can be an important contributing factor to the selectivity of the catalyst. In all cases, the palladium to silver molar ratio of these bi-metallic nanoparticles should be in the range of from 0.01:1 to 100:1. However, it is preferred that the silver and palladium are present in these bi-metallic nanoparticles at a palladium to silver molar ratio within a much narrower range. In particular, the palladium to silver molar ratio in these bi-metallic nanoparticles is in the range of from 0.01 to 10:1. However, preferably, the palladium to silver ratio is in the range of from 0.1:1 to 5:1. More preferably, the palladium to silver ratio is in the range of from 0.1:1 to 3:1, and most preferably, the palladium to silver ratio is from 0.2:1 to 2:1.

[0030] These bi-metallic nanoparticles can take several forms, including particles that are alloys of silver and palladium and particles that have a core-shell structure, where one metal component forms the core of the particle and the other metal component forms a shell surrounding the core.

[0031] With respect to the core-shell structure form of bi-metallic nanoparticles, the approach of the reacting molecules to the different metal components of these nanoparticles may be affected by their core-shell structure. For example, if the palladium metal component of the particle forms the shell and the silver metal component of the particle forms the core, the reacting molecules may have an easier or more favorable approach to the palladium metal of the shell than to the silver metal of the core. The reaction may be affected by the relative differences in the approach of the reacting molecules to the different metals of the bi-metallic nanoparticles.

[0032] The core-shell structure of these bimetallic nanoparticles includes an inner core and an outer shell surrounding the core, wherein the inner core has a first major portion that is a first metal component and the outer shell has a second major portion that is a second metal component. Although the geometric shapes of these bimetallic nanoparticles and their inner cores are not perfectly spherical, they are approximately spherical in shape.

[0033] Therefore, these core-shell bimetallic nanoparticles are characterized herein as two concentric spheres, including an outer diameter (D o ) surrounds a core with a diameter (D i ) of the overall spherical nanoparticle with an internal spherical core, where D o Greater than D i , and the area between the two spheres defines an outer shell surrounding the inner spherical core. The outer shell has a shell thickness (θ). The shell thickness θ is approximately the outer diameter D of the spherical particle. o The diameter D of the inner core i The difference between them is divided by 2, that is, θ = [(D o -D i ) / 2]. The ratio of the shell thickness to the outer diameter of the bimetallic nanoparticles having a core-shell structure (i.e., θ / D o ) is in the range of from 0.01 to 0.8 (1% to 80%). However, preferably, the ratio is in the range of from 0.03 to 0.6 (3% to 60%), and more preferably, the ratio is in the range of from 0.05 to 0.4 (5% to 40%).

[0034] The first metal component of the core of these bi-metallic nanoparticles can be silver or palladium, and the second metal component of the outer shell of these bi-metallic nanoparticles can be palladium or silver. If the first metal component of the inner core is silver, then palladium is the second metal component of the outer shell. Alternatively, if the first metal component of the inner core is palladium, then silver is the second metal component of the outer shell.

[0035] The bimetallic nanoparticles of the catalyst of the present invention are prepared by the method described in this specification. The method provides an aqueous dispersion of nanoparticles for preparing the catalyst. The catalyst preparation includes incorporating the aqueous dispersion of the bimetallic nanoparticles into a shaped inorganic oxide support, thereby dispersing the bimetallic nanoparticles on the surface of the shaped inorganic oxide support, and then drying and calcining to provide a catalyst.

[0036] Incorporating the aqueous dispersion of bimetallic nanoparticles onto the shaped inorganic oxide support results in the bimetallic nanoparticles being dispersed on the surface of the shaped inorganic oxide support. 2 The resulting metal surface area measured by chemisorption is less than 25% of the BET surface area of ​​the shaped inorganic oxide support. More typically, it is in the range of from 0.01% to 22%, and most typically, in the range of from 0.02% to 20%.

[0037] H for measuring the dispersion of nanoparticles on the surface of shaped inorganic oxide supports 2 The chemical adsorption method was performed according to ASTM D3908.

