High-density corrosion-resistant layer arrangement for electrostatic chucks
By using a composition of high-purity alumina and tantalum oxide in the layer arrangement of the electrostatic chuck, the liquid Ta2O5 phase is formed, which solves the problem of the electrostatic chuck not durable in a high-temperature corrosion environment in the prior art, and improves its dielectric strike Wear strength and mechanical integrity.
Patent Information
- Application Number
- CN202080022107.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-03
- Filing Date
- 2020-04-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-04-10
AI Technical Summary
Existing electrostatic chucks are easily eroded by corrosive gases during semiconductor manufacturing, and have a high impurity content, which makes them not durable in high-temperature processing environments and are not suitable for maintaining mechanical integrity for a long time.
A layer arrangement is adopted, including a metallization layer between the first ceramic layer and the second ceramic layer, the first ceramic layer containing high purity alumina, ZrO2, Y2O3, AlN, Si3N4, SiC or a combination thereof, and is co-fired Tantalum oxide (Ta2O5) is added as a sintering aid during the process to form a liquid Ta2O5 phase to improve the density and corrosion resistance of the ceramic.
It realizes reliable operation of electrostatic chucks in high-temperature corrosion environments, reduces impurity migration, improves dielectric breakdown strength and mechanical integrity, and extends the service life of the equipment.
Smart Images

Figure CN113597665B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a layer arrangement for an electrostatic chuck, a method of manufacturing the same, and an electrostatic chuck containing the layer arrangement. In particular, the present disclosure relates to a metallization layer disposed between a top dielectric layer and an insulating layer in an electrostatic chuck. Background Art
[0002] Electrostatic chucks (ESCs) are widely used in semiconductor device manufacturing processes to clamp substrates, such as silicon wafers. ESCs are layered structures in which conductive layers are sandwiched between ceramic insulators to prevent them from making direct contact with the device. Aluminum oxide and aluminum nitride are the most commonly used ceramics in ESCs. The conductive layers, often called "traces" or "electrodes," are usually made of refractory metals such as molybdenum and tungsten. The traces are further connected by interlayer conductive conduits called "vias" that pass through the ceramic layers to provide electrical energy from an external power source.
[0003] U.S. Patent 5,671,116 teaches a co-firing method for making ceramic ESCs. In this process, ceramic tapes are first formed by tape casting powders that are mixed with various organic and inorganic binders to hold them together. Conductive traces are then metallized on top of the ceramic tapes in the green state. The metallized green tapes are then stacked on top of each other and then pressed to laminate them. Vias are formed by inserting refractory metal slurries or powders into through holes drilled in the ceramic layers. The resulting laminated green parts are then co-fired at high temperatures to make the monolithic ESC body.
[0004] The top ceramic layer of the ESC is usually called the dielectric layer, which is in direct contact with the wafer and is the most critical ceramic layer in the ESC. Its main function is to provide an insulating layer between the wafer and the electrode below. Its dielectric strength must withstand the breakdown force of the electric field applied to clamp the wafer. It also prevents any metallic impurities from migrating from the electrode material to the device during processing. In processing chambers such as etching and deposition, harsh gases are used, such as fluorine and chlorine, which are increasingly corrosive in nature. In such cases, it is most important that the composition of the ceramic layer must not be dissolved by the corrosive processing gas and contaminate the device.
[0005] In order to maintain high dielectric breakdown strength, the ceramic must be nearly fully dense. U.S. Patents 4,678,683, 5,207,437, and 5,104,834 all disclose the use of silicon dioxide with calcium oxide and magnesium oxide as liquid phase sintering aids to densify the ceramic when sintering the layered metallization structure. Although such compositions in alumina yield dense sintered bodies, they have several drawbacks:
[0006] During the semiconductor manufacturing process, the composition is attacked by halogen plasma gases such as fluorine and chlorine; and
[0007] The composition has a relatively high level of impurities associated with liquid phase formation. The high impurity level makes the composition unsuitable for high temperature processing environments because the impurities can more easily migrate through the dielectric layer; and enter the gas processing environment and undesirably onto the surface of the silicon wafer.
[0008] Therefore, it is necessary to develop ESCs that are both corrosion resistant and resistant to the migration of impurities into the processing environment. Summary of the invention
[0009] In a first aspect, there is provided a layer arrangement for an electrostatic chuck comprising:
[0010] A. first ceramic layer;
[0011] B. second ceramic layer;
[0012] C. a metallization layer disposed between the first ceramic layer and the second ceramic layer,
[0013] The first ceramic layer comprises at least 90.0 wt % of the following substances:
[0014] (i) Alumina, titanium dioxide, ZrO2, Y2O3, AlN, Si3N4, SiC or a combination thereof; or
[0015] (ii) aluminum oxide doped with a transition metal oxide; and
[0016] Preferably, tantalum oxide (Ta2O5) is present in an amount sufficient to densify the first ceramic layer to at least 97%, or 98%, or 98.5%, or 99.0% of the theoretical maximum density (i.e., 0% porosity) of the first ceramic layer. Tantalum oxide (Ta2O5) is preferably present in an amount in the range of 0.05 wt% to 10.0 wt%.
[0017] In some embodiments, it has been found that relatively small amounts of tantalum oxide (e.g., less than 2.0 wt%) (used as a sintering aid) can produce high density, high purity ceramics. In these embodiments, the first ceramic layer preferably includes at least 90.0 wt% alumina, titania, ZrO2, Y2O3, AlN, Si3N4, SiC, or a combination thereof.
