Photosensitive resin composition, photosensitive resin sheet, cured film and method for producing the same, organic EL display device and electronic component

By using a combination of a polyimide precursor, a phenolic compound with an electron-withdrawing group, and a photosensitive compound in an organic EL display device, the problems of low imidization rate and poor pattern processability in the prior art have been solved and achieved. High imidization rate and long-term reliability below 200°C.

CN113544585BActive Publication Date: 2024-10-22TORAY INDUSTRIES INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202080018551.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-14
Filing Date
2020-03-04
Publication Date
2024-10-22
Estimated Expiration
2040-03-04

AI Technical Summary

Technical Problem

The existing technology is difficult to achieve a high imidization rate at temperatures below 200°C, and when strong acid or strong base is used as an imidization accelerator, it will cause the photosensitive resin composition to decompose and pattern processability to deteriorate, making it unable to meet the requirements of organic EL. Display devices require high reliability.

Method used

A photosensitive resin composition containing a polyimide precursor, a phenolic compound with an electron-withdrawing group, and a photosensitive compound is used. Through the combination of specific structural units of the polyimide precursor and the phenolic compound, the temperature below 200°C is achieved. High imidization rate and good pattern processability.

Benefits of technology

A high imidization rate is achieved at temperatures below 200°C, improving the long-term reliability and pattern processability of organic EL display devices, and meeting reliability requirements under accelerated conditions such as high temperature, high humidity, and light irradiation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113544585B_ABST
    Figure CN113544585B_ABST
Patent Text Reader

Abstract

The object of the present invention is to provide a photosensitive resin composition having a good imidization rate even when fired at a temperature below 200°C, high pattern processability, and high long-term reliability when a cured film is used in an organic EL display device. In order to solve the above-mentioned problems, the photosensitive resin composition of the present invention contains a polyimide precursor (a), a phenol compound (b) having an electron-withdrawing group, and a photosensitive compound (c), wherein the polyimide precursor (a) has a residue derived from a diamine having an ionization potential of less than 7.1 eV.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a photosensitive resin composition which can be suitably used for a planarization layer, an insulating layer, an interlayer insulating layer, a surface protective layer, etc. of an organic EL display device, and an electronic component. Background Art

[0002] In display devices with thin displays such as smartphones, tablet PCs, and televisions, a large number of products using organic electroluminescent (hereinafter, "organic EL") display devices have been developed. Generally speaking, an organic EL display device has a driving circuit, a planarization layer, a first electrode, an insulating layer, a light-emitting layer, and a second electrode on a substrate, and can emit light by applying a voltage between the opposing first electrode and the second electrode. Among them, as a material for a planarization layer and a material for an insulating layer, a photosensitive resin composition that can form a pattern by ultraviolet irradiation is generally used. The photosensitive resin composition in which a polyimide-based resin is used is suitable for use in an organic EL display device that can provide high reliability because the resin has high heat resistance and generates less gas components from the cured film.

[0003] Usually, a film of a polyimide precursor is subjected to thermal dehydration and cyclic closure to obtain a film having excellent heat resistance and mechanical properties. In this case, a high temperature sintering at 300°C or above is usually required. However, an organic EL display device such as a white OLED (organic light emitting diode) + color filter requires a low temperature curing process in the post-process due to the low heat resistance of the color filter. Furthermore, polyimide, polyphenylene sulfide, and polyimide precursors are preferably used as the precursors of polyimide. Polyimide resins are also widely used as surface protection layers and interlayer insulation layers of semiconductor elements. However, for example, MRAM (Magnetoresistive Random Access Memory), which is expected to be the next generation of memory, and sealing resins are not resistant to high temperatures. Therefore, in order to be used for insulating layers, planarization layers, and protective layers of such elements, it is required that the imidization rate is good even when cured by firing at a low temperature below 200°C, and that polyimide resins with properties comparable to those obtained when conventional materials are fired at a high temperature of around 300°C can be obtained.

[0004] As a technology for lowering the temperature of imidization, a negative photosensitive resin composition comprising a polyimide precursor having a weight average molecular weight of 3000 or more and less than 16000 and a photopolymerization initiator in which the carboxyl group of the polyamic acid is substituted with a specific structure is disclosed (see Patent Document 1). In addition, in addition to the technology of adding a catalytic amount of p-toluenesulfonic acid, which is a well-known strong acid, to a polyamic acid solution, a technology of adding a catalytic amount of 1,4-diazabicyclo[2.2.2]octane and 1,8-diazabicyclo[5.4.0]-7-undecene as a strong base to a polyamic acid solution is also disclosed (see Non-Patent Document 1). According to the method of using a strong acid or a strong base as an imidization accelerator in this way, a polyimide with a high imidization rate can be obtained at a temperature below 200°C.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: International Publication No. 2018 / 037997

[0008] Non-patent literature

[0009] Non-patent document 1: M. Ueda et al. Chem. Lett, 33(9), p.1156-1157, 2004 Summary of the invention

[0010] Problems to be solved by the invention

[0011] However, the applicant has conducted research and found that the imidization rate of the cured film of the composition described in Patent Document 1 fired at 200°C cannot be said to be sufficient. In addition, it was found that when the method of using a strong acid or a strong base described in Non-Patent Document 1 as an imidization accelerator is applied to a photosensitive resin composition, there are problems such as decomposition of the photosensitive compound due to the added imidization accelerator and deterioration of pattern processability due to imidization caused by heating of the solvent drying process (prebaking) of the photosensitive resin composition used to form a photosensitive resin film. Therefore, a material is required that does not undergo imidization during prebaking and is well imidized in the firing process of the photosensitive resin film after pattern processing.

[0012] In addition, the requirements for high reliability of organic EL display devices are becoming more stringent year by year. For materials for planarization layers and insulating layers, it is required to maintain high film properties even after reliability tests under accelerated conditions such as high temperature, high humidity, and light irradiation, and to obtain materials with properties that are not inferior to those when fired at high temperatures even when fired at low temperatures.

[0013] Therefore, an object of the present invention is to provide a photosensitive resin composition having a good imidization rate even when fired at a temperature of 200° C. or lower, high pattern processability, and high long-term reliability when a cured film is used in an organic EL display device.

[0014] Methods for solving problems

[0015] In order to solve the above problems, the photosensitive resin composition of the present invention contains a polyimide precursor (a) having a residue derived from a diamine having an ionization potential of less than 7.1 eV, a phenol compound (b) having an electron-withdrawing group, and a photosensitive compound (c).

[0016] Effects of the Invention

[0017] The photosensitive resin composition of the present invention has a good imidization rate even when fired at a temperature of 200° C. or lower, has high pattern processability, and has high long-term reliability when a cured film is used in an organic EL display device. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a diagram showing a reaction scheme of a dissociation reaction of an acid (proton).

[0019] Figure 2 This is a cross-sectional view of an example of a TFT substrate.

[0020] Figure 3 This is an enlarged cross-sectional view of an example of a pad portion of a semiconductor device having a bump.

[0021] Figure 4 This is a schematic diagram showing an example of a method for manufacturing a semiconductor device having bumps.

[0022] Figure 5 This is a schematic diagram of the steps for producing the organic EL display device in the example. DETAILED DESCRIPTION

[0023] Embodiments of the present invention will be described in detail.

[0024] The photosensitive resin composition of the present invention contains a polyimide precursor (a) having a residue derived from a diamine having an ionization potential of less than 7.1 eV, a phenol compound (b) having an electron-withdrawing group, and a photosensitive compound (c).

[0025] <Polyimide precursor (a)>

[0026] The photosensitive resin composition of the present invention contains a polyimide precursor (a). The polyimide precursor (a) has a residue derived from a diamine having an ionization potential of less than 7.1 eV. By containing a polyimide precursor (a) and a phenol compound (b) having an electron-withdrawing group described later, a cured film with a high imidization rate can be obtained even when calcined at a temperature below 200°C. In addition, the long-term reliability of the cured film of the present invention described later as a planarization layer and / or insulating layer of an organic EL display device can be improved. The so-called polyimide precursor refers to a resin that is converted into a polyimide by heat treatment or chemical treatment. As a polyimide precursor, for example, polyamic acid, polyamic acid ester, etc. can be cited.

[0027] In the present invention, the polyimide precursor preferably has alkali solubility. The so-called alkali solubility in the present invention means that a solution of the polyimide precursor (a) dissolved in γ-butyrolactone is coated on a silicon wafer, pre-baked at 120°C for 4 minutes to form a pre-baked film with a film thickness of 10 μm±0.5 μm, and the pre-baked film is immersed in a 2.38 mass % tetramethylammonium hydroxide aqueous solution at 23±1°C for 1 minute, and then rinsed with pure water, and the dissolution rate obtained by the reduction in film thickness at this time is 50 nm / minute or more.

[0028] In order to impart alkali solubility, the polyimide precursor (a) in the present invention preferably has a hydroxyl group and / or an acidic group in the structural unit of the polyimide precursor (a) and / or at the main chain terminal thereof. Examples of the acidic group include a carboxyl group, a phenolic hydroxyl group, and a sulfonic acid group.

[0029] The polyimide precursor (a) preferably has fluorine atoms. Fluorine atoms can impart hydrophobicity to the cured film.

[0030] The polyimide precursor (a) in the present invention preferably has a structural unit represented by the following general formula (3).

[0031]

[0032] In the general formula (3), X represents a 4- to 7-valent organic group, and Y represents a 2- to 11-valent organic group. 11 and R 13 Each independently represents a hydroxyl group or a sulfonic acid group, and each may be a single group or a mixture of different groups. 12 and R 14 Each independently represents a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms. t and w each independently represent an integer of 0 to 3, and v represents an integer of 0 to 6.

[0033] The polyimide precursor (a) preferably has 5 to 100,000 structural units represented by the general formula (3). In addition to the structural units represented by the general formula (3), the polyimide precursor (a) may also have other structural units. In this case, the polyimide precursor (a) preferably has structural units represented by the general formula (3) in an amount of 50 mol% or more of all structural units.

[0034] In the above general formula (3), X(R 11 ) t (COOR 12 )2 represents an acid residue. X is a 4- to 7-valent organic group, and preferably an organic group having 5 to 40 carbon atoms and containing an aromatic ring or a cyclic aliphatic group.

[0035] Examples of the acid include pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4'-biphenyltetracarboxylic acid, 2,2',3,3'-biphenyltetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2',3,3'-benzophenonetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, 2,2-bis(2,3-dicarboxyphenyl)hexafluoropropane, 1,1-bis(3,4-dicarboxyphenyl)ethane, 1,1-bis(2,3-dicarboxyphenyl)ethane, and 1,1-bis(2,3-dicarboxyphenyl)ethane. Tetracarboxylic acids such as bis(3,4-dicarboxyphenyl)ethane, bis(2,3-dicarboxyphenyl)methane, bis(3,4-dicarboxyphenyl)ether, 1,2,5,6-naphthalenetetracarboxylic acid, 2,3,6,7-naphthalenetetracarboxylic acid, 2,3,5,6-pyridinetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid and aromatic tetracarboxylic acids of the structures shown below, aliphatic tetracarboxylic acids such as butanetetracarboxylic acid, and aliphatic tetracarboxylic acids containing a cyclic aliphatic group such as 1,2,3,4-cyclopentanetetracarboxylic acid, etc., etc., can be used in combination of two or more.

[0036]

[0037] R 20 represents an oxygen atom, C(CF3)2 or C(CH3)2. 21 and R 22 Each independently represents a hydrogen atom or a hydroxyl group.

[0038] Among the above acids, in the case of tetracarboxylic acids, two carboxyl groups correspond to (COOR 12 )2.

[0039] These acids may be used directly or in the form of anhydrides, active esters, or active amides. Examples of active esters include N-hydroxysuccinimide ester compounds obtained by reacting the carboxyl group of an acid with N-hydroxysuccinimide, and examples of active amides include N-acylimidazole compounds obtained by reacting the carboxyl group of an acid with N,N'-carbonyldiimidazole.

[0040] Specific examples of the acid dianhydride include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,3,3',4'-biphenyltetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)propane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, and bis(2,3-dicarboxyphenyl) Aromatic tetracarboxylic acid dianhydrides such as methane dianhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, 1,2,5,6-naphthalenetetracarboxylic acid dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 9,9-bis{4-(3,4-dicarboxyphenoxy)phenyl}fluorene dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 2,3,5,6-pyridinetetracarboxylic acid dianhydride, 3,4,9,10-perylenetetracarboxylic acid dianhydride, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride, and acid dianhydrides of the following structures, aliphatic tetracarboxylic acid dianhydrides such as butanetetracarboxylic acid dianhydride, and aliphatic tetracarboxylic acid dianhydrides containing cyclic aliphatic groups such as 1,2,3,4-cyclopentanetetracarboxylic acid dianhydride. Two or more of these may be used.

[0041]

[0042] R 20 represents an oxygen atom, C(CF3)2 or C(CH3)2. 21 and R 22 Each independently represents a hydrogen atom or a hydroxyl group.

[0043] Y(R 13 ) v (COOR 14 ) w represents a residue of a diamine. Y is a 2- to 11-valent organic group. The polyimide precursor (a) in the present invention has a residue derived from a diamine having an ionization potential (hereinafter, sometimes described as "Ip") of less than 7.1 eV.

[0044] In the present invention, by using a polyimide precursor (a) having a residue derived from a diamine having an ionization potential of less than 7.1 eV, the mechanism by which a cured film showing a high imidization rate can be obtained even when calcined at a temperature below 200°C is uncertain, but, for example, it can be inferred as follows. That is, the imidization reaction of the polyimide precursor (a) is carried out by a nucleophilic attack of the nitrogen atom of the residue derived from the diamine on the carbonyl carbon of the residue derived from the acid dianhydride. The ionization potential is low, that is, the nucleophilicity of the nitrogen atom of the polyimide precursor having a residue derived from an electron-rich diamine is high. Therefore, it can be inferred that the reactivity of the imidization reaction is high, and a cured film with a high imidization rate can be obtained even at a temperature below 200°C.

