Cathode catalyst layer of fuel cell and fuel cell

By adopting a two-layer structure in the cathode catalyst layer of the fuel cell, the load density and composition of the catalyst are optimized, and the problems of increasing the catalyst particle size and decreasing proton conductivity are solved, and the power generation performance and gas diffusion properties of the fuel cell are improved. .

CN113544884BActive Publication Date: 2024-11-05PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080018396.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-05
Filing Date
2020-02-26
Publication Date
2024-11-05
Estimated Expiration
2040-02-26

AI Technical Summary

Technical Problem

When using a proton-conducting polymer electrolyte membrane, the catalyst support density of the existing fuel cell cathode catalyst layer increases the catalyst particle size, the reaction area decreases, and the proton conductivity decreases under low humidification conditions, resulting in a decrease in the catalyst particle size, resulting in a decrease in the catalyst particle size, which causes a decrease in the reaction area. Fuel cell performance declines.

Method used

A cathode catalyst layer adopts a two-layer structure, the first layer includes a first particle-like conductive member, a first catalyst particle and a first fibrous conductive member, the second layer includes a second particle-like conductive member and a second catalyst particle, the second The catalyst support density is greater than the first catalyst support density, and the utilization efficiency and gas diffusion properties of the catalyst are improved by optimizing the configuration of the catalyst layer.

Benefits of technology

The power generation performance of the fuel cell is improved, especially under low humidification conditions, the performance reduction is suppressed, the reaction efficiency and gas diffusion of the catalyst are enhanced, and the increase in the catalyst particle size and the increase in the proton movement resistance are avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113544884B_ABST
    Figure CN113544884B_ABST
Patent Text Reader

Abstract

The cathode catalyst layer (121) includes two layers, namely, a first catalyst layer (121A) on the gas diffusion layer side and a second catalyst layer (121B) on the electrolyte membrane (110) side. The first catalyst layer (121A) includes a first particle-shaped conductive member (123), a first catalyst particle (124) and a first fiber-shaped conductive member (125), and at least a portion of the first catalyst particle is supported on the first particle-shaped conductive member. The second catalyst layer (121B) includes a second particle-shaped conductive member (126) and a second catalyst particle (127), and at least a portion of the second catalyst particle is supported on the second particle-shaped conductive member. The catalyst supporting density D2 of the second catalyst particle in the second particle-shaped conductive member is greater than the catalyst supporting density D1 of the first catalyst particle in the first particle-shaped conductive member.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a cathode catalyst layer of a fuel cell and a fuel cell. Background Art

[0002] The fuel cell includes a membrane electrode assembly having an electrolyte membrane and a pair of electrodes sandwiching the electrolyte membrane. The pair of electrodes each includes a catalyst layer and a gas diffusion layer in this order from the electrolyte membrane side.

[0003] As the catalyst layer on the cathode side, Patent Document 1 discloses the following structure: a two-layer structure of a first layer on the electrolyte membrane side and a second layer on the gas diffusion layer side is formed, so that the loading density of the catalyst in the first layer relative to the catalyst support is 3 to 6 times the loading density of the catalyst in the second layer relative to the catalyst support.

[0004] However, when a proton-conductive polymer electrolyte membrane is used as the electrolyte membrane, water is required to improve the proton conductivity of the polymer electrolyte membrane. Therefore, water is usually supplied to the catalyst layer on the basis of humidifying the fuel gas or the oxidizing gas. In this case, a device (humidifier) ​​for generating water vapor gas and humidifying the fuel gas or the oxidizing gas is usually provided separately from the fuel cell unit.

[0005] On the other hand, it is desirable to be able to use a fuel cell even in an environment where sufficient space for installing a humidifier cannot be secured. In addition, it is also desirable to miniaturize the humidifier. Therefore, it is desirable to have a fuel cell with high output performance under low humidification conditions (for example, relative humidity 20% to 40%).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2010-73419 Summary of the invention

[0009] Problems to be solved by the invention

[0010] When the cathode catalyst layer is configured as a two-layer structure with different catalyst loading densities as in Patent Document 1, if only the catalyst loading density on the electrolyte membrane side is increased, the increase in catalyst loading density may increase the catalyst particle size and reduce the reaction area.

[0011] On the other hand, when the catalyst loading density on the gas diffusion layer side is reduced, in order to obtain the same catalyst reaction, the thickness of the catalyst layer needs to be increased. For example, when the catalyst loading density is reduced to about 1 / 3, in order to keep the catalyst loading amount the same, the thickness of the catalyst layer needs to be increased to about 3 times. As a result, the resistance to proton migration may increase.