[0018] In other embodiments, more Ta2O5 (e.g., 2.0 wt% to 6.0 wt% or 10 wt% or more) may be needed to form a Ta2O5 liquid phase to densify the first ceramic layer. In these embodiments, the first ceramic layer preferably includes at least 90.0 wt% alumina doped with a transition metal oxide (e.g., titanium dioxide).
[0019] Ta2O5 is very inert in most environments and therefore has a low tendency to migrate into the process environment. The process environment may be above 450°C, or above 550°C, or above 650°C, or above 750°C.
[0020] Preferably, there is at least 92.0 wt%, or at least 94.0 wt%, or at least 96.0 wt%, or at least 98.0 wt%, or at least 99.0 wt% alumina, titania, ZrO2, Y2O3, AlN, Si3N4, SiC, transition metal oxides or combinations thereof.
[0021] The first layer may include at least 95.0 wt%, or at least 97.0 wt%, or at least 98.0 wt%, or at least 99.0 wt%, or at least 99.5 wt%, or at least 99.8 wt% of tantalum oxide and aluminum oxide, titanium dioxide, ZrO2, Y2O3, AlN, Si3N4, SiC, transition metal oxides, or combinations thereof.
[0022] The first ceramic layer preferably comprises aluminum oxide or AlN.
[0023] The first ceramic layer preferably includes less than or equal to 8.0 wt % Ta2O5, or less than or equal to 6.0 wt % or less than or equal to 4.0 wt % Ta2O5, or less than or equal to 2.0 wt % or less than or equal to 1.5 wt % Ta2O5, or less than or equal to 1.0 wt % or less than or equal to 0.8 wt % Ta2O5, or less than or equal to 0.7 wt % or less than or equal to 0.6 wt % Ta2O5, or less than or equal to 0.5 wt % or less than or equal to 0.4 wt %. Preferably, the first ceramic layer includes greater than or equal to 0.2 wt % Ta2O5, or greater than or equal to 0.3 wt % Ta2O5. The amount of Ta2O5 required may depend on: the composition of the first ceramic layer; the desired target density and / or target sintering temperature and time; and the processing environment to which the layer arrangement will be exposed. Higher levels of Ta2O5 may not provide significant additional benefits during densification; while lower levels may be insufficient to provide the target density requirements under the target conditions.
[0024] Preferably, the first ceramic layer is a top dielectric layer.The top dielectric layer may be in direct contact with the wafer in a processing chamber, and thus the surface of the dielectric layer is preferably substantially free of volatile impurity species (eg, Cu and Na).
[0025] Preferably, the first ceramic layer comprises a Ta2O5 phase at an interface of the first ceramic layer and the metallization layer.
[0026] In one embodiment, during the co-firing process of manufacturing the layer arrangement, the layer arrangement is heated to below the melting point of Ta2O5 for a set period of time, resulting in the formation of a liquid Ta2O5-alumina phase, which is attracted to the more porous areas around the metallization layer and the adjacent second ceramic layer. Preferably, Ta2O5 is capable of forming a liquid phase within the first ceramic layer at or below 1600°C, and more preferably at or below 1400°C.
[0027] As a result, the Ta2O5 concentration at the top surface of the top dielectric layer (Ta2O5 deficient phase) is lower than the Ta2O5 concentration of the Ta2O5 phase (e.g., glass) at the interface of the first ceramic layer and the metallization layer. Preferably, the Ta2O5 concentration at the top surface of the first ceramic layer is 20%, or 50%, or 80% lower than the Ta2O5 concentration in the Ta2O5 phase at the interface between the metallization layer and the first ceramic layer. This distribution of Ta2O5 is advantageous because, although Ta2O5 is not reactive to most gas environments, it readily reacts with fluorine gas. Therefore, there is less Ta2O5 on the surface in direct contact with the gas environment. In addition, in embodiments where the ceramic oxide used is alumina, it is believed that Ta2O5 forms an alumina-based glass that is more resistant to chlorine corrosion than Ta2O5 alone.
[0028] In some embodiments, the cross-sectional area of the tantalum phase near the metallization layer (e.g., a minimum sample cross-sectional area of approximately 300 μm2 or more (e.g., 20 μm×15 μm) at a maximum point no more than 30 μm from the metallization layer) is 20% larger, or 40% larger, or 80% larger, or 100% larger, or 150% larger, or 200% larger than the cross-sectional area of the tantalum phase near the surface of the top dielectric layer (e.g., a minimum sample cross-sectional area of approximately 300 μm2 or more (e.g., 20 μm×15 μm) at a maximum point no more than 30 μm from the surface).
[0029] The Ta2O5 phase has a relatively high melting point and a relatively low vapor pressure. Not only is the Ta2O5 phase corrosion resistant and non-volatile at temperatures up to 1000°C or more, it also forms a barrier that prevents more volatile impurities from migrating through the first ceramic layer and entering the processing chamber. The layer arrangement thus has the benefit of being able to operate reliably in high temperature corrosive environments while not contaminating wafers in semiconductor production.
[0030] In particular, in non-etching applications such as ion implantation chambers, tantalum oxide doped alumina ESCs result in a much cleaner processing environment because Ta2O5 has a lower vapor pressure than other binders such as magnesium oxide and calcium oxide.