[0038] The carrier component of the catalyst of the present invention is prepared by any suitable method known to those skilled in the art for preparing a shaped porous catalyst carrier for carrying catalytically active metals. The carrier or shaped inorganic oxide carrier comprises a porous refractory oxide or inorganic oxide component, such as aluminum oxide, silicon dioxide, aluminum oxide-silicon dioxide, titanium dioxide, zirconium oxide, boron oxide, magnesium oxide, zeolite, and a combination thereof. The preferred inorganic oxide for the shaped inorganic oxide carrier of the catalyst is one selected from the group consisting of the following items: aluminum oxide, silicon dioxide, aluminum oxide-silicon dioxide and titanium dioxide. Among them, the most preferred inorganic oxide is aluminum oxide.

[0039] The inorganic oxide of the support is formed into a shaped structure by any known suitable method. The extruded shaped structure is usually prepared by mixing the inorganic oxide powder with water and one or more additives to form a mixture having plastic properties, and then forming the mixture into an extrudate by any known extrusion method. The formed extrudate can be cylindrical, leaf-shaped and twisted, with a nominal extrudate diameter in the range of from 0.5 mm to 25 mm and an extrudate length in the range of from 1 mm to 50 mm.

[0040] The spherical structures or balls of the inorganic oxide support can be made by applying any known granulation method, which uses an inclined rotating disk or pan to which the inorganic oxide particles are fed while spraying the viscous slurry onto the particles. By this method, the particles are formed into spherical particles. The diameter of the spherical support particles ranges from 0.5 mm to 25 mm.

[0041] Dry tableting can also be used to prepare shaped support structures. In this method, cylindrical granules or pellets of inorganic oxides are made by pressing dried inorganic oxide powders, optionally mixed with additives such as lubricants and binders, between two punches in a tablet press. The support particles, which are cylindrical granules, have a granule diameter in the range of from 0.5 mm to 25 mm and a granule length in the range of from 1 mm to 50 mm.

[0042] The shaped support particles are then dried under standard drying conditions, which may include drying temperatures in the range from 50 to 200°C, preferably from 75 to 175°C and more preferably from 90 to 150°C.

[0043] After drying, the shaped support particles are calcined under standard calcination conditions including a calcination temperature in the range from 800°C to 1,500°C, preferably from 900°C to 1,400°C and most preferably from 1,000°C to 1,300°C.

[0044] The calcined shaped support should have a surface area and pore volume that allows for impregnation of the shaped support with the bimetallic nanoparticles. The calcined shaped support may have a surface area of ​​from 1 m 2 / g to 100m 2 / g, preferably from 5m 2 / g to 50m 2 / g and most preferably from 5m 2 / g to 35m 2 / g range (by using N 2 The BET method is determined by ASTM test method D3037).

[0045] The calcined shaped support The average pore size in units ranges from 50 to 200, preferably from 70 to 150 and most preferably from 75 to 125.

[0046] The pore volume of the calcined shaped support should exceed 0.2cc / g, and is typically in the range of from 0.3cc / g to 1.1cc / g. More typically, the pore volume is in the range of from 0.35cc / g to 0.9cc / g, and most typically, in the range of from 0.4cc / g to 0.7cc / g.

[0047] References herein to the pore size distribution and pore volume of the calcined shaped particles are directed to those properties as measured by mercury intrusion porosimetry, ASTM test method D 4284. The pore size distribution of the calcined shaped particles is measured using any suitable measuring instrument using a contact angle of 140° and a mercury surface tension of 474 dynes / cm at 25°C.

[0048] One preferred attribute of the catalyst of the present invention is that it is a so-called eggshell catalyst in which the bi-metallic nanoparticles incorporated into the shaped support structure are primarily deposited and accumulated in a thin surface layer near the periphery and surface of the shaped support structure. This feature is important because it helps to increase the selectivity of the catalyst. This enhanced selectivity results from the use of the bi-metallic nanoparticles in combination with their placement near the periphery and surface or surface layer skin of the catalyst support. This combination of features provides greater catalytic benefit than the eggshell property alone.

[0049] Certain other embodiments of the catalyst of the present invention include features that help achieve even greater benefits than the eggshell properties alone or the combination of bi-metallic nanoparticles used in an eggshell catalyst. A preferred feature of the catalyst of the present invention is that the core-shell bi-metallic nanoparticles of the present invention are used in combination with depositing the majority of these bi-metallic nanoparticles within a skin layer at the outer periphery and surface of a shaped support structure. Thus, for this embodiment, the bi-metallic nanoparticles of the catalyst are core-shell and are contained within a shaped support structure in a manner that provides an eggshell catalyst composition.

