Packaging mold and preparation method thereof
By forming a copper or chromium metal layer with a columnar crystal structure on the surface of the packaging mold and forming an oxide layer, the problem of adhesion between the packaging material and the mold surface is solved, and the stability of the packaging process and product quality are improved.
Patent Information
- Application Number
- CN202110900820.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-08-06
AI Technical Summary
The adhesion between the packaging materials and the surface of the packaging mold leads to problems with the packaging process stability and product quality, especially the silicone-containing materials used in the LED industry are more likely to form adhesion.
Using copper or chromium metal layer with a columnar crystal structure as the anti-adhesive coating, a closely-bonded coating is formed on the surface of the packaging mold through magnetron sputtering process, and an oxide layer is formed on the surface to reduce the interface energy to improve the anti-adhesive coating. Effect.
It effectively reduces the adhesion between the packaging material and the mold surface, improves the stability of the packaging process and product quality, and improves the overall performance of the packaging process.
Smart Images

Figure CN113628982B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of packaging process and the technical field of coating, and in particular to a packaging mold with an anti-sticking coating. Background Art
[0002] In the packaging process, one of the problems faced by current packaging molds during use is that the packaging material and the surface of the mold are easy to stick to each other. The packaging material (e.g., epoxy resin) is mostly a non-Newtonian fluid with a high viscosity coefficient, which easily forms sticky residues on the surface of the packaging mold. The packaging material remaining on the mold not only affects the stability of the packaging process and the appearance of the product, but also affects the performance of the product in some high-precision packaging processes.
[0003] With the rise of the LED industry, the research and development and application of packaging materials containing silicon (Si) glue have increased. Compared with traditional resin packaging materials containing silicon (Si) glue, it is easier to form adhesion with the surface of the packaging mold. Therefore, it is necessary to further study and improve the surface or coating of the packaging mold. Summary of the invention
[0004] The present application provides a packaging mold with a self-adjusting anti-sticking coating and a method for preparing the packaging mold. The self-adjusting anti-sticking coating is a copper layer or a chromium layer with a columnar crystal structure, which can form a tightly bonded structure with the surface of the packaging mold substrate and effectively reduce the adhesion between the packaging material and the surface of the mold substrate, thereby improving the stability of the packaging process and the yield of the product.
[0005] According to one aspect of the present application, a packaging mold is provided, which includes: a packaging film substrate and a coating. The coating is disposed on a portion of the surface of the packaging film substrate, wherein the coating includes a metal layer having a columnar crystal structure, and the metal layer includes one of copper or chromium.
[0006] In some embodiments, the coating further comprises an oxide layer disposed on the surface of the metal layer, the oxide layer being one of copper oxide or chromium oxide.
[0007] In some embodiments, the oxide layer has a thickness of 100 nm to 1 μm.
[0008] In some embodiments, the coating thickness is 2 μm to 10 μm.
[0009] In some embodiments, the crystal structure of the columnar crystal structure of the metal layer is a cubic crystal system, and the crystal structure belongs to a body-centered cubic structure.
[0010] In some embodiments, the grain size of the columnar crystal structure of the metal layer is 30 nm to 100 nm.
[0011] According to another aspect of the present application, the present application provides a method for preparing a packaging mold, which includes the following steps: providing a packaging film substrate and using a magnetron sputtering process to form a metal layer with a columnar crystal structure on the surface of the packaging film substrate, and the metal layer contains one of copper or chromium.
[0012] In some embodiments, the bias voltage used in the magnetron sputtering process is 30V to 100V, and the target power is 5Kw to 15Kw.
[0013] In some embodiments, the gas pressure of the closed chamber furnace in the magnetron sputtering process is 0.1 Pa to 1 Pa, and the sputtering deposition time is 40 minutes to 120 minutes.
[0014] In some embodiments, after the metal layer is formed, the method further comprises the following steps: placing the packaging mold in a pure oxygen environment to form an oxide layer on the surface of the metal layer, wherein the oxide layer is one of copper oxide or chromium oxide.
[0015] In some embodiments, the temperature in the oxygen-containing environment is 75°C to 90°C.
[0016] In some embodiments, after the step of providing a packaging film substrate and before the step of forming a metal layer, it further includes using argon ion cleaning on the surface of the packaging film substrate. The argon ion cleaning step includes the following steps: introducing argon gas into a closed chamber furnace, applying a bias voltage of 100V to 800V, and cleaning the surface of the packaging film substrate.
