A test method for the stability of supercooling behavior of phase change energy storage materials
By controlling different residence times in the molten state of phase change energy storage materials, combined with T-history method and DSC method testing, the stability of the supercooling behavior of the hydrated salt system is evaluated, which solves the problem of evaluating the impact of liquid phase residence time in the existing technology. Accurate questions improve the accuracy of assessment and application prospects.
Patent Information
- Application Number
- CN202110757557.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-07-05
AI Technical Summary
When testing the supercooling behavior of hydrated salt system phase change energy storage materials, the existing technology fails to effectively consider the impact of the material's residence time in the liquid phase on the supercooling behavior, resulting in inaccurate stability assessment.
By carrying out multiple cycles in the molten state of the phase change energy storage material system, controlling different residence times, using the T-history method and DSC method to test the degree of supercooling, set the supercooling threshold and difference threshold, and evaluate the material's Stability of supercooling behavior.
This method improves the accuracy of the stability assessment of supercooling behavior of phase change energy storage materials and takes into account the impact of liquid phase residence time on supercooling behavior, which has important engineering significance and application prospects.
Smart Images

Figure CN113390915B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of phase change energy storage materials, and in particular relates to a method for testing the stability of supercooling behavior of a phase change energy storage material system. Background Art
[0002] At present, the supercooling behavior test of hydrated salt system phase change energy storage materials is mainly achieved by single or multiple supercooling measurements, and little attention is paid to the influence of the residence time of the material in the liquid phase (above the phase change temperature) on the supercooling behavior. When the material is modified by a thickener (such as improving the cycle stability), its supercooling behavior will be affected by the residence time of the material in the liquid phase, but in practical applications, the residence time of the material in the liquid phase cannot be determined because it will be affected by the environment, and the uncertainty of the residence time of the material in the liquid phase will affect the accuracy of the stability assessment of the material's supercooling behavior.
[0003] Therefore, it is very necessary to characterize the stability of the supercooling behavior of the material when it stays in the liquid phase for different times. Summary of the invention
[0004] In order to solve the problems existing in the above-mentioned prior art, the present invention provides a testing method for the stability of the supercooling behavior of a phase change energy storage material system. The method determines the stability of the supercooling behavior of the material system by regulating the influence of different staying times of the phase change energy storage material system in a molten state on the supercooling degree of the material system.
[0005] To achieve the above-mentioned purpose, the present invention provides a method for testing the stability of supercooling behavior of a phase change energy storage material system, which comprises:
[0006] S10, subjecting the phase-change energy storage material system to be tested to multiple cycles of endothermic melting-exothermic crystallization, controlling the phase-change energy storage material system to stay in a molten state for different first predetermined times during the multiple cycles, wherein the first predetermined times include a first residence time and a second residence time, and the second residence time is greater than the first residence time by more than 3 hours;
[0007] S20, testing the supercooling of the phase-change energy storage material system by using a T-history method at least during the cycle process in which the phase-change energy storage material system stays in a molten state for the first residence time and the second residence time, to obtain a first supercooling corresponding to the first residence time and a second supercooling corresponding to the second residence time;
[0008] S30. Based on the comparison between the first degree of supercooling and the second degree of supercooling and a preset degree of supercooling threshold and a difference threshold, the stability of the supercooling behavior of the phase change energy storage material system is evaluated.
[0009] Preferably, judging the stability of the supercooling behavior of the phase change energy storage material system based on the comparison of the first supercooling degree and the second supercooling degree with a preset supercooling degree threshold and a difference threshold comprises:
[0010] (I) if both the first degree of supercooling and the second degree of supercooling are not greater than the degree of supercooling threshold, it is determined that the supercooling behavior of the phase change energy storage material system is stably suppressed;
[0011] (II), at least one of the first degree of supercooling and the second degree of supercooling is greater than the supercooling threshold, and the difference between the first degree of supercooling and the second degree of supercooling is not greater than the difference threshold, then it is determined that the supercooling behavior of the phase change energy storage material system is suppressed to a certain extent;
[0012] (III) If at least one of the first degree of supercooling and the second degree of supercooling is greater than the supercooling threshold, and the difference between the first degree of supercooling and the second degree of supercooling is greater than the difference threshold, it is determined that the supercooling behavior of the phase change energy storage material system is unstable.
[0013] Preferably, the first residence time is 2 hours to 3 hours, and the second residence time is 6 hours to 10 hours.