[0050] Thus, a preferred embodiment of the catalyst of the present invention is that it has an eggshell character, wherein the bimetallic nanoparticles (preferably core-shell nanoparticles) are primarily present in the outer shell region of the shaped support structure.

[0051] In characterizing the catalyst, the shaped support structure defines a particle volume through its exterior surface. The specification further characterizes the shaped support structure as having an exterior shell region and an interior region.

[0052] The outer shell region is defined as a peripheral region or outer skin having a certain depth within the particle volume. The inner boundary of the outer shell region can be defined by the endpoints of each vector extending vertically from each point on the outer surface of the shaped structure from a tangent line at each such point inwardly toward the interior of the shaped structure by the vector length (also referred to herein as the depth).

[0053] The interior region of the shaped support structure is the volume of the particle excluding the outer shell region.

[0054] The depth of the outer shell region should range from as small as 20 nm (0.02 μm), approaching the depth of a monolayer of bi-metallic nanoparticles, to a maximum of 500 μm (500,000 nm). As described above, it is desirable that the bi-metallic nanoparticles be concentrated in a thin boundary layer of the shaped support structure, and therefore the depth of the outer shell region should be relatively narrow. Therefore, it is preferred that the depth of the outer shell region range from 5,000 nm (5 μm) to 400 μm (400,000 nm), and more preferably, the depth ranges from 10,000 nm (10 μm) to 300 μm (300,000 nm).

[0055] An important embodiment of the present invention is the method of making the bi-metallic nanoparticles and incorporating them into a support for the catalyst. It is the specific method of making the bi-metallic nanoparticles that provides the particles with the necessary characteristics that contribute to the improved properties of the selective hydrogenation catalysts of the present invention. The catalysts of the present invention are prepared by incorporating an aqueous dispersion of the bi-metallic nanoparticles made by the methods described herein into a support for the catalyst.

[0056] An aqueous dispersion of bi-metallic nanoparticles is prepared by mixing a salt of palladium metal, a salt of silver metal, and a surfactant in water. The mixture is heated at low temperature, preferably while stirring the mixture, for a sufficient time to allow the bi-metallic nanoparticles to form and disperse within the aqueous phase of the aqueous dispersion.

[0057] An important feature of the preparation method is that the surfactant has a bifunctional property, which can reduce palladium ions and silver ions to metals and disperse the formed nanoparticles. Therefore, one difference between this method and many other methods for preparing metal nanoparticles described in the art is that it does not use an additional separate reducing agent. Instead, the surfactant acts as a reducing agent. Due to the dual role of the surfactant used to prepare the aqueous dispersion of palladium and silver nanoparticles, one embodiment of the present invention includes preparing a mixture comprising a silver salt, a palladium salt, a surfactant and water, but substantially without a separately added reducing agent. A separate reducing agent should not be added to the mixture during preparation.

[0058] Another difference of this preparation method over other methods is that bimetallic nanoparticles, particularly palladium and silver nanoparticles, are formed rather than monometallic nanoparticles. When preparing an aqueous mixture of a palladium salt, a silver salt, and a surfactant, the relative amounts of the metal salts mixed together are used to provide nanoparticles having the desired palladium to silver molar ratio discussed in this specification. The aqueous mixture will also have a metal concentration such that when the aqueous dispersion is incorporated into a catalyst support, the final catalyst has the metal concentration discussed in the specification.

[0059] It is believed that the surfactant used in the preparation of the aqueous dispersion of bimetallic nanoparticles provides the formation of unique core-shell nanoparticles of the present invention. In the preparation of an aqueous mixture of a metal salt and a surfactant, a spherical micelle is formed with a surfactant that acts as both a stabilizer and a reducing agent. The mixture is heated at low temperatures for a time sufficient to reduce the two metals and form bimetallic nanoparticles. During the heating of the mixture, a portion of the surfactant is hydrolyzed, thereby causing the reducing compound to release. The reduced metal accumulates in the center of the micelle and forms nanoparticles. However, the reduction rates of the two metals are different for each of them. This difference in their reduction rates helps to form the core-shell structure of nanoparticles.

[0060] The heating of the mixture is carried out at a low temperature in the range of from 30°C to 120°C. Preferably, the heating temperature is in the range of from 40°C to 110°C, and more preferably, from 50°C to 100°C. The heating temperature is important for the preparation of nanoparticles. Too high a temperature will result in excessive hydrolysis of the surfactant. If the temperature is too low, the nanoparticles will not be properly formed.