[0031] The inert nature of the ESC with the Ta2O5 dielectric top layer in corrosive gases also enables the ESC to maintain its mechanical integrity over a longer period of time compared to conventional ESCs.
[0032] The formation of a liquid Ta2O5 phase during high temperature sintering also facilitates the bonding of the ceramic layer to the metallization layer, thus avoiding delamination of different layers in the ESC.
[0033] Depending on the specific application and the composition of the first ceramic layer, the thickness of the first ceramic layer is typically between 10 μm and 1.0 mm, or between 20 μm and 500 μm, or between 30 μm and 400 μm, or between 40 micrometers and 300 μm, or between 50 μm and 200 μm, including all subranges and values therebetween. When the first ceramic layer is the top dielectric layer of an ESC for an ion implantation process, the dielectric layer needs to withstand a voltage range of 500 V to 2000 V. For an ESC for an etching or deposition process, the dielectric layer may need to withstand a voltage of 3000 V to 6000 V, preferably 1000 V to 3000 V.
[0034] In one embodiment, the breakdown voltage of the top dielectric layer is at least 60 V / μm, or at least 70 V / μm, or at least 80 V / μm.
[0035] For Al2O3 (99.5wt%)-Ta2O5 (0.5wt%) dielectric layers, the dielectric breakdown voltage is about 2000V / mil or 80V / μm. When a safety margin is added, the approximate thickness of the dielectric layer may be between 10μm or 20μm and 200μm. Compared to conventional high-purity dielectric layers (such as, Al-995TM and Al-998TM (available from Morgan Advanced Ceramics, Hayward, CA)), the superior dielectric breakdown strength of the layer arrangement of the embodiments of the present invention allows thinner dielectric layers to be used for the same application voltage.
[0036] The density of the first ceramic layer is preferably greater than 97%, more preferably greater than 98%, and even more preferably greater than 99% of the theoretical maximum density of the ceramic material (porosity 0%). Alternatively, the porosity of the first ceramic layer is preferably less than 3% v / v, more preferably less than 2% v / v, and even more preferably less than 1% v / v.
[0037] The density of the first ceramic layer may be greater than 3.90 g / cm 3 , or greater than 3.91g / cm 3 , or greater than 3.92g / cm 3 , or greater than 3.93g / cm 3 , or greater than 3.94g / cm 3, or greater than 3.95g / cm 3 .
[0038] The density of the second ceramic layer is preferably lower than that of the first ceramic layer.The second ceramic layer preferably comprises at least 95 wt % and more preferably at least 95 wt % of alumina, titania, ZrO2, Y2O3, AlN, Si3N4, SiC or a combination thereof.
[0039] The average grain size of the ceramic material forming the first layer and the second layer is preferably between about 0.5 μm and 5 μm, and more preferably between 1 μm and 3 μm.
[0040] The first ceramic layer and the second ceramic layer preferably include the same ceramic component. In a preferred embodiment, the first ceramic layer and the second ceramic layer include aluminum oxide. In this embodiment, the second ceramic layer preferably has a high aluminum oxide content (e.g., Al-998TM). Due to the substantial absence of sintering aids, higher purity aluminum oxide is more difficult to sinter and densify. Therefore, the density of the second ceramic layer is generally lower than that of the first ceramic layer, and is therefore conducive to the migration of liquid Ta2O5 to the second ceramic phase and entering the second ceramic phase. The migration of liquid Ta2O5 into the second ceramic phase may only be near the metallization layer interface (i.e., not extending to the entire second ceramic layer).
[0041] In another embodiment, the first ceramic layer comprises a static charge dissipative material comprising aluminum oxide doped with a transition metal oxide and between 0.1 wt % or 0.5 wt % and 10.0 wt % tantalum oxide (Ta2O5). The transition metal oxide is preferably present in an amount in the range of 1.0 wt % to 8.0 wt % (preferably in the range of 1.5 wt % to 7.5 wt % or in the range of 2.0 wt % to 7.0 wt %) based on the total weight of the ceramic material in the first ceramic layer. In this embodiment, the aluminum oxide doped with the transition metal oxide preferably accounts for at least 90 wt % of the first ceramic layer.
[0042] Doping of alumina enables the resistivity of the doped alumina to be controlled as disclosed in US 6,641,939, which is incorporated herein by reference.
[0043] The transition metal oxide may be selected from the group consisting of oxides of Re, Ti, V, Fe, Cr, Co, Mn, Ni, Mo and Nb. The transition metal oxide is preferably titanium dioxide.
[0044] It is believed that the continuity of the grain boundary phase and the wetting angle of the Ta2O5-titanate liquid phase control the resistivity of the doped alumina. Compared with high purity alumina, a larger amount of Ta2O5 needs to be added to the titania-doped alumina to form the Ta2O5-titanate liquid phase (e.g., in the range of 2.0 wt% to 10 wt% Ta2O5) at a co-firing temperature equal to or lower than 1600°C.
[0045] In embodiments comprising a transition metal oxide doped aluminum oxide first ceramic layer, the breakdown voltage of the first ceramic layer is preferably at least 20 V / μm, or at least 30 V / μm, or at least 40 V / μm.
[0046] In a second aspect, an electrostatic chuck is provided comprising the layer arrangement of the first aspect.
