Method for producing chromium oxide coated tinplate

By electrolyzing the chromium oxide layer on the tin-plated steel plate to form a closed chromium oxide layer, the problem of growth of tin oxide film of tin-plated steel plate is solved, corrosion resistance and paintability are improved, and passivation treatment that is consistent with REACH is provided The solution replaces the traditional Cr(VI) treatment.

CN113574209BActive Publication Date: 2024-11-26TATA STEEL IJMUIDEN BV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202080021692.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-02-25
Filing Date
2020-02-25
Publication Date
2024-11-26
Estimated Expiration
2040-02-25

AI Technical Summary

Technical Problem

Existing tin-plated steel plates are prone to form tin oxide films during storage, resulting in poor corrosion resistance and paintability, and traditional Cr(VI)-based passivation treatment violates REACH regulations and needs to be found.

Method used

In the continuous high-speed plating production line, water-soluble chromium (III) salt electrolyte solution without halide ions is used, and the chromium oxide layer is electrolytically deposited onto the tin-plated steel plate to form a closed chromium oxide layer to avoid the use of Cr(VI). The pH value of the electrolyte is adjusted by sulfate to ensure the stability and adhesion of the deposited layer.

Benefits of technology

Effectively prevent the growth of tin oxide film, improve the corrosion resistance and paintability of tin-plated steel plates, comply with REACH regulations, provides an alternative to Cr(VI) passivation treatment, and enhances the adhesion between the organic coating and the chromium oxide layer. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113574209B_ABST
    Figure CN113574209B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for electroplating a steel strip having a coating and improvements thereto.
Need to check novelty before this filing date? Find Prior Art

Description

Field of the Invention

[0001] The present invention relates to a method for electroplating tinplate with a protective layer and to the tinplate produced thereby. Background of the Invention

[0003] Tin mill products traditionally include electrolytic tin plated steel, electrolytic chrome plated steel (also known as tin free steel or TFS) and black steel. Although not limited thereto, most applications of tin mill products are used by the container industry in the manufacture of cans, end caps and closures for the food and beverage industry.

[0004] In continuous steel strip plating, a cold rolled steel strip is provided, which is usually annealed after cold rolling to soften the steel by recrystallization annealing or recovery annealing. After annealing and before plating, the steel strip is first cleaned for removing oil and other surface contaminants. After the cleaning step, the steel strip is pickled in a sulfuric acid or hydrochloric acid solution to remove the oxide film. Between the different treatment steps, the steel strip is rinsed to prevent contamination by the solution used for the next treatment step. During the rinsing and transportation of the steel strip to the plating section, a new thin oxide layer is immediately formed on the exposed steel surface. It is necessary to protect the exposed steel surface from further oxidation by depositing a coating layer on the steel.

[0005] This protection is provided by a process called electrodeposition used in electroplating. The part to be plated (steel strip) is the cathode of the circuit. The anode of the circuit can be made of the metal to be plated on the part (dissolving anodes, such as those used in conventional electrotin plating) or dimensionally stable anodes (which do not dissolve during the plating process). The anode and cathode are immersed in an electrolyte solution containing ions of the metal to be deposited on the black steel plate substrate.

[0006] Black steel plate is a tin rolled product that has not (yet) received any metallic coating during the production process. It is the base material for the production of other tin rolled products. Black steel plate can be single-thinned or double-thinned. For single-thinned black steel plate, the hot rolled strip is thinned to the desired thickness in a cold rolling mill and then recrystallized or recovery annealed in a continuous or batch annealing process and optionally temper rolled. For double-thinned black steel plate, the single-rolled substrate is subjected to a second rolling reduction of more than 5%. Single-thinned black steel plate that is temper rolled is generally not considered to be double-thinned black steel plate, because the temper rolling reduction is less than 5%.

[0007] SR or DR black steel plates are usually supplied in the form of coiled strip.

