Solid electrolyte material and battery using the same
By using the combination of solid electrolyte materials of Li, Zr, Y, M and X, the problems of low lithium ion conductivity and safety of hydrogen sulfide in the prior art are solved, and high lithium ion conductivity and excellent charge and discharge characteristics are achieved.
Patent Information
- Application Number
- CN201980092634.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-15
- Filing Date
- 2019-12-11
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-12-11
AI Technical Summary
The prior art is difficult to provide solid electrolyte materials with high lithium ion conductivity, and sulfide electrolyte materials are prone to hydrogen sulfide in the atmosphere, affecting safety.
Using solid electrolyte materials including Li, Zr, Y, M and X, where M is Nb or Ta and X is a combination of Cl or Br, it is prepared by mechanochemical grinding method to ensure that the material does not contain sulfur and has high lithium ion conduction. Rate.
A solid electrolyte material with high lithium ion conductivity is achieved, ensuring the safety of the material and excellent charging and discharging characteristics, and avoiding the production of hydrogen sulfide.
Smart Images

Figure CN113474910B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a solid electrolyte material and a battery using the solid electrolyte material. Background Art
[0002] Patent Document 1 discloses an all-solid-state battery using a sulfide solid electrolyte material.
[0003] Patent document 2 discloses a method using a composition formula Li 6-3z Y z A solid electrolyte material represented by X6 (0<z<2, X=Cl or Br).
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2011-129312
[0007] Patent Document 2: International Publication No. 2018 / 025582 Summary of the invention
[0008] Problems to be solved by the invention
[0009] An object of the present invention is to provide a solid electrolyte material having high lithium ion conductivity.
[0010] Means for solving problems
[0011] The solid electrolyte material of the present invention comprises Li, Zr, Y, M and X, M is at least one element selected from Nb and Ta, and X is at least one element selected from Cl and Br.
[0012] Effects of the Invention
[0013] The present invention provides a solid electrolyte material with high lithium ion conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 A cross-sectional view of a battery 1000 according to a second embodiment is shown.
[0015] Figure 2 A schematic diagram showing a press mold 300 used to evaluate the ion conductivity of a solid electrolyte material.
[0016] Figure 3 This is a graph showing a Cole-Cole plot of the impedance measurement results of the solid electrolyte material of Example 1.
[0017] Figure 4 This is a graph showing the initial discharge characteristics of the battery of Example 1. DETAILED DESCRIPTION
[0018] Below, while referring to the attached Figure 1 Embodiments of the present invention will be described below.
[0019] (First Embodiment)
[0020] The solid electrolyte material of the first embodiment includes Li, Zr, Y, M, and X. M is at least one element selected from Nb and Ta. X is at least one element selected from Cl and Br. The solid electrolyte material of the first embodiment has high lithium ion conductivity.
[0021] The solid electrolyte material of the first embodiment can be used to obtain a battery having excellent charge and discharge characteristics. An example of such a battery is an all-solid secondary battery.
[0022] The solid electrolyte material of the first embodiment preferably does not contain sulfur. A solid electrolyte material that does not contain sulfur does not generate hydrogen sulfide even when exposed to the atmosphere, and therefore has excellent safety. When the sulfide solid electrolyte material disclosed in Patent Document 1 is exposed to the atmosphere, it should be noted that hydrogen sulfide may be generated.
[0023] The solid electrolyte material of the first embodiment may also be substantially composed of Li, Zr, Y, M and X. “The solid electrolyte material of the first embodiment is substantially composed of Li, Zr, Y, M and X” means that in the solid electrolyte material of the first embodiment, the total molar ratio of the amount of Li, Zr, Y, M and X relative to the total amount of all elements constituting the solid electrolyte material is 90% or more. As an example, the molar ratio may also be 95% or more. The solid electrolyte material of the first embodiment may also be composed only of Li, Zr, Y, M and X. This solid electrolyte material has high lithium ion conductivity.