[0045] Examples of diamines having an ionization potential of less than 7.1 eV include 2,7-diaminofluorene (Ip 6.48 eV, literature value), o-tolidine (Ip 6.58 eV, literature value), benzidine (Ip 6.73 eV, literature value), 4,4'-diaminodiphenyl ether (Ip 6.78 eV, literature value), 1,4-bis(4-aminophenoxy)benzene (Ip 6.80 eV, literature value), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (Ip 6.6. 84eV, calculated value), 9,9-bis(4-aminophenyl)fluorene (Ip 6.88eV, literature value), 4,4'-diaminodiphenylmethane (Ip 6.94eV, literature value), p-phenylenediamine (Ip 7.03eV, literature value), 3,3'-diaminodiphenylmethane (Ip 7.08eV, literature value), m-tolidine (Ip 7.08eV, literature value), 1,3-bis(4-aminophenoxy)benzene (Ip 7.08eV, calculated value), etc. Two or more of these may be used.

[0046] From the viewpoint of being able to more easily achieve a high imidization rate even when calcined at a temperature of 200° C. or lower, the ionization potential is preferably less than 7.0 eV, more preferably 6.9 eV, and even more preferably 6.8 eV. The lower limit of the ionization potential is not particularly limited, but is approximately 6.0 eV.

[0047] Among them, from the viewpoint of improving sensitivity, the residue derived from a diamine having an ionization potential of less than 7.1 eV preferably has an ether bond. Among them, the diamine having an ionization potential of less than 7.1 eV more preferably includes one or more diamines selected from 4,4'-diaminodiphenyl ether (Ip 6.78 eV, literature value), 1,4-bis(4-aminophenoxy)benzene (Ip 6.80 eV, literature value), 2,2-bis[4-(4-aminophenoxy)phenyl]propane (Ip 6.84 eV, calculated value), and 1,3-bis(4-aminophenoxy)benzene (Ip 7.08 eV, calculated value).

[0048] In addition, the Ip in the present invention uses the literature value described in "New Edition of Latest Polyimide" ("Newly Edited Latest Polyimide" (page 102, written by Shinji Ando). In addition, the value (calculated value) obtained by calculation using Gaussian09, using B3LYP as the universal function, and using 6-311G(d) (structure optimization calculation) and 6-311++G(d, p) (energy calculation) as the basis function system in the same manner as the literature value was used for the Ip without description.

[0049] In addition, the polyimide precursor (a) used in the present invention may contain a diamine residue having an ionization potential of 7.1 eV or more, in addition to a diamine residue having an ionization potential of less than 7.1 eV, within the range that does not reduce the above-mentioned characteristics. In the case of containing a diamine residue having an ionization potential of 7.1 eV or more, from the viewpoint that it is easier to achieve a high imidization rate even when calcined at a temperature below 200°C, the content of the residue derived from the diamine having an ionization potential of less than 7.1 eV in 100 mol% of the diamine residues constituting the polyimide precursor (a) is preferably 5 mol% or more, more preferably 10 mol% or more, and more preferably 20 mol% or more. In addition, from the viewpoint of further improving the sensitivity, it is preferably 50 mol% or less, and more preferably 40 mol% or less.

[0050] Examples of diamines having an ionization potential of 7.1 eV or more include 3,3'-diaminodiphenyl ether (Ip 7.12 eV, literature value), 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane (Ip 7.15 eV, calculated value), 1,3-bis(3-aminophenoxy)benzene (Ip 7.18 eV, literature value), 9,9-bis(3-amino-4-hydroxyphenyl)fluorene (Ip 7.28 eV, calculated value). )、3,3'-bis(trifluoromethyl)benzidine (Ip7.30eV, literature value), 2,2-bis(3-amino-4-methylphenyl)hexafluoropropane (Ip7.32eV, calculated value), m-phenylenediamine (Ip7.39eV, literature value), 2,2-bis(4-aminophenyl)hexafluoropropane (Ip7.41eV, calculated value), 4,4'-diaminodiphenyl sulfone (Ip7.50eV, literature value), 2, 2'-bis(trifluoromethyl)benzidine (Ip 7.55 eV, literature value), 3,3'-diaminodiphenyl sulfone (Ip 7.68 eV, literature value), 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (Ip 7.88 eV, calculated value), bis(3-amino-4-hydroxyphenyl) sulfone (Ip 8.02 eV, calculated value), at least part of the hydrogen atoms of these aromatic rings are substituted with alkyl or halogen atoms Aromatic diamines such as compounds of, 4,4'-diaminodicyclohexylmethane (Ip8.15eV, literature value), aliphatic diamines containing cyclic aliphatic groups such as 1,4-cyclohexanediamine (Ip8.61eV, literature value), diamines containing silicon atoms such as 1,3-bis(3-aminopropyl)tetramethyldisiloxane (Ip8.03eV, calculated value), and diamines of the structure shown below (Ip7.16eV, calculated value), etc. Two or more of them may be used.

[0051]

[0052] These diamines may be used as they are, or in the form of a diisocyanate compound obtained by, for example, reacting an amino group of a diamine with phosgene, or in the form of a trimethylsilylated diamine obtained by reacting an amino group of a diamine with chlorotrimethylsilane.

[0053] Furthermore, by blocking the terminals of these resins with monoamine, acid anhydride, acid chloride, monocarboxylic acid, or active ester compounds having an acidic group, a resin having an acidic group at the terminal of the main chain can be obtained.

[0054] Preferred examples of monoamines having an acidic group include 2-aminobenzoic acid, 3-aminobenzoic acid, 4-aminobenzoic acid, 4-aminosalicylic acid, 5-aminosalicylic acid, 6-aminosalicylic acid, 3-amino-4,6-dihydroxypyrimidine, 2-aminophenol, 3-aminophenol, 4-aminophenol, 2-aminothiophenol, 3-aminothiophenol, 4-aminothiophenol, etc. Two or more of these may be used.

[0055] Preferred examples of the acid anhydride include phthalic anhydride, maleic anhydride, nadic anhydride, cyclohexanedicarboxylic anhydride, 3-hydroxyphthalic anhydride, etc. Two or more of these may be used.

[0056] Preferred examples of the monocarboxylic acid include 3-carboxyphenol, 4-carboxyphenol, 3-carboxythiophenol, 4-carboxythiophenol, etc. Two or more of these may be used.

[0057] Preferred examples of the acid chloride include monoacyl chloride compounds in which the carboxyl group of the above-mentioned monocarboxylic acid is chlorinated, monoacyl chloride compounds in which only one carboxyl group of dicarboxylic acids such as terephthalic acid, phthalic acid, maleic acid, cyclohexanedicarboxylic acid, 1,5-dicarboxynaphthalene, 1,6-dicarboxynaphthalene, 1,7-dicarboxynaphthalene, and 2,6-dicarboxynaphthalene is chlorinated, etc. Two or more of these may be used.

[0058] Preferred examples of the active ester compound include reaction products of the above-mentioned monoacyl chloride compound with N-hydroxybenzotriazole or N-hydroxy-5-norbornene-2,3-dicarboximide, etc. Two or more of these may be used.

[0059] The polyimide precursor (a) in the present invention can be synthesized by a known method.

[0060] As a manufacturing method of the polyamic acid which is a polyimide precursor, the method etc. which make tetracarboxylic dianhydride and a diamine compound react in a solvent at low temperature are mentioned, for example.

[0061] Similarly, as a method for manufacturing polyamic acid ester as a polyimide precursor, in addition to the above-mentioned method of reacting polyamic acid with an esterifying agent, it is also possible to cite: a method of obtaining a diester by tetracarboxylic dianhydride and alcohol, and then reacting with an amine in a solvent in the presence of a condensing agent; a method of obtaining a diester by tetracarboxylic dianhydride and alcohol, and then chlorinating the remaining dicarboxylic acid to react with an amine in a solvent, etc. From the viewpoint of ease of synthesis, it is preferred to include a process of reacting polyamic acid with an esterifying agent. As an esterifying agent, there is no particular limitation, and a known method can be applied, but from the perspective of the ease of refining the resulting resin, N, N-dimethylformamide dialkyl acetal is preferably used.

[0062] The polymerization solvent is not particularly limited, and examples thereof include alkylene glycol monoalkyl ethers such as ethylene glycol monomethyl ether and propylene glycol monomethyl ether, alkyl acetates such as propyl acetate, butyl acetate, and isobutyl acetate, ketones such as methyl isobutyl ketone and methyl propyl ketone, alcohols such as butanol and isobutyl alcohol, ethyl lactate, butyl lactate, dipropylene glycol dimethyl ether, diethylene glycol dimethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol diethyl ether, 3-methoxybutyl acetate, ethylene glycol monoethyl ether acetate, γ-butyrolactone, N-methyl-2-pyrrolidone, diacetone alcohol, N-cyclohexyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, propylene glycol monomethyl Ether acetate, N,N-dimethyl isobutyric acid amide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, 1,3-dimethyl-2-imidazolidinone, N,N-dimethylpropylene urea, delta valerolactone, 2-phenoxyethanol, 2-pyrrolidone, 2-methyl-1,3-propanediol, diethylene glycol butyl ether, triacetin, butyl benzoate, cyclohexylbenzene, bicyclohexane, o-nitroanisole, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, N-(2-hydroxyethyl)-2-pyrrolidone, N,N-dimethylpropaneamide, N,N-dimethyl isobutylamide, N,N,N',N'-tetramethylurea, 3-methyl-2- Oxazolidinone, etc.

[0063] <Phenol compound having an electron-withdrawing group (b)>

[0064] The photosensitive resin composition of the present invention contains a phenol compound (b) having an electron-withdrawing group (hereinafter, sometimes simply described as "phenol compound (b)"). By containing the above-mentioned polyimide precursor (a) and the phenol compound (b), a cured film with a high imidization rate can be obtained even when calcined at a temperature of 200° C. or less, and the long-term reliability of the cured film of the present invention described later when used as a planarization layer and / or an insulating layer of an organic EL display device can be improved.

[0065] The electron-withdrawing group is the Hammett substituent constant σ defined in "Chemical Handbook Basics Revised 5th Edition" II-379 to II-380 (edited by the Chemical Society of Japan, published by Maruzen Co., Ltd.) p 0 The phenol compound (b) having an electron-withdrawing group has an electron-withdrawing group in the molecule, thereby increasing the acidity of the phenolic hydroxyl group and acting as an acid catalyst to promote imidization of the polyimide precursor (a).

[0066] As specific examples of electron-withdrawing groups, sulfonyl, sulfonic acid, sulfonic acid ester, sulfonic acid amide, sulfonic acid imide, carboxyl, carbonyl, carboxylate, cyano, halogen, trifluoromethyl, nitro, etc. can be cited, but it is not limited to this, as long as it is any known electron-withdrawing group. Among them, from the viewpoint of further promoting the imidization of the polyimide precursor (a), carbonyl, trifluoromethyl, halogen, sulfonyl are preferred, and trifluoromethyl and sulfonyl are particularly preferred.

[0067] As a preferred form of the phenol compound (b), the phenol compound (b) preferably contains a compound (b1) having a phenolic hydroxyl group whose acid dissociation constant (pKa) is 11.0 or less as determined by quantum chemical calculation based on density functional theory. The compound (b1) having a phenolic hydroxyl group whose pKa is 11.0 or less has a higher acidity of the phenolic hydroxyl group than the acidity of unsubstituted phenol (pKa=12.2) determined by the calculation. On the other hand, since the acidity is not as high as that of the sulfonic acid compound (pKa<0) known as an imidization accelerator, imidization is not promoted in the solvent drying step (prebaking) of the photosensitive resin composition described later, and the effect of promoting imidization in the firing step of the photosensitive resin film after pattern processing can be improved. The lower limit of pKa is not particularly limited, but is about 1.0.

[0068] The acid dissociation constant (pKa) is the logarithm of the reciprocal of the acid dissociation constant. In the case of multi-stage dissociation, the first-stage dissociation constant (i.e., pKa1) is used. In addition, as the acid dissociation constant (pKa) in the present invention, the acid dissociation constant calculated by quantum chemical calculation based on the density functional method (DFT method) is used. In such quantum chemical calculations, the values ​​calculated by calculation using an electronic computer, Gaussian09, B3LYP as a functional, and 6-311G(d) (structure optimization calculation) and 6-311++G(d, p) (energy calculation and vibration analysis) as a basis function are used. In addition, in such quantum chemical calculations, Figure 1 The calculation of thermodynamic quantities shown in the reaction scheme of the acid dissociation reaction (proton dissociation reaction) of the acid (acid represented by the formula: HA) described above. Figure 1 In the formula, HA represents acid, A - The ion representing the acid, H + represents a hydrogen ion (proton). In addition, Figure 1 In the formula: HA(aq)→H + (aq)+A - (aq) represents the dissociation reaction of protons in water, formula: HA(g)→H + (g)+A - (g) represents the dissociation reaction of protons in the gas phase.

[0069] First, using Gaussian09, the Gibbs free energy G of HA in the gas phase was calculated: 0 gas After HA was added, the Gibbs free energy difference ΔG between HA in the gas phase and in water was calculated using the SMD solvation model. * solv (HA). In addition, in the SMD solvation model, the molecular cavity is assigned to RADII = UAHF. The same operation is performed to obtain A - The Gibbs free energy in the gas phase G 0 gas (A - ) and then calculate A - The difference in Gibbs free energy between the gas phase and water is ΔG * solv (A - ). Then, using the obtained value, pKa is calculated based on mathematical formulas (1) to (4). In addition, regarding this calculation, H + Gibbs free energy G 0 gas (H + ) is set to -6.275 kcal / mol, H + The difference in Gibbs free energy between the gas phase and water is ΔG * solv (H + ) is set to -1112.5 kJ / mol, the gas constant (R) is set to 8.314 J / (K·mol) = 0.0821 atm·L / (K·mol), and the absolute temperature (T) is set to 298.15 K.

[0070]

[0071]

[0072]

[0073]

[0074] Specific examples of the compound (b1) having a phenolic hydroxyl group and having a pKa of 11.0 or less include bisphenol S (pKa=9.8), bisphenol AF (pKa=10.8), and 4-(trifluoromethyl)phenol (pKa=10.5).

[0075] As another preferred embodiment of the phenol compound (b), the phenol compound (b) preferably contains a compound (b2) represented by the general formula (1).