[0047] In a third aspect, there is provided a method of manufacturing a layer arrangement for an electrostatic chuck, comprising the steps of:
[0048] A. forming a first ceramic layer or a second ceramic layer to obtain a base layer in a green state;
[0049] B. applying a metallization layer to the substrate layer;
[0050] C. placing a first ceramic layer or a second ceramic layer on top of the metallized layer to form a top layer in a green state; the first ceramic layer (in a co-fired state) comprising:
[0051] At least 90 wt% of aluminum oxide, titanium dioxide, ZrO2, Y2O3, AlN, Si3N4, SiC, transition metal oxides, or combinations thereof; and sufficient to densify the first ceramic layer to at least 97%, or 98%, or 98.5%, or 99.0% of the theoretical density of the first ceramic layer. Tantalum oxide (Ta2O5) is preferably in the range of 0.1 wt% to 10.0 wt%.
[0052] D. Co-firing the layers at sufficient temperature and time to form a liquid Ta2O5 phase,
[0053] The liquid Ta2O5 phase migrates toward the interface between the first ceramic layer, the metallization layer and the second ceramic layer.
[0054] In a fourth aspect, there is provided a method of manufacturing a layer arrangement for an electrostatic chuck, comprising the steps of:
[0055] A. forming a substrate layer comprising a first material in a green state;
[0056] B. applying a refractory metallization forming material to the base layer to form a metallization layer;
[0057] C. disposing a top layer comprising a second material in a green state over the metallization layer;
[0058] D. co-firing the base layer, metallization layer and top layer at a sufficient temperature and time to form a liquid Ta2O5 phase,
[0059] wherein the liquid Ta2O5 phase migrates toward the interface between the top layer, the metallization layer and the base layer; and
[0060] In the co-fired state, the top layer includes a first ceramic material, which includes: at least 90.0wt% of aluminum oxide, titanium dioxide, ZrO2, Y2O3, AlN, Si3N4, SiC or a combination thereof; and tantalum oxide (Ta2O5) in the range of 0.1wt% to 10.0wt%.
[0061] Other methods of forming the layer arrangement are possible, for example, using a binder to bond the layers together, rather than co-firing. However, in general, co-firing is preferred because it promotes a Ta2O5 concentration gradient from the top surface to the metallization layer, thereby:
[0062] Creating a barrier at or near the metallization layer to prevent the migration of volatile impurities to the surface of the dielectric layer;
[0063] creating an adhesion layer between the dielectric layer and the metallization layer to prevent delamination of the dielectric layer and the metallization layer; and
[0064] An inert dielectric layer surface is provided that is substantially free of volatile impurities and is capable of operating in an atmosphere critical environment, such as in an ion implantation chamber.
[0065] Preferably, the second ceramic layer is a base layer and the first ceramic layer is a top layer.
[0066] Additional layers (eg heater layers) may be added to the arrangement prior to co-firing. The additional layers are preferably added to the base layer, thereby maintaining the first ceramic layer as the top layer.
[0067] The interface between the metallization layer and the adjacent ceramic layer is prone to delamination and void formation, in part due to thermal expansion mismatch and / or void formation. The liquid Ta2O5 phase in the first ceramic layer migrates to the metallization layer interface to form a more reliable bond between the metallization layer and the adjacent ceramic layer.
[0068] Typically, the temperature and time for densifying the first ceramic layer to greater than 97.0 wt % of the theoretical maximum density of the first ceramic layer are sufficient to allow the liquid Ta2O5 phase to improve the adhesion of the metallization layer. However, maintaining the co-firing conditions for an extended time (e.g., greater than 1 hour or greater than 2 hours) can have additional positive effects. The extended co-firing time can also result in a reduced level of Ta2O5 on the surface of the first ceramic layer compared to the surface in the green state due to the migration of the Ta2O5 phase. The lower level of Ta2O5 in the surface layer (e.g., 10%, 20%, or 50% less than the surface in the green state) makes the surface suitable for use in a chlorine (Cl2 and BCl3) gas environment or even a fluorine gas environment.
[0069] Preferably, during the densification process, the density of the second ceramic layer is lower than that of the first ceramic layer, because the higher void fraction in the second ceramic phase and around the layer boundaries promotes the migration of the liquid Ta2O5 phase into the second ceramic layer.
[0070] The first ceramic layer and the second ceramic layer can be realized by any suitable technique (including dry pressing or casting). In one embodiment, the second layer is formed by dry pressing, and the first layer is formed by casting. The details of this process are provided in US20170057880, which is incorporated herein by reference. When the thickness of the dielectric layer is less than 200 μm and more preferably less than 100 μm, casting is preferably used.
[0071] The thickness of the green second ceramic layer can vary widely, depending primarily on its specific application. However, in general, its thickness ranges from about 0.1 mm to about 5 mm. Preferably, the green ceramic layer has a uniform or at least substantially uniform thickness.
[0072] Metallization
[0073] The metallization layer may include a refractory metallization forming material, i.e., during co-firing, the refractory metallization forming material forms a conductive refractory metal phase on the substrate. In general, metallization forming materials are known in the art and can be purchased commercially. The melting temperature of the metallization forming material is preferably significantly lower than the co-firing temperature (e.g., 50° C. or 100° C. lower). The metallization material is preferably a metal selected from the group consisting of platinum, palladium, tungsten, molybdenum, niobium, tantalum and alloys thereof.
[0074] Typically, the metallization forming material is in the form of a paste or ink comprising refractory metal particles suspended in an organic binder and a solvent. The metallization material may also contain some glass-forming components (e.g., SiO2, MgCO3, kaolin), which further aids in the bonding of the metal to the substrate. However, such addition is optional because the liquid Ta2O5 phase formed can improve the bonding of the metallization layer to the substrate.