[0061] A benefit provided by the nanoparticle preparation method of the present invention is that it accelerates the reduction of metal and shortens the required heating time for realizing metal reduction and nanoparticle formation. The mixture is heated enough to provide the time for nanoparticle formation, and this time should be no more than 10 hours. However, the heating time is preferably from 0.1 hour to 8 hours, and more preferably, in the scope of from 0.2 hour to 6 hours.

[0062] The pH of the aqueous dispersion of bi-metallic nanoparticles is typically set by the components used in its preparation, and is usually less than 9. More typically, the pH is in the neutral or acidic pH range, such as acidic to 7 or about 7. Most typically, the pH is in the range from 1 to 5 or 6.

[0063] The silver salt used to prepare the aqueous dispersion of bi-metallic nanoparticles of the present invention is selected from the group of silver salts consisting of silver nitrate, silver halide, silver carbonate, silver phosphate, silver acetate, silver hydroxide, silver oxide and silver sulfate. The preferred silver salt is silver nitrate.

[0064] The palladium salt used to prepare the aqueous dispersion of bi-metallic nanoparticles of the present invention is selected from the group consisting of palladium salts: palladium nitrate, palladium halide, palladium carbonate, palladium phosphate, palladium acetate, palladium oxide and palladium sulfate. The preferred palladium salt is palladium nitrate.

[0065] The surfactant used to prepare the aqueous dispersion of the bi-metallic nanoparticles of the present invention can be any suitable cationic, anionic or non-ionic surfactant which acts as both a stabilizer and a reducing agent, as discussed above, and provides for the formation of micelles in water within which the bi-metallic nanoparticles are formed or grown.

[0066] Suitable anionic surfactants may be selected from the group consisting of organic sulfate compounds, organic sulfite compounds, organic sulfonate compounds, organic phosphate compounds and organic carboxylate compounds. Preferred surfactants are organic sulfate compounds, and among them, sodium lauryl sulfate is the most preferred surfactant.

[0067] Suitable cationic surfactants can be selected from the group of surfactant compounds consisting of ammonium salts of primary, secondary and tertiary amines. Examples of cationic surfactants that can be used include quaternary ammonium surfactant compounds such as cetyltrimethylammonium bromide, cetylpyridinium chloride, benzalkonium chloride, benzethonium chloride, dimethyldioctadecylammonium chloride and dioctadecyldimethylammonium bromide.

[0068] Suitable nonionic surfactants can be selected from the group of compounds consisting of ethoxylates, fatty alcohol ethoxylates, alkylphenol ethoxylates and fatty acid esters. Examples of fatty alcohol nonionic surfactants that can be used include octaethylene glycol monododecyl ether and pentaethylene glycol monododecyl ether. Examples of alkylphenol ethoxylates include nonoxynol ether and Triton X-100. Examples of fatty acid esters that can be used as nonionic surfactants include glyceryl monostearate, glyceryl monolaurate, sorbitan monolaurate, sorbitan monostearate and sorbitan tristearate.

[0069] The nanoparticles of the present invention are incorporated into the catalyst support by any suitable method to disperse them over the surface area of ​​the shaped inorganic oxide support. As previously mentioned, the dispersion rate of the bimetallic nanoparticles over the surface area of ​​the catalyst support should be less than 25% of the surface area of ​​the shaped inorganic oxide support, such as by H 2 Measured by chemical adsorption method.

[0070] It is preferred to impregnate the shaped inorganic oxide support with the aqueous dispersion of the bi-metallic nanoparticles by applying any known impregnation method, such as incipient wetness impregnation and wet impregnation. Incipient wetness impregnation is accomplished by contacting the support particles with a volume of the impregnation solution (i.e., aqueous dispersion of the bi-metallic nanoparticles) that is substantially equal to the total aqueous pore volume of the support particles. Wet impregnation methods involve contacting the support particles by dipping or immersing the support particles in the impregnation solution or passing the impregnation solution over the support particles for a defined period of time.