[0008] Tinplate consists of a black steel plate coated with one or more thin tin layers. Tin is usually applied on both sides of the black steel plate by electrodeposition. The tin layer can be melted, for example, by induction or resistance heating, so as to enhance the corrosion resistance of the product by the formation of an inactive FeSn2-alloy layer. Tinplate can be provided with tin of the same thickness or tin of different thicknesses (different coatings) on both sides. The flowing molten tin plate has a thin tin oxide film on the surface, which can grow during storage if it is not treated. In order to improve corrosion resistance and paintability (laquerability), electrochemical passivation (passivation code 311) is applied to the flowing molten tin plate (called 311 passivation) immediately after plating. Tinplate that has not been reflowed and reflowed can be treated by chemical passivation (passivation code 300). These passivation treatments involve treatment in a dichromate solution. This treatment deposits a complex layer of chromium and its hydrated oxide, which inhibits the growth of tin oxide, prevents yellowing, improves paint adhesion and minimizes staining by sulfur compounds. Dichromates or chromic acid solutions contain Cr(VI) compounds. REACH (EU Chemicals Directive) prohibits the use of these hexavalent chromium compounds. Therefore, alternatives have been developed over time based on harmless compounds.

[0009] A particular type of tinplate is provided with a FeSn (50 atomic % iron and 50 atomic % tin) alloy layer. This is produced by diffusion annealing a tinplate containing up to 1000 mg / m2 and preferably between at least 100 and / or up to 600 mg / m2 of deposited tin in a reducing atmosphere at a temperature of at least 513°C, at which temperature the tin layer is converted into an iron-tin alloy consisting of FeSn. The FeSn layer may be coated with an additional tin layer, which, like ordinary tinplate, would normally require a passivation treatment.

[0010] Purpose of the Invention

[0011] The object of the present invention is to provide a REACH compliant alternative to Cr(VI) based passivation treatments for preventing the growth of tin oxide films on tin plated steel sheets.

[0012] It is also an object of the present invention to provide a REACH-compliant alternative to Cr(VI)-based passivation treatments which improves the adhesion of paints to tinplate steel.

[0013] Description of the invention

[0014] One or more objects are achieved by a method for the electrolytic deposition of a chromium oxide layer onto a tinplate steel substrate from an aqueous electrolyte solution free of halide ions comprising a trivalent chromium compound provided by a water-soluble chromium (III) salt in a continuous high-speed plating line operating at a line speed of at least 50 m / min, wherein the steel substrate serves as the cathode and wherein the anode comprises a catalytic coating of i) iridium oxide or ii) a mixed metal oxide comprising iridium oxide and tantalum oxide, for reducing or eliminating Cr 3+ - ions oxidized to Cr 6+ -ions, and wherein the electrolyte solution contains at least 50 mM and at most 1000 mM Cr 3+ ions, a total of 25-2800 mM sodium sulfate or potassium sulfate, a pH measured at 25°C between 2.50 and 3.6, and wherein the plating temperature is between 40 and 70°C and wherein no other compounds are added to the electrolyte, except optionally sulfuric acid or sodium or potassium hydroxide to adjust the pH to the desired value.

[0015] For the sake of clarity, note that 1 mM means 1 millimole / l. It should also be noted that there are two potential sources of sodium sulfate in the electrolyte. First, if basic chromium sulfate is used as the water-soluble chromium (III) salt, its chemical formula is (CrOHSO4)2×Na2SO4, then 0.5 mM of Na2SO4 is also added to the electrolyte for each mM of Cr. However, Na2SO4 can also be added as a salt, for example as a salt that enhances conductivity, or to increase the dynamic viscosity of the electrolyte. The total amount of Na2SO4 is the sum of the addition of Na2SO4 and the amount together with the basic chromium (III) sulfate. If basic chromium sulfate is not used as the water-soluble chromium (III), and for example chromium (III) sulfate or chromium (III) nitrate is used, any Na2SO4 present in the electrolyte is added as sodium sulfate. The above Cr (III) salts, including basic chromium (III) sulfate, can be provided alone or in combination.

[0016] A steel substrate in the sense of the present invention is intended to mean a steel substrate comprising a tin-based metal layer which has been deposited on the steel substrate before the chromium oxide layer is deposited according to the invention.