[0012] Means for solving problems

[0013] One aspect of the present invention relates to a cathode catalyst layer of a fuel cell, comprising: a first catalyst layer and a second catalyst layer, wherein the first catalyst layer comprises a first particle-shaped conductive member, a first catalyst particle and a first fiber-shaped conductive member, at least a portion of the first catalyst particle is supported on the first particle-shaped conductive member, and the second catalyst layer comprises a second particle-shaped conductive member and a second catalyst particle, at least a portion of the second catalyst particle is supported on the second particle-shaped conductive member, and a second catalyst supporting density D 2 Greater than the first catalyst loading density D 1 , the second catalyst loading density D 2 The first catalyst loading density D is expressed as the ratio of the mass of the second catalyst particles carried on the second particle-shaped conductive member to the total mass of the second catalyst particles carried on the second particle-shaped conductive member and the second particle-shaped conductive member. 1 The mass of the first catalyst particles carried on the first particulate conductive member is expressed as a ratio of the mass of the first catalyst particles carried on the first particulate conductive member to the total mass of the first catalyst particles carried on the first particulate conductive member and the first particulate conductive member.

[0014] Another aspect of the present invention relates to a fuel cell comprising: a cathode having the cathode catalyst layer; an anode; and an electrolyte membrane interposed between the cathode and the anode, wherein the second catalyst layer is interposed between the first catalyst layer and the electrolyte membrane.

[0015] Effects of the Invention

[0016] According to the present invention, the utilization efficiency of the cathode catalyst is improved, and the power generation performance of the fuel cell can be improved.

[0017] The novel features of the present invention are described in the attached technical solutions, which relate to both the structure and the content of the present invention, and together with other objects and features of the present invention, can be better understood through the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1It is a cross-sectional view schematically showing the structure of a single cell of a fuel cell according to an embodiment of the present invention.

[0019] Figure 2 This is a diagram schematically showing the interior of a catalyst layer according to an embodiment of the present invention. DETAILED DESCRIPTION

[0020] The cathode catalyst layer of the fuel cell of the embodiment of the present invention is a two-layer structure having a first catalyst layer and a second catalyst layer. The first catalyst layer includes a first particle-shaped conductive member, a first catalyst particle and a first fibrous conductive member, and at least a portion of the first catalyst particle is supported on the first particle-shaped conductive member. The second catalyst layer includes a second particle-shaped conductive member and a second catalyst particle, and at least a portion of the second catalyst particle is supported on the second particle-shaped conductive member. It should be noted that, in the case of constituting a fuel cell, the electrolyte membrane and the cathode catalyst layer are stacked in such a manner that the second catalyst layer of the cathode catalyst layer is located on the electrolyte membrane side. A gas diffusion layer can be stacked on the first catalyst layer side of the cathode catalyst layer.

[0021] Here, the ratio of the mass of the first catalyst particles supported on the first particulate conductive member to the total mass of the first catalyst particles supported on the first particulate conductive member and the first particulate conductive member is referred to as the first catalyst supporting density D. 1 The ratio of the mass of the second catalyst particles supported on the second particulate conductive member to the total mass of the second catalyst particles supported on the second particulate conductive member and the second particulate conductive member is defined as the second catalyst supporting density D. 2 The second catalyst loading density is greater than the first catalyst loading density (D 1 <D 2 ).

[0022] When the fuel cell generates electricity, protons (hydrogen ions) react with oxide ions in the cathode catalyst layer to generate water. Oxide ions are generated by the oxidizing gas (e.g., air) supplied from the first catalyst layer side through the catalytic reaction of the catalyst disposed in the cathode catalyst layer. On the other hand, protons are generated in the anode and diffuse to the cathode catalyst layer through the electrolyte membrane. Therefore, the proton concentration on the side of the cathode catalyst layer close to the electrolyte membrane tends to be higher than the side away from the electrolyte membrane, and the catalyst reaction tends to be concentrated on the side close to the electrolyte membrane.

[0023] Therefore, by setting the catalyst loading density D of the second catalyst layer disposed on the electrolyte membrane side 2 The catalyst loading density D of the first catalyst layer is 1 Large, can improve the utilization efficiency of the catalyst.