[0014] Further preferably, except for the first stay time and the second stay time, the other scheduled stay times among the plurality of first scheduled times are all shorter than the first stay time.
[0015] Preferably, the supercooling threshold is 1.2°C to 1.5°C, and the difference threshold is 4°C to 6°C.
[0016] Further preferably, the supercooling threshold is 1.5°C, and the difference threshold is 5°C.
[0017] Preferably, when the supercooling behavior of the phase change energy storage material system is determined to be unstable, the testing method further comprises:
[0018] S40, subjecting the phase change energy storage material system to multiple cycles of endothermic melting-exothermic crystallization, controlling the phase change energy storage material system to stay in a molten state for different second predetermined times during the multiple cycles, testing the supercooling degree of the phase change energy storage material system by DSC method, and making a final judgment on the stability of the supercooling behavior of the phase change energy storage material system according to the test results of the DSC method, including:
[0019] If the test result according to the DSC method shows that the supercooling behavior of the phase change energy storage material system is unstable, it is finally determined that the supercooling behavior of the phase change energy storage material system is unstable;
[0020] If the test result according to the DSC method shows that the supercooling behavior of the phase change energy storage material system is stable, it cannot be determined that the supercooling behavior of the phase change energy storage material system is unstable, and the test process of steps S10-S30 needs to be repeated.
[0021] More preferably, the second predetermined time is 0.1 min to 30 min.
[0022] The present invention provides a method for testing the stability of supercooling behavior of a phase-change energy storage material system. By combining the T-history test method and the DSC test method, the influence of different residence times of the phase-change energy storage material system in a molten state on the supercooling degree of the material system is regulated, and the stability of the supercooling behavior of the material system is judged. The test method takes into account the influence of the residence time of the phase-change energy storage material in the liquid phase on its supercooling behavior, improves the accuracy of the evaluation of the stability of the supercooling behavior of the phase-change energy storage material, and has important engineering significance and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a flow chart of a method for testing the stability of supercooling behavior of a phase change energy storage material system in an embodiment of the present invention;
[0024] Figure 2 is a flow chart of a method for testing the stability of supercooling behavior of a phase change energy storage material system in an embodiment of the present invention;
[0025] Figure 3 is a cooling curve diagram of the phase change energy storage material system in Example 1 of the present invention;
[0026] Figure 4 This is a distribution diagram of the supercooling degree of the phase change energy storage material system in Example 1 of the present invention in 100 melting-crystallization cycles as the number of cycles increases;
[0027] Figure 5 is a cooling curve diagram of the phase change energy storage material system in Example 2 of the present invention;
[0028] Figure 6 is a cooling curve diagram of the phase change energy storage material system in Example 3 of the present invention;
[0029] Figure 7 This is a DSC curve diagram of the phase change energy storage material system in Example 3 of the present invention. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Examples of these preferred embodiments are illustrated in the accompanying drawings. The embodiments of the present invention shown in the accompanying drawings and described according to the accompanying drawings are merely exemplary, and the present invention is not limited to these embodiments.
[0031] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the solutions according to the present invention are shown in the accompanying drawings, while other details that are not closely related to the present invention are omitted.
[0032] The present invention provides a method for testing the stability of supercooling behavior of a phase change energy storage material system. Figure 1 , the method comprising:
[0033] Step S10, subjecting the phase change energy storage material system to be tested to multiple cycles of endothermic melting-exothermic crystallization, and controlling the phase change energy storage material system to stay in a molten state for different first predetermined times during the multiple cycles.
[0034] Preferably, the plurality of first predetermined times include a first stay time and a second stay time.
[0035] Further preferably, the second residence time is greater than the first residence time by more than 3 hours.
[0036] Preferably, the first residence time is 2 hours to 3 hours, and the second residence time is 6 hours to 10 hours.
[0037] Further preferably, except for the first stay time and the second stay time, the other scheduled stay times among the plurality of first scheduled times are all shorter than the first stay time, for example, 30 minutes, 1 hour or 1.5 hours.
[0038] Step S20, testing the supercooling of the phase-change energy storage material system by using the T-history method at least during the cycle process in which the phase-change energy storage material system stays in the molten state for the first residence time and the second residence time, to obtain a first supercooling corresponding to the first residence time and a second supercooling corresponding to the second residence time.
[0039] Step S30: Based on the comparison between the first degree of supercooling and the second degree of supercooling and a preset degree of supercooling threshold and a difference threshold, the stability of the supercooling behavior of the phase change energy storage material system is judged.