[0075] Generally, the refractory metal particles range in size from about 0.1 microns to about 20 microns.
[0076] The refractory metal may be any metal whose particles can sinter together during sintering of the sinterable ceramic composition of the present invention to produce a continuous conductive phase. The refractory metal must be solid during sintering of the ceramic composition and preferably, it is tungsten or molybdenum.
[0077] The metallization material can be contacted with the ceramic layer by many conventional techniques. Generally, it is deposited or printed on and / or in the middle of the preselected electrostatic chuck electrode pattern. Typically, it is screen printed on top.
[0078] manufacture
[0079] In the manufacture of a monolithic body with a multilayer ceramic substrate, a plurality of green ceramic layers are produced and metallization material is contacted to them or printed on most, if not all, of them in a preselected pattern. Through holes or through-holes may be punched in the sheets as required for interconnection of the layers and filled with metallization material, usually in the form of a paste. The sheets are then stacked together in a preselected manner, usually forming a sandwich, i.e., on top of one another. The stack may be laminated to form a laminated structure at a pressure and temperature, which is primarily determined by its specific composition, but is usually below about 100°C, and then co-fired.
[0080] After the metallization coating is applied, isostatic pressing can be used to assemble the multilayer green tapes and / or dry pressed green sheets. Typical pressures are up to about 103 MPa (15 kpsi), but higher pressures can be used as needed. Isostatic pressing not only produces good lamination between the tapes, but also ensures uniform shrinkage of the multilayer tape structure during firing.
[0081] When the fired laminate assembly is used as an electrostatic chuck, the outer surface or face of the co-fired ceramic component needs to be substantially flat in order to ensure maximum surface area contact between the substrate wafer and the supporting surface of the dielectric layer. In order to provide flatness of the co-fired ceramic component, a method of flattening the fired layer arrangement includes the following steps:
[0082] a) arranging a support layer on an insulating setter having at least one substantially flat surface;
[0083] b) installing or mounting an insulating weight having at least one substantially flat surface on the layer arrangement such that the layer arrangement is located between the insulating setter and the substantially flat surface of the insulating weight.
[0084] Steps (a) and (b) are then fired to a sintering temperature in an inert (e.g., N2) or reducing (e.g., H2) gas environment. Preferably, at least one surface of the setter and / or weight adjacent to the article is machined to be substantially flat. By machining at least one surface of the setter and / or weight in contact with the green article to be substantially flat, the green layer arrangement will maintain its flatness during firing or adopt the flatness of the setter and / or weight surface. For example, in the latter case, when the green layer arrangement is not completely flat or has defects due to its formation process (such as dry pressing or isostatic pressing or even processing), by firing the green layer arrangement between the substantially flat surface of the setter and the weight, the pressure applied by the weight causes the layer arrangement to substantially adopt the flatness of the flat surface of the setter and / or weight.
[0085] The structures of the present invention are preferably co-fired to produce a sintered structure comprising a sintered ceramic substrate free of voids greater than about 5 microns and a bonded refractory metal conductive phase.
[0086] During sintering, the first ceramic layer preferably includes a Ta2O5 liquid phase for producing a ceramic substrate of the desired density. Preferably, the Ta2O5 liquid phase bonds the sintered metal particles to the adjacent ceramic layer. During sintering, a portion of the liquid phase that achieves sintering of the ceramic migrates through capillaries into the voids between the sintered refractory metal particles to obtain a phase, typically a glass phase, which mixes with the continuous phase of the refractory metal and helps to bond the refractory metal phase to the substrate. The sintering temperature can vary greatly, depending primarily on the specific ceramic composition, but is generally above 1300°C and typically ranges from about 1350°C to about 2100°C. For example, for a sinterable liquid phase Ta2O5-alumina composition, a typical sintering temperature is about 1500°C to about 1600°C.
[0087] Further details regarding machining components to form an electrostatic chuck can be found in US20170057880, which is incorporated herein by reference.
[0088] For convenience, tantalum is described as being in the oxide form (Ta2O5), and it is understood that tantalum may exist in other forms. BRIEF DESCRIPTION OF THE DRAWINGS
[0089] Figure 1 is an exploded view (not to scale) of the arrangement of layers that form an electrostatic chuck.
[0090] Figure 2 is a SEM image of a first ceramic layer (top), a metallization layer, and a second ceramic layer according to an embodiment.
[0091] Figure 3 yes Figure 2 Magnified SEM image of .
[0092] Figure 4 is the weight loss of Al2O3-Ta2O5 composite after corrosion test (×10-4 g / cm 2 ) in the table below.
[0093] Figure 5 is the flexural strength (MPa) of the Al2O3-Ta2O5 composition after corrosion testing.
[0094] Figure 6 is a SEM image of a cross section of the layer arrangement.
[0095] Figure 7 is a SEM image of a cross section of the top portion of the dielectric layer.
[0096] Figure 8 is a SEM image of a cross section of the middle portion of the dielectric layer.
[0097] Fig. 9 is a SEM image of a cross section of the bottom portion of the dielectric layer.
[0098] Fig.10 are SEM images and EDS spectra highlighting the presence of the tantalum phase in the dielectric layer.