[0017] The absence of complexing agents in the electrolyte means that there are no necessary components for the deposition of Cr-metal. Complexing agents are required for the very stable [Cr(H2O)6] 3+The complex is unstable. The inventors unexpectedly found that by avoiding the use of complexing agents (such as NaCOOH), the deposition of chromium metal was prevented but a closed chromium oxide layer was deposited instead. With a closed oxide layer, the oxide layer is meant to cover the entire surface of the substrate and adhere well to the surface. In addition, the absence of a carbon-containing complexing agent also prevents the co-deposition of chromium carbide in the oxide layer. If present in a detectable amount in the oxide layer, any residual amount of chromium carbide is therefore the result of a small and unavoidable amount of residual other compounds present in the base material that produces the electrolyte. The presence of sulfate in the electrolyte causes the presence of sulfate in the chromium oxide coating layer under the plating conditions according to the present invention. The maximum amount of sulfate detected at the surface is about 10%. The minimum amount of sulfate at the surface is 0.5%, and in most cases at least 2%. These values ​​are obtained from the XPS depth distribution within the first 3nm starting from the outer surface.

[0018] Due to the closed chromium oxide layer on the substrate, the adhesion between the substrate on which the closed chromium oxide layer is deposited and the organic coating layer is greatly improved.

[0019] If the pH of the electrolyte solution becomes too high or too low, sulfuric acid or sodium hydroxide may be added to adjust the pH to a value within the desired range. Likewise, different acids or bases may be used, but sulfuric acid and sodium hydroxide are preferred in view of simplifying the bath chemistry.

[0020] Sodium sulfate or potassium sulfate also acts as a salt that enhances conductivity. In order to keep the electrolyte as simple as possible, and to prevent the formation of chlorine or bromine, the salt that enhances conductivity is a sulfate. The cation is preferably sodium or potassium. In order for the electrolyte not to become too viscous, a maximum amount of 2800mM sodium sulfate or potassium sulfate is still allowed. For reasons of simplicity, the cation is preferably sodium. A pH exceeding 4 leads to a colloidal reaction in the electrolyte, making it unusable for electroplating. A pH below 2.50 is undesirable because the increase in surface pH at the cathode required for the deposition of chromium oxide (CrOx) cannot be obtained in the electrolyte at these low pH values. High pH also enables the use of lower current densities during deposition, resulting in less hydrogen precipitation. Excessive hydrogen evolution is believed to cause a streaky appearance of the surface at lower pH (below 2.50). A relatively high electrolyte temperature electrolyte of at least 40°C also allows the use of lower current densities, which also helps to reduce hydrogen evolution.

[0021] It is preferred to use only sodium sulfate in the electrolyte, since this keeps the composition of the electrolyte as simple as possible.

[0022] Halides such as chloride or bromide may be absent in the electrolyte. This absence is required to prevent the formation of, for example, chlorine or bromine at the anode. The electrolyte also does not contain a depolarizing agent. In many similar baths, potassium bromide is used as a depolarizing agent. The absence of this compound mitigates any risk of bromine formation at the anode. Likewise, buffers such as the commonly used boric acid (H3BO3) are absent in the electrolyte.

[0023] It is essential in the method according to the invention that the anode comprises i) a catalytic coating of iridium oxide or ii) a mixed metal oxide comprising iridium oxide and tantalum oxide. The catalytic coating is usually deposited onto a titanium anode, wherein the titanium covering is such that the titanium is not exposed to the electrolyte. It is found that the use of any other practical anode such as platinum, platinum-plated titanium or nickel-chromium leads to Cr(VI) compounds which are to be avoided due to their toxic and carcinogenic properties. 6+ - Formation of ions. Carbon as anode material breaks down over time due to the high current densities used in industrial high-speed plating lines and should also not be used.

[0024] In the method according to the invention, the steel substrate is a black steel sheet coated with tin (tin-plated steel sheet) or a black steel sheet coated with a FeSn-alloy layer (see Figure 3 ). WO2012045791 discloses a method for producing a black steel sheet coated with a FeSn-alloy layer.

[0025] The steel used for the black steel plate may be any steel grade suitable for producing packaging steel. By way of example, but not intended to be limiting, reference is made to steel grades used for packaging applications in EN 10202:2001 and ASTM 623-08:2008.