[0040] Preferably, the supercooling threshold is 1.2°C to 1.5°C, and the difference threshold is 4°C to 6°C.
[0041] Further preferably, the supercooling threshold is 1.5°C, and the difference threshold is 5°C.
[0042] Wherein, judging the stability of the supercooling behavior of the phase change energy storage material system based on the comparison between the first supercooling degree and the second supercooling degree and a preset supercooling degree threshold and a difference threshold comprises:
[0043] (I) if both the first degree of supercooling and the second degree of supercooling are not greater than the degree of supercooling threshold, it is determined that the supercooling behavior of the phase change energy storage material system is stably suppressed;
[0044] (II), at least one of the first degree of supercooling and the second degree of supercooling is greater than the supercooling threshold, and the difference between the first degree of supercooling and the second degree of supercooling is not greater than the difference threshold, then it is determined that the supercooling behavior of the phase change energy storage material system is suppressed to a certain extent;
[0045] (III) If at least one of the first degree of supercooling and the second degree of supercooling is greater than the supercooling threshold, and the difference between the first degree of supercooling and the second degree of supercooling is greater than the difference threshold, it is determined that the supercooling behavior of the phase change energy storage material system is unstable.
[0046] In a further preferred embodiment, see Figure 2 , when the supercooling behavior of the phase change energy storage material system is determined to be unstable, the testing method further comprises:
[0047] Step S40, subjecting the phase change energy storage material system to multiple cycles of endothermic melting-exothermic crystallization, controlling the phase change energy storage material system to stay in a molten state for different second predetermined times during the multiple cycles, testing the supercooling degree of the phase change energy storage material system by DSC method, and making a final judgment on the stability of the supercooling behavior of the phase change energy storage material system based on the test results of the DSC method.
[0048] Among them, the final evaluation of the supercooling behavior stability of the phase change energy storage material system is carried out according to the test results of the DSC method, including:
[0049] If the test result according to the DSC method shows that the supercooling behavior of the phase change energy storage material system is unstable, it is finally determined that the supercooling behavior of the phase change energy storage material system is unstable;
[0050] If the test result according to the DSC method shows that the supercooling behavior of the phase change energy storage material system is stable, it cannot be determined that the supercooling behavior of the phase change energy storage material system is unstable, and the test process of steps S10-S30 needs to be repeated.
[0051] Among them, it is necessary to test the supercooling result and crystallization exothermic peak of the phase change energy storage material system according to the DSC method to determine whether the supercooling behavior of the phase change energy storage material system is stable:
[0052] (1) Determine whether the supercooling behavior of the phase change energy storage material system is stable: Take at least 4 dwell time intervals uniformly distributed in the time scale of 0.1min to 60min, and determine whether the supercooling degree and the temperature span of the crystallization exothermic peak obtained by the test change regularly with the delay of the dwell time. If the supercooling degree is relatively stable (the change is within 5°C, and there is no obvious trend of continuous increase or continuous decrease), and the temperature span of the crystallization exothermic peak changes less than 1.5°C and there is no obvious pattern of first increasing and then decreasing to the equilibrium value, then the supercooling behavior of the system is determined to be stable.
[0053] (2) Determine whether the supercooling behavior of the phase change energy storage material system is unstable: Take at least 4 residence time intervals uniformly distributed in the time scale of 0.1min to 60min, and determine whether the supercooling degree and the temperature span of the crystallization exothermic peak obtained by the test change regularly with the delay of the residence time. If the supercooling degree changes by more than 5°C and has an obvious trend of continuous increase, and the temperature span of the crystallization exothermic peak changes by more than 1.5°C and has an obvious pattern of first increasing and then decreasing to the equilibrium value, then it is determined that the supercooling behavior of the system is easily affected by the uneven local supercooling and exhibits unstable supercooling behavior.
[0054] Since the sample tested by the DSC method is only a few milligrams, while the sample tested by the T-history method is usually tens or even hundreds of grams, the test results obtained by the DSC method and the T-history method may be inconsistent. Since the sample amount tested by the T-history method is higher, the test results of the T-history method are usually taken as the standard. However, when the test results obtained by the DSC method and the T-history method are inconsistent, it is also necessary to consider whether other external factors interfere with the test results of the T-history method. Therefore, when the conclusions of the two are inconsistent, it is necessary to repeat the T-history method test process of steps S10-S30.