[0076]

[0077] In the general formula (1), A represents a divalent group selected from the structures represented by the general formula (2), a and b each independently represent an integer of 0 to 3, and a+b is an integer of 2 to 4. 1 and R 2 Each independently represents a halogen atom or a monovalent organic group having 1 to 20 carbon atoms substituted with a halogen atom.

[0078] The compound (b2) represented by the general formula (1) has high heat resistance and has two or more phenolic hydroxyl groups, and therefore can further enhance the effect of improving the long-term reliability when the cured film of the present invention described below is used as a planarizing layer and / or insulating layer of an organic EL display device.

[0079] Specific examples of the compound represented by the general formula (1) include bisphenol S (pKa=9.8), bisphenol AF (pKa=10.8), and 4,4′-dihydroxybenzophenone (pKa=11.3).

[0080] The content of the phenol compound (b) is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and further preferably 10 parts by mass or more relative to 100 parts by mass of the polyimide precursor (a). By being in such a range, it is easy to achieve a high imidization rate even when calcined at a temperature below 200°C. In addition, the content of the phenol compound (b) is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and further preferably 30 parts by mass or less. By being in such a range, it is easy to suppress the reduction of the residual film rate after alkali development.

[0081] <Photosensitive compound (c)>

[0082] The photosensitive resin composition of the present invention contains a photosensitive compound (c). Examples of the photosensitive compound (c) include a photoacid generator (c1) and a photopolymerization initiator (c2). The photoacid generator (c1) is a compound that generates an acid by light irradiation, and the photopolymerization initiator (c2) is a compound that generates free radicals by bond cleavage and / or reaction by exposure.

[0083] By containing a photoacid generator (c1), an acid is generated in the light-irradiated portion, and the solubility of the light-irradiated portion in the alkaline aqueous solution is increased, so that a positive relief pattern in which the light-irradiated portion is dissolved can be obtained. In addition, by containing a photoacid generator (c1) and an epoxy compound or a thermal crosslinking agent described later, the acid generated in the light-irradiated portion promotes the crosslinking reaction of the epoxy compound and the thermal crosslinking agent, and a negative relief pattern in which the light-irradiated portion is insoluble can be obtained. On the other hand, by containing a photopolymerization initiator (c2) and a free radical polymerizable compound described later, free radical polymerization is carried out in the light-irradiated portion, and a negative relief pattern in which the light-irradiated portion is insoluble can be obtained.

[0084] Examples of the photoacid generator (c1) include quinone diazonium compounds, sulfonium salts, Salt, diazo Salt, iodine Salts, etc. It is preferred that two or more photoacid generators are contained. When two or more photoacid generators are contained, a photosensitive resin composition with higher sensitivity can be obtained. From the perspective of long-term reliability when the cured film of the present invention described later is used as a planarization layer and / or insulating layer of an organic EL display device, the photoacid generator (c1) is particularly preferably a quinone diazine compound.

[0085] Examples of the quinone diazonium compound include compounds in which the sulfonic acid of quinone diazonium is bonded to a polyhydroxy compound via an ester, compounds in which the sulfonic acid of quinone diazonium is bonded to a polyamino compound via a sulfonamide bond, compounds in which the sulfonic acid of quinone diazonium is bonded to a polyhydroxy polyamino compound via an ester bond and / or a sulfonamide bond, etc. Preferably, 50 mol% or more of the functional groups of these polyhydroxy compounds and polyamino compounds are substituted with the sulfonic acid of quinone diazonium.

[0086] As the quinone diazo structure, it is preferred to use any one of 5-naphthoquinone diazo sulfonyl and 4-naphthoquinone diazo sulfonyl. It may contain a naphthoquinone diazo sulfonyl ester compound having a 4-naphthoquinone diazo sulfonyl group and a 5-naphthoquinone diazo sulfonyl group in the same molecule, or it may contain a 4-naphthoquinone diazo sulfonyl ester compound and a 5-naphthoquinone diazo sulfonyl ester compound. The 4-naphthoquinone diazo sulfonyl ester compound has absorption in the i-ray region of a mercury lamp and is suitable for i-ray exposure. The 5-naphthoquinone diazo sulfonyl ester compound has absorption extending to the g-ray region of a mercury lamp and is suitable for g-ray exposure.

[0087] It is preferred to select 4-naphthoquinone diazo sulfonyl ester compounds and 5-naphthoquinone diazo sulfonyl ester compounds according to the wavelength for exposure, and it is preferred to include 4-naphthoquinone diazo sulfonyl ester compounds from the viewpoint of high sensitivity. On the other hand, from the viewpoint of long-term reliability when the cured film of the present invention described later is used as a planarization layer and / or insulating layer of an organic EL display device, 5-naphthoquinone diazo sulfonyl ester compounds are preferred. However, in the present invention, by containing the above-mentioned polyimide precursor (a) and phenol compound (b), long-term reliability can be improved, so 4-naphthoquinone diazo sulfonyl ester compounds can be suitably used.

[0088] The quinone diazonium compound can be synthesized by any esterification reaction of a compound having a phenolic hydroxyl group and a quinone diazonium sulfonic acid compound. By using these quinone diazonium compounds, the resolution, sensitivity and residual film rate can be further improved.

[0089] In the present invention, among the photoacid generators (c1), sulfonium salts, Salt, diazo Salt, iodine Onium salts are preferred because they can moderately stabilize the acid component generated by exposure. Among them, sulfonium salts are preferred. A sensitizer or the like may also be contained as needed.

[0090] In the present invention, from the viewpoint of high sensitivity, when using a photoacid generator (c1), the content is preferably 0.1 parts by mass or more, more preferably 10 parts by mass or more, and further preferably 25 parts by mass or more relative to 100 parts by mass of a polyimide precursor (a). From the viewpoint of further improving the chemical resistance of the cured film, it is preferably 100 parts by mass or less. From the viewpoint of improving the long-term reliability when the cured film of the present invention described later is used as a planarization layer and / or an insulating layer of an organic EL display device, it is preferred that the content of the photoacid generator (c1) is small, but in the present invention, by containing the above-mentioned polyimide precursor (a) and the phenol compound (b), the long-term reliability can be improved, so the content of the photoacid generator (c1) can be increased for high sensitivity.

[0091] As the photopolymerization initiator (c2), for example, benzyl ketal photopolymerization initiator, α-hydroxy ketone photopolymerization initiator, α-amino ketone photopolymerization initiator, acyl phosphine oxide photopolymerization initiator, oxime ester photopolymerization initiator, acridine photopolymerization initiator, titanocene photopolymerization initiator, benzophenone photopolymerization initiator, acetophenone photopolymerization initiator, aromatic ketoester photopolymerization initiator, benzoate photopolymerization initiator, etc. can be mentioned. Two or more photopolymerization initiators (c2) can be contained. From the viewpoint of further improving the sensitivity, α-amino ketone photopolymerization initiator, acyl phosphine oxide photopolymerization initiator, oxime ester photopolymerization initiator are more preferred.

[0092] Examples of the α-aminoketone-based photopolymerization initiator include 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butane-1-one, 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholinophenyl)-butane-1-one, and 3,6-bis(2-methyl-2-morpholinopropionyl)-9-octyl-9H-carbazole.

[0093] Examples of the acylphosphine oxide-based photopolymerization initiator include 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-(2,4,4-trimethylpentyl)phosphine oxide.

[0094] Examples of the oxime ester photopolymerization initiator include 1-phenylpropane-1,2-dione-2-(O-ethoxycarbonyl)oxime, 1-phenylbutane-1,2-dione-2-(O-methoxycarbonyl)oxime, 1,3-diphenylpropane-1,2,3-trione-2-(O-ethoxycarbonyl)oxime, 1-[4-(phenylthio)phenyl]octane-1,2-dione-2-(O-benzoyl)oxime, 1-[4-[4-(carboxyphenyl)thio]phenyl]propane-1,2-dione-2-(O-acetyl)oxime, 1-[ 9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone-1-(O-acetyl)oxime, 1-[9-ethyl-6-[2-methyl-4-[1-(2,2-dimethyl-1,3-dioxolan-4-yl)methyloxy]benzoyl]-9H-carbazole-3-yl]ethanone-1-(O-acetyl)oxime or 1-(9-ethyl-6-nitro-9H-carbazole-3-yl)-1-[2-methyl-4-(1-methoxypropane-2-yloxy)phenyl]methanone-1-(O-acetyl)oxime, etc.

[0095] In the present invention, from the viewpoint of high sensitivity, when using a photopolymerization initiator (c2), relative to a total of 100 parts by mass of a polyimide precursor (a) and a free radical polymerizable compound described later, its content is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, and further preferably 10 parts by mass or more. On the other hand, from the viewpoint of further improving the resolution and reducing the cone angle, it is preferably 50 parts by mass or less. From the viewpoint of improving the long-term reliability when the cured film of the present invention described later is used as a planarization layer and / or an insulating layer of an organic EL display device, it is preferred that the content of the photopolymerization initiator (c2) is small, but in the present invention, by containing the above-mentioned polyimide precursor (a) and the phenol compound (b), the long-term reliability can be improved, so in order to achieve high sensitivity, the content of the photopolymerization initiator (c2) can be increased.

[0096] <Colorant (d)>

[0097] The photosensitive resin composition of the present invention preferably further contains a colorant (d). By containing a colorant (d), it is possible to impart light-shielding properties to light of a wavelength absorbed by the light-shielding colorant (d) from light passing through the film of the photosensitive resin composition or light reflected from the film of the photosensitive resin composition. By imparting light-shielding properties, it is possible to prevent degradation, malfunction, leakage current, etc. caused by light intrusion into TFT when the cured film of the present invention described later is used as a planarization layer and / or insulating layer of an organic EL display device. Furthermore, it is possible to suppress external light reflection from wiring and TFT, and improve the contrast between the luminous area and the non-luminous area.

[0098] As the colorant (d), a dye (d1) and / or a pigment (d2) are preferably used. The colorant (d) may contain at least one, and examples thereof include a method of using one dye or organic pigment, a method of mixing two or more dyes or pigments, and a method of using one or more dyes in combination with one or more pigments.

[0099] In the present invention, it is preferred to select a substance having an absorption maximum at 400 to 750 nm.

[0100] From the viewpoint of solvent solubility, the colorant (d) in the present invention is preferably a dye (d1). On the other hand, from the viewpoint of being able to suppress the fading of the colorant in the heat curing process of the photosensitive resin composition or photosensitive resin sheet of the present invention described later, a pigment (d2) is preferred. However, in the present invention, since the polyimide precursor (a) and the phenol compound (b) mentioned above are contained, curing can be performed even at a temperature below 200°C, so even if the dye (d1) is used, the fading of the colorant in the heat curing process can be suppressed. Therefore, the dye (d1) can also be suitably used.

[0101] In the photosensitive resin composition of the present invention, the colorant (d) preferably contains a dye (d1-1) and / or a pigment (d2-1) having an absorption maximum in the range of (d-1) wavelength of 400 nm or more and less than 490 nm. Hereinafter, they are sometimes referred to as component (d-1), component (d1-1), and component (d2-1), respectively.

[0102] In the present invention, from the viewpoint of storage stability, fading during curing and light irradiation, the dye (d1-1) used as the component (d-1) is preferably a dye that is soluble in the organic solvent that dissolves the polyimide precursor (a) and is compatible with the resin, and a dye with high heat resistance and light resistance. The component (d1-1) has an absorption maximum in the range of more than 400nm and less than 490nm, and examples thereof include yellow dyes, orange dyes, etc. As the type of dye, examples thereof include oil-soluble dyes, disperse dyes, reactive dyes, acid dyes, direct dyes, etc.

[0103] Examples of the skeleton structure of the dye include anthraquinone-based, azo-based, phthalocyanine-based, methine-based, Azine series, quinoline series, triarylmethane series, Among them, anthraquinone-based, azo-based, methine-based, triarylmethane-based, In addition, each of these dyes can be used alone or in the form of a metal complex salt system. Specifically, they can be selected from Sumilan, Lanyl dyes (manufactured by Sumitomo Chemical Industries, Ltd.), Orasol, Oracet, Filamid, Irgasperse dyes (manufactured by Chiba Spessary Chemicals Co., Ltd.), Zapon, Neozapon, Neptune, Acidol dyes (manufactured by BASF Corporation), Kayaset, Kayakalan dyes (manufactured by Nippon Kayaku Co., Ltd.), Valifast Colors dyes (manufactured by Olient Chemical Industries, Ltd.), Savinyl, Sandoplast, Polysynthren, Lanasyn dyes (manufactured by Clariant Japan Co., Ltd.), Aizen Spilon dyes (manufactured by Hodogaya Chemical Industries, Ltd.), functional pigments (manufactured by Yamada Chemical Industries, Ltd.), Plast Color dyes, Oil Color dyes (manufactured by Arimoto Chemical Industry Co., Ltd.) and the like are obtained, but the present invention is not limited thereto. These dyes are used alone or in combination.

[0104] In the present invention, the pigment (d2-1) used as the component (d-1) is preferably a pigment having high heat resistance and light resistance from the viewpoint of fading during curing or light irradiation.

[0105] The specific example of the organic pigment they use is represented by color index (CI) numbering. As the example of yellow pigment, pigment yellow 83, 117, 129, 138, 139, 150, 180 etc. can be enumerated. As the example of orange pigment, pigment orange 38, 43, 64, 71, 72 etc. can be enumerated. In addition, pigments other than these can also be used.

[0106] When used in the present invention, the content of the component (d-1) is preferably 0.1 to 300 parts by mass, more preferably 0.2 to 200 parts by mass, and particularly preferably 1 to 200 parts by mass relative to 100 parts by mass of the polyimide precursor (a). When the content of the component (d-1) is 0.1 parts by mass or more, light of the corresponding wavelength can be absorbed. In addition, when the content is 300 parts by mass or less, the adhesion strength between the photosensitive colored resin film and the substrate, the heat resistance of the film after heat treatment, and the mechanical properties can be maintained while absorbing light of the corresponding wavelength.