[0024] The solid electrolyte material of the first embodiment may also contain an element that is inevitably mixed in. Examples of such an element are hydrogen, nitrogen, or oxygen. Such an element may be present in the raw material powder of the solid electrolyte material or in the atmosphere used to manufacture or store the solid electrolyte material.
[0025] The solid electrolyte material of the first embodiment may be a material represented by the following composition formula (1).
[0026] Li 6-(4+a-b)c (Zr 1-a-b Y b M a ) c X6 (1)
[0027] Here, the following mathematical expressions a>0, b>0, (a+b)<1, and 0<c<1.5 are satisfied.
[0028] The material represented by formula (1) has high lithium ion conductivity. Since the solid electrolyte material does not contain sulfur, it is excellent in safety.
[0029] In order to improve the lithium ion conductivity of the solid electrolyte material, the composition formula (1) may satisfy the mathematical formula: 0.01≤a≤0.4 or the mathematical formula: 0.05≤a≤0.4. In order to further improve the lithium ion conductivity of the solid electrolyte material, the composition formula may satisfy the mathematical formula: 0.01≤a≤0.2 or the mathematical formula: 0.05≤a≤0.2.
[0030] In order to improve the lithium ion conductivity of the solid electrolyte material, the composition formula (1) may satisfy the mathematical formula: 0.8≤c≤1.3. In order to further improve the ion conductivity of the solid electrolyte material, the composition formula (1) may satisfy the mathematical formula: 1.0≤c≤1.1.
[0031] The solid electrolyte material of the first embodiment may be crystalline or amorphous.
[0032] The shape of the solid electrolyte material of the first embodiment is not limited. Examples of the shape are needle-shaped, spherical or ellipsoidal. The solid electrolyte material of the first embodiment may also be particles. The solid electrolyte material of the first embodiment may also be formed in a manner having a pellet or a plate shape.
[0033] In order to further improve the ion conductivity and form a good dispersion state of other materials such as active materials, when the shape of the solid electrolyte material in the first embodiment is particulate (e.g., spherical), the solid electrolyte material in the first embodiment may also have a median particle size of 0.1 μm or more and 100 μm or less. It may also be preferred to have a median particle size of 0.5 μm or more and 10 μm or less. The median particle size refers to the particle size when the cumulative volume in the volume-based particle size distribution is equal to 50%. The volume-based particle size distribution can be measured using a laser diffraction scattering method or an image analysis device.
[0034] In order to form a good dispersion state of the solid electrolyte material and the active material, the solid electrolyte material of the first embodiment may have a smaller median particle size than the active material.
[0035] The solid electrolyte material of the first embodiment is produced, for example, by the following method.
[0036] Prepare halide raw material powders of a target composition ratio. 2.2 Zr 0.6 Y 0.3 Nb 0.1When preparing the raw material powder of LiCl, ZrCl, YCl and NbCl (i.e., raw material powders of four halides) in a molar ratio of LiCl: ZrCl: YCl: NbCl of 2.2: 0.6: 0.3: 0.1. Alternatively, the raw material powders may be mixed in a pre-adjusted molar ratio so that the composition changes that may occur during the synthesis process are offset.
[0037] The raw powders react with each other in a mechanochemical manner (i.e., by a mechanochemical grinding method) in a mixing device such as a planetary ball mill to obtain a reactant. The reactant may also be fired in a vacuum or in an inert atmosphere. Alternatively, the mixture of the raw powders may also be fired in a vacuum or in an inert atmosphere to obtain a reactant. The firing may also be performed at a temperature of 100° C. to 650° C. for more than 1 hour.
[0038] Through these methods, the solid electrolyte material of the first embodiment is obtained.
[0039] (Second Embodiment)
[0040] The second embodiment will be described below, and matters described in the first embodiment will be appropriately omitted.
[0041] The battery of the second embodiment includes a positive electrode, an electrolyte layer, and a negative electrode. The electrolyte layer is disposed between the positive electrode and the negative electrode.
[0042] At least one selected from the positive electrode, the electrolyte layer, and the negative electrode contains the solid electrolyte material of the first embodiment.
[0043] The battery of the second embodiment has excellent charge and discharge characteristics.