[0024] In particular, under low-humidification power generation conditions, proton conductivity decreases, so it is difficult for protons to diffuse to an area far from the electrolyte membrane in the cathode catalyst layer, and the deviation of the distribution of proton concentration in the thickness direction of the cathode catalyst layer tends to become significant. Therefore, on the side close to the electrolyte membrane, the concentration of the catalyst reaction tends to become further increased. Under low-humidification conditions, for example, the following situation may also occur: the thickness of the cathode catalyst layer is set to T, and 3 / 4 of the total power generation current is generated in an area of ​​T / 4 thickness on the electrolyte membrane side of the cathode catalyst layer. According to the configuration of the present invention, even under such low-humidification conditions, the performance degradation of the fuel cell can be suppressed.

[0025] However, as the catalyst loading density of the first catalyst layer is reduced, the thickness of the first catalyst layer tends to become thicker. As a result, the gas diffusivity is reduced, and sometimes the resistance to proton movement increases. In this embodiment, the gas diffusivity is improved by including the first fibrous conductive member in the first catalyst layer, and the increase in the resistance to proton movement is suppressed. In addition, water generated by power generation is easily discharged.

[0026] In the first catalyst layer, the first catalyst particles can be carried on the first fibrous conductive member. However, the lower the catalyst loading density of the first fibrous conductive member, the higher the hydrophobicity of the first fibrous conductive member becomes. Therefore, the lower the catalyst loading density of the first fibrous conductive member, the higher the water drainage of the first catalyst layer, and the higher the gas diffusivity can be improved. The first catalyst particles are preferably not substantially carried on the first fibrous conductive member, but are substantially only carried on the first particle-shaped conductive member. Here, in the case where the proportion of the mass of the first catalyst particles carried on the first fibrous conductive member in the overall mass of the first catalyst particles is less than 0.5%, it can be said that the first catalyst particles are substantially only carried on the first particle-shaped conductive member.

[0027] The second catalyst loading density D 2 The first catalyst loading density D 1 The second catalyst loading density D 2 When the lower limit of is as described above, the utilization efficiency of the catalyst can be easily improved.

[0028] The second catalyst loading density D 2 The first catalyst loading density D 1 When the ratio of the second catalyst loading density to the first catalyst loading density is too large, the particle size of the second catalyst particles may increase, and the reaction area may decrease. In addition, the overall thickness of the cathode catalyst layer may become too thick, and the resistance to the movement of protons may increase. 2is the first catalyst loading density D 1 The second catalyst loading density D is less than 3 times of that of the cathode catalyst layer, which can suppress the increase in the particle size of the catalyst particles and the decrease in the catalyst reaction area. In addition, the thickness of the cathode catalyst layer as a whole becomes an appropriate thickness, which can suppress the increase in the proton transfer resistance. 2 The first catalyst loading density D 1 Less than 2 times.

[0029] The second catalyst loading density D 2 For example, it is 20% to 60%. 2 On the other hand, by increasing the second catalyst loading density D 2 By limiting the catalyst loading density to 60% or less, the increase in the particle size of the catalyst particles can be suppressed, and the decrease in the reaction area can be suppressed. 2 It may be 30% to 60% or 30% to 50%.

[0030] In contrast, the first catalyst loading density D 1 For example, it is 5% to 40%. The first catalyst loading density D 1 It may be 10% to 40% or 10% to 30%.

[0031] From the viewpoint of improving the reactivity of the catalyst layer, the first catalyst layer and the second catalyst layer preferably further include a proton conductive resin. In this case, the proton conductive resin covers at least a portion of the particle-shaped conductive member (the first and second particle-shaped conductive members), the fibrous conductive member (the first fibrous conductive member) and / or the catalyst particles (the first and second catalyst particles).

[0032] Similar to the first catalyst layer, the second catalyst layer may include a fibrous conductive member (second fibrous conductive member). However, when the second catalyst layer includes the second fibrous conductive member, the ratio F of the mass of the second fibrous conductive member to the total mass of the second particle-shaped conductive member and the second fibrous conductive member is 2 The ratio F of the mass of the first fibrous conductive member to the total mass of the first particulate conductive member and the first fibrous conductive member in the first catalyst layer may be smaller than 1 The second catalyst layer preferably does not substantially contain the second fibrous conductive member. In this case, the second catalyst layer serves as a buffer layer, and damage to the electrolyte membrane caused by the first fibrous conductive member piercing the electrolyte membrane is suppressed, thereby preventing gas leakage from the damaged portion.

[0033] It should be noted that the ratio F 2 For example, it may be less than 20%, or less than 10%.2 If the content is 0.5% or less, it can be said that the second catalyst layer does not substantially contain the second fibrous conductive member.