[0107] In the present invention, the organic pigment used as component (d2-1) may be a substance that has been subjected to surface treatment such as rosin treatment, acidic treatment, or alkaline treatment as required. In addition, it may be used together with a dispersant as appropriate. The dispersant may include, for example, cationic, anionic, nonionic, amphoteric, silicone, or fluorine-based surfactants.

[0108] The colorant (d) used in the photosensitive resin composition of the present invention preferably contains (d-2) a dye (d1-2) and / or a pigment (d2-2) having an absorption maximum in the wavelength range of 490 nm or more and less than 580 nm. Hereinafter, they are sometimes referred to as component (d-2), component (d1-2), and component (d2-2), respectively.

[0109] In the present invention, from the viewpoint of storage stability, fading during curing and light irradiation, the dye used as the component (d1-2) is preferably a dye that is soluble in the organic solvent that dissolves the polyimide precursor (a) and is compatible with the resin, a dye with high heat resistance and light resistance. The component (d1-2) has an absorption maximum value in the range of more than 490nm and less than 580nm, and for example, red dyes, purple dyes, etc. can be cited. As the type of dye, for example, oil-soluble dyes, disperse dyes, reactive dyes, acid dyes or direct dyes can be cited.

[0110] Examples of the skeleton structure of the dye include anthraquinone-based, azo-based, phthalocyanine-based, methine-based, Azine series, quinoline series, triarylmethane series, Among them, from the viewpoint of solubility in organic solvents and heat resistance, anthraquinone-based, azo-based, methine-based, triarylmethane-based, In addition, each of these dyes can be used alone or in the form of a metal complex salt system. Specifically, they can be selected from Sumilan, Lanyl dyes (manufactured by Sumitomo Chemical Industries, Ltd.), Orasol, Oracet, Filamid, Irgasperse dyes (manufactured by Chiba Spessary Chemicals Co., Ltd.), Zapon, Neozapon, Neptune, Acidol dyes (manufactured by BASF Corporation), Kayaset, Kayakalan dyes (manufactured by Nippon Kayaku Co., Ltd.), Valifast Colors dyes (manufactured by Olient Chemical Industries, Ltd.), Savinyl, Sandoplast, Polysynthren, Lanasyn dyes (manufactured by Clariant Japan Co., Ltd.), Aizen Spilon dyes (manufactured by Hodogaya Chemical Industries, Ltd.), functional pigments (manufactured by Yamada Chemical Industries, Ltd.), Plast Color dyes, Oil Color dyes (manufactured by Arimoto Chemical Industry Co., Ltd.) and the like are obtained, but the present invention is not limited thereto. These dyes are used alone or in combination.

[0111] In the present invention, the pigment (d2-2) used as the component (d-2) is preferably a pigment having high heat resistance and light resistance from the viewpoint of fading during curing or light irradiation.

[0112] The specific examples of the organic pigments used are represented by color index (CI) numbers. Examples of red pigments include Pigment Red 48:1, 122, 168, 177, 202, 206, 207, 209, 224, 242, 254, etc. Examples of violet pigments include Pigment Violet 19, 23, 29, 32, 33, 36, 37, 38, etc. In addition, pigments other than these can also be used.

[0113] When used in the present invention, the content of the component (d-2) is preferably 0.1 to 300 parts by mass, more preferably 0.2 to 200 parts by mass, and particularly preferably 1 to 200 parts by mass relative to 100 parts by mass of the polyimide precursor (a). When the content of the component (d-2) is 0.1 parts by mass or more, light of the corresponding wavelength can be absorbed. In addition, when the content is 300 parts by mass or less, the adhesion strength between the photosensitive colored resin film and the substrate, the heat resistance of the film after heat treatment, and the mechanical properties can be maintained while absorbing light of the corresponding wavelength.

[0114] In the present invention, the organic pigment used as component (d2-2) may be a substance that has been subjected to surface treatments such as rosin treatment, acidic treatment, and alkaline treatment as required. In addition, it may be used together with a dispersant as appropriate. Dispersants include, for example, cationic, anionic, nonionic, amphoteric, silicone-based, and fluorine-based surfactants.

[0115] The colorant (d) used in the photosensitive resin composition of the present invention preferably contains (d-3) a dye (d1-3) and / or a pigment (d2-3) having an absorption maximum in a wavelength range of 580 nm to less than 800 nm.

[0116] In the present invention, from the viewpoint of storage stability, fading during curing and light irradiation, the dye (d1-3) used as the component (d-3) is preferably a dye that is soluble in the organic solvent that dissolves the polyimide precursor (a) and is compatible with the resin, or a dye that has high heat resistance and light resistance. The component (d1-3) has an absorption maximum in the range of a wavelength of 580 nm or more and less than 800 nm, and examples thereof include blue dyes and green dyes.

[0117] Examples of the dye include oil-soluble dyes, disperse dyes, reactive dyes, acid dyes, and direct dyes.

[0118] Examples of the skeleton structure of the dye include anthraquinone-based, azo-based, phthalocyanine-based, methine-based, Azine series, quinoline series, triarylmethane series, Among them, anthraquinone-based, azo-based, methine-based, triarylmethane-based, In addition, each of these dyes can be used alone or as a metal salt system. Specifically, they can be selected from Sumilan, Lanyl dyes (manufactured by Sumitomo Chemical Industries, Ltd.), Orasol, Oracet, Filamid, Irgasperse dyes (manufactured by Chiba Spessary Chemicals Co., Ltd.), Zapon, Neozapon, Neptune, Acidol dyes (manufactured by BASF Corporation), Kayaset, Kayakalan dyes (manufactured by Nippon Kayaku Co., Ltd.), Valifast Colors dyes (manufactured by Olient Chemical Industries, Ltd.), Savinyl, Sandoplast, Polysynthren, Lanasyn dyes (manufactured by Clariant Japan Co., Ltd.), Aizen Spilon dyes (manufactured by Hodogaya Chemical Industries, Ltd.), functional pigments (manufactured by Yamada Chemical Industries, Ltd.), Plast Color dyes, Oil Color dyes (manufactured by Arimoto Chemical Industry Co., Ltd.) and the like are obtained, but the present invention is not limited thereto. These dyes may be used alone or in combination.

[0119] In the present invention, the pigment (d2-3) used as the component (d-3) is preferably a pigment having high heat resistance and light resistance from the viewpoint of discoloration during curing or light irradiation.

[0120] Specific examples of the organic pigments used are indicated by color index (CI) numbers. Examples of blue pigments include pigment blue 15 (15:3, 15:4, 15:6, etc.), 21, 22, 60, 64, etc. Examples of green pigments include pigment green 7, 10, 36, 47, 58, etc. In addition, pigments other than these may be used.

[0121] In the present invention, the content of the component (d-3) is preferably 0.1 to 300 parts by mass, more preferably 0.2 to 200 parts by mass, and particularly preferably 1 to 200 parts by mass, relative to 100 parts by mass of the polyimide precursor (a). When the content of the component (d-3) is 0.1 parts by mass or more, light of the corresponding wavelength can be absorbed. In addition, when the content is 300 parts by mass or less, the adhesion strength between the photosensitive colored resin film and the substrate, the heat resistance of the film after heat treatment, and the mechanical properties can be maintained while absorbing light of the corresponding wavelength.

[0122] In the present invention, the organic pigment used as component (d2-3) may be a substance that has been subjected to surface treatments such as rosin treatment, acidic treatment, and alkaline treatment as required. In addition, it may be used together with a dispersant as appropriate. Dispersants include, for example, cationic, anionic, nonionic, amphoteric, silicone-based, and fluorine-based surfactants.

[0123] In addition, in the present invention, by using the components (d-1), (d-2) and (d-3) together, blackening can be achieved. Blackening can be represented by optical density (OD value), preferably the OD value is 0.3 or more, more preferably 0.6 or more, and further preferably 1.0 or more.

[0124] <Thermochromic compounds>

[0125] The photosensitive resin composition of the present invention may further contain a thermochromic compound. The thermochromic compound is a thermochromic compound that develops color by heat treatment and has an absorption maximum at 350 nm to 700 nm, and more preferably a thermochromic compound that develops color by heat treatment and has an absorption maximum at 350 nm to 500 nm. By using a thermochromic compound instead of the above-mentioned component (d-1) or in combination with the component (d-1), the absorption of the photosensitive resin composition in the exposure wavelength region of 350-450 nm can be suppressed, thereby suppressing the reduction in sensitivity.

[0126] In the present invention, the thermochromic compound is preferably a compound that develops color at a temperature higher than 120° C., and more preferably a thermochromic compound that develops color at a temperature higher than 180° C. The higher the color development temperature of the thermochromic compound, the better the heat resistance under high temperature conditions, and the less fading by long-term irradiation with ultraviolet light and visible light, and the better the light resistance.

[0127] In the present invention, the thermochromic compound may be a general thermosensitive pigment or a pressure-sensitive pigment, or may be other compounds. Examples of thermochromic compounds include substances that develop color by changing their chemical structure or charge state through the action of coexisting acidic groups in the system during heat treatment, and substances that develop color by undergoing a thermal oxidation reaction or the like due to the presence of oxygen in the air.

[0128] Examples of the skeleton structure of the thermochromic compound include a triarylmethane skeleton, a diarylmethane skeleton, a fluorane skeleton, a dilactone skeleton, a phthalide skeleton, Tonne skeleton, rhodamine lactam skeleton, fluorene skeleton, phenothiazine skeleton, phen Among them, the triarylmethane skeleton is preferred because of its high thermal color development temperature and excellent heat resistance.

[0129] Specific examples of the triarylmethane skeleton include 2,4',4"-methylenetriphenol, 4,4',4"-methylenetriphenol, 4,4'-[(4-hydroxyphenyl)methylene]bis(aniline), 4,4'-[(4-aminophenyl)methylene]bisphenol, 4,4'-[(4-aminophenyl)methylene]bis[3,5-dimethylphenol], 4,4'-[(2-hydroxyphenyl)methylene]bis[2,3,6-trimethylphenol], 4- [Bis(4-hydroxyphenyl)methyl]-2-methoxyphenol, 4,4'-[(2-hydroxyphenyl)methylene]bis[2-methylphenol], 4,4'-[(4-hydroxyphenyl)methylene]bis[2-methylphenol], 4-[bis(4-hydroxyphenyl)methyl]-2-ethoxyphenol, 4,4'-[(4-hydroxyphenyl)methylene]bis[2,6-dimethylphenol], 2,2'-[(4-hydroxyphenyl)methylene]bis[3,5-dimethylphenol] phenol], 4,4'-[(4-hydroxy-3-methoxyphenyl)methylene]bis[2,6-dimethylphenol], 2,2'-[(2-hydroxyphenyl)methylene]bis[2,3,5-trimethylphenol], 4,4'-[(4-hydroxyphenyl)methylene]bis[2,3,6-trimethylphenol], 4,4'-[(2-hydroxyphenyl)methylene]bis[2-cyclohexyl-5-methylphenol], 4,4'-[(4-hydroxyphenyl)methylene]bis[2-cyclohexyl-5-methylphenol], ]bis[2-cyclohexyl-5-methylphenol], 4,4'-[(3-methoxy-4-hydroxyphenyl)methylene]bis[2-cyclohexyl-5-methylphenol], 4,4'-[(3,4-dihydroxyphenyl)methylene]bis[2-methylphenol], 4,4'-[(3,4-dihydroxyphenyl)methylene]bis[2,6-dimethylphenol], 4,4'-[(3,4-dihydroxyphenyl)methylene]bis[2,3,6-trimethylphenol], etc. They can be used alone or in combination. In addition, with respect to the hydroxyl-containing compound having a triarylmethane skeleton, the sulfonic acid of naphthoquinone diazonium can be ester-bonded with the compound and used as a quinone diazonium compound.

[0130] In the present invention, the content of the thermochromic compound is preferably 5 to 80 parts by mass, particularly preferably 10 to 60 parts by mass, relative to 100 parts by mass of the polyimide precursor (a). If the content of the thermochromic compound is 5 parts by mass or more, the transmittance in the ultraviolet visible region of the cured film can be reduced. In addition, if it is 80 parts by mass or less, the heat resistance and strength of the cured film can be maintained and the water absorption can be reduced.

[0131] <Resins other than polyimide precursor (a)>

[0132] The photosensitive resin composition of the present invention may contain a resin other than the polyimide precursor (a). Examples of the resin (a) other than the polyimide precursor (a) include polyimide, polybenzoic acid, The present invention is not limited to oxazole precursors, polyamide-imide, polyamide-imide precursors, polyamide, polymers of radical polymerizable monomers having an acidic group, phenol resins, etc. These resins are preferably alkali-soluble, and two or more of these resins may be contained. Among these resins, polyimide, polybenzophenone, and polybenzophenone are more preferred because they have high adhesion by development, excellent heat resistance, and low outgassing at high temperatures, thereby providing a high long-term reliability when the cured film described later is used in an organic EL display device. Here, the so-called polybenzoic acid Azole precursor refers to a product that is converted into polybenzoic acid by heating or chemical treatment. Examples of the oxazole resin include polyhydroxyamide and the like.

[0133] <Radical polymerizable compounds>

[0134] The photosensitive resin composition of the present invention may further contain a radical polymerizable compound.

[0135] The so-called free radical polymerizable compound refers to a compound having multiple ethylenically unsaturated double bonds in the molecule. During exposure, free radical polymerization of the free radical polymerizable compound is carried out by the free radicals generated from the above-mentioned photopolymerization initiator (c2), and the light irradiated part is insolubilized, thereby obtaining a negative pattern. By further containing a free radical polymerizable compound, the photocuring of the light irradiated part is promoted, and the sensitivity is further improved. In addition, since the crosslinking density after thermal curing is increased, the hardness of the cured film can be increased.

[0136] As the free radical polymerizable compound, a compound having a (meth)acryloyl group that is easy to be free radically polymerized is preferred. From the viewpoint of improving the sensitivity during exposure and improving the hardness of the cured film, a compound having two or more (meth)acryloyl groups in the molecule is more preferred. As the double bond equivalent of the free radical polymerizable compound, from the viewpoint of improving the sensitivity during exposure and improving the hardness of the cured film, it is preferably 80 to 400 g / mol.