[0026] Black steel sheets are usually provided in the form of low carbon (LC), extra low carbon (ELC) or ultra low carbon (ULC) strips, wherein the carbon content, expressed as a weight percentage, is between 0.05 and 0.15 (LC), between 0.02 and 0.05 (ELC) or less than 0.02 (ULC), respectively. Alloying elements such as manganese, aluminum, nitrogen, but sometimes also elements such as boron are added to improve the mechanical properties (see EN 10202, 10205 and 10239). Black steel sheets may consist of interstitial-free low carbon steels, extra low carbon steels or ultra low carbon steels, such as titanium stabilized, niobium stabilized or titanium-niobium stabilized interstitial-free steels.

[0027] Single-reduced (SR) black steel sheets (as defined in international standards) fall within the range of 0.15mm to 0.49mm; double-reduced (DR) black steel sheets 0.13mm-0.29mm, with a typical range of DR being 0.14-0.24mm. For special applications, lower specifications down to 0.08mm are now available in single or double-reduced base materials.

[0028] The method according to the invention allows good control of the oxide layer, allows the deposition of a closed oxide layer, ie an oxide layer covering the entire surface of the substrate, and allows the properties of the oxide layer to be improved in terms of improved adhesion to organic coatings.

[0029] The method according to the invention also allows the deposition of a closed chromium oxide layer on top of the tin layer or FeSn layer. The absence of a complexing agent means that there is no co-deposition or only a very small amount of metallic chromium is co-deposited. This chromium oxide layer acts as a passivation layer and because it is deposited by means of a Cr (III)-technology, this deposition process complies with REACH. The chromium oxide layer also improves the adhesion to the organic coating. The paintability of the tinplate is at the same level as the steel or tinplate coated with FeSn treated with a known passivation treatment based on Cr (VI). In the case of covering the FeSn diffusion layer with a tin layer, the material passivation and adhesion behavior are considered to be similar to the tinplate in the context of the present invention.

[0030] So, although the substrates may be different, the effect of the enclosed chromium oxide layer deposited on the substrate in each case results in improved adhesion between the substrate and the organic coating. There is also the additional benefit of providing a REACH compliant passivation treatment that can replace current Cr(VI) based passivation treatments such as 311 and 300 treatments.

[0031] Preferred embodiments are provided in the dependent claims.

[0032] As water-soluble chromium(III) salts, one or more salts are selected from the group consisting of basic chromium(III) sulfate, chromium(III) sulfate and chromium(III) nitrate. From the point of view of keeping the bath chemistry as simple as possible, it is preferred to use only basic chromium(III) sulfate.

[0033] In embodiments, the electrolyte solution contains up to 500 mM Cr 3+ -ions, preferably up to 350 mM, more preferably up to 250 mM or even up to 225 mM Cr 3+ - ions. The electrolyte solution preferably contains at least 100 mM Cr 3+ -ions, preferably at least 125 mM Cr 3+ -ions. These preferred ranges provide good results.

[0034] In a preferred embodiment, the pH of the electrolyte is measured at 25°C between 2.50 and 3.25. Preferably the plating temperature is between 35 and 65°C. In an embodiment, the pH of the electrolyte solution is at most 3.30, preferably at most 3.00. In an embodiment, the pH is at least 2.60 or even at least 2.70. The pH range between 2.55 and 3.25 provides excellent results in terms of coating quality. Likewise, at values ​​greater than 3.25, there is no risk of colloidal reactions in the electrolyte making it unusable for electroplating in the method according to the invention. In the pH range between 3.25 and 4, the risk increases from acceptable just above 3.25 to unacceptable if the pH value is greater than 4. Less than 2.55, the process becomes less economical because the effort required to increase the surface pH at the cathode at lower pH is greater.