[0034] In contrast, the ratio F 1 For example, it may be 20% or more, or 30% or more, or 45% or more. 1 For example, it may be 80% or less, or 65% or more. 1 The lower and upper limits can be combined in any way.

[0035] Hereinafter, the constituent elements of the cathode catalyst layer will be described in detail.

[0036] (Particle-shaped conductive member)

[0037] The first particle-shaped conductive member and the second particle-shaped conductive member are not particularly limited, but carbon black is preferred from the perspective of excellent conductivity. As carbon black, acetylene black, Ketjen black, pyrolytic black, furnace black, channel black, etc. can be cited. The particle size (or the length of the structure composed of a plurality of connected primary particles) is not particularly limited, and the particle size of the catalyst layer used in the past for fuel cells can be used.

[0038] (Fiber-shaped conductive member)

[0039] Examples of the first fibrous conductive member and the second fibrous conductive member include fibrous carbon materials such as vapor grown carbon fiber (VGCF (registered trademark)), carbon nanotubes, and carbon nanofibers. F , is not particularly limited, but is preferably 200 nm or less, more preferably 5 nm or more and 200 nm or less, and further preferably 10 nm or more and 170 nm or less. In this case, the volume ratio of the fibrous conductive member in the catalyst layer can be reduced, and the gas path can be fully ensured, thereby improving gas diffusivity. The diameter D of the fibrous conductive member is F The diameter is obtained by randomly taking out 10 fibrous conductive members from the catalyst layer and averaging the diameters thereof. The diameter is the length in a direction perpendicular to the longitudinal direction of the fibrous conductive member.

[0040] Regarding the length L of the fibrous conductive member F , is not particularly limited, and is preferably 0.2 μm or more and 20 μm or less, and more preferably 0.2 μm or more and 10 μm or less. In this case, at least a portion of the fibrous conductive member is oriented along the thickness direction of the catalyst layer, making it easy to ensure a gas diffusion path. The length L of the fibrous conductive member FThe average fiber length is obtained by taking out 10 fibrous conductive members at random from the catalyst layer and averaging the fiber lengths of these fibrous conductive members. It should be noted that in the case of a substantially linear fibrous conductive member, the fiber length of the fibrous conductive member refers to the length of the straight line connecting one end and the other end of the fibrous conductive member. The aspect ratio L of the fibrous conductive member is F / D F Although not particularly limited, it is preferably 10 or more and 500 or less, and more preferably 20 or more and 250 or less.

[0041] The fibrous conductive member may have a hollow space (hollow portion) inside. At this time, in the catalyst layer, the two ends of the length direction of the fibrous conductive member may be opened respectively. The two ends of the length direction of the fibrous conductive member are opened respectively, which means that the hollow portion is connected to the outside through the opening. That is, the openings at the two ends of the fibrous conductive member are not blocked by any one of the electrolyte membrane and the gas diffusion layer, and the gas can enter and exit from the two ends.

[0042] A through hole connecting the hollow part with the outside can be provided on the side wall of the fibrous conductive member having a hollow part. Catalyst particles can be arranged on the side wall of the fibrous conductive member and fixed in a manner that blocks at least a portion of the through hole. The catalyst particles carried on the side wall in a manner that blocks at least a portion of the through hole can more effectively contact the reaction gas, greatly improving the reaction efficiency of the catalyst layer.

[0043] (Catalyst particles)

[0044] The first catalyst particles and the second catalyst particles are not particularly limited, and examples thereof include alloys or simple substances containing at least one selected from Sc, Y, Ti, Zr, V, Nb, Fe, Co, Ni, Ru, Rh, Pd, Pt, Os, Ir, lanthanides, and actinides. For example, catalyst particles used in the anode include Pt and Pt-Ru alloys. Catalyst particles used in the cathode include Pt and Pt-Co alloys. At least a portion of the catalyst particles is carried on a particle-like conductive member. From the viewpoint of improving the reaction efficiency of the gas, the catalyst particles are carried on a fibrous conductive member in addition to being carried on a particle-like conductive member.

[0045] From the viewpoint of immobilization of the catalyst particles, the diameter X of the catalyst particles is preferably 1 nm or more and 10 nm or less, more preferably 2 nm or more and 5 nm or less. When X is 1 nm or more, the catalytic effect brought by the catalyst particles can be fully obtained. When X is 10 nm or less, it is easy to carry the catalyst particles on the sidewalls of the fibrous conductive member.

[0046] The diameter X of the catalyst particles is determined as follows.