[0044] Figure 1 A cross-sectional view of a battery 1000 according to a second embodiment is shown.
[0045] The battery 1000 includes a positive electrode 201 , an electrolyte layer 202 , and a negative electrode 203 . The electrolyte layer 202 is disposed between the positive electrode 201 and the negative electrode 203 .
[0046] The positive electrode 201 includes positive electrode active material particles 204 and solid electrolyte particles 100 .
[0047] The electrolyte layer 202 contains an electrolyte material (eg, a solid electrolyte material).
[0048] The negative electrode 203 includes negative electrode active material particles 205 and solid electrolyte particles 100 .
[0049] The solid electrolyte particle 100 is a particle containing the solid electrolyte material of the first embodiment as a main component. The particle containing the solid electrolyte material of the first embodiment as a main component refers to a particle containing the solid electrolyte material of the first embodiment as the largest component. The solid electrolyte particle 100 may also be a particle composed of the solid electrolyte material of the first embodiment.
[0050] The positive electrode 201 contains a material capable of inserting and removing metal ions such as lithium ions. The positive electrode 201 contains, for example, a positive electrode active material (for example, positive electrode active material particles 204).
[0051] Examples of positive electrode active materials are lithium-containing transition metal oxides, transition metal fluorides, polyanionic materials, fluorinated polyanionic materials, transition metal sulfides, transition metal fluorides, transition metal oxysulfides or transition metal oxynitrides. Examples of lithium-containing transition metal oxides are Li(NiCoAl)O2 or LiCoO2.
[0052] The positive electrode active material particles 204 may also have a median particle size of 0.1 μm or more and 100 μm or less. When the positive electrode active material particles 204 have a median particle size of 0.1 μm or more, the positive electrode active material particles 204 and the solid electrolyte particles 100 can be well dispersed in the positive electrode 201. As a result, the battery has high charge and discharge characteristics. When the positive electrode active material particles 204 have a median particle size of 100 μm or less, the lithium diffusion rate in the positive electrode active material particles 204 is increased. As a result, the battery can operate at a high output power.
[0053] The positive electrode active material particles 204 may have a larger median diameter than the solid electrolyte particles 100. This allows the positive electrode active material particles 204 and the solid electrolyte particles 100 to be well dispersed.
[0054] From the viewpoint of battery energy density and output, in the positive electrode 201 , the ratio of the volume of the positive electrode active material particles 204 to the total volume of the positive electrode active material particles 204 and the volume of the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.
[0055] From the viewpoint of the energy density and output of the battery, the positive electrode 201 may have a thickness of 10 μm or more and 500 μm or less.
[0056] The electrolyte layer 202 contains an electrolyte material. The electrolyte material is, for example, a solid electrolyte material. The electrolyte layer 202 may also be a solid electrolyte layer. The solid electrolyte material contained in the electrolyte layer 202 may also be the solid electrolyte material of the first embodiment.
[0057] The electrolyte layer 202 may be composed only of the solid electrolyte material of the first embodiment.
[0058] The electrolyte layer 202 may also be composed only of a solid electrolyte material different from the solid electrolyte material of the first embodiment. Examples of solid electrolyte materials different from the solid electrolyte material of the first embodiment are Li2MgX'4, Li2FeX'4, Li(Al, Ga, In)X'4, Li3(Al, Ga, In)X'6, or LiI. Here, X' is at least one element selected from F, Cl, Br, and I.
[0059] Hereinafter, the solid electrolyte material of the first embodiment is referred to as a first solid electrolyte material. A solid electrolyte material different from the solid electrolyte material of the first embodiment is referred to as a second solid electrolyte material.
[0060] The electrolyte layer 202 may contain not only the first solid electrolyte material but also the second solid electrolyte material. In this case, the first solid electrolyte material and the second solid electrolyte material may be uniformly dispersed.
[0061] The layer composed of the first solid electrolyte material and the layer composed of the second solid electrolyte material may be stacked in sequence along the stacking direction of the battery 1000 .