[0055] Preferably, the second predetermined time is 0.1 min to 30 min.
[0056] The following will illustrate the test method for the stability of the supercooling behavior of the above-mentioned phase change energy storage material system in conjunction with specific embodiments. Those skilled in the art will understand that the following embodiments are specific examples of the test method for the stability of the supercooling behavior of the above-mentioned phase change energy storage material system of the present invention, and are not intended to limit the entirety of the present invention.
[0057] Example 1: Evaluation of the supercooling behavior stability of EPCM+0.5%SrCl2·6H2O+0.5%HEC
[0058] Step 1, subjecting the EPCM+0.5%SrCl2·6H2O+0.5%HEC phase change energy storage material system to be tested to multiple cycles of endothermic melting-exothermic crystallization, wherein EPCM: 43%MgCl2+57%Mg(NO3)2-6H2O, HEC: hydroxyethyl cellulose; during the multiple cycles, the phase change energy storage material system is controlled to stay in a molten state for different first predetermined times, wherein the first predetermined times include 2h and 8h.
[0059] Step 2, using the T-history method to cyclically test 100 times the supercooling of the phase change energy storage material system in the molten state corresponding to several different first predetermined time periods; wherein, arbitrarily select one or more times in the test process to measure the supercooling of the phase change energy storage material system when it stays in the molten state for 2h and 8h, respectively, and the predetermined stay times corresponding to the remaining test processes are all less than 2h and can be arbitrarily selected according to actual needs; then take the maximum values of the measurement results corresponding to 2h and corresponding to 8h as the first supercooling and the second supercooling, respectively.
[0060] Figure 3 is the cooling curve diagram of the phase change energy storage material system, Figure 3 It can be seen that the first supercooling degree of the phase change energy storage material is 0.2°C, and the second supercooling degree is 0.6°C.
[0061] Step 3: Based on the obtained first undercooling degree of 0.2°C and second undercooling degree of 0.6°C, therefore, both the first undercooling degree and the second undercooling degree are not greater than 1.5°C. In addition, Figure 4 is the distribution diagram of the supercooling degree of the phase change energy storage material system in 100 melting-crystallization cycles as a function of the number of cycles, Figure 4 It can be seen that the supercooling degree of the phase change energy storage material system is less than 1.5°C during 100 melting-crystallization cycles; therefore, it is determined that the supercooling behavior of the phase change energy storage material system is stably suppressed.
[0062] Example 2: Evaluation of the supercooling behavior stability of EPCM+0.5%SrCl2·6H2O+1.0%HEC
[0063] Step 1, subjecting the EPCM+0.5%SrCl2·6H2O+1.0%HEC phase change energy storage material system to be tested to multiple cycles of endothermic melting-exothermic crystallization, wherein EPCM: 43%MgCl2+57%Mg(NO3)2-6H2O, HEC: hydroxyethyl cellulose; during the multiple cycles, the phase change energy storage material system is controlled to stay in a molten state for different first predetermined times, wherein the first predetermined times include 2h and 8h.
[0064] Step 2, using the T-history method to test 50 times the supercooling of the phase change energy storage material system in the molten state corresponding to several different first predetermined time periods during the cycle; wherein, arbitrarily select one or more times during the test process to measure the supercooling of the phase change energy storage material system when it stays in the molten state for 2h and 8h, respectively, and the corresponding predetermined stay times in the remaining test processes are all less than 2h and can be arbitrarily selected according to actual needs; then take the maximum values of the measurement results corresponding to 2h and corresponding to 8h as the first supercooling and the second supercooling, respectively.
[0065] Figure 5 is the cooling curve diagram of the phase change energy storage material system, Figure 5 It can be seen that the first supercooling degree of the phase change energy storage material is 0.9°C, and the second supercooling degree is 1.7°C.
[0066] Step 3: Based on the obtained first supercooling of 0.9°C and second supercooling of 1.7°C, the second supercooling is greater than 1.5°C, and the difference between the first supercooling and the second supercooling is 0.6°C, which is not greater than 5°C. Therefore, it is determined that the supercooling behavior of the phase change energy storage material system has been suppressed to a certain extent, and it can be decided later whether the supercooling of the phase change energy storage material system needs to be tested by the DSC method according to actual conditions.