[0035] The plating time, i.e. the duration of applying current to the cathode (which is significantly shorter than the immersion time), is preferably as short as possible to allow the method to be used in an industrial production line. At low production line speeds and / or long anode lengths, the plating time is at most 3 seconds. A maximum plating time of at most 1000ms is still permissible, preferably at most 900ms. At very high production line speeds, it may be necessary to increase the current density and / or total anode length to keep the production line at a practical minimum. Although it is preferred that there is no complexing agent at all in the electrolyte in the method according to the present invention, it may still occur that, despite all appropriate care and the use of an intermediate rinse bath, a small amount is inevitably present as an inevitable impurity in the electrolyte due to the introduction of the previous upstream electrolyte bath in the plating production line. The maximum permissible value is 10mM of a complexing agent such as NaCOOH, preferably at most 5mM, preferably at most 2mM. It was found that these amounts did not result in any significant chromium metal deposition and the deposited oxide layer adhesion quality appeared unaffected. Nevertheless, it is preferred that there is no such complexing agent in the electrolyte according to the method of the present invention.

[0036] In embodiments, the electrolyte solution contains at least 210 mM and / or at most 845 mM sodium sulfate.

[0037] In a preferred embodiment the plating temperature is at least 50°C, preferably at least 55°C.

[0038] In embodiments the line speed of the continuous plating line is at least 100 m / min, more preferably at least 200 m / min.

[0039] In a preferred embodiment, the aqueous electrolyte consists only of basic chromium (III) sulfate, sodium sulfate and optionally sulfuric acid or sodium hydroxide in an amount sufficient to adjust the pH of the electrolyte to the desired value, and unavoidable impurities. The pH is preferably adjusted to a value of 2.55 or greater, and preferably to a value of 3.25 or less.

[0040] In an embodiment of the present invention, a black steel sheet or a tin-plated steel sheet provided with a FeSn layer is provided with a chromium oxide layer applied using the method according to the present invention, and is further coated on one or both sides with an organic coating consisting of a paint, a thermoplastic single layer or a thermoplastic multilayer polymer by a painting step, a film lamination step or a direct extrusion step, preferably wherein the thermoplastic polymer coating is a polymer coating system comprising one or more layers, the layers comprising thermoplastic resins such as polyesters or polyolefins, acrylic resins, polyamides, polyvinyl chloride, fluorocarbon resins, polycarbonates, styrene-type resins, ABS resins, chlorinated polyethers, ionomers, urethane resins and functionalized polymers, and / or their copolymers, and or their blends.

[0041] Preferably the thermoplastic polymer coating is a polymer coating system comprising one or more layers of a thermoplastic resin such as a polyester or polyolefin, but may also include acrylic resins, polyamides, polyvinyl chloride, fluorocarbon resins, polycarbonates, styrenic resins, ABS resins, chlorinated polyethers, ionomers, urethane resins and functionalized polymers. To illustrate:

[0042] Polyester is a polymer composed of a dicarboxylic acid and a diol. Examples of suitable dicarboxylic acids include terephthalic acid, isophthalic acid (IPA), naphthalene dicarboxylic acid, and cyclohexane dicarboxylic acid. Examples of suitable diols include ethylene glycol, propylene glycol, butanediol, hexanediol, cyclohexane diol, cyclohexanedimethanol (CHDM), neopentyl glycol, and the like. More than two dicarboxylic acids or diols may be used together.

[0043] Polyolefins include, for example, polymers or copolymers of ethylene, propylene, 1-butene, 1-pentene, 1-hexene or 1-octene.

[0044] Acrylic resins include, for example, polymers or copolymers of acrylic acid, methacrylic acid, acrylate, methacrylate or acrylamide.

[0045] The polyamide resin includes so-called nylon 6, nylon 66, nylon 46, nylon 610, and nylon 11, for example.

[0046] Polyvinyl chloride includes homopolymers and copolymers, for example using ethylene or vinyl acetate.

[0047] Fluorocarbon resins include, for example, polyethylene tetrafluoride, polyethylene trifluoride, chloromonofluoride, ethylene-propylene hexafluoride, polyvinyl fluoride, and polyvinylidene fluoride.

[0048] • Functionalized polymers, for example by grafting with maleic anhydride, including, for example, modified polyethylene, modified polypropylene, modified ethylene acrylate copolymers and modified ethylene vinyl acetate.