[0047] For any catalyst particle observed in the TEM image of the catalyst layer, the diameter of a circle equal to the cross-sectional area of ​​the particle is taken as the particle size. This operation is performed for 100 to 300 catalyst particles observed in the TEM image, and the particle sizes of each are calculated. The average value of these particle sizes is taken as the diameter X of the catalyst particle.

[0048] (Proton conductive resin)

[0049] The proton conductive resin is not particularly limited, and examples thereof include perfluorocarbon sulfonic acid polymers, hydrocarbon polymers, etc. Among them, perfluorocarbon sulfonic acid polymers, etc. are preferred from the perspective of excellent heat resistance and chemical stability. Examples of perfluorocarbon sulfonic acid polymers include Nafion (registered trademark).

[0050] From the perspective of miniaturization of the fuel cell and maintaining low proton resistance and obtaining high output, the thickness of the catalyst layer is preferably as thin as possible. On the other hand, from the perspective of strength, it is preferably not too thin. Generally, if the proportion of the fibrous conductive member increases, the thickness of the catalyst layer tends to become thicker.

[0051] The thickness of the cathode catalyst layer is, for example, greater than 4 μm and less than 15 μm. Among them, the thickness of the first catalyst layer can be greater than 2 μm and less than 12 μm. The thickness of the second catalyst layer can be greater than 1 μm and less than 7 μm. The ratio of the thickness of the first catalyst layer to the thickness of the second catalyst layer can be greater than 1 and less than 4, or greater than 2 and less than 3. Here, the thickness of the catalyst layer is an average thickness, which is obtained by averaging the distance when a straight line along the thickness direction of the catalyst layer is drawn from one main surface to another main surface at any 10 locations in the cross section of the catalyst layer.

[0052] The catalyst layer is produced, for example, as follows.

[0053] First, a particulate conductive member carrying catalyst particles is mixed in a dispersion medium (e.g., water, ethanol, propanol, etc.). Next, while stirring the obtained dispersion, a proton conductive resin and a fibrous carbon material as required are added in sequence to obtain a catalyst dispersion. The proton conductive resin can be added in two or more times. In this case, the second and subsequent additions of the proton conductive resin can be performed together with the fibrous carbon material. Then, the obtained catalyst dispersion is applied to the surface of an electrolyte membrane or an appropriate transfer substrate sheet with a uniform thickness and dried to obtain a catalyst layer.

[0054] As the coating method, conventional coating methods can be cited, such as spraying, screen printing, and coating methods using various coating machines such as blade coaters, knife coaters, and gravure coaters. As a transfer substrate sheet, for example, a sheet with a smooth surface such as polyethylene terephthalate (PET) and polypropylene is preferably used. When using a transfer substrate sheet, the resulting catalyst layer is transferred to an electrolyte membrane or a gas diffusion layer described later.

[0055] The transfer of the catalyst layer to the electrolyte membrane or the gas diffusion layer is performed by bringing the surface of the catalyst layer opposite to the transfer substrate sheet into contact with the electrolyte membrane or the gas diffusion layer. By bringing the smooth surface of the catalyst layer into contact with the electrolyte membrane or the gas diffusion layer, the interface resistance with the catalyst layer is reduced, and the performance of the fuel cell is improved. The catalyst dispersion can be directly coated on the electrolyte layer.

[0056] The fuel cell according to the embodiment of the present invention comprises a cathode having the cathode catalyst layer, an anode, and an electrolyte membrane interposed between the cathode and the anode. In this case, the second catalyst layer of the cathode catalyst layer is interposed between the first catalyst layer of the cathode catalyst layer and the electrolyte membrane.

[0057] Below, while referring to Figure 1 An example of the structure of the fuel cell according to the present embodiment will be described. Figure 1 1 is a cross-sectional view schematically showing the structure of a single cell configured in a fuel cell according to one embodiment. Generally, a plurality of single cells are stacked and configured in a fuel cell in the form of a cell stack. Figure 1 In the figure, for convenience, one single battery is shown.

[0058] The unit cell 200 includes a membrane electrode assembly 100, which includes an electrolyte membrane 110, a cathode catalyst layer 121 and an anode catalyst layer 122 arranged so as to sandwich the electrolyte membrane 110, and a cathode side gas diffusion layer 131 and an anode side gas diffusion layer 132 arranged so as to sandwich the electrolyte membrane 110, respectively, with the cathode catalyst layer 121 and the anode catalyst layer 122 interposed therebetween. In addition, the unit cell 200 includes a cathode side separator 241 and an anode side separator 242 sandwiching the membrane electrode assembly 100. The electrolyte membrane 110 is larger than the cathode catalyst layer 121 and the anode catalyst layer 122, so that the peripheral edge of the electrolyte membrane 110 is exposed from the cathode catalyst layer 121 and the anode catalyst layer 122. The peripheral edge of the electrolyte membrane 110 is sandwiched by a pair of sealing members 251 and 252.