[0067] Example 3: Evaluation of the supercooling behavior stability of EPCM+0.5%SrCl2·6H2O+1.5%HEC
[0068] Step 1, subjecting the EPCM+0.5%SrCl2·6H2O+1.5%HEC phase change energy storage material system to be tested to multiple cycles of endothermic melting-exothermic crystallization, wherein EPCM: 43%MgCl2+57%Mg(NO3)2-6H2O, HEC: hydroxyethyl cellulose; during the multiple cycles, the phase change energy storage material system is controlled to stay in a molten state for different first predetermined times, wherein the first predetermined times include 2h and 8h.
[0069] Step 2, using the T-history method to test 50 times the supercooling of the phase change energy storage material system in the molten state corresponding to several different first predetermined time periods during the cycle; wherein, arbitrarily select one or more times during the test process to measure the supercooling of the phase change energy storage material system when it stays in the molten state for 2h and 8h, respectively, and the predetermined stay times corresponding to the remaining tests are all less than 2h and can be arbitrarily selected according to actual needs; then take the maximum values of the measurement results corresponding to 2h and corresponding to 8h as the first supercooling and the second supercooling, respectively.
[0070] Figure 6is the cooling curve diagram of the phase change energy storage material system, Figure 6 It can be seen that the first supercooling degree of the phase change energy storage material is 3.8°C, and the second supercooling degree is 9.5°C.
[0071] Step 3: Based on the obtained first supercooling of 3.8°C and second supercooling of 9.5°C, the first supercooling and second supercooling are both greater than 1.5°C; and the difference between the first supercooling and the second supercooling is 5.7°C, which is greater than 5°C. Therefore, it is determined that the supercooling behavior of the phase change energy storage material system is unstable.
[0072] Step 4: subject the phase change energy storage material system to multiple cycles of endothermic melting-exothermic crystallization. During the multiple cycles, the phase change energy storage material system is controlled to stay in a molten state at 80°C for several different second predetermined times (0.1 min, 1 min, 5 min, 10 min and 30 min), and the supercooling of the phase change energy storage material system is tested by DSC method.
[0073] Since the quality levels of the samples tested by the T-history method and the DSC method are different, the scales of their residence time are also different. It takes more than several hours to reflect the fluctuations of the T-history method, while when using the DSC method, the difference can be reflected in a residence time of only a few minutes.
[0074] Figure 7 is the DSC curve of the phase change energy storage material system, and the crystallization temperature is 60°C. When it stays in the molten state for 0.1 min, the initial crystallization temperature is 49.09°C, the corresponding supercooling is 10.91°C, and the span of the crystallization exothermic peak is 14.03°C; when it stays in the molten state for 1 min, the initial crystallization temperature is 46.81°C, the corresponding supercooling is 13.19°C, and the span of the crystallization exothermic peak is 15.87°C; when it stays in the molten state for 5 min, the initial crystallization temperature is 48.01°C, the corresponding supercooling is 11.99°C, and the span of the crystallization exothermic peak is 15.73°C; when it stays in the molten state for 10 min, the initial crystallization temperature is 34.81°C, the corresponding supercooling is 25.19°C, and the span of the crystallization exothermic peak is 12.00°C; when it stays in the molten state for 30 min, the initial crystallization temperature is 35.69°C, the corresponding supercooling is 24.31°C, and the span of the crystallization exothermic peak is 11.93°C.
[0075] Depend on Figure 7It can be seen that in this embodiment, based on the DSC method to test the supercooling of the phase change energy storage material system, the supercooling changes by more than 5°C with the delay (increase) of the residence time, and the supercooling has a trend of continuous increase. At the same time, the temperature span of the crystallization exothermic peak changes by more than 1.5°C and has an obvious pattern of first increasing and then decreasing to the equilibrium value. Therefore, it is determined that the supercooling behavior of the phase change energy storage material system is unstable.
[0076] In summary, the test results of the T-history method and the DSC method show that the supercooling behavior of the phase change energy storage material system is unstable. Finally, it can be judged that the supercooling behavior of the phase change energy storage material system is unstable, and the different time it stays in the molten state has a great influence on the supercooling behavior. It is necessary to further optimize its supercooling behavior in order to achieve the purpose of "stably achieving the suppression of supercooling".
[0077] If the difference in supercooling obtained by the T-history method is large, but the broadening of the exothermic peak of the crystallization peak in the test results obtained by the DSC method is not obvious, it can be explained that the difference in supercooling measured by the T-history method is not caused by the heterogeneity of local supercooling, but by other reasons such as external interference. At this time, it cannot be determined that the supercooling behavior of the phase change energy storage material system is unstable, and it is necessary to re-conduct the T-history method test experiment to determine the result.