[0062] The electrolyte layer 202 may have a thickness of 1 μm or more and 100 μm or less. When the electrolyte layer 202 has a thickness of 1 μm or more, the positive electrode 201 and the negative electrode 203 are less likely to short-circuit. When the electrolyte layer 202 has a thickness of 100 μm or less, the battery can operate at a high output.
[0063] The negative electrode 203 contains a material capable of inserting and removing metal ions such as lithium ions. The negative electrode 203 contains, for example, a negative electrode active material (for example, negative electrode active material particles 205).
[0064] Examples of negative electrode active materials are metal materials, carbon materials, oxides, nitrides, tin compounds or silicon compounds. The metal material may be a simple metal or an alloy. Examples of metal materials are lithium metal or lithium alloys. Examples of carbon materials are natural graphite, coke, graphitizable carbon, carbon fiber, spherical carbon, artificial graphite or amorphous carbon. From the viewpoint of capacity density, preferred examples of negative electrode active materials are silicon (i.e. Si), tin (i.e. Sn), silicon compounds or tin compounds.
[0065] The negative electrode active material particles 205 may also have a median particle size of 0.1 μm or more and 100 μm or less. When the negative electrode active material particles 205 have a median particle size of 0.1 μm or more, the negative electrode active material particles 205 and the solid electrolyte particles 100 can be well dispersed in the negative electrode 203. As a result, the charge and discharge characteristics of the battery are improved. When the negative electrode active material particles 205 have a median particle size of 100 μm or less, the lithium diffusion rate in the negative electrode active material particles 205 is increased. As a result, the battery can operate at a high output power.
[0066] The negative electrode active material particles 205 may have a larger median diameter than the solid electrolyte particles 100. This allows the negative electrode active material particles 205 and the solid electrolyte particles 100 to be well dispersed.
[0067] From the viewpoint of battery energy density and output, in the negative electrode 203 , the ratio of the volume of the negative electrode active material particles 205 to the total volume of the negative electrode active material particles 205 and the volume of the solid electrolyte particles 100 may be 0.30 or more and 0.95 or less.
[0068] From the viewpoint of the energy density and output of the battery, the negative electrode 203 may have a thickness of 10 μm or more and 500 μm or less.
[0069] At least one selected from the positive electrode 201 , the electrolyte layer 202 , and the negative electrode 203 may contain a second solid electrolyte material for the purpose of improving ion conductivity, chemical stability, and electrochemical stability.
[0070] The second solid electrolyte material may also be a sulfide solid electrolyte.
[0071] Examples of sulfide solid electrolytes are Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, Li2S-GeS2, Li 3.25 Ge 0.25 P 0.75 S4 or Li 10 GeP2S 12 .
[0072] The second solid electrolyte material may also be an oxide solid electrolyte.
[0073] Examples of oxide solid electrolytes are
[0074] (i) NASICON type solid electrolytes such as LiTi2(PO4)3 or its element substitution products,
[0075] (ii) Perovskite-type solid electrolytes such as (LaLi)TiO3,
[0076] (iii)Li 14 ZnGe4O 16 , LISICON type solid electrolytes such as Li4SiO4, LiGeO4 or their element substitution bodies,
[0077] (iv)Li7La3Zr2O 12 or its element substitution body, such as garnet-type solid electrolyte, or
[0078] (v) Li3PO4 or its N-substituted form.
[0079] The second solid electrolyte material may also be a halide solid electrolyte.
[0080] An example of a halide solid electrolyte is Li p Me q Y r The compound represented by Z6. Here, p+m′q+3r=6 and r>0 are satisfied. Me is at least one element selected from metal elements and semi-metal elements other than Li and Y. Z is at least one element selected from F, Cl, Br and I. The value of m′ represents the valence of Me.
[0081] “Semi-metallic element” refers to B, Si, Ge, As, Sb and Te.
[0082] “Metal elements” refer to all elements included in Groups 1 to 12 of the periodic table (except hydrogen) and all elements included in Groups 13 to 16 of the periodic table (except B, Si, Ge, As, Sb, Te, C, N, P, O, S and Se).