[0099] Fig.11a -c is Fig. 9 A portion of a SEM image that has been processed using digital imaging software. DETAILED DESCRIPTION
[0100] refer to Figure 1 , there is an electrostatic chuck 10 with a diameter of 300 mm, which includes: a top dielectric layer 20 with a thickness of 150 μm formed by dry pressing, which has a top surface 22; a metallization layer 30 (20 μm) comprising a molybdenum-based coating composition; a dry-pressed insulating layer 40 with a thickness of about 50 μm; a heater layer (20 μm) 50, which includes a molybdenum-based coating composition; and a base layer with a thickness of 150 μm.
[0101] Each of the dielectric layer 20, the insulating layer 40 and the base layer 60 comprises high purity alumina. The dielectric layer 20 comprises 99.5 wt% Al2O3, 0.5 wt% Ta2O5 and trace levels of impurities. The thin insulating layer 40 and the base layer 60 are both formed from alumina powder having a nominal purity of 99.8 wt% Al2O3 (Al-998TM). Other suitable alumina powders include Al-995TM. High purity alumina forms the basis of alumina formulations (Al-998TM, AL-995TM and E-1 formulations) in which the average particle size of the alumina particles is about 1.2 μm; the surface area is about 3.5 m 2 / g.
[0102] The ceramic layer is dry pressed using spray dried alumina; binders, dispersants and other additives as described in paragraphs 57 to 62 of US20170057880.
[0103] refer to Figure 2 , the co-fired layer arrangement 10 includes a dielectric layer 20 including small voids distributed therein. The top portion 70 of the dielectric layer 20 is expected to have a lower proportion of Ta2O5 relative to the interface region 80 between the dielectric layer 20 and the metallization layer 30. The metallization layer includes sintered metal particles and a glass phase, some of which may be part of the metallization composition and some of which may be derived from the Ta2O5 in the dielectric layer. The insulating layer 40 includes a larger proportion of voids than the dielectric layer 20.
[0104] The enlarged image of the interface region 80 shows that the proportion of voids in this region is larger than in the majority of the dielectric layer 20 .
[0105] Example:
[0106] sample
[0107] The composition of sample E-1 is 99.5wt% Al2O3 and 0.5wt% Ta2O5. Other impurities are less than 0.1wt%. The average particle size of Ta2O5 is less than 1.0μm, and the smaller particle size distribution (compared with Al2O3) helps to evenly disperse Ta2O5 in Al2O3. The density of E-1 is 3.96g / cm3.
[0108] Sample CE-1 is Al-995TM available from Morgan Advanced Ceramics (Hayward, CA) and has a composition of 99.5 wt% Al2O3 and 0.5 wt% other materials (excluding Ta2O5), including glass forming materials. The density of CE-1 is 3.91 g / cm 3 The samples (E-1 and CE-1) were laminated at room temperature under 15 Kpsi pressure and then co-fired at 1575°C in H2 for 2 hours.
[0109] The composition of sample E-2 is 2.0 wt% TiO2, 4.0 wt% Ta2O5, less than 0.1 wt% other impurities and the remainder is Al2O3. The density of E-2 is 3.96 g / cm3.
[0110] Sample CE-2 is a commercial composition in which energy dispersive X-ray spectroscopy (EDS) analysis confirmed the presence of a major Al2O3 component and minor components TiO2, MgO, CaO and SiO2. The density of CE-2 is 3.85 g / cm3.
[0111] The samples (E-2 and CE-2) were laminated at room temperature under 15 Kpsi pressure and then co-fired at 1600°C in H2 for 2 hours.
[0112] Corrosion resistance and flexural strength
[0113] The samples were of known weight and flexural strength and each had an average surface area of 15.5 cm 2 Samples CE1 and E1 were placed in Teflon™ test containers with 150 ml of 20% v / v aqueous hydrochloric acid, sulfuric acid, nitric acid or potassium hydroxide at 90°C for 11 weeks. The samples were then reweighed and retested for flexural strength, with the average results provided in Figure 4 and Figure 5 middle.
[0114] The results show that the corrosion resistance and flexural strength of sample E-1 (alumina-Ta2O5) are improved compared to sample CE-1 (alumina-MgO-silica).
[0115] Dielectric properties
[0116] Sample E-1
[0117] The breakdown voltage was determined at room temperature according to ASTM D149. The results (Table 1) indicate that the breakdown voltage of the Al2O3-Ta2O5 dielectric layer is more than twice that of a conventional high purity alumina dielectric layer, thereby enabling the use of thinner dielectric layers.
[0118] Table 1
[0119]
[0120]
[0121] Sample CE-1 is reported to have a dielectric breakdown voltage of 800 V / mil at room temperature.
[0122] The breakdown voltage was also determined in an ESC comprising a top dielectric layer comprising 99.8 wt% alumina (Al998™ from Morgan Advanced Ceramics) processed under the same conditions as E-1 and CE-1. The density was 3.92 g / cm 3 , and the breakdown voltage varies between 569V / mil and 943V / mil, with an average value of 741V / mil.
[0123] Table 2
[0124] Thickness(mil) Breakdown voltage(V) Breakdown voltage (V / mil) [V / μm] 7.0 6659 951[37.5] 7.0 6582 940[37.0] 7.0 6418 917[36.1] 7.0 8044 1149[45.2] average value 6926 989[38.9]
[0125] The breakdown voltage of CE-2 is 11V / μm.
[0126] The volume resistivity of E-2 is 2×10-11Ωcm, compared to 1×10-11Ωcm of CE-2.