[0078] The present invention provides a method for testing the stability of supercooling behavior of a phase-change energy storage material system. By adjusting the different time the phase-change energy storage material system stays in a molten state, the supercooling degree of the material system is tested by combining the T-history method and the DSC method, thereby obtaining the influence of different time of staying in a molten state on the supercooling degree of the material system, and then judging the stability of the supercooling behavior of the material system. The testing method takes into account the influence of the residence time of the phase-change energy storage material in the liquid phase on its supercooling behavior, improves the accuracy of the evaluation of the stability of the supercooling behavior of the phase-change energy storage material, and has important engineering significance and application prospects.
[0079] The above is only a specific implementation of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A test method for the stability of supercooling behavior of a phase change energy storage material system. It is characterized in that include: S10, subjecting the phase-change energy storage material system to be tested to multiple cycles of endothermic melting-exothermic crystallization, controlling the phase-change energy storage material system to stay in a molten state for different first predetermined times during the multiple cycles, wherein the first predetermined times include a first residence time and a second residence time, and the second residence time is greater than the first residence time by more than 3 hours; S20, testing the supercooling of the phase-change energy storage material system by using a T-history method at least during the cycle process in which the phase-change energy storage material system stays in a molten state for the first residence time and the second residence time, to obtain a first supercooling corresponding to the first residence time and a second supercooling corresponding to the second residence time; S30, judging the stability of the supercooling behavior of the phase change energy storage material system based on the comparison between the first supercooling degree and the second supercooling degree and a preset supercooling degree threshold and a difference threshold; Wherein, judging the stability of the supercooling behavior of the phase change energy storage material system based on the comparison between the first supercooling degree and the second supercooling degree and a preset supercooling degree threshold and a difference threshold comprises: (I) if both the first degree of supercooling and the second degree of supercooling are not greater than the degree of supercooling threshold, it is determined that the supercooling behavior of the phase change energy storage material system is stably suppressed; (II), at least one of the first degree of supercooling and the second degree of supercooling is greater than the supercooling threshold, and the difference between the first degree of supercooling and the second degree of supercooling is not greater than the difference threshold, then it is determined that the supercooling behavior of the phase change energy storage material system is suppressed to a certain extent; (III), at least one of the first supercooling degree and the second supercooling degree is greater than the supercooling degree threshold, and the difference between the first supercooling degree and the second supercooling degree is greater than the difference threshold, then it is determined that the supercooling behavior of the phase change energy storage material system is unstable; Wherein, when the supercooling behavior of the phase change energy storage material system is determined to be unstable, the testing method further comprises: S40, subjecting the phase change energy storage material system to multiple cycles of endothermic melting-exothermic crystallization, controlling the phase change energy storage material system to stay in a molten state for different second predetermined times during the multiple cycles, testing the supercooling degree of the phase change energy storage material system by DSC method, and making a final judgment on the stability of the supercooling behavior of the phase change energy storage material system according to the test results of the DSC method, including: If the test result according to the DSC method shows that the supercooling behavior of the phase change energy storage material system is unstable, it is finally determined that the supercooling behavior of the phase change energy storage material system is unstable; If the test result according to the DSC method shows that the supercooling behavior of the phase change energy storage material system is stable, it cannot be determined that the supercooling behavior of the phase change energy storage material system is unstable, and the test process of steps S10-S30 needs to be repeated.
2. The method for testing the supercooling behavior stability of the phase change energy storage material system according to claim 1, It is characterized in that The first stay time is 2 hours to 3 hours, and the second stay time is 6 hours to 10 hours.
3. The method for testing the supercooling behavior stability of the phase change energy storage material system according to claim 2, It is characterized in that Except for the first stay time and the second stay time, all other scheduled stay times among the plurality of first scheduled times are shorter than the first stay time.
4. The method for testing the supercooling behavior stability of the phase change energy storage material system according to claim 1, It is characterized in that The supercooling threshold is 1.2°C to 1.5°C, and the difference threshold is 4°C to 6°C.
5. The method for testing the supercooling behavior stability of the phase change energy storage material system according to claim 4, It is characterized in that The undercooling threshold is 1.5°C, and the difference threshold is 5°C.
6. A method for testing the supercooling behavior stability of a phase change energy storage material system according to any one of claims 1 to 5, It is characterized in that The second predetermined time is 0.1 min to 30 min.