[0137] Examples of the radical polymerizable compound include trimethylolpropane tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, 2,2-bis[4-(3-(meth)acrylate]propane

[0063] The invention also includes the following:

[0064] bis((meth)acryloyloxy-2-hydroxypropoxy)phenyl]propane, 1,3,5-tris((meth)acryloyloxyethyl)isocyanuric acid, 1,3-bis((meth)acryloyloxyethyl)isocyanuric acid, 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene, 9,9-bis[4-(3-(meth)acryloyloxypropoxy)phenyl]fluorene, 9,9-bis(4-(meth)acryloyloxyphenyl)fluorene, or acid-modified forms thereof, ethylene oxide-modified forms thereof, propylene oxide-modified forms thereof, and the like.

[0138] In the photosensitive resin composition of the present invention, from the viewpoint of further improving sensitivity and reducing the taper angle, the content of the radical polymerizable compound is preferably 15 parts by mass or more, more preferably 30 parts by mass or more, relative to 100 parts by mass of the total of the polyimide precursor (a) and the radical polymerizable compound. On the other hand, from the viewpoint of further improving the heat resistance of the cured film and reducing the taper angle, it is preferably 65 parts by mass or less, more preferably 50 parts by mass or less.

[0139] <Thermal cross-linking agent>

[0140] The photosensitive resin composition of the present invention may further contain a thermal crosslinking agent. The so-called thermal crosslinking agent refers to a compound having at least 2 alkoxymethyl, methylol, epoxy, oxetane and other heat-reactive functional groups in the molecule. By containing a thermal crosslinking agent, the polyimide precursor (a) or other added components can be crosslinked, so that the heat resistance, chemical resistance and bending resistance of the film after thermal curing are improved. On the other hand, from the perspective of improving the imidization rate during low-temperature sintering and improving the long-term reliability when the cured film of the present invention described later is used as a planarization layer and / or insulating layer of an organic EL display device, it is preferably a thermal crosslinking agent that does not contain epoxy and oxetane. It is speculated that this is because, in the case where the photosensitive resin composition of the present invention contains a thermal crosslinking agent that reacts with a phenolic hydroxyl group such as an epoxy and oxetane, the phenolic hydroxyl of the phenol compound (b) reacts with the thermal crosslinking agent, and the effect of the present invention becomes smaller.

[0141] Preferred examples of the compound having at least two alkoxymethyl groups or hydroxymethyl groups include DML-PC, DML-PEP, DML-OC, DML-OEP, DML-34X, DML-PTBP, DML-PCHP, DML-OCHP, DML-PFP, DML-PSBP, DML-POP, DML-MBOC, DML-MBPC, DML-MTrisPC, DML-BisOC-Z, DML-BisOCHP-Z, DML-BPC, DML-BisOC-P, DMOM-PC, DMOM-PTBP, DMOM-MBPC, TriML-P, TriML-35XL, TML-HQ, TML-BP, TML-pp-BPF, TML-BPE, TML-BPA, TML-BPAF, TML-BPAP, TMOM-BP, TMOM-BPE, TMOM-BPA, TMOM-BPAF, TMOM-BPAP, HML-TPPHBA, HML-TPHAP, HMOM-TPPHBA, HMOM-TPHAP (the above are trade names, manufactured by Honshu Chemical Industry Co., Ltd.), "NIKALAC" (registered trademark) MX-290, "NIKALAC" MX-280, "NIKALAC" MX-270, "NIKALAC" MX-279, "NIKALAC" MW-100LM, "NIKALAC" MX-750LM (the above are trade names, manufactured by Sanwa Chemical Co., Ltd.).

[0142] Preferred examples of the compound having at least two epoxy groups include Epilite (registered trademark) 40E, Epilite 100E, Epilite 200E, Epilite 400E, Epilite 70P, Epilite 200P, Epilite 400P, Epilite 1500NP, Epilite 80MF, Epilite 4000, Epilite 3000, and Epilite 4000. 002 (above, manufactured by Kyoeisha Chemical Co., Ltd.), "Doctor" (registered trademark) EX-212L, "Doctor" EX-214L, "Doctor" EX-216L, "Doctor" EX -850L (above, manufactured by Nagas Co., Ltd.), GAN, GOT (above, Nippon Kayaku Co., Ltd.), "Etotron" (registered trademark) 828, "Etotron" 1002, "Etotron" "エピコート" 1007, YX8100-BH30, E1256, E4 250. E4275 (above, manufactured by Semantec Co., Ltd.), "Ebocon" (note Registered trademarks) EXA-9583, HP4032 (above, manufactured by DIC Co., Ltd.), VG3101 (manufactured by Mitsui Chemicals Co., Ltd.), "テピック" (registered trademark) S, "テピック" G, "テピック" P ( The above, Nissan Chemical Industries, Ltd.), "Denacol" EX-321L (manufactured by Nagase Chemtex Co., Ltd.), NC6000 (manufactured by Nippon Kayaku Co., Ltd.), "Epote" (registered trademark) YH-434L (manufactured by Tohto Kasei Co., Ltd.), EPPN502H, NC3000 (manufactured by Nippon Kayaku Co., Ltd.), "Epicron" (registered trademark) N695, HP7200 (the above, manufactured by DIC Corporation), etc.

[0143] Preferred examples of the compound having at least two oxetane groups include Etanacol EHO, Etanacol OXBP, Etanacol OXTP, Etanacol OXMA (all manufactured by Ube Industries, Ltd.), and oxetane-containing phenol novolac.

[0144] Two or more thermal crosslinking agents may be contained in combination.

[0145] When a thermal crosslinking agent is contained, its content is preferably 1% by mass or more and 30% by mass or less in 100% by mass of the total amount of the photosensitive resin composition excluding the solvent. If the content of the thermal crosslinking agent is 1 part by mass or more, the chemical resistance and bending resistance of the cured film can be further improved. In addition, if the content of the thermal crosslinking agent is 30 parts by mass or less, the amount of outgassing from the cured film can be further reduced, the long-term reliability of the organic EL display device can be further improved, and the storage stability of the photosensitive resin composition is also excellent.

[0146] <Solvent>

[0147] The photosensitive resin composition of the present invention may further contain a solvent. By containing a solvent, a varnish state can be formed, and coating properties can be improved.

[0148] Examples of the solvent include polar aprotic solvents such as γ-butyrolactone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol mono-n-propyl ether, diethylene glycol mono-n-butyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, propylene glycol mono-n-butyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tetrahydrofuran, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, dipropylene glycol mono-n-butyl ether, tripropylene glycol monomethyl ether, tripropylene glycol monoethyl ether, tetrahydrofuran, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, tetrahydrofuran, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, tetrahydrofuran, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, tetrahydrofuran, dipropylene glycol monoethyl ether ...ethyl ether, dipropylene glycol monoethyl Ethers such as alkanes, acetone, methyl ethyl ketone, diisobutyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, ketones such as diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, esters such as ethyl lactate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, methyl 3-ethoxypropionate, ethyl 3-ethoxypropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutyrate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxy Butyl propionate, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-amyl formate, isoamyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, methyl pyruvate, ethyl pyruvate, n-propyl pyruvate, methyl acetoacetate, ethyl acetoacetate, ethyl 2-oxobutyrate and other esters, aromatic hydrocarbons such as toluene and xylene, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, 3-methoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropaneamide, N,N-dimethylpropaneamide, N,N-dimethylisobutylamide and other amides, 3-methyl-2- Oxazolidinone, etc. Two or more of these may be contained.

[0149] When a solvent is contained, its content is not particularly limited, but is preferably 100 to 3000 parts by mass, and more preferably 150 to 2000 parts by mass, relative to 100 parts by mass of the total amount of the photosensitive resin composition excluding the solvent. In addition, the proportion of solvents having a boiling point of 180° C. or higher in the total amount of 100% by mass of the solvent is preferably 20% by mass or less, and more preferably 10% by mass or less. By making the proportion of solvents having a boiling point of 180° C. or higher 20% by mass or less, the outgassing amount after thermal curing can be further reduced, and the long-term reliability of the organic EL device can be further improved.

[0150] <Adhesion Improver>

[0151] The photosensitive resin composition of the present invention can further contain a close fit improver. As a close fit improver, silane coupling agents such as vinyl trimethoxy silane, vinyl triethoxy silane, epoxy cyclohexyl ethyl trimethoxy silane, 3-glycidoxy propyl trimethoxy silane, 3-glycidoxy propyl triethoxy silane, p-phenyl trimethoxy silane, 3-aminopropyl trimethoxy silane, 3-aminopropyl triethoxy silane, N-phenyl-3-aminopropyl trimethoxy silane, titanium chelate, aluminum chelate, compounds obtained by reacting aromatic amine compounds with silicon compounds containing alkoxy groups, etc. can be enumerated. Two or more of them can be contained. By containing these close fit improvers, the development closeness of the base substrates such as silicon wafer, indium tin oxide (ITO), SiO2, silicon nitride can be improved when the resin film is developed. In addition, the resistance to oxygen plasma used for washing, UV ozone treatment, etc. can be improved. When the adhesion improver is contained, the content is preferably 0.01 to 10% by mass in 100% by mass of the total amount of the photosensitive resin composition excluding the solvent.

[0152] <Surfactant>

[0153] The photosensitive resin composition of the present invention may further contain a surfactant as needed to improve wettability with the substrate. Examples of the surfactant include SH series, SD series, and ST series of Toray Daw Coning Co., Ltd., BYK series of Bick Chemie Japan Co., Ltd., KP series of Shin-Etsu Chemical Co., Ltd., Diesflow series of NOF Corporation, Megafac (registered trademark) series of DIC Corporation, Fluorade series of Sumitomo Slide Corporation, and the like. Fluorine-based surfactants such as the "SURFLON (registered trademark)" series and the "ASHIGADO (registered trademark)" series of Asahi Glass Co., Ltd. and the "POLYFOX" series of Omnova Solar Co., Ltd.; acrylic and / or methacrylic surfactants such as the "POLYFLO" series of Kyoeisha Chemical Co., Ltd. and the "DISPARON (registered trademark)" series of Kusumoto Chemicals Co., Ltd.

[0154] When a surfactant is contained, the content thereof is preferably 0.001 to 1% by mass based on 100% by mass of the total amount of the photosensitive resin composition excluding the solvent.

[0155] <Inorganic particles>

[0156] The photosensitive resin composition of the present invention may further contain inorganic particles. Preferred specific examples of inorganic particles include silicon oxide, titanium oxide, barium titanate, aluminum oxide, talc, etc. The primary particle size of the inorganic particles is preferably 100 nm or less, more preferably 60 nm or less.

[0157] When inorganic particles are contained, the content thereof is preferably 5 to 90% by mass based on 100% by mass of the total amount of the photosensitive resin composition excluding the solvent.

[0158] <Method for producing photosensitive resin composition>

[0159] Next, the method for producing the photosensitive resin composition of the present invention is described. For example, the photosensitive resin composition of the present invention can be obtained by dissolving a polyimide precursor (a), a phenol compound (b), a photosensitive compound (c), and, if necessary, a colorant (d), a thermochromic compound, a radical polymerizable compound, a thermal crosslinking agent, a solvent, a close contact improving agent, a surfactant, inorganic particles, and the like.

[0160] As the dissolving method, stirring and heating can be mentioned. In the case of heating, the heating temperature is preferably set within a range that does not damage the performance of the photosensitive resin composition, usually room temperature to 80°C. In addition, the dissolution order of each component is not particularly limited, and for example, a method of dissolving in order from compounds with low solubility can be mentioned. In addition, regarding components such as surfactants and a part of the adhesion improver that are prone to generate bubbles when stirred and dissolved, the other components are dissolved and then added last, thereby preventing poor dissolution of other components caused by the generation of bubbles.

[0161] The obtained photosensitive resin composition is preferably filtered using a filter to remove garbage and particles. The filter pore size can be, for example, 0.5 μm, 0.2 μm, 0.1 μm, 0.07 μm, 0.05 μm, 0.02 μm, etc., but is not limited thereto. Among the materials of the filter, polypropylene (PP), polyethylene (PE), nylon (NY), polytetrafluoroethylene (PTFE), etc. can be cited. Among them, polyethylene and nylon are preferred.

[0162] <Photosensitive resin film, photosensitive resin sheet>

[0163] The photosensitive resin sheet of the present invention is a photosensitive resin sheet formed from the photosensitive resin composition of the present invention. The photosensitive resin sheet of the present invention can be obtained by, for example, applying the photosensitive resin composition of the present invention on a releasable substrate such as polyethylene terephthalate and drying it.

[0164] In the present invention, the photosensitive resin film can be obtained by applying the photosensitive resin composition of the present invention to obtain a coating film of the photosensitive resin composition, and drying the coating film. Alternatively, a photosensitive resin sheet can be made into a photosensitive resin film.

[0165] As a method for coating the photosensitive resin composition of the present invention, for example, spin coating, slit coating, dip coating, spray coating, printing, etc. can be cited. Among them, the slit coating method is preferred because it can be coated with a small amount of coating liquid, which is conducive to cost reduction. The amount of coating liquid required for the slit coating method is about 1 / 5 to 1 / 10 of that for the spin coating method. As the slit nozzle used for coating, for example, the slit nozzles listed by multiple manufacturers such as "Liner Coder" manufactured by Dainippon Screen Manufacturing Co., Ltd., "Spinless" manufactured by Tokyo Ohka Industry Co., Ltd., "TS Coder" manufactured by Toray Engineering Co., Ltd., "Technical Coder" manufactured by Chugai Route Industry Co., Ltd., "CS Series" and "CL Series" manufactured by Tokyo Electron Co., Ltd., "Inline Slit Coder" manufactured by Samatronix Trading Co., Ltd., and "Hedd Coder HC Series" manufactured by Hirata Machinery Co., Ltd. can be selected. The coating speed is generally in the range of 10 mm / sec to 400 mm / sec. The film thickness of the coating film varies depending on the solid content concentration, viscosity, etc. of the resin composition, but the coating is usually performed so that the film thickness after drying becomes 0.1 to 10 μm, preferably 0.3 to 5 μm.