[0059] Figure 2 1 is a diagram schematically showing the interior of the cathode catalyst layer 121 , and is a diagram showing the interior of the cathode catalyst layer as viewed from a planar direction. Figure 2Also shown is an electrolyte membrane 110. Figure 2 As shown, the cathode catalyst layer 121 includes two layers, a first catalyst layer 121A and a second catalyst layer 121B. The first catalyst layer 121A includes a first particle-shaped conductive member 123, a first catalyst particle 124, and a first fiber-shaped conductive member 125. On the other hand, the second catalyst layer 121B includes a second particle-shaped conductive member 126 and a second catalyst particle 127, and does not substantially include a fiber-shaped conductive member (a second fiber-shaped conductive member).

[0060] In the first catalyst layer 121A, the first catalyst particles 124 are carried on the first particle-shaped conductive member 123. In the second catalyst layer 121B, the second catalyst particles 127 are carried on the second particle-shaped conductive member 126. The carrying density of the second catalyst particles 127 in the second particle-shaped conductive member 126 (the second catalyst carrying density) is greater than the carrying density of the first catalyst particles 124 in the first particle-shaped conductive member 123 (the first catalyst carrying density). Thus, the utilization efficiency of the catalyst can be improved.

[0061] In the first catalyst layer 121A, a part of the first catalyst particles 124 may be carried on the first fibrous conductive member 125. However, from the viewpoint of improving the drainage property of the first catalyst layer 121A and improving the gas diffusion property, the amount of the first catalyst particles 124 carried on the first fibrous conductive member 125 may be reduced. It is more preferable that the first fibrous conductive member 125 does not substantially carry the first catalyst particles 124.

[0062] The anode catalyst layer 122 may be made of a known material and a known structure. Like the cathode catalyst layer, the anode catalyst layer may include a conductive member, catalyst particles supported on the conductive member, and a proton conductive resin. Furthermore, the conductive member may include a particle-shaped conductive member and / or a fibrous conductive member.

[0063] The anode catalyst layer is not exposed to a highly oxidizing environment like the cathode catalyst layer, and water is not generated by the reaction, so it is easy to become a lower humidity environment than the cathode catalyst layer. As a result, the proton conductivity is easy to decrease. The composition and content ratio of the particle-shaped conductive member, the fibrous conductive member and the proton conductive resin can be changed to obtain a higher proton conductivity than the cathode catalyst layer.

[0064] (Electrolyte membrane)

[0065] A polymer electrolyte membrane is preferably used as the electrolyte membrane 110. As a material of the polymer electrolyte membrane, the polymer electrolytes exemplified as the proton conductive resin can be mentioned. The thickness of the electrolyte membrane is, for example, 5 to 30 μm.

[0066] (Gas Diffusion Layer)

[0067] The cathode side gas diffusion layer 131 and the anode side gas diffusion layer 132 may have a substrate layer or may not have a substrate layer. As a structure having a substrate layer, for example, a structure having a substrate layer and a microporous layer disposed on the catalyst layer side thereof may be cited. The substrate layer may be made of a conductive porous sheet such as carbon cloth or carbon paper. The microporous layer may be made of a mixture of a hydrophobic resin such as a fluororesin, a conductive carbon material, and a proton conductive resin (polymer electrolyte).

[0068] (Spacer)

[0069] The cathode side spacer 241 and the anode side spacer 242 can be made of any material as long as they have airtightness, electronic conductivity and electrochemical stability. As such a material, a carbon material, a metal material, etc. are preferred. Carbon can also be coated on a metal material. For example, the cathode side spacer 241 and the anode side spacer 242 are obtained by forming a metal plate into a prescribed shape and performing a surface treatment.

[0070] In the present embodiment, a gas flow path 261 is formed on the surface of the cathode-side separator 241 that contacts the cathode-side gas diffusion layer 131. On the other hand, a gas flow path 262 is formed on the surface of the anode-side separator 242 that contacts the anode-side gas diffusion layer 132. The shape of the gas flow path is not particularly limited, and may be formed in a straight line, a serpentine shape, or the like.