[0071] These methods provide accumulation of a majority of the nanoparticles within the outer shell region of the shaped inorganic oxide support. When the surface of the inorganic oxide support is contacted with the aqueous dispersion of the bi-metallic nanoparticles, the nanoparticles contained in the aqueous dispersion tend to settle and accumulate within the outer shell region of the shaped inorganic oxide support. Thus, at least 90% by weight of the nanoparticles accumulate and settle within the outer shell region of the shaped support structure. Very few, if any, of the nanoparticles accumulate or deposit on the support surface within the interior region of the shaped support structure. The deposition of the nanoparticles within the outer shell region of the shaped support structure provides the eggshell characteristics of the catalyst of the present invention.

[0072] The impregnated support is dried using conventional drying methods at a drying temperature ranging from 40° C. to 180° C. Preferably, the drying temperature is in the range from 50° C. to 160° C., and more preferably, from 50° C. to 150° C.

[0073] After the impregnated support is dried, it is then calcined in the presence of oxygen (preferably air) at a calcination temperature ranging from 250° C. to 600° C. to provide the selective hydrogenation catalyst composition of the present invention. Preferably, the calcination temperature is in the range of from 320° C. to 550° C., and more preferably, from 350° C. to 525° C.

[0074] After incorporating the nanoparticles into the support, drying the impregnated support, and calcining the dried support, the selective hydrogenation catalyst composition of the present invention has a total silver content in the range of from 0.01 wt % to 1 wt %, and a total palladium content in the range of from 0.01 wt % to 1 wt %. Preferably, the total silver content is in the range of from 0.015 wt % to 0.09 wt %, and more preferably, from 0.02 wt % to 0.08 wt %. Preferably, the total palladium content of the selective hydrogenation catalyst composition is in the range of from 0.015 wt % to 0.09 wt %, and more preferably, from 0.02 wt % to 0.08 wt %. Assuming that silver is a metal, regardless of its actual form, the weight percentage of silver is based on the total weight of the catalyst composition. Assuming that palladium is a metal, regardless of its actual form, the weight percentage of palladium is based on the total weight of the catalyst composition.

[0075] The selective hydrogenation process of the present invention uses the catalyst composition described herein. The selective hydrogenation process can be carried out in a single reactor or in more than one reactor connected with any suitable flow arrangement. If more than one reactor is used, the reactors can be arranged in parallel flow or serial flow or a combination of these two flow arrangements. Each reactor defines a reaction zone containing a certain volume of selective hydrogenation catalyst. Each of these reactors is equipped with a feed inlet device for receiving a feed stream and introducing the feed stream into its reaction zone, which operates under selective hydrogenation reaction conditions. Each of these reactors is also equipped with a reactor effluent outlet device for discharging reactor effluent from its reaction zone.

[0076] In the selective hydrogenation process, olefin feed is introduced into the reaction zone containing the selective hydrogenation catalyst. The olefin feed contacts with the catalyst under the selective hydrogenation reaction conditions in the reaction zone. The olefin feed is an olefin product stream, which comprises monounsaturated hydrocarbons. Preferred monounsaturated hydrocarbon product streams can be product streams of a combination of ethylene, propylene or butylene or these low molecular weight olefins.

[0077] The olefin feed or olefin product stream treated by the selective hydrogenation process of the present invention may also contain contaminating concentrations of highly unsaturated hydrocarbons (such as alkynes, e.g., acetylene or methylacetylene) and polyunsaturated hydrocarbons (such as dienes, e.g., propadiene). The selective hydrogenation catalyst of the present invention provides for the selective hydrogenation of highly unsaturated hydrocarbons contained in the olefin feed to their respective monosaturated hydrocarbons (i.e., olefins), with only minimal hydrogenation of the olefins in the olefin feed to saturated hydrocarbons.

[0078] The preferred use of the selective hydrogenation catalyst is the selective hydrogenation of acetylene contained in an ethylene product stream or the selective hydrogenation of methylacetylene and propadiene contained in a propylene product stream. In both processes, the selective hydrogenation catalyst of the present invention is particularly suitable for the selective hydrogenation of acetylene contained in an ethylene product stream.

[0079] The ethylene product feed entering the selective acetylene hydrogenation process can typically have an acetylene concentration exceeding 100ppmm to 2 mole %. The selective hydrogenation process can reduce the concentration of acetylene contained in the ethylene product feed to produce a reactor effluent or treated ethylene product with a reduced acetylene concentration (typically having a concentration significantly lower than 100ppmm). The process has a high degree of selectivity in acetylene hydrogenation. The selectivity is typically greater than 70%. More typically, the selectivity is greater than 72%, and even greater than 74%. The ethylene selectivity is defined as the volume of ethylene in the reactor outlet effluent minus the volume of ethylene in the reactor inlet feed divided by the difference of the acetylene in the reactor inlet feed and the acetylene in the reactor outlet effluent, multiplied by 100.