[0166] Before coating, the substrate to be coated with the photosensitive resin composition may be pre-treated with the above-mentioned adhesion improver. As a pre-treatment method, for example, a method of treating the substrate surface using a solution obtained by dissolving 0.5 to 20% by mass of the adhesion improver in a solvent such as isopropanol, ethanol, methanol, water, tetrahydrofuran, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether, ethyl lactate, diethyl adipate, etc. As a method for treating the substrate surface, a spin coating method, a slit die coating method, a rod coating method, a dip coating method, a spray coating method, a steam treatment method, etc. may be mentioned.

[0167] After coating, a reduced pressure drying treatment is performed as necessary.

[0168] The vacuum drying speed is related to the volume of the vacuum chamber, the capacity of the vacuum pump, the diameter of the pipe between the chamber and the pump, etc., but for example, in the state without a coated substrate, it is preferably set to a condition where the vacuum chamber is depressurized to 40 Pa after 60 seconds. The general vacuum drying time is about 30 seconds to 100 seconds, and the pressure in the vacuum chamber at the end of the vacuum drying is usually below 100 Pa in the state with a coated substrate. By making the reaching pressure below 100 Pa, a dry state with reduced stickiness on the surface of the coating film can be formed, thereby suppressing surface contamination and particle generation in the subsequent substrate transportation.

[0169] After coating or drying under reduced pressure, the coating film is generally heated and dried. This process is also called prebaking. Drying uses a hot plate, an oven, infrared rays, etc. When a hot plate is used, the coating film is directly held on the plate for heating or held on a fixture such as a contact pin set on the plate for heating. The heating time is preferably 1 minute to several hours. The heating temperature varies depending on the type and purpose of the coating film, but from the viewpoint of promoting the drying of the solvent during prebaking, it is preferably 80°C or more, and more preferably 90°C or more. On the other hand, from the viewpoint of reducing the imidization during prebaking, it is preferably 150°C or less, and more preferably 140°C or less. The photosensitive resin composition in the present invention contains the above-mentioned polyimide precursor (a) and the phenol compound (b), thereby suppressing the imidization during prebaking, but even when calcined at a temperature below 200°C, a cured film with a high imidization rate can be obtained.

[0170] The photosensitive resin film and the photosensitive resin sheet can be patterned. For example, the photosensitive resin film and the photosensitive resin sheet can be exposed to chemical rays through a mask having a desired pattern, and then developed to form a desired pattern.

[0171] As chemical rays used for exposure, ultraviolet rays, visible rays, electron rays, X-rays, etc. can be cited. In the present invention, i-rays (365nm), h-rays (405nm), and g-rays (436nm) of a mercury lamp are preferably used. In the case of positive photosensitivity, the exposed portion dissolves in the developer. In the case of negative photosensitivity, the exposed portion solidifies and becomes insoluble in the developer.

[0172] After exposure, the exposed part is removed in the case of positive type, and the non-exposed part is removed in the case of negative type by a developer to form a desired pattern. As a developer, aqueous solutions of alkaline compounds such as tetramethylammonium hydroxide, diethanolamine, diethylaminoethanol, sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, triethylamine, diethylamine, methylamine, dimethylamine, dimethylaminoethyl acetate, dimethylaminoethanol, dimethylaminoethyl methacrylate, cyclohexylamine, ethylenediamine, and 1,6-hexanediamine are preferred. In these alkaline aqueous solutions, one or more polar solvents such as N-methyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, γ-butyrolactone, and dimethylacrylamide, alcohols such as methanol, ethanol, and isopropanol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, ketones such as cyclopentanone, cyclohexanone, isobutyl ketone, and methyl isobutyl ketone can be added. Examples of the developing method include spraying, paddle, dipping, and ultrasonic methods.

[0173] Next, the pattern formed by development is preferably rinsed with distilled water. The rinsing treatment can be performed by adding alcohols such as ethanol and isopropyl alcohol, esters such as ethyl lactate and propylene glycol monomethyl ether acetate, etc. to distilled water.

[0174] <Cured film>

[0175] The cured film of the present invention is a cured film obtained by curing the photosensitive resin composition of the present invention or the photosensitive resin sheet of the present invention. By heat-curing the photosensitive resin composition of the present invention or the photosensitive resin sheet of the present invention, components with low heat resistance can be removed, thereby further improving heat resistance and chemical resistance. In particular, since the photosensitive resin composition of the present invention or the photosensitive resin sheet of the present invention contains a polyimide precursor, an imide ring is formed by heat curing, thereby further improving heat resistance and chemical resistance.

[0176] The cured film of the present invention can be suitably used, for example, as a planarizing layer and / or insulating layer in an organic EL display device having a driving circuit, a planarizing layer, a first electrode, an insulating layer, a light-emitting layer, and a second electrode on a substrate.

[0177] Furthermore, the cured film of the present invention can be suitably used, for example, for an interlayer insulating layer and / or a surface protective layer in an electronic component having an electrode, a metal wiring, an interlayer insulating layer and / or a surface protective layer on a substrate.

[0178] <Method for producing cured film>

[0179] A first embodiment of the method for producing a cured film of the present invention comprises the following steps: a step of forming a photosensitive resin film made of the photosensitive resin composition of the present invention or the photosensitive resin sheet of the present invention on a substrate; a step of exposing the photosensitive resin film; a step of developing the exposed photosensitive resin film; and a step of heat-treating the developed photosensitive resin film at 200° C. or less.

[0180] The second embodiment of the method for producing a cured film of the present invention comprises the following steps: forming a photosensitive resin film made of the photosensitive resin composition of the present invention or the photosensitive resin sheet of the present invention on a substrate; exposing the photosensitive resin film; developing the exposed photosensitive resin film; and heat-treating the developed photosensitive resin film in an atmosphere having an oxygen concentration of 1% or more. In the present invention, oxygen concentration refers to volume concentration.

[0181] The steps of forming a photosensitive resin film, exposing the photosensitive resin film, and developing the exposed photosensitive resin film in the method for producing a cured film of the present invention are as described in the above section <Photosensitive resin film, photosensitive resin sheet>.

[0182] The first embodiment of the method for producing a cured film of the present invention comprises a step of heat-treating a photosensitive resin film at 200° C. or less. The photosensitive resin composition of the present invention contains a polyimide precursor (a) and a phenol compound (b), so that a cured film with a high imidization rate can be obtained even when heat-treated at 200° C. or less. In particular, when the photosensitive resin composition further contains a colorant (d), it is preferred to heat-treat at 200° C. or less from the viewpoint of more easily suppressing fading of the colorant (d).

[0183] In the method for producing a cured film of the present invention, the temperature in the heat treatment step may be increased stepwise or continuously.

[0184] In the method for producing a cured film of the present invention, from the viewpoint of further reducing the amount of outgassing generated from the cured film and improving the long-term reliability when the cured film is used as a planarization layer and / or an insulating layer of an organic EL display device, the atmosphere during heat curing is preferably an inert gas atmosphere. Specific examples of the inert gas include nitrogen gas, argon gas, and the like.

[0185] In the first aspect of the method for producing a cured film of the present invention, the oxygen concentration in the inert gas atmosphere is preferably 5% or less, more preferably 1% or less, further preferably 0.5% or less, particularly preferably 0.01% or less.

[0186] In the first embodiment of the method for manufacturing a cured film of the present invention, from the viewpoint of further reducing the amount of outgassing, the heating time in the heat treatment process is preferably 30 minutes or more. In addition, in the present invention, the so-called heating time refers to the holding time at the highest reached temperature in the heat treatment process. In addition, from the viewpoint of improving the film toughness of the cured film, it is preferably 3 hours or less. As a method for heat treatment, for example, a method of heat treatment at 200°C for 30 minutes, a method of heat treatment at 150°C and 200°C for 30 minutes each, a method of heat treatment while linearly heating from room temperature to 200°C over 2 hours, etc. can be cited.

[0187] The second embodiment of the method for producing a cured film of the present invention comprises a step of heat-treating the developed photosensitive resin film in an atmosphere with an oxygen concentration of 1% or more. The photosensitive resin composition of the present invention contains a polyimide precursor (a) and a phenol compound (b), so that the long-term reliability of the cured film when used as a planarization layer and / or an insulating layer of an organic EL display device can be improved, and thus heat curing can be suitably performed even at an oxygen concentration of 1% or more.

[0188] In the second aspect of the method for producing a cured film of the present invention, from the viewpoint of further reducing the amount of outgassing generated from the cured film, the temperature in the heat treatment step is preferably 180° C. or higher, more preferably 200° C. or higher, further preferably 230° C. or higher, and particularly preferably 250° C. or higher. On the other hand, from the viewpoint of improving the film toughness of the cured film, the temperature is preferably 500° C. or lower, more preferably 450° C. or lower.

[0189] In the second embodiment of the method for producing a cured film of the present invention, when the photosensitive resin composition further contains a colorant (d), the temperature in the heat treatment step is preferably 230° C. or less, and more preferably 200° C. or less, from the viewpoint of easily suppressing fading of the colorant (d).

[0190] In the second embodiment of the method for producing a cured film of the present invention, from the viewpoint of further reducing the amount of outgassing, the heating time in the heat treatment process is preferably 30 minutes or more. In addition, from the viewpoint of improving the film toughness of the cured film, it is preferably 3 hours or less. As the method of heat treatment, for example, a method of heat treatment at 250°C for 30 minutes, a method of heat treatment at 150°C and 250°C for 30 minutes each, a method of heat treatment while linearly increasing the temperature from room temperature to 300°C over 2 hours, etc. can be cited.

[0191] <Application examples of the photosensitive resin composition, the photosensitive resin sheet, and the cured film>

[0192] The photosensitive resin composition, photosensitive resin sheet and cured film of the present invention are suitable for use as surface protection layers, interlayer insulating layers, insulating layers of organic electroluminescence (EL) elements, planarization layers of thin film transistors (TFT) substrates for driving display devices using organic EL elements, wiring protection insulating layers of circuit substrates, on-chip microlenses of solid-state imaging elements, and planarization layers for various displays / solid-state imaging elements. For example, they are suitable as surface protection layers and interlayer insulating layers of MRAM with low heat resistance, polymer memories (PFRAM) expected to be the next generation of memories, phase change memories (PCRAM, Ovonics Unified Memory: OUM), etc. In addition, they can also be used in insulating layers of display devices including a first electrode formed on a substrate and a second electrode arranged opposite to the first electrode, such as LCDs, ECDs, ELDs, display devices using organic electroluminescent elements (organic electroluminescent devices), etc. The following description will be given by taking an organic EL display device, a semiconductor device, and a semiconductor electronic component as examples.

[0193] <Organic EL display device>

[0194] The organic EL display device of the present invention is an organic EL display device having a driving circuit, a planarization layer, a first electrode, an insulating layer, a light-emitting layer and a second electrode on a substrate, and the planarization layer and / or the insulating layer have a cured film of the present invention. Organic light-emitting materials are generally not resistant to gas components and moisture, and exposure to them causes a decrease in luminous brightness and pixel reduction. Here, the so-called pixel reduction refers to a phenomenon in which the luminous brightness from the end of the pixel decreases or becomes unlit. The organic EL display device of the present invention can improve long-term reliability by including the cured film of the present invention in the planarization layer and / or the insulating layer of the organic EL display device. In particular, since the insulating layer is adjacent to the organic light-emitting material, it has a greater impact on long-term reliability than the planarization layer. Therefore, in order to obtain an organic EL display device with high long-term reliability, it is preferred that at least the insulating layer contains the cured film of the present invention.

[0195] If an active matrix display device is taken as an example, a TFT and wiring located on the side of the TFT and connected to the TFT are provided on a substrate such as glass or various plastics, a planarization layer is provided thereon in a manner covering the concave and convex, and a display element is further provided on the planarization layer. The display element and the wiring are connected via contact holes formed in the planarization layer. In particular, in recent years, the flexibility of organic EL display devices has become the mainstream, so it is preferred that the organic EL display device has a substrate containing a resin film having the above-mentioned driving circuit. If a cured film obtained by curing the photosensitive resin composition or photosensitive sheet of the present invention is used as an insulating layer or a planarization layer of such a flexible display, the bending resistance is excellent, so it is particularly preferred to use it. From the viewpoint of improving the adhesion with the cured film obtained by curing the photosensitive resin composition or photosensitive sheet of the present invention, polyimide is particularly preferred as a resin film.

[0196] When the cured film of the present invention is used as the above-mentioned planarization layer, the film thickness is preferably 1.0 to 5.0 μm, and more preferably 2.0 μm or more. By making the planarization layer within the above range, the flatness of the TFTs and wirings that are densely packed due to high precision can be improved. If the planarization layer is thickened, the outgassing increases, which becomes the cause of the reduction in the long-term reliability of the organic EL display device, but the cured film of the present invention can improve the long-term reliability even when it is thickened. In addition, for high precision, TFTs and wirings can also be arranged along the film thickness direction, so the above-mentioned planarization layer is preferably multi-layered, and the above-mentioned planarization layer is more preferably composed of 2 to 5 layers.

[0197] exist Figure 2 A cross-sectional view of an example of a TFT substrate is shown in FIG. TFTs (thin film transistors) 1 of a bottom gate type or a top gate type are arranged in a matrix on a substrate 6, and a TFT insulating layer 3 is formed in a state of covering the TFTs 1. In addition, wiring 2 connected to the TFTs 1 is arranged on the TFT insulating layer 3. Further, a planarizing layer 4 is arranged in a state of burying the wiring 2 on the TFT insulating layer 3. A contact hole 7 reaching the wiring 2 is provided in the planarizing layer 4. Furthermore, an ITO (transparent electrode) 5 is formed on the planarizing layer 4 in a state of being connected to the wiring 2 via the contact hole 7. Here, the ITO 5 becomes an electrode of a display element (for example, an organic EL element). Furthermore, an insulating layer 8 is formed in a manner covering the periphery of the ITO 5. The organic EL element can be a top emission type that emits light from the opposite side of the substrate 6, or a bottom emission type that extracts light from the substrate 6 side. In this way, an active matrix organic EL display device is obtained in which the TFTs 1 used to drive each organic EL element are connected to each organic EL element.

[0198] Such a TFT insulating layer 3, planarizing layer 4 and / or insulating layer 8 can be formed as described above by the following steps: a step of forming a photosensitive resin film formed from the photosensitive resin composition or photosensitive resin sheet of the present invention; a step of exposing the photosensitive resin film; a step of developing the exposed photosensitive resin film; and a step of heat-treating the developed photosensitive resin film. An organic EL display device can be obtained by a manufacturing method having these steps.