[0127] Compared to conventional electrostatic charge dissipative materials of the prior art (eg US 6,641,939), the layer arrangements herein are able to provide greater breakdown voltage (Table 2), corrosion resistance and density.
[0128] Densification of the first ceramic layer
[0129] The samples were processed as previously described, except that the sintering temperature and time were adjusted. The density of the first ceramic layer is affected by the temperature and the duration maintained at the sintering temperature. As shown in Table 3, the combination of sintering temperature and time affects the densification process. If the sintering temperature is high enough, then time may be the limiting factor for the liquid phase to penetrate the voids and increase densification.
[0130] Table 3
[0131] Sintering temperature(℃) Time (hours) <![CDATA[Density (g / cm 3 ) [*% of theoretical value]]]> 1600 2 3.96[99.25%] 1530 2 3.95[99.00%] 1530 0.5 3.89[97.49%]
[0132] *The density of Al2O3 is 3.99 g / cm 3 Distribution of Tantalum in the First Ceramic Layer
[0133] refer to Figure 6-Figure 9 , the Ta2O5 concentration was measured at a cross-sectional area 170 near the surface in the top dielectric (top (sample A)), at a cross-sectional area 120 in the middle of the dielectric layer (middle (sample B)), and at a cross-sectional area 180 at the bottom of the dielectric layer adjacent to the metallization layer 130 (bottom (sample C)). No significant amount of Ta2O5 was found in the second ceramic layer 140, but it is more likely to exist at the interface between the first ceramic layer and the second ceramic layer rather than being separated by the metallization layer 130.
[0134] The cross-sectional surface area of each component of the dielectric layer was determined using the image processing software tool ImageJTM. Voids and artifacts in the image (identified as black) were excluded from the total cross-sectional area. The graphical data were then converted into a binary format (white - tantalum part; black - others) using a threshold based on the hue of the tantalum part, with the composition verified from the corresponding EDS spectra, as indicated by the verification of the tantalum phase in the middle (sample B) ( Fig.10 ). The ratio of black to white pixels was then used to calculate the cross-sectional area ratio of the tantalum portion of the top (sample A), middle (sample B), and bottom (sample C) of the dielectric layer.
[0135] The image analysis process of the bottom (sample C) is shown in Figure 11a-Figure 11c In the first step, we use image processing tools to analyze the sample image area ( Fig.11a) to remove gaps and artifacts ( Fig.11b ), which is then used to identify the area relative to the remaining area (excluding Fig.11b The identified gaps and artifacts in Fig.11c ) Cross-sectional area of the tantalum phase (white). The same processing steps were used to calculate the cross-sectional area of the tantalum phase in the top (sample A) and in the middle (sample B).
[0136] Using a maximum point of no more than 30 μm from the metallization layer for the bottom (sample C) and a maximum point of no more than 30 μm from the dielectric layer surface for the top (sample A) of about 312 μm. 2 The top (sample A), middle (sample B), and bottom (sample C) portions of the dielectric layer were analyzed using EDS analysis with a sample cross-sectional area of (26 μm × 12 μm), and the results are shown in Table 4. As shown in Table 4, the proportion of tantalum (relative to the total effective area of the sample, i.e., the total sample area minus the sample area occupied by voids and artifacts) is the highest at the bottom of the dielectric layer (sample C), and the proportion of tantalum decreases toward the top of the dielectric layer (sample A). This is the case at the top (sample A) ( Figure 7 )、Middle(Sample B)( Figure 8 ) and bottom (sample C) ( Fig. 9 ) was referenced in the SEM image of Fig. 9 The Ta2O5 phase (the speckled white phase) above the middle metallization layer 130 is significantly more abundant.
[0137] Table 4
[0138] Dielectric layer location Cross-sectional area of Ta phase % Change from Top (Sample A) Top (Sample A) 0.29% - Middle (Sample B) 0.50% 172% Bottom (Sample C) 0.73% 252%
[0139] Throughout this specification, references to "one embodiment," "certain embodiments," "various embodiments," "one or more embodiments," or "an embodiment" mean that a particular feature, structure, material, or characteristic described in conjunction with the embodiment is included in at least one embodiment of the present disclosure. Thus, phrases such as "in one or more embodiments," "in certain embodiments," "in various embodiments," "in one embodiment," or "in an embodiment" appearing in various places throughout this specification do not necessarily refer to the same embodiment of the present disclosure. Furthermore, in one or more embodiments, the particular features, structures, materials, or characteristics may be combined in any suitable manner.
[0140] Although the present disclosure has been described herein with reference to specific embodiments, it should be understood that these embodiments are merely illustrations of the principles and applications of the present disclosure. It will be apparent to those skilled in the art that various modifications and variations may be made to the present disclosure without departing from the spirit and scope of the present disclosure. Therefore, the present disclosure is intended to include modifications and variations within the scope of the appended claims and their equivalents.
Claims
1. A layer arrangement for an electrostatic chuck, the layer arrangement comprising: A. first ceramic layer; B. second ceramic layer; C. a metallization layer, the metallization layer being disposed between the first ceramic layer and the second ceramic layer, The first ceramic layer comprises: At least 90.0 wt % of alumina, titania, ZrO2, Y2O3, AlN, Si3N4, SiC, transition metal oxides, or combinations thereof; and Tantalum oxide (Ta2O5) in the range of 0.1wt% to 10.0wt%, Wherein a concentration of Ta2O5 at or near a top surface of the first ceramic layer is lower than a concentration of Ta2O5 at or near an interface between the first ceramic layer and the metallization layer.