[0080] The selective hydrogenation of acetylene in an ethylene stream to form ethylene is typically carried out as a gas phase process at a space velocity of the gaseous ethylene stream of from 500 v / vh to 15,000 v / vh (based on the catalyst volume), a temperature in the range of from 10° C. to 250° C. and a pressure of from 0.01 bar to 90 bar.

[0081] The molar ratio of hydrogen to acetylene in the feed contacting the selective hydrogenation catalyst is typically in the range of from 0.8 to 1.8.

[0082] The selective hydrogenation of methylacetylene or propadiene or both contained in the propylene stream to form propylene is generally carried out as a gas phase process or a mixed gas-liquid phase process at a space velocity of the liquid propylene stream of from 1 v / vh to 50 v / vh (based on the catalyst volume), a temperature in the range of from 10° C. to 180° C. and a pressure of from 0.01 bar to 50 bar. The molar ratio of hydrogen to methylacetylene and propadiene in the propylene stream in the feed contacted with the selective hydrogenation catalyst is typically in the range of from 0.8 to 2.

[0083] The following examples are provided to illustrate the invention, but they should not be construed as limiting the invention in any way.

[0084] Example

[0085] Example 1

[0086] This Example 1 describes the preparation of Catalyst 1 which is representative of the catalyst according to the invention.

[0087] In 0.1M sodium dodecyl sulfate solution, Pd(NO 3 ) 2 and AgNO 3 Mix in water and heat to 75°C for 10 hours. 400 g of α-alumina support (4×4 mm tablets) were impregnated with this mixture. The amount of metal salts was calculated to give 0.035 wt% Pd and 0.025 wt% Ag on the catalyst.

[0088] The impregnated support was dried in air at 120°C for 2 hours and then calcined in a rotary kiln at 500°C for 3 hours.

[0089] Example 2

[0090] This Example 2 describes the preparation of Catalyst 2 which also represents a catalyst according to the invention.

[0091] In 0.1M sodium dodecyl sulfate solution, Pd(NO 3 ) 2 and AgNO 3 Mix in water and heat to 80°C for 10 hours. 400 g of α-alumina support (4×4 mm tablets) were impregnated with this mixture. The amount of metal salts was calculated to give 0.035 wt% Pd and 0.040 wt% Ag on the catalyst.

[0092] The impregnated support was dried in air at 100°C for 2 hours and then calcined in a rotary kiln at 500°C for 3 hours.

[0093] Example 3

[0094] This Example 3 describes the preparation of Comparative Catalyst 3, which is similar to the catalyst disclosed in PCT Publication No. WO 2011 / 113881.

[0095] 400 g of α-alumina support (4×4 mm tablets) were impregnated with an aqueous hydrazine solution (2% hydrazine content). The volume of the solution corresponded to 35% of the total pore volume of the support. Subsequently, AgNO 3 and Pd(NO 3 )2 The support is impregnated with an aqueous solution of . The concentration of the noble metal in the solution is chosen to give a palladium content of 0.035% by weight and a silver content of 0.025% by weight in the catalyst. The volume of the noble metal-containing solution corresponds to 65% of the total pore volume of the support.

[0096] The impregnated catalyst precursor was completely dried in a moving bed and subsequently calcined at 630°C for five hours under a nitrogen atmosphere.

[0097] Example 4

[0098] This Example 4 describes the performance tests performed to characterize the catalyst compositions of Examples 1 to 3.

[0099] Experimental conditions were chosen that were very similar to those of the first tail reactor of a steam cracker unit.

[0100] The laboratory reactor was filled with 15 ml of catalyst, divided into five layers, diluted with 85 ml of α-alumina balls. The feed having the composition shown in the table below was fed into the reactor at a rate to provide a GHSV of 4,000 v / vh. The reactor was operated at a pressure of 10 bar and a temperature adjusted and maintained so as to provide an acetylene conversion of 70%, i.e. an acetylene concentration of 3,000 ppm, at the reactor outlet.