[0199] <Electronic components>

[0200] The electronic component of the present invention has electrodes and metal wiring on a substrate and further has an interlayer insulating layer and / or a surface protective layer, and at least a portion of the interlayer insulating layer and / or the surface protective layer has the cured film of the present invention.

[0201] Specific examples of electronic components include active components including semiconductors such as transistors, diodes, integrated circuits (hereinafter, ICs), and memories, and passive components such as resistors, capacitors, and inductors. Hereinafter, electronic components using semiconductors may be referred to as semiconductor devices.

[0202] Specific examples of cured films within electronic components include passivation films of semiconductors, surface protective films of semiconductor elements, TFTs, etc., interlayer insulating films in multilayer wiring for high-density mounting of 2 to 10 layers, insulating films and protective films of touch panel displays, but are not limited to these and various structures can be used.

[0203] Taking a semiconductor device as an example, since the cured film of the present invention has excellent mechanical properties, stress from the sealing resin can be relaxed during mounting, and damage to the low-k layer can be suppressed, so that a highly reliable semiconductor device can be provided.

[0204] exist Figure 3 FIG. 1 is an enlarged cross-sectional view showing an example of a pad portion of a semiconductor device having a bump. An Al pad 10 for input and output and a passivation layer 11 having a through hole are formed on a silicon wafer 9. Further, an insulating layer 12 is formed on the passivation layer 11, and further, a metal layer 13 formed of Cr, Ti, etc. is formed in a manner connected to the Al pad 10, and a metal wiring 14 formed of Al, Cu, etc. is formed by electrolytic plating, etc. The pads are insulated by etching the metal layer 13 located around the solder bump 18. A barrier metal 16 and a solder bump 18 are formed on the insulated pad. When the insulating film 15 is processed, a scratch line 17 is formed.

[0205] Next, a method for manufacturing a semiconductor device will be described using the accompanying drawings. Figure 4An example of a method for manufacturing a semiconductor device with a bump is shown in FIG. In step 3a, the photosensitive resin composition of the present invention is applied on a silicon wafer 9 on which an Al pad 10 and a passivation layer 11 are formed, and a patterned insulating layer 12 is formed by a photolithography process. Next, in step 3b, a metal layer 13 is formed by a sputtering method. In step 3c, a metal wiring 14 is formed on the metal layer 13 by a plating method. Next, in step 3d', the photosensitive resin composition of the present invention is applied, and in step 3d, a pattern of an insulating layer 15 is formed by a photolithography process. At this time, the resin composition constituting the insulating layer 15 is processed into a thick film in the scratch line 17. Wiring (so-called rewiring) can be further formed on the insulating layer 15. In the case of forming a multilayer wiring structure with more than two layers, the above steps are repeated, so that a multilayer wiring structure in which more than two layers of rewiring are separated by an interlayer insulating layer constituted by the cured film of the present invention can be formed. There is no upper limit to the number of layers of the multilayer wiring structure, but materials with less than 10 layers are often used. Next, in step 3e, barrier metal 16 is formed, and in step 3f, solder bumps 18 are formed. Furthermore, by dicing along the final scribe line 17 to separate into individual pieces, semiconductor devices having bumps can be obtained.

[0206] Example

[0207] Hereinafter, the present invention will be described with reference to Examples etc., but the present invention is not limited to these Examples. In addition, each evaluation in the Examples was performed by the following methods.

[0208] (1) Imidization rate

[0209] The varnish obtained by each example and comparative example was applied to a silicon wafer by spin coating at an arbitrary rotation speed using a spin coater (MS-A100; manufactured by Mikasa Co., Ltd.). Next, it was baked at 120°C for 2 minutes using a hot plate (SCW-636; manufactured by Dainippon Screen Manufacturing Co., Ltd.) to prepare a pre-baked film with a film thickness of 2.0 μm. In addition, the film thickness was measured using a Lamdace STM-602 manufactured by Dainippon Screen Manufacturing Co., Ltd. under the condition of a refractive index of 1.63. The obtained prebaked film was cut into three pieces, the first one was not subjected to any treatment, the second one was heat-treated at 200°C in a nitrogen atmosphere with an oxygen concentration of 0.01% for 1 hour using an inert oven CLH-21CD-S (manufactured by Koyo Sound System Co., Ltd.), and the third one was heat-treated at 250°C in a nitrogen atmosphere with an oxygen concentration of 0.01% for 1 hour to produce a photosensitive resin composition prebaked film and cured films at 200°C and 250°C.

[0210] The infrared absorption spectra of the obtained prebaked film, 200°C and 250°C cured films were obtained by the ATR method using a Fourier transform infrared spectrophotometer (manufactured by JASCO Corporation). Based on the mathematical formula (5), the cured film after heating at 250°C for 1 hour was set to an imidization rate of 100%, and the 1371 cm-1 wavelength derived from the polyimide CNC of each sample was used as the infrared absorption spectra of the obtained prebaked film, 200°C and 250°C cured films. -1 The absorption intensity (A(1371cm -1 )) and 1437cm -1 The absorption intensity (A(1437cm -1 )) to calculate the imidization rate (%) of each of the prebaked film and the cured film at 200°C. In mathematical formula (5), X (%) represents the imidization rate. When the imidization rate of the cured film at 200°C is 90% or more, it is judged as "A", when it is less than 90% and 75% or more, it is judged as "B", and when it is less than 75%, it is judged as "C". In addition, even if the imidization rate of the cured film at 200°C is 75% or more, it is judged as "C" when the imidization rate of the prebaked film is 30% or more.

[0211]

[0212] (2) Sensitivity (pattern processing)

[0213] The varnish obtained by each embodiment and comparative example was applied on an 8-inch silicon wafer by spin coating using a coating and developing device ACT-8 (manufactured by Tokyo Electron Co., Ltd.), and baked at 120°C for 2 minutes to produce a pre-baked film with a film thickness of 3.0 μm. In addition, the film thickness was measured using a Lamdace STM-602 manufactured by Dainippon Screen Manufacturing Co., Ltd. under the condition of a refractive index of 1.63. Then, an exposure machine, an i-ray stepper exposure machine NSR-2005i9C (manufactured by Nikon Co., Ltd.), was used to expose the film at an exposure amount of 50 to 300 mJ / cm through a mask having a pattern of contact holes of 10 μm. 2 The range is 5mJ / cm 2 After exposure, the film was developed using the above-mentioned ACT-8 developing device with a 2.38 mass % tetramethylammonium aqueous solution (hereinafter referred to as TMAH, manufactured by Tama Chemical Industry Co., Ltd.) as a developer until the film reduction amount became 0.5 μm, and then rinsed with distilled water and twirled to dry to obtain a pattern.

[0214] The obtained pattern was observed at a magnification of 20 times using an FDP microscope MX61 (manufactured by Orinpass Co., Ltd.) to measure the opening diameter of the contact hole. The minimum exposure amount at which the opening diameter of the contact hole reached 10 μm was determined and defined as the sensitivity. When the sensitivity was less than 150 mJ / cm 2In the case of 150mJ / cm 2 Above and less than 200mJ / cm 2 In the case of 200mJ / cm 2 Above and less than 250mJ / cm 2 In the case of 250mJ / m 2 The above cases are judged as "C".

[0215] (3)Residual film rate

[0216] The pre-baked film with a thickness of 3.0 μm obtained by the same operation as the sensitivity evaluation (2) was developed using an ACT-8 developing device, using a 2.38 mass % TMAH aqueous solution as a developer, and after developing for 60 seconds, it was rinsed with distilled water and swung dry to obtain a developed film. The ratio of the film thickness of the developed film to the film thickness of the pre-baked film was set as the residual film rate (residual film rate = (film thickness of the developed film) / (film thickness of the pre-baked film) × 100). When the residual film rate is 80% or more, it is judged as "A", when it is less than 80% and 65% or more, it is judged as "B", and when it is less than 65%, it is judged as "C".

[0217] (4) Long-term reliability evaluation of organic EL display devices

[0218] exist Figure 5A schematic diagram of the steps for making an organic EL display device is shown in the figure. First, a 10 nm ITO transparent conductive film is formed on the entire surface of a 38 mm × 46 mm alkali-free glass substrate 19 by sputtering, and then etched as a first electrode (transparent electrode) 20. At the same time, an auxiliary electrode 21 for taking out the second electrode is also formed. The obtained substrate is ultrasonically cleaned with Semico Clean 56 (trade name, manufactured by Fruuchi Chemical Co., Ltd.) for 10 minutes, and then washed with ultrapure water. Next, the photosensitive resin composition shown in Tables 2 and 3 is applied to the entire surface of the substrate by spin coating, and pre-baked on a hot plate at 120°C for 2 minutes. After the film is exposed to UV through a photomask, it is developed with a 2.38 mass % TMAH aqueous solution to dissolve the unnecessary parts and rinsed with pure water. The obtained resin pattern was heat treated at 200°C for 1 hour in a nitrogen atmosphere with an oxygen concentration of 0.01% using an inert oven CLH-21CD-S (manufactured by Koyo Sound System Co., Ltd.). In this way, openings with a width of 70 μm and a length of 260 μm were arranged at a spacing of 155 μm in the width direction, and openings with a width of 70 μm and a length of 260 μm were arranged at a spacing of 465 μm in the length direction. Each opening was limited to the effective area of ​​the substrate to form an insulating layer 22 in a shape that exposed the first electrode. In this way, an insulating layer with an insulating layer opening ratio of 25% was formed in the effective area of ​​the substrate in a quadrilateral with a side length of 16 mm. The thickness of the insulating layer is about 1.0 μm.

[0219] Next, after nitrogen plasma treatment as a pretreatment, the organic EL layer 23 including the light-emitting layer was formed by vacuum deposition. The vacuum degree during deposition was 1×10 -3 Pa or less, and the substrate is rotated relative to the deposition source during the evaporation. First, 10 nm of compound (HT-1) is evaporated as a hole injection layer, and 50 nm of compound (HT-2) is evaporated as a hole transport layer. Next, on the light-emitting layer, the compound (GH-1) as the main material and the compound (GD-1) as the doping material are evaporated to a thickness of 40 nm in such a way that the doping concentration becomes 10%. Next, the compound (ET-1) as the electron transport material and the compound (LiQ) are stacked with a volume ratio of 1:1 to a thickness of 40 nm. The structure of the compounds used in the organic EL layer is shown below.

[0220]

[0221] Next, after evaporating the compound (LiQ) 2nm, Mg and Ag were evaporated at a volume ratio of 10:1 for 10nm to form a second electrode (non-transparent electrode) 24. Finally, the cover glass plate was bonded with an epoxy resin adhesive in a low-humidity nitrogen atmosphere to seal it, and a top-emitting organic EL display device with four quadrilaterals with a side length of 5mm was produced on one substrate. In addition, the film thickness here refers to the display value of the crystal vibration film thickness monitor.

[0222] The prepared organic EL display device was placed on a hot plate heated to 80°C with the light-emitting surface facing up and irradiated with a wavelength of 365 nm and an illuminance of 0.6 mW / cm 2 UV light. Immediately after irradiation (0 hour), 250 hours, 500 hours, and 1000 hours later, the organic EL display device was driven by a DC current of 0.625 mA to emit light, and the area ratio of the light-emitting portion relative to the area of ​​the light-emitting pixel (pixel light-emitting area ratio) was measured. As the pixel light-emitting area ratio after 1000 hours obtained by this evaluation method, it was judged as "S" when it was 80% or more, "A" when it was less than 80% and more than 70%, "B" when it was less than 70% and more than 60%, and "C" when it was less than 60%.

[0223] Synthesis Example 1 Synthesis of a hydroxyl-containing diamine compound (α)

[0224] 18.3 g (0.05 mol) of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (hereinafter referred to as BAHF) was dissolved in 100 mL of acetone and 17.4 g (0.3 mol) of propylene oxide, and the mixture was cooled to -15°C. A solution of 20.4 g (0.11 mol) of 3-nitrobenzoyl chloride dissolved in 100 mL of acetone was added dropwise thereto. After the addition was completed, the mixture was reacted at -15°C for 4 hours, and then returned to room temperature. The precipitated white solid was separated by filtration and dried in vacuo at 50°C.

[0225] 30 g of the solid was added to a 300 mL stainless steel autoclave, dispersed in 250 mL of methyl cellosolve, and 2 g of 5% palladium-carbon was added. Hydrogen was introduced into the autoclave using a balloon, and the reduction reaction was carried out at room temperature. After about 2 hours, it was confirmed that the balloon was no longer deflated and the reaction was terminated. After the reaction was completed, the palladium compound used as a catalyst was removed by filtration, and concentrated using a rotary evaporator to obtain a hydroxyl-containing diamine compound (α) (Ip7.16 eV, calculated value) shown in the following formula.

[0226]

[0227] Synthesis Example 2 Synthesis of Quinone Diazo Compound (c-1)

[0228] Under a dry nitrogen stream, 21.22 g (0.05 mol) of TrisP-PA (trade name, manufactured by Honshu Chemical Industry Co., Ltd.) and 36.27 g (0.135 mol) of 5-naphthoquinonediazidesulfonyl chloride were dissolved in 1,4-dihydroquinone. 450 g of alkane was added to the mixture and the temperature was set to room temperature. 1,4-dioxane was added dropwise so that the temperature in the system did not rise above 35°C. 15.18 g of triethylamine was mixed with 50 g of oxane. After the addition, the mixture was stirred at 30°C for 2 hours. The triethylamine salt was filtered and the filtrate was poured into water. Then, the precipitate was collected by filtration. The precipitate was dried in a vacuum dryer to obtain a quinone diazonium compound (c-1) represented by the following formula.