[0071] (Sealing member)

[0072] The sealing members 251 and 252 are made of elastic materials and prevent the fuel and / or oxidant from leaking from the gas flow paths 261 and 262. The sealing members 251 and 252 have, for example, a frame-like shape that annularly surrounds the peripheral edge of the cathode catalyst layer 121 and the anode catalyst layer 122. As the sealing members 251 and 252, known materials and known structures can be used respectively.

[0073] Hereinafter, the present invention will be described in more detail based on examples. However, the present invention is not limited to the following examples.

[0074] [Example 1]

[0075] <Preparation of Dispersion Liquid for Cathode Catalyst Layer>

[0076] A particulate conductive member (carbon black) carrying catalyst particles (Pt-Co alloy) is added to an appropriate amount of water and stirred to disperse. After adding an appropriate amount of ethanol while stirring the obtained dispersion, 35 parts by mass of a fibrous conductive member (vapor-grown carbon fiber, average diameter of 150 nm, average fiber length of 10 μm) and 100 parts by mass of a proton conductive resin (perfluorocarbon sulfonic acid polymer) are added to 100 parts by mass of the above-mentioned particulate conductive member carrying catalyst particles, and stirred to prepare a catalyst dispersion for the first catalyst layer of the cathode catalyst layer.

[0077] In the catalyst dispersion for the first catalyst layer, the ratio of the mass of the catalyst particles to the total mass of the particulate conductive member and the catalyst particles (the first catalyst loading density D 1 ) is 30%.

[0078] Separately, a particulate conductive member (carbon black) carrying catalyst particles (Pt-Co alloy) was added to an appropriate amount of water and stirred to disperse it. After adding an appropriate amount of ethanol while stirring the obtained dispersion, 100 parts by mass of a proton conductive resin (perfluorocarbon sulfonic acid polymer) was added to 100 parts by mass of the above-mentioned particulate conductive member carrying catalyst particles and stirred to prepare a catalyst dispersion for the second catalyst layer of the cathode catalyst layer.

[0079] In the catalyst dispersion for the second catalyst layer, the ratio of the mass of the catalyst particles to the total mass of the particulate conductive member and the catalyst particles (the second catalyst loading density D 2 ) is 50%.

[0080] <Preparation of Dispersion Liquid for Anode Catalyst Layer>

[0081] A particulate conductive member (carbon black) carrying catalyst particles (Pt) is added to an appropriate amount of water and stirred to disperse. After adding an appropriate amount of ethanol while stirring the obtained dispersion, 35 parts by mass of a fibrous conductive member (vapor-grown carbon fiber, average diameter of 150 nm, average fiber length of 10 μm) and 120 parts by mass of a proton conductive resin (perfluorocarbon sulfonic acid polymer) are added to 100 parts by mass of the above-mentioned particulate conductive member carrying catalyst particles, and stirred to prepare a catalyst dispersion for an anode catalyst layer.

[0082] <Production of single cell>

[0083] The obtained catalyst dispersion for the second catalyst layer of the cathode catalyst layer was applied to the surface of an electrolyte membrane (perfluorocarbon sulfonic acid polymer membrane) having a thickness of 15 μm by spraying at a uniform thickness and then dried to form a second catalyst layer.

[0084] Furthermore, the catalyst dispersion for the first catalyst layer is applied to the second catalyst layer in a uniform thickness and then dried to form a cathode catalyst layer composed of two layers, the first catalyst layer and the second catalyst layer.

[0085] The cathode catalyst layer had a film thickness of 6 μm, of which the first catalyst layer had a film thickness of 4 μm and the second catalyst layer had a film thickness of 2 μm.

[0086] Similarly, the catalyst dispersion for the anode catalyst layer was applied to the other surface of the electrolyte membrane by spraying at a uniform thickness, and then dried to form the anode catalyst layer. The thickness of the anode catalyst layer was 4.5 μm.

[0087] Next, two porous conductive carbon sheets were prepared as gas diffusion layers, one of which was placed in contact with the anode catalyst layer and the other was placed in contact with the cathode catalyst layer.

[0088] Next, a frame-shaped sealing member was arranged so as to surround the anode and cathode, and the whole was sandwiched by a pair of stainless steel flat plates (spacers) having gas flow paths at the portions in contact with the gas diffusion layers, thereby completing the test unit cell A1.