[0049] Mixtures of two or more resins may be used. In addition, the resins may be mixed with antioxidants, heat stabilizers, UV absorbers, plasticizers, pigments, nucleating agents, antistatic agents, mold release agents, antiblocking agents, etc. The use of such thermoplastic polymer coating systems has been shown to provide excellent properties in can preparation and can use, such as shelf life.

[0050] Preferably the thermoplastic polymer coating is a polymer coating system comprising one or more layers comprising a thermoplastic resin such as polyester or polyolefin, acrylic resin, polyamide, polyvinyl chloride, fluorocarbon resin, polycarbonate, styrene-type resin, ABS resin, chlorinated polyether, ionomer, urethane resin and functionalized polymers, and / or copolymers thereof, and or blends thereof.

[0051] Preferably, the thermoplastic polymer coating on one or both sides of the coated black steel plate is a multi-layer coating system, the coating system comprising at least an adhesive layer for adhering to the coated black steel plate, a surface layer and a bulk layer between the adhesive layer and the surface layer, wherein the layers of the multi-layer coating system comprise or consist of polyesters, such as polyethylene terephthalate, isophthalic acid (IPA)-modified polyethylene terephthalate, cyclohexanedimethanol (CHDM)-modified polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, or copolymers or blends thereof.

[0052] The application process of the thermoplastic polymer coating is preferably carried out by laminating the polymer film to the coated black steel plate by means of extrusion coating and lamination, wherein the polymer resin is melted and formed into a hot film, which is applied to a moving substrate. The coated substrate is then usually passed between a set of counter-rotating rollers, which press the coating onto the substrate to ensure complete contact and adhesion. An alternative is film lamination, wherein a polymer film is provided and applied to a heated substrate and passed through a set of counter-rotating rollers and pressed onto the substrate between them to ensure complete contact and adhesion. Example

[0053] The materials according to Table 1 were used as substrates.

[0054] Table 1: Substrate

[0055]

[0056] Table 2: Cr(III) electrolyte composition

[0057] Components unit 1 Cr(III) concentration <![CDATA[gl -1 ]]> 20 Additional Sodium Sulfate <![CDATA[gl -1 ]]> 0 Complexing agent <![CDATA[gl -1 ]]> 0

[0058] exist Figure 2 The results of the RCE experiments are presented in the following. Using electrolyte 1 (20 g / l basic chromium (III) sulfate (385 mM Cr3+ ). The experiments were performed at 55°C and pH 2.7 (and some at 3.2) on a cylindrical electrode rotating at 776 rpm. 776 rpm corresponds to a line speed of 100 m / s in an industrial coating line. For the electrodeposition experiments, a titanium anode comprising a catalytic mixed metal oxide of iridium oxide and tantalum oxide was selected. The rotation speed of the RCE was kept constant at 776 RPM (Ω 0.7 =6.0s 0.7 ). The substrates are listed in Table 1 and the dimensions of the cylinders are 113.3 mm x φ73 mm. The plating time is 800 ms. Figure 2 For the black steel sheet (1) and the tinned steel sheet (3), the CrOx coating weight (expressed as Cr metal, in mg / m 2 The current density is plotted as a function of the current density.

[0059] The amount of Cr oxide deposited is plotted on the Y axis. The amount of Cr oxide is determined by means of XRF. The XRF measurements were performed as described in the previously cited paper, which is included herein by reference. Initially no Cr or CrOx was present on the new substrate. By measuring the sample with XRF, the total amount of chromium deposited (i.e. metal, oxide, sulfate and (if present) carbide) was measured. The difference (Δ(XRF)) is then attributed to the Cr oxide, and this is Figure 2 For samples 1 and 3, no CrOx was present on the new substrate before coating the substrate using the method according to the invention.

[0060] Table 3: Figure 2 Details of the RCE experiment drawn in

[0061]

[0062] Removal of SnOx means removing the tin oxide (SnOx) layer using a well-known sodium carbonate treatment such as by (but not limited to) immersing the substrate in a sodium carbonate solution containing between 1 and 50 g / l Na2CO3 at a temperature between 35 and 65°C and wherein a pressure between 0.5 and 2 A / dm 2 The cathodic current density is maintained for a time between 0.5 and 5 seconds.