[0083] Me may be at least one element selected from the group consisting of Mg, Ca, Sr, Ba, Zn, Sc, Al, Ga, Bi, Zr, Hf, Ti, Sn, Ta, and Nb.
[0084] Examples of halide solid electrolytes are Li3YCl6 or Li3YBr6.
[0085] The second solid electrolyte material may also be an organic polymer solid electrolyte.
[0086] Examples of the organic polymer solid electrolyte include compounds of a polymer compound and a lithium salt.
[0087] The polymer compound may have an ethylene oxide structure. A polymer compound having an ethylene oxide structure can contain a large amount of lithium salt, and thus can further improve ion conductivity.
[0088] Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used.
[0089] At least one selected from the positive electrode 201, the electrolyte layer 202, and the negative electrode 203 may contain a non-aqueous electrolyte solution, a gel electrolyte, or an ionic liquid for the purpose of facilitating the transfer of lithium ions and improving the output characteristics of the battery.
[0090] The non-aqueous electrolyte comprises a non-aqueous solvent and a lithium salt dissolved in the non-aqueous solvent. Examples of non-aqueous solvents are cyclic carbonate solvents, chain carbonate solvents, cyclic ether solvents, chain ether solvents, cyclic ester solvents, chain ester solvents or fluorine solvents. Examples of cyclic carbonate solvents are ethylene carbonate, propylene carbonate or butylene carbonate. Examples of chain carbonate solvents are dimethyl carbonate, ethyl methyl carbonate or diethyl carbonate. Examples of cyclic ether solvents are tetrahydrofuran, 1,4-dioxane or 1,3-dioxolane. Examples of chain ether solvents are 1,2-dimethoxyethane or 1,2-diethoxyethane. Examples of cyclic ester solvents are γ-butyrolactone. Examples of chain ester solvents are methyl acetate. Examples of fluorine solvents are fluoroethylene carbonate, methyl fluoropropionate, fluorobenzene, ethyl fluoromethyl carbonate or dimethylene fluorocarbonate. A non-aqueous solvent selected from one of them may also be used alone. Alternatively, a mixture of two or more non-aqueous solvents selected from these may be used.
[0091] Examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiSO3CF3, LiN(SO2CF3)2, LiN(SO2C2F5)2, LiN(SO2CF3)(SO2C4F9) or LiC(SO2CF3)3. One lithium salt selected from these may be used alone. Alternatively, a mixture of two or more lithium salts selected from these may be used. The concentration of the lithium salt may be, for example, 0.5 mol / liter or more and 2 mol / liter or less.
[0092] As the gel electrolyte, a polymer material impregnated with a non-aqueous electrolyte can be used. Examples of the polymer material are polyethylene oxide, polyacrylonitrile, polyvinylidene fluoride, polymethyl methacrylate, or a polymer having an ethylene oxide bond.
[0093] Examples of cations contained in ionic liquids are
[0094] (i) aliphatic chain quaternary salts such as tetraalkylammonium or tetraalkylphosphonium,
[0095] (ii) an aliphatic cyclic ammonium such as a pyrrolidinium, morpholinium, imidazolinium, tetrahydropyrimidinium, piperazinium or piperidinium, or
[0096] (iii) Nitrogen-containing heterocyclic aromatic cations such as pyridinium and imidazolium cations.
[0097] An example of an anion contained in an ionic liquid is PF6 - 、BF4 - 、SbF6 - 、AsF6 - 、SO3CF3 - 、N(SO2CF3)2 - 、N(SO2C2F5)2 - 、N(SO2CF3)(SO2C4F9) - or C(SO2CF3)3 - .
[0098] The ionic liquid may also contain a lithium salt.
[0099] At least one selected from the positive electrode 201 , the electrolyte layer 202 , and the negative electrode 203 may contain a binder for the purpose of improving the adhesion between particles.