[0017] The packaging mold with a self-adjusting anti-sticking coating provided by the present application, a metal copper layer or a metal chromium layer with a columnar crystal structure formed by a magnetron sputtering process, can form a compact coating structure, and its columnar crystal structure has a typical growth preference, which is conducive to the diffusion of oxygen elements in the air, so that it can self-adjust to form a stable metal oxide layer on the surface of the coating, and reduce the interface energy of the coating surface, which is conducive to the anti-sticking effect. Therefore, the packaging mold with a self-adjusting anti-sticking coating provided by the present application can be used in the packaging process to effectively improve the stability of the packaging process and the product quality.
[0018] Additional aspects and advantages of the embodiments of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The following will briefly describe the drawings necessary for describing the embodiments of the present application or the prior art to facilitate the description of the embodiments of the present application. Obviously, the drawings described below are only some of the embodiments in the present application. For those skilled in the art, without the need for creative work, drawings of other embodiments can still be obtained based on the structures illustrated in these drawings.
[0020] Figure 1 Schematic cross-sectional view of a packaging mold according to some embodiments of the present application.
[0021] Figure 2 FIG. 4 is a cross-sectional electron microscope image of a coating layer of a packaging mold according to an embodiment of the present application.
[0022] Figure 3 The figure is a top-view electron microscope image of a coating layer of a packaging mold according to an embodiment of the present application.
[0023] Figure 4 Schematic cross-sectional view of a packaging mold according to some embodiments of the present application.
[0024] Figure 5 The figure is a cross-sectional electron microscope image of a coating layer of a packaging mold according to an embodiment of the present application. DETAILED DESCRIPTION
[0025] The embodiments of the present application will be described in detail below. In the full text of the present application specification, the same or similar components and components with the same or similar functions are represented by similar reference numerals. The embodiments of the accompanying drawings described herein are illustrative, graphical, and are used to provide a basic understanding of the present application. The embodiments of the present application should not be interpreted as limiting the present application.
[0026] As used herein, the terms "about," "substantially," and "essentially" are used to describe and illustrate small variations. When used in conjunction with an event or circumstance, the terms may refer to instances where the event or circumstance occurred exactly as well as instances where the event or circumstance occurred very approximately. For example, when used in conjunction with a numerical value, the terms may refer to a range of variation less than or equal to ±10% of the numerical value, such as less than or equal to ±5%, less than or equal to ±0.5%, or less than or equal to ±0.05%. For example, two numerical values may be considered "substantially" the same if the difference between the two values is less than or equal to ±10% of the average of the values.
[0027] In the packaging process, one of the main problems encountered by the currently used packaging molds is how to avoid the adhesion between the packaging material and the surface of the packaging mold. The adhesion between the packaging material and the surface of the packaging mold will cause part of the packaging material to remain on the surface of the packaging mold, thereby affecting the stability of the packaging process. In severe cases, it will even cause defects in the packaged product. Therefore, the present application provides a packaging mold with an anti-sticking coating, which is used in the packaging process to effectively improve the stability of the packaging process and the product quality.
[0028] Figure 1 is a schematic cross-sectional view of a packaging mold 10 according to some embodiments of the present application.
[0029] According to one aspect of the present application, the present application provides a packaging mold. Figure 1 As shown, the packaging mold 10 includes: a packaging film substrate 101 and a coating 102. The coating 102 is disposed on a portion of the surface of the packaging film substrate 101, wherein the coating includes a metal layer 102A having a columnar crystal structure, and the metal layer 102A is a metal copper layer or a metal chromium layer.
[0030] Figure 2 and 3 They are respectively a cross-sectional view and a top view electron microscope image of a coating of a packaging mold according to an embodiment of the present application.
[0031] like Figure 2 As shown, the metal copper layer or metal chromium layer 102A having a columnar crystal structure can form a stable coating structure that is tightly bonded to the surface of the packaging mold 101. Figure 3 As shown, the coating surface with a columnar crystal structure can form a dense dot structure, and the dot structure of the metal copper layer or the metal chromium layer can effectively reduce the interfacial energy of the coating surface, thereby reducing the adhesion between the packaging material and the coating.
[0032] In some embodiments, the crystal structure of the columnar crystal structure of the metal copper layer or the metal chromium layer is a cubic crystal system, and its crystal structure belongs to a body-centered cubic structure. The columnar crystal structure of the cubic crystal system has a tighter coating structure, and the structure of the coating surface is also smoother. In some embodiments, the grain size of the columnar crystal structure of the metal copper layer or the metal chromium layer is 30nm to 100nm, so as to optimize the arrangement of the coating structure and the coating surface structure and improve the anti-sticking effect of the coating.