[0063] The RCE results closely match those of coil testing in an industrial scale pilot line with similar settings 14 g / l Cr, T = 55 °C, line speed = 150 m / min 1 , current density = 18.75A dm -2 , plating time: 600ms, Figure 24, even though the Cr(III) concentration is slightly lower. It was also found that pretreatment of the strip had little effect on the amount of CrOx deposited on the strip.

[0064] Similar experiments conducted at pH values ​​less than 2.50, such as those disclosed in US6099714, show unsatisfactory streaky surface quality when conducted on tinplate in an industrial production line. US6099714 discloses a 3×5 inch 2 Experiments on tinplate samples, ie in a laboratory setting and intended for piece-by-piece plating. In addition to an appearance that may be perceived by consumers as aesthetically unappealing, streaking can also result in non-uniform oxide layer thickness and / or composition, which can affect the performance of the coated black steel panel as a whole.

[0065] The tests were carried out with tinplate using electrolyte 1 in Table 2. The substrate on which the oxide was deposited according to the method of the invention was an unpassivated, flow-melted tinplate (2.8 g / m 2 Sn). The black steel plate in all cases was 0.223 mm thick, continuously annealed SR low carbon steel (TH340, 0.045 wt% C, 0.205 wt% Mn, 0.045 wt% Al_solute).

[0066] The samples were investigated by XPS to determine the composition, which showed that the deposited layer consisted only of chromium oxide.

[0067] Table 4: Results of Cr as CrOx on tinned steel sheets

[0068] Go to SnOx pH i t Cr <![CDATA[A / dm 2 ]]> ms <![CDATA[mg / m 2 ]]> yes 2.7 20 800 27.0 yes 2.7 40 800 35.0 yes 2.7 60 800 64.1 no 2.7 40 800 32.9 yes 2.7 0 - 0.9 yes 2.7 20 400 6.3 yes 2.7 20 200 3.3 yes 2.7 20 2 x 400 16.8 no 3.2 0 - 0 yes 3.2 0 - 0.1 yes 3.2 20 400 38.4

[0069] In most cases the tin oxide layer was removed so that the surface was that of a new tin surface. The experiments without deposition clearly showed that no chromium oxide was present in those cases.

[0070] The samples were investigated by XPS to determine the composition, which showed that the deposit consisted only of chromium oxide and no chromium metal was present. The presence of sulfate in the electrolyte caused the presence of sulfate in the chromium oxide coating under the plating conditions according to the invention. The maximum amount of sulfate detected at the surface was about 10%. The minimum amount of sulfate at the surface was about 0.5%, and in most cases at least 2%.

[0071] BRIEF DESCRIPTION OF THE DRAWINGS

[0072] The invention will now be explained by way of the following non-limiting drawings.

[0073] Figure 1Schematic overview of the process steps to obtain a coated product starting from a hot rolled strip.Before cold rolling, the hot rolled strip is usually pickled (not shown) to remove the hot mill scale and cleaned (not shown) to remove any contaminants from the strip.

[0074] Figure 2 : Amount of Cr-oxide as a function of current density in the RCE experiment for experiments performed at pH=2.7.

[0075] Figure 3 : Schematic diagram of a tinplate that can be produced with a top layer of CrOx deposited according to the invention:

[0076] a.Tin-plated steel sheet (not reflowed)

[0077] b.Tin-plated steel sheet (soft melting)

[0078] c. Tinned steel (soft melt) with additional tin

[0079] d.FeSn

[0080] e.FeSn and tin

Claims

1. A method for electrolytically depositing a chromium oxide layer onto a tinplate substrate from an aqueous halide-free electrolyte solution comprising a trivalent chromium compound provided by a water-soluble trivalent chromium salt in a continuous high-speed plating line operating at a line speed of at least 50 m / min, wherein the tinplate substrate serves as the cathode and wherein the anode comprises i) iridium oxide or ii) a catalytic coating of a mixed metal oxide comprising iridium oxide and tantalum oxide, for reducing or eliminating Cr 3+ Ion to Cr 6+ ions, and wherein the aqueous electrolyte contains at least 50 mM and at most 1000 mM Cr 3+ ions, a total of 25-2800 mM sodium sulfate or potassium sulfate, a pH measured at 25°C between 2.50 and 3.6, and wherein the plating temperature is between 40 and 70°C and wherein no other compounds are added to the aqueous electrolyte solution, except optionally sulfuric acid or sodium or potassium hydroxide to adjust the pH to the desired value.