[0100] The example of binder is polyvinylidene fluoride, polytetrafluoroethylene, polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamide-imide, polyacrylonitrile, polyacrylic acid, polymethyl acrylate, polyethyl acrylate, polyhexyl acrylate, polymethacrylic acid, polymethyl methacrylate, polyethyl methacrylate, polyhexyl methacrylate, polyvinyl acetate, polyvinyl pyrrolidone, polyether, polyether sulfone, polyhexafluoropropylene, styrene-butadiene rubber or carboxymethyl cellulose. Copolymer can also be used as binder. The example of this binder is a copolymer of two or more materials selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid and hexadiene. A mixture selected from two or more of the above-mentioned materials can also be used as binder.
[0101] At least one selected from the positive electrode 201 and the negative electrode 203 may contain a conductive auxiliary agent for the purpose of improving electron conductivity.
[0102] Examples of conductive additives are
[0103] (i) Graphites such as natural graphite or artificial graphite,
[0104] (ii) Carbon black such as acetylene black or Ketjen black,
[0105] (iii) Conductive fibers such as carbon fibers or metal fibers,
[0106] (iv) Fluorinated carbon
[0107] (v) Metal powders such as aluminum,
[0108] (vi) Conductive metal whiskers such as zinc oxide or potassium titanate,
[0109] (vii) conductive metal oxides such as titanium oxide, or
[0110] (viii) Conductive polymer compounds such as polyaniline, polypyrrole or polythiophene.
[0111] For the purpose of cost reduction, the above-mentioned (i) or (ii) may be used as the conductive auxiliary agent.
[0112] Examples of the shape of the battery of the second embodiment are a coin type, a cylindrical type, a square type, a sheet type, a button type, a flat type, or a laminate type.
[0113] (Example)
[0114] Hereinafter, the present invention will be described in more detail with reference to Examples.
[0115] (Example 1)
[0116] [Production of solid electrolyte materials]
[0117] In an argon atmosphere with a dew point below -60°C (hereinafter referred to as "argon atmosphere"), LiCl, ZrCl4, YCl3 and NbCl5 are prepared as raw material powders in a molar ratio of LiCl: ZrCl4: YCl3: NbCl5 of 2.2: 0.6: 0.3: 0.1. These raw material powders are crushed and mixed in a mortar. In this way, a mixed powder is obtained. Using a planetary ball mill, the mixed powder is ground for 12 hours at 600 rpm. In this way, a powder of the solid electrolyte material of Example 1 is obtained. The solid electrolyte material of Example 1 has a Li 2.2 Zr 0.6 Y 0.3 Nb 0.1 The composition represented by Cl6.
[0118] The Li content per unit weight of the solid electrolyte material of Example 1 was measured by atomic absorption spectrometry. The Zr content, Y content and Nb content per unit weight of the solid electrolyte material of Example 1 were measured by high-frequency inductively coupled plasma emission spectrometry. Based on the contents of Li, Zr, Y and Nb obtained from these measurement results, the molar ratio of Li: Zr: Y: Nb was calculated. As a result, the solid electrolyte material of Example 1 had a Li: Zr: Y: Nb molar ratio of 2.2: 0.6: 0.3: 0.1.
[0119] [Evaluation of ion conductivity]
[0120] Figure 2 A schematic diagram showing a press mold 300 used to evaluate the ion conductivity of a solid electrolyte material.
[0121] The press forming die 300 includes a frame die 301, a punch lower portion 302, and a punch upper portion 303. The frame die 301 is formed of insulating polycarbonate. The punch lower portion 302 and the punch upper portion 303 are both formed of electron conductive stainless steel.
[0122] use Figure 2 The pressure forming die 300 shown was used to measure the impedance of the solid electrolyte material of Example 1 by the following method.
[0123] In a dry argon atmosphere, the solid electrolyte material ( Figure 2 The powder 101 equivalent to the solid electrolyte material in the embodiment 1 is filled in the press mold 300. In the press mold 300, a pressure of 300 MPa is applied to the solid electrolyte material of Example 1 using the punch lower part 302 and the punch upper part 303.