[0089] <Evaluation>

[0090] The power generation performance of the single cell A1 of Example 1 was evaluated. Specifically, the single cell A1 was heated to 80°C, a fuel gas with a relative humidity of 30% was supplied to the anode, and an oxidant gas (air) with a relative humidity of 30% was supplied to the cathode. The fuel gas and the oxidant gas were pressurized to a cell inlet gas pressure of 50 kPa to 70 kPa at each current density and supplied. Then, the load control device was controlled in such a way that the current flows constantly, and while changing the current density relative to the electrode area of ​​the anode and cathode, the voltage (initial voltage) V and the output density P of the single cell A1 were measured, and the maximum output density P at which the output density is the largest was calculated. max .

[0091] [Comparative Example 1]

[0092] In the production of a single cell, only the catalyst dispersion for the first catalyst layer of the cathode catalyst layer in Example 1 was applied to the surface of the electrolyte membrane in a uniform thickness and then dried to form a cathode catalyst layer.

[0093] The cathode catalyst layer had a thickness of 8 μm.

[0094] The test cell B1 was completed in the same manner as in Example 1 except for the above, and was evaluated in the same manner as in Example 1. It should be noted that the amount of catalyst particles in the entire cathode catalyst layer was the same in the cell A1 and the cell B2.

[0095] When the maximum output density of battery cell B1 is set to 100, the maximum output density P of battery cell A1 is max The cathode catalyst layer is formed into two layers, namely, a first catalyst layer on the gas diffusion layer side and a second catalyst layer on the electrolyte membrane side, so that the catalyst loading density of the second catalyst layer is higher than that of the first catalyst layer, thereby significantly improving the power generation performance.

[0096] Industrial Applicability

[0097] The fuel cell of the present invention can be suitably used as a power source for a stationary household cogeneration system or a vehicle power source. The present invention is suitably applied to a polymer electrolyte fuel cell, but is not limited thereto and can be applied to fuel cells in general.

[0098] The present invention has been described with respect to the present preferred embodiment, but such disclosure should not be interpreted in a limiting manner. By reading the above disclosure, various deformations and changes are undoubtedly clear to those skilled in the art in the technical field to which the present invention belongs. Therefore, the attached technical scheme should be interpreted as including all deformations and changes without departing from the true spirit and scope of the present invention.

[0099] Description of Reference Numerals

[0100] 100: Membrane electrode assembly

[0101] 110: Electrolyte membrane

[0102] 121: Cathode catalyst layer

[0103] 121A: First catalyst layer

[0104] 123: First particle-shaped conductive member

[0105] 124: First Catalyst Particle

[0106] 125: First fibrous conductive member

[0107] 121B: Second catalyst layer

[0108] 126: Second particle-shaped conductive member

[0109] 127: Second catalyst particle

[0110] 122: Anode catalyst layer

[0111] 131: Cathode side gas diffusion layer

[0112] 132: Anode side gas diffusion layer

[0113] 200: Fuel cell (single cell)

[0114] 241: Cathode side separator

[0115] 242: Anode side spacer

[0116] 251, 252: Sealing components

[0117] 261, 262: Gas flow path

Claims

1. A cathode catalyst layer of a fuel cell, comprising: a first catalyst layer, the first catalyst layer comprising a first particulate conductive member, first catalyst particles, a first fibrous conductive member, and a proton conductive resin, wherein at least a portion of the first catalyst particles is supported on the first particulate conductive member; and a second catalyst layer, the second catalyst layer comprising a second particulate conductive member, second catalyst particles, and a proton conductive resin, wherein at least a portion of the second catalyst particles is supported on the second particulate conductive member, The second catalyst loading density D2 is greater than the first catalyst loading density D1, The second catalyst loading density D2 is represented by the ratio of the mass of the second catalyst particles loaded on the second particle-shaped conductive member to the total mass of the second catalyst particles loaded on the second particle-shaped conductive member and the second particle-shaped conductive member. The first catalyst loading density D1 is represented by the ratio of the mass of the first catalyst particles loaded on the first particle-shaped conductive member to the total mass of the first catalyst particles loaded on the first particle-shaped conductive member and the first particle-shaped conductive member. In the first catalyst layer, a ratio of the mass of the first catalyst particles carried on the first fibrous conductive member to the total mass of the first catalyst particles is 0.5% or less.

2. The cathode catalyst layer according to claim 1, wherein The second catalyst loading density is less than 3 times the first catalyst loading density.

3. A fuel cell comprising: A cathode having a cathode catalyst layer according to claim 1 or 2; an anode; and an electrolyte membrane between the cathode and the anode, The second catalyst layer is interposed between the first catalyst layer and the electrolyte membrane.