[0033] In some embodiments, the coating thickness is 2 μm to 10 μm. Within this thickness range, the prepared metal layer has excellent bonding strength with the packaging mold substrate, and the coating has good structural strength.
[0034] Figure 4 is a schematic cross-sectional view of a packaging mold 20 according to some embodiments of the present application.
[0035] like Figure 4 As shown, in some embodiments, the coating layer 102 can further include an oxide layer 102B disposed on the surface of the metal layer, and the oxide layer 102B is a copper oxide layer or a chromium oxide layer.
[0036] Figure 5 The cross-sectional electron microscope image of a metal copper coating having a columnar crystal structure of a packaging mold according to an embodiment of the present application.
[0037] like Figure 5As shown, since the metal copper layer 102A with a columnar crystal structure has a typical growth preference, it is conducive to the diffusion of oxygen elements in the air in the columnar crystal structure. Therefore, the metal copper layer with a columnar crystal structure can form a metal oxide layer 102B on the surface of the coating, and the metal oxide layer 102B (copper oxide layer) has a lower interface energy, which can further reduce the adhesion between the packaging material and the coating. In some embodiments of the present application, the metal chromium layer with a columnar crystal structure can also form a metal oxide layer on the surface of the coating, and the chromium oxide layer has a lower interface energy, which can further reduce the adhesion between the packaging material and the coating.
[0038] Although the metal oxide layer has a dense structure, the transitional oxidation may cause the columnar crystal structure in the metal layer to be destroyed, thereby affecting the overall structural stability of the coating. In some embodiments, the thickness of the oxide layer is 100 nm to 1 μm to improve the bonding force between the oxide layer and the metal layer, thereby improving the overall structural strength of the coating. In some embodiments, the thickness of the oxide layer is less than or equal to 0.8 μm.
[0039] According to another aspect of the present application, the present application provides a method for preparing a packaging mold, which includes the following steps: providing a packaging film substrate and using a magnetron sputtering process to form a metal layer with a columnar crystal structure on the surface of the packaging film substrate, and the metal layer contains one of copper or chromium.
[0040] In some embodiments, the bias voltage used in the magnetron sputtering process is 30V to 100V, and the target power is 5Kw to 15Kw.
[0041] In some embodiments, the gas pressure of the closed chamber furnace in the magnetron sputtering process is 0.1 Pa to 1 Pa, and the sputtering deposition time is 40 minutes to 120 minutes.
[0042] In some embodiments, after the metal layer is formed, the method further comprises the following steps: placing the packaging mold in an oxygen-containing environment to form an oxide layer on the surface of the metal layer, wherein the oxide layer is one of copper oxide or chromium oxide.
[0043] In some embodiments, the temperature in the oxygen-containing environment is 75° C. to 90° C. to reduce the time for the oxide layer to form and to improve the structural strength of the oxide layer.
[0044] In some embodiments, the oxygen-containing environment may be a pure oxygen environment to further form a more compact oxide layer structure.
[0045] In some embodiments, the thickness of the metal oxide layer can be controlled by adjusting the oxygen content, temperature and oxidation time in the oxidation environment. In some embodiments, after the oxidation step, the metal oxide layer is placed in an atmospheric environment and at room temperature, and the metal oxide layer can form a stable structure with a fixed thickness and density, and can effectively block the contact between the metal layer and the oxidizing components in the atmosphere to avoid the metal in the metal layer from continuing to oxidize, thereby maintaining the double-layer structure of the metal layer and the metal oxide layer in the coating, so that the coating has good structural stability and service life. In some embodiments, after the step of providing a packaging film substrate and before the step of forming a metal layer, it further includes using argon ion cleaning on the surface of the packaging film substrate, and the argon ion cleaning step includes the following steps: introducing argon gas in a closed chamber furnace, applying a bias voltage of 100V to 800V, and cleaning the surface of the packaging film substrate. Argon ion cleaning of the surface of the packaging mold substrate can improve the bonding strength between the metal layer and the surface of the packaging mold substrate.
[0046] The preparation method of the present application adopts a magnetron sputtering process. By controlling the bias range and power in the magnetron sputtering process, a metal copper layer or a metal chromium layer with a specific columnar crystal structure can be formed, and a tight coating structure is formed with the packaging mold substrate. The columnar crystal structure has typical growth preference, which is conducive to the diffusion of oxygen elements in the air, so that a stable metal oxide layer can be self-regulated on the surface of the coating, and the interfacial energy of the coating surface is reduced, which helps to achieve an anti-sticking effect.