[0124] While maintaining the pressure applied, the punch was connected to a potentiostat (Versa STAT4, Princeton Applied Research) equipped with a frequency response analyzer via the punch lower portion 302 and the punch upper portion 303. The impedance of the solid electrolyte material of Example 1 was measured at room temperature by electrochemical impedance spectroscopy.
[0125] Figure 3 This is a graph showing a Cole-Cole plot of the impedance measurement results of the solid electrolyte material of Example 1.
[0126] Figure 3 In the example, the real value of the impedance at the measurement point where the absolute value of the phase of the complex impedance is the smallest is regarded as the resistance value of the solid electrolyte material of Example 1 to ion conduction. Figure 3 The arrow R SEUsing this resistance value, the ion conductivity was calculated based on the following mathematical formula (2).
[0127] σ=(R SE ×S / t) -1 (2)
[0128] Here, σ is the ion conductivity. S is the contact area between the solid electrolyte material and the upper portion 303 of the punch ( Figure 2 is equivalent to the area of the hollow part of the frame mold 301). SE is the resistance value of the solid electrolyte material in the impedance measurement. t is the thickness of the solid electrolyte material ( Figure 2 is equivalent to the thickness of the layer formed by the powder 101 of the solid electrolyte material).
[0129] The ionic conductivity of the solid electrolyte material of Example 1 measured at 22°C was 1.78×10 -3 S / cm.
[0130] [Battery production]
[0131] In a dry argon atmosphere, the solid electrolyte material of Example 1 and LiCoO 2 were prepared so as to have a volume ratio of 70:30. These materials were mixed in a mortar to obtain a mixture.
[0132] In an insulating cylinder having an inner diameter of 9.5 mm, the solid electrolyte material of Example 1 (100 mg), the above mixture (11.80 mg) and aluminum powder (14.7 mg) were stacked in order to obtain a stack. A pressure of 300 MPa was applied to the stack to form a solid electrolyte layer and a first electrode. The solid electrolyte layer had a thickness of 500 μm.
[0133] Next, metal In (thickness: 200 μm) was stacked on the solid electrolyte layer to obtain a stacked body. A pressure of 80 MPa was applied to the stacked body to form a second electrode. The first electrode was a positive electrode, and the second electrode was a negative electrode.
[0134] Next, a current collector made of stainless steel was attached to the first electrode and the second electrode, and a current collecting lead was attached to the current collector.
[0135] Finally, an insulating hoop is used to block the inside of the insulating tube from the outside atmosphere and seal it.
[0136] In this way, the battery of Example 1 was obtained.
[0137] [Charge and discharge test]
[0138] Figure 4 This is a graph showing the initial discharge characteristics of the battery of Example 1. The initial charge and discharge characteristics were measured by the following method.
[0139] The battery of Example 1 was placed in a constant temperature chamber at 25°C.
[0140] At 72μA / cm 2 The battery of Example 1 was charged at a current density of 0.05C to a voltage of 3.7V. This current density is equivalent to a 0.05C rate.
[0141] Next, at 72 μA / cm 2 The battery of Example 1 was discharged at a current density of 1.000 V to a voltage of 1.9 V. This current density is equivalent to a 0.05C rate.
[0142] As a result of the charge and discharge test, the battery of Example 1 had an initial discharge capacity of 0.77 mAh.
[0143] (Examples 2 to 38)
[0144] In Examples 2 to 36, LiCl, ZrCl4, YCl3 and MCl5 were prepared as raw material powders in such a manner as to achieve a molar ratio of LiCl:ZrCl4:YCl3:MCl5 of {6-(4+ab)c}:(1-ab)c:bc:ac.
[0145] In Examples 37 and 38, LiCl, LiBr, YBr3, MCl5 and ZrCl4 were prepared as raw material powders in a manner to achieve a molar ratio of LiCl:LiBr:YBr3:MCl5:ZrCl4 of 0.9:1.5:0.5:0.1:0.4.
[0146] Solid electrolyte materials of Examples 2 to 38 were obtained in the same manner as in Example 1 except for the above matters.
[0147] The ion conductivity of the solid electrolyte materials of Examples 2 to 38 was measured in the same manner as in Example 1. Table 1 shows the measurement results.