2. The process according to claim 1, wherein the pH is adjusted to a value of 2.55-3.

6.

3. The process according to claim 1, wherein the pH is adjusted to a value of 2.55-3.

25.

4. The method according to claim 1 or 2, wherein the plating time, i.e. the duration of applying the current to the cathode, is at most 1000 ms.

5. The method according to claim 1, wherein the water-soluble trivalent chromium salt is basic chromium sulfate.

6. The method according to claim 1 or 2, wherein the amount of chromium deposited as chromium oxide is at least 5 mg / m 2 .

7. The method according to claim 1 or 2, wherein the amount of chromium deposited as chromium oxide is at least 6 mg / m 2 .

8. The method according to claim 1 or 2, wherein the amount of chromium deposited as chromium oxide is at least 7 mg / m 2 .

9. The method according to claim 1 or 2, wherein the amount of chromium deposited as chromium oxide is at least 8 mg / m 2 .

10. The method according to claim 1 or 2, wherein the aqueous electrolyte solution contains up to 10 mM of sodium formate as an inevitable impurity in the electrolyte.

11. The method according to claim 1 or 2, wherein the aqueous electrolyte solution contains at least 210 mM and at most 845 mM sodium sulfate.

12. The method of claim 1 or 2, wherein the plating temperature is at least 50°C.

13. The method of claim 1 or 2, wherein the plating temperature is at least 55°C.

14. The method of claim 1 or 2, wherein the line speed of the plating line is at least 100 m / min.

15. The method according to claim 1 or 2, wherein the aqueous electrolyte solution consists only of basic chromium sulfate, sodium sulfate and optionally sulfuric acid or sodium hydroxide in an amount sufficient to adjust the pH of the electrolyte to a desired value, and unavoidable impurities.

16. The method according to any one of claims 1 to 3, wherein the tinplate substrate is further coated on one or both sides with an organic coating consisting of a thermoplastic monolayer or thermoplastic multilayer polymer by a film lamination step or a direct extrusion step.

17. The method of claim 16, wherein the thermoplastic polymer coating is a polymer coating system comprising one or more layers comprising a thermoplastic resin.

18. The method according to claim 17, wherein the thermoplastic resin is selected from polyester or polyolefin, acrylic resin, polyamide, polyvinyl chloride, fluorocarbon resin, polycarbonate, styrene type resin, ABS resin, chlorinated polyether, ionomer, urethane resin, and / or copolymers thereof, and / or blends thereof.

19. A method according to claim 17 or 18, wherein the thermoplastic polymer coating on one or both sides of the coated tinplate substrate is a multilayer coating system, the coating system comprising at least an adhesion layer for adhesion to the coated tinplate substrate, a surface layer and a bulk layer between the adhesion layer and the surface layer, wherein the layers of the multilayer coating system comprise or consist of polyester.

20. The method according to claim 19, wherein the polyester is selected from polyethylene terephthalate, isophthalic acid-modified polyethylene terephthalate, cyclohexanedimethanol-modified polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, or copolymers or blends thereof.

21. Coated metal substrate obtainable by a process according to any one of claims 1 to 20.

22. Use of a coated metal substrate according to claim 21 in a process for producing containers for packaging purposes.

Citation Information

Patent Citations

  • Passification of tin surfaces

    US6099714A

  • Process for producing an iron-tin layer on a packaging steel substrate

    WO2012045791A1

  • Coated substrate for packaging applications and a method for producing said coated substrate

    CN104302814A

  • Chromium-chromium oxide coatings applied to steel substrates for packaging applications and a method for producing said coatings

    CN105102685A

  • Method for manufacturing chromium-chromium oxide coated blackplate

    EP3378973A1