[0047] To further illustrate the beneficial effects of the packaging mold of the self-adjusting anti-sticking coating of the present application, the present application provides the following specific embodiments and the results of the bonding force and high temperature contact angle tests:
[0048] Example 1
[0049] The pre-treated uncoated molds were evenly loaded onto the coating machine rotating rack, the rack speed was adjusted to 5 rpm, and the furnace chamber was closed. When the vacuum in the closed furnace chamber reached 3x10 -3 Pa, turn on the heater, heat to 500 ° C, and introduce argon, turn on the ion cleaning power, set the bias voltage to 600 V, and perform argon ion cleaning of the substrate for 40 minutes. Then turn off the cleaning power, turn on the copper target, introduce nitrogen until the pressure of the closed furnace chamber is 0.5 Pa, set the power to 12Kw, the substrate bias voltage to 60V, deposit the copper metal layer, and the deposition time is 80min.
[0050] Subsequently, the prepared mold was cooled and taken out of the oven. The film thickness was measured by a film thickness ball mill, and basically no surface oxide layer was detected. The metal layer was 7μm, and the bonding force between the coating and the substrate was 80N. The contact angle between the mold surface and the resin was measured by a high-temperature contact angle meter and was 60±5°.
[0051] Example 2
[0052] The pre-treated uncoated molds were evenly loaded onto the coating machine rotating rack, the rack speed was adjusted to 5 rpm, and the furnace chamber was closed. When the vacuum in the closed furnace chamber reached 3x10 -3 Pa, turn on the heater, heat to 500 ° C, and introduce argon, turn on the ion cleaning power, set the bias voltage to 600 V, and perform argon ion cleaning of the substrate for 40 minutes. Then turn off the cleaning power, turn on the copper target, introduce nitrogen until the pressure of the closed furnace chamber is 0.5 Pa, set the power to 12Kw, the substrate bias voltage to 60V, deposit the copper metal layer, and the deposition time is 80min.
[0053] Subsequently, the prepared mold was cooled to 80°C in a vacuum furnace, and then high-purity oxygen was introduced for 90 minutes. The prepared mold was cooled out of the furnace, and the film thickness was measured by a film thickness ball mill. The surface oxide layer was 1.5μm, the metal layer was 7μm, and the bonding force between the coating and the substrate was 30N. The contact angle between the mold surface and the resin was measured by a high-temperature contact angle meter and was 75±5°.
[0054] Example 3
[0055] The pre-treated uncoated molds were evenly loaded onto the coating machine rotating rack, the rack speed was adjusted to 5 rpm, and the furnace chamber was closed. When the vacuum in the closed furnace chamber reached 3x10 -3 Pa, turn on the heater, heat to 500 ° C, and introduce argon, turn on the ion cleaning power, set the bias voltage to 600 V, and perform argon ion cleaning of the substrate for 40 minutes. Then turn off the cleaning power, turn on the copper target, introduce nitrogen until the pressure of the closed furnace chamber is 0.5 Pa, set the power to 12Kw, the substrate bias voltage to 60V, deposit the copper metal layer, and the deposition time is 80min.
[0056] Subsequently, the prepared mold was cooled to 80°C in a vacuum furnace, and then high-purity oxygen was introduced for 40 minutes. The prepared mold was cooled out of the furnace, and the film thickness was measured by a film thickness ball mill. The surface oxide layer was 0.8μm, the metal layer was 7μm, and the bonding force between the coating and the substrate was 60N. The contact angle between the mold surface and the resin was measured by a high-temperature contact angle meter and was 85±5°.
[0057] Example 4
[0058] The pre-treated uncoated molds were evenly loaded onto the coating machine rotating rack, the rack speed was adjusted to 5 rpm, and the furnace chamber was closed. When the vacuum in the closed furnace chamber reached 3x10 -3Pa, turn on the heater, heat to 500 ° C, and introduce argon, turn on the ion cleaning power, set the bias voltage to 600 V, and perform argon ion cleaning of the substrate for 40 minutes. Then turn off the cleaning power, turn on the copper target, introduce nitrogen until the pressure of the closed furnace chamber is 0.5 Pa, set the power to 12Kw, the substrate bias voltage to 60V, and deposit the copper metal layer for 120 minutes.
[0059] Subsequently, the prepared mold was cooled to 80°C in a vacuum furnace, and then high-purity oxygen was introduced for 40 minutes. The prepared mold was cooled out of the furnace, and the film thickness was measured by a film thickness ball mill. The surface oxide layer was 0.8μm, the metal layer was 10μm, and the bonding force between the coating and the substrate was 55N. The contact angle between the mold surface and the resin was measured by a high-temperature contact angle meter and was 84±5°.