2. The layer arrangement of claim 1, wherein the first ceramic layer is a top dielectric layer. 3 . The layer arrangement according to claim 2 , wherein the thickness of the top dielectric layer is in the range of 20 μm to 200 μm.
4. The layer arrangement according to claim 1, wherein the first ceramic layer comprises at least 98 wt% aluminum oxide.
5. The layer arrangement according to claim 1, wherein the first ceramic layer comprises at least 99.0 wt% of the sum of tantalum oxide, aluminum oxide, titanium dioxide, ZrO2, Y2O3, AlN, Si3N4, SiC and transition metal oxides. 6 . The layer arrangement according to claim 1 , wherein the metallization layer comprises a metal selected from the group consisting of platinum, palladium, tungsten, molybdenum, niobium, tantalum and alloys thereof.
7. The layer arrangement according to claim 1, wherein the second ceramic layer comprises aluminum oxide, titanium dioxide, ZrO2, Y2O3, AlN, Si3N4, SiC or a combination thereof.
8. The layer arrangement of claim 1, further comprising a Ta2O5 phase at an interface of the first ceramic layer and the metallization layer.
9. The layer arrangement of claim 1, wherein a cross-sectional area of the Ta2O5 phase in the first ceramic layer close to the metallization layer is more than 20% larger than a cross-sectional area of the Ta2O5 phase in the first ceramic layer close to a top surface of the first ceramic layer.
10. The layer arrangement according to claim 1, wherein the density of the first ceramic layer is greater than 97% of its theoretical maximum density. The layer arrangement according to claim 1 , wherein the density of the second ceramic layer is lower than the density of the first ceramic layer.
12. A layer arrangement according to claim 1, wherein the first ceramic layer comprises an electrostatic charge dissipative material, the material comprising aluminum oxide doped with a transition metal oxide and 0.5 wt % to 10.0 wt % Ta2O5, wherein the transition metal oxide is present in an amount ranging from 1.0 wt % to 8.0 wt % based on the total weight of the ceramic material in the first ceramic layer.
13. The layer arrangement according to claim 12, wherein the transition metal oxide comprises titanium dioxide (TiO2).
14. The layer arrangement of claim 12, wherein the first ceramic layer comprises between 2.0 wt% and 6.0 wt% Ta2O5.
15. The layer arrangement according to claim 1, wherein the layer arrangement is a co-fired layer arrangement.
16. An electrostatic chuck comprising the layer arrangement according to claim 1.
17. The electrostatic chuck of claim 16, wherein the first ceramic layer has a breakdown voltage of at least 60 V / μm.
18. A method of manufacturing a layer arrangement for an electrostatic chuck, the method comprising: A. forming a substrate layer, the substrate layer comprising a first material in a green state; B. applying a refractory metallization forming material to the base layer to form a metallization layer; C. disposing a top layer comprising a second material in a green state over the metallization layer; D. co-firing the base layer, metallization layer and top layer at a sufficient temperature and time to form a liquid Ta2O5 phase, wherein the liquid Ta2O5 phase migrates toward the interface between the top layer, the metallization layer and the base layer; and In the co-fired state, the top layer includes a first ceramic material, which includes: at least 90.0wt% of aluminum oxide, titanium dioxide, ZrO2, Y2O3, AlN, Si3N4, SiC or a combination thereof; and tantalum oxide (Ta2O5) in the range of 0.1wt% to 10.0wt%, and the Ta2O5 concentration at or near the top surface of the first ceramic layer is lower than the Ta2O5 concentration at or near the interface between the first ceramic layer and the metallization layer.
19. The method of claim 18, wherein the first ceramic material comprises greater than 99.0 wt% alumina and less than 1.0 wt% Ta2O5.
20. An electrostatic chuck comprising a layer arrangement formed by the method of claim 18.
21. A method of manufacturing a silicon wafer in a halogen gas environment, wherein the silicon wafer is electrostatically held by an electrostatic chuck formed by the method according to claim 18.
22. The method of claim 21, wherein the halogen gas environment comprises chlorine gas or boron trichloride gas.
23. The method of claim 21, wherein the method comprises ion implantation.
24. A layer arrangement for an electrostatic chuck, the layer arrangement comprising: A. first ceramic layer; B. second ceramic layer; C. A metallized layer disposed between the first ceramic layer and the second ceramic layer, wherein the first ceramic layer comprises an electrostatic charge dissipative material comprising aluminum oxide doped with a transition metal oxide and between 2.0 wt % and 10.0 wt % Ta2O5, wherein the transition metal oxide is present in an amount ranging from 1.0 wt % to 8.0 wt % based on the total weight of the ceramic material in the first ceramic layer, and a concentration of Ta2O5 at or near a top surface of the first ceramic layer is lower than a concentration of Ta2O5 at or near an interface between the first ceramic layer and the metallized layer.
25. The layer arrangement of claim 24, wherein the aluminum oxide doped with a transition metal oxide comprises at least 90 wt% of the first ceramic layer.
Citation Information
Patent Citations
Method for manufacturing large ceramic co-fired articles
US20170057880A1
Process for cofiring structure comprised of ceramic substrate and refractory metal metallization
US4678683A
Dielectric ceramics for electrostatic chucks and method of making them
US5104834A
Ceramic electrostatic wafer chuck
US5207437A
Multilayered electrostatic chuck and method of manufacture thereof
US5671116A