[0148] Using the solid electrolyte materials of Examples 2 to 38, batteries were obtained in the same manner as in Example 1. As in Example 1, the batteries of Examples 2 to 38 had good charge and discharge characteristics.
[0149] Table 1 shows the element types of M and X and the values of a, b, and c in each of Examples 2 to 38.
[0150] (Comparative Example 1)
[0151] In Comparative Example 1, LiCl and YCl 3 were prepared as raw material powders so as to achieve a LiCl:YCl 3 molar ratio of 3: 1. A solid electrolyte material of Comparative Example 1 was obtained in the same manner as in Example 1 except for the above matters.
[0152] The ion conductivity of the solid electrolyte material of Comparative Example 1 was measured in the same manner as in Example 1. As a result, the ion conductivity of the solid electrolyte material of Comparative Example 1 at 22° C. was 5.70×10 -4 S / cm.
[0153] [Table 1]
[0154]
[0155] (Inspection)
[0156] Table 1 shows that the solid electrolyte materials of Examples 1 to 38 have a strength of 5.8×10 -4 High ion conductivity of more than S / cm.
[0157] Table 1 shows that when the value of a is greater than 0.05 and less than 0.4, the solid electrolyte material has high ion conductivity. Comparing Examples 4, 9 and 14 with Example 16, it is shown that when the value of a is greater than 0.05 and less than 0.2, the ion conductivity is further improved. Even if the value of a is less than 0.05, it can be considered that the solid electrolyte material has high ion conductivity. The value of a can also be, for example, greater than 0.01 and less than 0.3.
[0158] Table 1 shows that when the value of c is 0.8 or more and 1.3 or less, the solid electrolyte material has high ion conductivity. Comparison of Examples 9, 22, 24 and 25 with Examples 19, 20, 26 and 27 shows that when the value of c is 1.0 or more and 1.1 or less, the ion conductivity is further improved.
[0159] In all of Examples 1 to 38, the batteries were charged and discharged at room temperature.
[0160] Since the solid electrolyte materials of Examples 1 to 38 do not contain sulfur, hydrogen sulfide will not be generated.
[0161] As described above, the solid electrolyte material of the present invention is suitable for providing a battery having high lithium ion conductivity and capable of good charge and discharge.
[0162] Industrial Applicability
[0163] The solid electrolyte material of the present invention can be applied to, for example, a battery (eg, an all-solid lithium ion secondary battery).
[0164] Explanation of symbols:
[0165] 100 Solid Electrolyte Particles
[0166] 101 Powder of solid electrolyte material
[0167] 201 Positive electrode
[0168] 202 electrolyte layer
[0169] 203 Negative electrode
[0170] 204 Positive electrode active material particles
[0171] 205 Negative electrode active material particles
[0172] 300 Pressurized Forming Die
[0173] 301 frame mold
[0174] 302 punch lower part
[0175] 303 Punch upper part
[0176] 1000 Batteries
Claims
1. A solid electrolyte material represented by the following composition formula (1): Li 6-(4+a-b)c (Zr 1-a-b Y b M a ) c X6(1) Here, the following mathematical formula is satisfied a>0, b>0, (a+b)<1, and 0<c<1.5, M is at least one element selected from Nb and Ta, and X is at least one element selected from Cl and Br.
2. The solid electrolyte material according to claim 1, wherein Satisfies the mathematical formula: 0.01≤a≤0.
4.
3. The solid electrolyte material according to claim 2, wherein Satisfies the mathematical formula: 0.01≤a≤0.
2.
4. The solid electrolyte material according to any one of claims 1 to 3, wherein Satisfies the mathematical formula: 0.8≤c≤1.
3.
5. The solid electrolyte material according to claim 4, wherein Satisfies the mathematical formula: 1.0≤c≤1.
1.
6. A battery having positive electrode, Negative electrode, and an electrolyte layer disposed between the positive electrode and the negative electrode, At least one selected from the positive electrode, the negative electrode, and the electrolyte layer contains the solid electrolyte material according to any one of claims 1 to 5.