[0101] Feed composition (in mol%)

[0102] <![CDATA[C 2 H 2 (Acetylene)]]> 1.0(10,000ppm) <![CDATA[H 2 ]]> 1.0 <![CDATA[C 2 H 4 (Ethylene)]]> 30 <![CDATA[C 3 H 8 (Propane)]]> 1.0 <![CDATA[N 2 ]]> balance

[0103] The following table presents the results from the performance tests of the catalysts of the present invention and comparative catalysts. The selectivity was calculated as follows: [(ethylene outlet concentration - ethylene inlet concentration) / (acetylene inlet concentration - acetylene outlet concentration)]*100.

[0104] Performance test results of the catalyst of the present invention and the comparative catalyst

[0105]

[0106] The performance data presented in the above table show that the catalyst of the present invention provides significantly better selectivity for the conversion of acetylene to ethylene than the comparative catalyst. When compared with the comparative catalyst, this improvement in the selectivity for the conversion of acetylene when using the catalyst of the present invention provides a higher ethylene yield and a lower green oil yield.

[0107] The rate of decrease in ethylene selectivity when using the catalyst of the present invention is much lower than the rate of decrease in ethylene selectivity when using the comparative catalyst. Therefore, the catalyst of the present invention is more stable and can provide a longer service life than the comparative catalyst. The stability of the catalyst of the present invention is also demonstrated by the smaller rate of increase in reactor temperature required for 70% acetylene conversion exhibited by the catalyst of the present invention relative to the comparative catalyst.

[0108] Example 5

[0109] This embodiment presents Figure 2 , which is a transmission electron micrograph of a catalyst of the present invention prepared as described in Example 1. The magnification of the TEM scan is ×100,000 (200 kV), and it shows the alumina support of the catalyst, and the bimetallic nanoparticles present on the surface of the alumina support. The arrows on the image point to the nanoparticles.

[0110] This embodiment also presents Figure 3 , which is a transmission electron micrograph of the bimetallic nanoparticles of the aqueous dispersion used to prepare the catalyst of the present invention. The magnification of the TEM scan is x100,000 (200 kV), and it shows the nanoparticles after drying the aqueous dispersion.

[0111] Example 6

[0112] This embodiment presents Figure 4 , which is an exemplary particle size distribution of micelle-stabilized nanoparticles in aqueous dispersion. 3 ) 2 and AgNO 3 The particle size distribution was measured after mixing into a 0.1 M aqueous sodium dodecyl sulfate solution (as described in Examples 1 and 2) and stirring for 12 hours at 80° C. The method applied was dynamic light scattering.

Claims

1. A composition for use as a selective hydrogenation catalyst or a selective hydrogenation catalyst precursor, wherein the composition comprises a carrier comprising bimetallic nanoparticles, wherein the bi-metallic nanoparticles comprise a silver component and a palladium component and have an average particle size in a range from 1 nm to 10 nm, and a total molar ratio of palladium to silver in a range from 0.01:1 to 100:1, wherein the composition comprises a total silver content in the range of from 0.01 wt % to 1 wt % and a total palladium content in the range of from 0.01 wt % to 1 wt %, wherein the weight percent of silver is based on the weight of the composition and silver as metal and the weight percent of palladium is based on the weight of the composition and palladium as metal, wherein the bi-metallic nanoparticles comprise core-shell nanoparticles, and wherein the support is a shaped inorganic oxide support and the dispersion of the bi-metallic nanoparticles on the surface of the support is in the range of from 0.01% to 22% of the BET surface area of ​​the support as measured by H2 chemisorption.

2. The composition of claim 1, wherein the bi-metallic nanoparticles comprise metal alloy nanoparticles comprising silver and palladium.

3. The composition of claim 1, wherein the core-shell nanoparticle comprises a core and a shell surrounding the core, the core having a first major portion being palladium and the shell having a second major portion being silver.

4. The composition of claim 1, wherein the core-shell nanoparticle comprises a core and a shell surrounding the core, the core having a first major portion being silver, and the shell having a second major portion being palladium.