[0229]

[0230] Synthesis Example 3 Synthesis of Alkali-Soluble Resin (a-1)

[0231] Under a dry nitrogen stream, ODPA31.02g (0.10 mol) was dissolved in NMP500g. BAHF23.81g (0.065 mol), o-tolidine4.25g (0.02 mol), and SiDA1.24g (0.005 mol) were added together with NMP50g, and the mixture was reacted at 40°C for 2 hours. Next, MAP2.18g (0.02 mol) as a capping agent was added together with NMP5g, and the mixture was reacted at 50°C for 2 hours. Then, a solution in which 32.39g (0.22 mol) of N,N-dimethylformamide diethyl acetal was diluted with NMP50g was added. After addition, the mixture was stirred at 50°C for 3 hours. After the stirring was completed, the solution was cooled to room temperature, and then the solution was added to 3L of water to obtain a white precipitate. The precipitate was collected by filtration, washed with water three times, and then dried in a vacuum dryer at 80° C. for 24 hours to obtain a polyimide precursor (a-1).

[0232] Synthesis Examples 4 to 15, Comparative Synthesis Examples 1 to 3

[0233] Except having changed the amine component and the acid component as described in Table 1, it carried out similarly to Synthesis Example 3, and obtained the polyimide precursor (a-2) - (a-13), (a'-1) - (a'-3).

[0234] The names of the compounds used in the respective synthesis examples, comparative synthesis examples, examples, and comparative examples, and the structural formulas of HMOM-TPHAP and VG3101L are shown below.

[0235] o-Tolidine: o-Tolidine (Ip 6.58 eV, literature value)

[0236] DAE: 4,4'-diaminodiphenyl ether (Ip 6.78 eV, literature value) (diamine with ether bond)

[0237] MDA: 4,4'-diaminodiphenylmethane (Ip 6.94 eV, literature value)

[0238] TDE-R: 1,3-bis(4-aminophenoxy)benzene (Ip 7.08 eV, calculated value) (diamine having an ether bond)

[0239] BAHF: 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (Ip 7.88 eV, calculated value)

[0240] SiDA: 1,3-bis(3-aminopropyl)tetramethyldisiloxane (Ip 8.03 eV, calculated value)

[0241] MAP: 3-aminophenol

[0242] ODPA: 3,3',4,4'-diphenyl ether tetracarboxylic dianhydride

[0243] 6FDA: 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane dianhydride

[0244] b-1: Bisphenol AF (pKa = 10.8) (a phenol compound (b) having an electron-withdrawing group satisfying the requirements of (b1) and (b2))

[0245] b-2: Bisphenol S (pKa = 9.8) (phenol compound (b) having an electron-withdrawing group satisfying the requirements of (b1) and (b2))

[0246] b-3: 4,4'-dihydroxybenzophenone (pKa = 11.3) (phenol compound (b) having an electron-withdrawing group satisfying the requirement of (b2))

[0247] b-4: 4-(Trifluoromethyl)phenol (pKa=10.5) (phenol compound (b) having an electron-withdrawing group satisfying the requirement of (b1))

[0248] b-5: 3-(Trifluoromethyl)phenol (pKa=11.2) (phenol compound (b) having an electron-withdrawing group)

[0249] b'-1: bisphenol A (pKa = 11.6) (phenol compound having no electron-withdrawing group)

[0250] b'-2: p-cresol (pKa=12.8) (phenol compound without electron-withdrawing group)

[0251] GBL: gamma-butyrolactone

[0252] NMP: N-methylpyrrolidone

[0253] TsOH: p-Toluenesulfonic acid

[0254] DBU: 1,8-diazabicyclo[5.4.0]-7-undecene

[0255]

[0256] Example 1

[0257] 10.0 g of polyimide precursor (a-1), 2.0 g of phenol compound (b-1), and 2.0 g of quinone diazide compound (c-1) were added to 30 g of GBL to obtain a varnish of a positive photosensitive resin composition. The obtained varnish was used to evaluate the imidization rate, sensitivity, residual film rate, and long-term reliability of the organic EL display device as described above.

[0258] Examples 2 to 23, Comparative Examples 1 to 7, Comparative Examples 10 to 15

[0259] A varnish of a positive photosensitive resin composition was obtained in the same manner as in Example 1 except that the polyimide precursor (a), the phenol compound (b), the photosensitive compound (c), and other additives were changed as shown in Table 2. Using the obtained varnish, the imidization rate, sensitivity, residual film rate, and long-term reliability of the organic EL display device were evaluated as described above.

[0260] Embodiment 24

[0261] The long-term reliability of the organic EL display device was evaluated in the same manner as in Example 2, except that the varnish obtained in Example 2 was used and the heating temperature of the resin pattern was changed from 200° C. to 250° C.

[0262] Embodiment 25

[0263] The long-term reliability of the organic EL display device was evaluated in the same manner as in Example 2 except that the varnish obtained in Example 2 was used and the heat treatment atmosphere of the resin pattern was changed from a nitrogen atmosphere with an oxygen concentration of 0.01% to a nitrogen atmosphere with an oxygen concentration of 1%.

[0264] Embodiment 26

[0265] The long-term reliability of the organic EL display device was evaluated in the same manner as in Example 2 except that the varnish obtained in Example 2 was used and the heat treatment atmosphere of the resin pattern was changed from a nitrogen atmosphere with an oxygen concentration of 0.01% to a nitrogen atmosphere with an oxygen concentration of 5%.

[0266] Embodiment 27

[0267] The long-term reliability of the organic EL display device was evaluated in the same manner as in Example 2 except that the varnish obtained in Example 2 was used and the heat treatment atmosphere of the resin pattern was changed from a nitrogen atmosphere with an oxygen concentration of 0.01% to an air atmosphere with an oxygen concentration of 21%.

[0268] Embodiment 28

[0269] 10.0 g of a polyimide precursor (a-2), 2.0 g of a phenol compound (b-1), 2.0 g of a quinone diazine compound (c-1), 2.5 g of 4,4',4"-methylenetriphenol (e-1), 1.5 g of Valifast Red 1308 (d1-2-1), and 2.5 g of Oil Blue 613 (d1-3-1) were added to 30 g of GBL to obtain a varnish of a positive photosensitive resin composition. Using the obtained varnish, the imidization rate, sensitivity, residual film rate, and long-term reliability of the organic EL display device were evaluated as described above. In addition, the heat treatment atmosphere of the resin pattern was an air atmosphere with an oxygen concentration of 21%, and the heat treatment temperature was set to 200°C.

[0270] Next, a cured film having a film thickness of 1.0 μm and subjected to a heat treatment at 200° C. was prepared on an alkali-free glass substrate by the same method as in (1) for the imidization ratio. The incident light intensity (I0) and the transmitted light intensity (I) of the prepared cured film were measured using a transmission densitometer (X-Rite 361T (V); manufactured by X-Rite). The OD value was calculated as an index of light-shielding properties by the following formula, and the OD value was 0.6.

[0271] OD value = log 10 (I0 / I).

[0272] Embodiment 29

[0273] The long-term reliability of the organic EL display device was evaluated in the same manner as in Example 28, except that the varnish obtained in Example 28 was used and the heat treatment temperature of the resin pattern was changed from 200° C. to 250° C.

[0274] Next, the OD value of the cured film was calculated in the same manner as in Example 28 except that the heat treatment temperature was changed from 200° C. to 250° C. As a result, fading of a part of the colorant progressed during the heat treatment, and the OD value was 0.3.

[0275] Comparative Example 8

[0276] 10.0 g of the polyimide precursor (a'-1) and 2.0 g of the quinone diazine compound (c-1) were added to 30 g of GBL. 1.0 g of TsOH was added thereto to obtain a varnish of a positive photosensitive resin composition. The obtained varnish was used to evaluate the imidization rate, sensitivity, residual film rate, and long-term reliability of the organic EL display device as described above.

[0277] Comparative Example 9

[0278] 10.0 g of the polyimide precursor (a'-1) and 2.0 g of the quinone diazide compound (c-1) were added to 30 g of GBL, and 1.0 g of DBU was added thereto. As a result, the varnish turned black and a decomposition product of the quinone diazide compound was precipitated, so the evaluation was stopped.

[0279] Comparative Example 16

[0280] The long-term reliability of the organic EL display device was evaluated in the same manner as in Comparative Example 1, except that the heat treatment temperature of the resin pattern was changed from 200° C. to 250° C., using the varnish obtained in Comparative Example 1.

[0281] Comparative Example 17

[0282] The long-term reliability of the organic EL display device was evaluated in the same manner as in Comparative Example 1 except that the varnish obtained in Comparative Example 1 was used and the heat treatment atmosphere of the resin pattern was changed from an oxygen concentration of 0.01% to a nitrogen atmosphere of 1%.

[0283] Comparative Example 18

[0284] The long-term reliability of the organic EL display device was evaluated in the same manner as in Comparative Example 1 except that the varnish obtained in Comparative Example 1 was used and the heat treatment atmosphere of the resin pattern was changed from an oxygen concentration of 0.01% to a nitrogen atmosphere of 5%.

[0285] Comparative Example 19

[0286] The long-term reliability of the organic EL display device was evaluated in the same manner as in Comparative Example 1 except that the varnish obtained in Comparative Example 1 was used and the heat treatment atmosphere of the resin pattern was changed from a nitrogen atmosphere with an oxygen concentration of 0.01% to an air atmosphere with an oxygen concentration of 21%.

[0287] The composition and evaluation results of each example and comparative example are shown in Tables 2 to 5.

[0288] [Table 1]

[0289]

[0290] [Table 2-1]

[0291]

Table 2-1

[0292]

[0293] [Table 2-2]

[0294]

Table 2-2

[0295]

[0296] [Table 3]

[0297]

Table 3

[0298]

[0299] [Table 4-1]

[0300]

[0301] [Table 4-2]

[0302]

[0303] [Table 5-1]

[0304]

[0305] [Table 5-2]

[0306]

[0307] Description of Reference Numerals

[0308] 1: TFT (Thin Film Transistor)

[0309] 2: Wiring

[0310] 3: TFT insulation layer

[0311] 4: Flattening layer

[0312] 5: ITO (transparent electrode)

[0313] 6: Substrate

[0314] 7: Contact hole

[0315] 8: Insulation layer

[0316] 9: Silicon wafer

[0317] 10: Al liner

[0318] 11: Passivation layer

[0319] 12: Insulation layer

[0320] 13: Metal (Cr, Ti, etc.) layer

[0321] 14: Metal wiring (Al, Cu, etc.)

[0322] 15: Insulation layer

[0323] 16: Barrier Metal

[0324] 17: Scratch Line

[0325] 18: Solder Bump

[0326] 19: Alkali-free glass substrate

[0327] 20: First electrode (transparent electrode)

[0328] 21: Auxiliary electrode

[0329] 22: Insulation layer

[0330] 23: Organic EL layer

[0331] 24: Second electrode (non-transparent electrode).

Claims

1. A photosensitive resin composition comprising a polyimide precursor (a), a phenol compound (b) having an electron-withdrawing group, and a photosensitive compound (c), wherein the polyimide precursor (a) has a residue derived from a diamine having an ionization potential of less than 7.1 eV, The phenol compound (b) having an electron-withdrawing group includes a compound (b2) represented by the general formula (1), In the general formula (1), A represents a divalent group selected from the structures represented by the general formula (2), a and b each independently represent an integer of 0 to 3, and a+b is an integer of 2 to 4; in the general formula (2), R 1 and R 2 each independently represents a halogen atom or a monovalent organic group having 1 to 20 carbon atoms substituted with a halogen atom, The content of the residue derived from the diamine having an ionization potential of less than 7.1 eV is 5 to 50 mol% in 100 mol% of the diamine residues constituting the polyimide precursor (a). The content of the phenol compound (b) having an electron-withdrawing group is 1 to 50 parts by mass relative to 100 parts by mass of the polyimide precursor (a). The photosensitive compound (c) is selected from a photoacid generator (c1) and a photopolymerization initiator (c2). 2 . The photosensitive resin composition according to claim 1 , wherein the residue derived from the diamine having an ionization potential of less than 7.1 eV has an ether bond.

3. The photosensitive resin composition according to claim 1, wherein the diamine having an ionization potential of less than 7.1 eV comprises one or more diamines selected from 4,4'-diaminodiphenyl ether, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, and 1,3-bis(4-aminophenoxy)benzene. 4 . The photosensitive resin composition according to claim 1 , wherein the phenol compound (b) having an electron-withdrawing group comprises a compound (b1) having a phenolic hydroxyl group and having a pKa of 11.0 or less. The photosensitive resin composition according to claim 1 , further comprising a colorant (d). 6 . A photosensitive resin sheet comprising the photosensitive resin composition according to claim 1 . 7 . A cured film obtained by curing the photosensitive resin composition according to claim 1 or the photosensitive resin sheet according to claim 6 .

8. A method for producing a cured film, comprising the following steps: forming a photosensitive resin film made of the photosensitive resin composition according to any one of claims 1 to 5 or the photosensitive resin sheet according to claim 6 on a substrate; exposing the photosensitive resin film; developing the exposed photosensitive resin film; and heating the developed photosensitive resin film at a temperature below 200°C.

9. A method for producing a cured film, comprising the following steps: forming a photosensitive resin film made of the photosensitive resin composition according to any one of claims 1 to 5 or the photosensitive resin sheet according to claim 6 on a substrate; exposing the photosensitive resin film; developing the exposed photosensitive resin film; and heat-treating the developed photosensitive resin film in an atmosphere with an oxygen concentration of 1% or more.

10. An organic EL display device comprising a drive circuit, a planarization layer, a first electrode, an insulating layer, a light-emitting layer and a second electrode on a substrate, wherein the planarization layer and / or the insulating layer comprises the cured film according to claim 7. 11 . The organic EL display device according to claim 10 , wherein the planarization layer is composed of 2 to 5 layers.

12. An electronic component comprising electrodes and metal wirings on a substrate and further comprising an interlayer insulating layer and / or a surface protective layer, wherein the cured film according to claim 7 is present on at least a portion of the interlayer insulating layer and / or the surface protective layer.

Citation Information

Patent Citations

  • Process for preparing butyl-p-benzoylbenzoates

    EP0000502A1

  • Photosensitive resin composition and method for producing cured relief pattern

    WO2018037997A1

  • Positive photosensitive resin composition

    JP2011197362A

  • Resin composition

    JP2015004000A

  • Photosensitive resin composition, method for manufacturing cured relief pattern, and semiconductor apparatus

    WO2017170600A1