5. The composition according to claim 1, wherein the support comprises an inorganic oxide and is a shaped structure defined by a shape having an outer shell region and an inner region, wherein the bimetallic nanoparticles are concentrated in the outer shell region, and wherein the shape is selected from the group consisting of spheres, cylindrical pellets, and extrudates that are cylindrical or lobed, wherein the sphere has a sphere diameter in the range from 0.5 mm to 25 mm, the cylindrical pellets have a pellet diameter in the range from 0.5 mm to 25 mm and a pellet length in the range from 1 mm to 50 mm, and the extrudate has an extrudate diameter in the range from 0.5 mm to 25 mm and an extrudate length in the range from 1 mm to 50 mm.

6. The composition of claim 5, wherein the outer shell region has a depth from the outer surface in the range of from 1 micron to 400 microns.

7. A method of making a composition for use as a selective hydrogenation catalyst or a selective hydrogenation catalyst precursor, wherein the method comprises: providing an aqueous dispersion of bi-metallic nanoparticles, the bi-metallic nanoparticles being formed by reducing a palladium salt and a silver salt in a mixture using a surfactant, wherein the bi-metallic nanoparticles include a core-shell structure, wherein the surfactant is selected from the group consisting of cationic surfactants, anionic surfactants and nonionic surfactants, wherein the silver salt is selected from the group consisting of silver nitrate, silver halide, silver carbonate, silver phosphate, silver acetate and silver sulfate, and wherein the palladium salt is selected from the group consisting of palladium salts consisting of palladium nitrate, palladium halide, palladium carbonate, palladium phosphate, palladium acetate and palladium sulfate; incorporating the aqueous dispersion into a carrier to provide an impregnated carrier; as well as The impregnated support is dried and then calcined in air at a low calcination temperature ranging from 250°C to 600°C to provide the composition.

8. The method of claim 7, wherein the step of providing an aqueous dispersion of bi-metallic nanoparticles comprises: mixing the palladium salt, the silver salt, and the surfactant in water to provide the mixture; as well as The mixture is heated at a low heating temperature ranging from 30° C. to 100° C. for a heating period sufficient to thereby provide the aqueous dispersion, and the heating period is up to 24 hours.

9. The method of claim 7 wherein said bi-metallic nanoparticles provide a molar ratio of palladium to silver in said aqueous dispersion in a range from 0.01:1 to 100:1 based on the total weight of said aqueous dispersion including both continuous and discontinuous phases.

10. The method according to claim 7, wherein the surfactant is selected from the group of anionic surfactants consisting of organic sulfate compounds, organic sulfite compounds, organic sulfonate compounds, organic phosphate compounds and organic carboxylate compounds.

11. The method according to claim 7, wherein the surfactant is selected from the group of cationic surfactant compounds consisting of ammonium salts of primary, secondary and tertiary amines.

12. The method according to claim 7, wherein the surfactant is selected from the group of nonionic surfactants consisting of ethoxylates, fatty alcohol ethoxylates, alkylphenol ethoxylates and fatty acid esters.

13. The method of claim 7, wherein the support is a shaped structure comprising an inorganic oxide and having a shape selected from the group consisting of a sphere, a cylindrical pellet, and an extrudate that is a cylinder or a leaf shape, wherein the sphere has a sphere diameter in the range from 0.5 mm to 25 mm, the cylindrical pellet has a pellet diameter in the range from 0.5 mm to 25 mm and a pellet length from 1 mm to 50 mm, and the extrudate has an extrudate diameter in the range from 0.5 mm to 25 mm, and an extrudate length in the range from 1 mm to 50 mm, and wherein the shaped structure is defined as having an outer shell region and an inner region.

14. The method of claim 13, wherein the incorporating step is a wet impregnation or incipient wetness impregnation that causes the bi-metallic nanoparticles to be incorporated and concentrated within the outer shell region having a depth in a range from 1 micron to 400 microns.

15. The method of claim 7, wherein the aqueous dispersion comprises a concentration of silver and a concentration of palladium such that upon incorporation into the support and calcination of the impregnated support, the composition comprises from 0.01 to 1 weight percent silver, based on the weight of the composition and silver as metal, and from 0.01 to 1 weight percent palladium, based on the weight of the composition and palladium as metal.

16. A selective hydrogenation process comprising: Under suitable selective hydrogenation reaction conditions, an olefin feed stream having a contaminating concentration of highly unsaturated hydrocarbons is contacted with any one of the catalysts according to claims 1 to 6 or with any one of the catalysts produced by the methods according to claims 7 to 15, and a treated olefin feed stream having a reduced concentration of highly unsaturated hydrocarbons is produced.