[0060] Example 5
[0061] The pre-treated uncoated molds were evenly loaded onto the coating machine rotating rack, the rack speed was adjusted to 5 rpm, and the furnace chamber was closed. When the vacuum in the closed furnace chamber reached 3x10 -3 Pa, turn on the heater, heat to 500 ° C, and introduce argon, turn on the ion cleaning power, set the bias voltage to 600 V, and perform argon ion cleaning of the substrate for 40 minutes. Then turn off the cleaning power, turn on the copper target, introduce nitrogen until the pressure of the closed furnace chamber is 0.5 Pa, set the power to 12Kw, the substrate bias voltage to 60V, and deposit the copper metal layer for 160 minutes.
[0062] Subsequently, the prepared mold was cooled to 80°C in a vacuum furnace, and then high-purity oxygen was introduced for 40 minutes. The prepared mold was cooled out of the furnace, and the film thickness was measured by a film thickness ball mill. The surface oxide layer was 0.8μm, the metal layer was 12μm, and the bonding force between the coating and the substrate was 40N. The contact angle between the mold surface and the resin was measured by a high-temperature contact angle meter and was 80±5°.
[0063] Example 6
[0064] The pre-treated uncoated molds were evenly loaded onto the coating machine rotating rack, the rack speed was adjusted to 5 rpm, and the furnace chamber was closed. When the vacuum in the closed furnace chamber reached 3x10 -3 Pa, turn on the heater, heat to 500 ° C, and introduce argon, turn on the ion cleaning power, set the bias voltage to 600 V, and clean the substrate with argon ions for 40 minutes. Then turn off the cleaning power, turn on the copper target, introduce nitrogen until the pressure of the closed furnace chamber is 0.5 Pa, set the power to 12Kw, the substrate bias voltage to 60V, and deposit the copper metal layer for 30 minutes.
[0065] Subsequently, the prepared mold was cooled to 80°C in a vacuum furnace, and then high-purity oxygen was introduced for 40 minutes. The prepared mold was cooled out of the furnace, and the film thickness was measured by a film thickness ball mill. The surface oxide layer was 0.8μm, the metal layer was 2μm, and the bonding force between the coating and the substrate was 50N. The contact angle between the mold surface and the resin was measured by a high-temperature contact angle meter and was 76±5°.
[0066] Bonding strength test:
[0067] The scratch tester (model: WS-2005, Lanzhou Zhongke Kaihua Technology Development Co., Ltd.) was used for the bonding test. The specific test parameters were as follows: load 100N, scratch rate 2mm / min, loading rate 100N / min, and scratch length 2mm. The sample was placed in the scratch tester, the sample was locked and fixed, and the pointer position and applied force were adjusted. Then the load pressure was gradually increased until the coating was scraped off and the scratch on the substrate was exposed. The applied force of the pointer when the scratch occurred was recorded to obtain the bonding force of the sample coating on the substrate.
[0068] High temperature contact angle test:
[0069] A high temperature contact angle measuring instrument was used to horizontally place the coating to be tested in the instrument, and a resin (model: CYD-128 epoxy resin) was used to test its static contact angle at a temperature of 60°C.
[0070] Table 1
[0071]
[0072] It can be seen from the above test results that the packaging mold with an anti-sticking coating of the present application can effectively reduce the interfacial energy of its surface. For the contact angle test of the packaging resin, it can reach a contact angle of more than 60±5°. The surface contact angle of the packaging mold with an oxide layer coating can even be increased to 85±5°, and the anti-sticking coating of the present application has a certain bonding force with the packaging mold. In addition, by controlling the thickness of the surface oxide layer, the packaging mold of the present application can effectively reduce the adhesion of the packaging material to its surface. The packaging mold with a self-adjusting anti-sticking coating provided by the present application is used in the packaging process to effectively improve the stability of the packaging process and product quality.
[0073] References throughout the specification to "some embodiments", "partial embodiments", "one embodiment", "another example", "example", "specific example" or "partial example" mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example", do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics herein may be combined in one or more embodiments or examples in any suitable manner.
[0074] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.
Claims
1. A packaging mold, comprising: The encapsulation film has a substrate; A coating layer, the coating layer being disposed on a portion of the surface of the packaging film substrate, wherein the coating layer comprises a metal layer having a columnar crystal structure, and the metal layer comprises one of copper or chromium, wherein a surface of the metal layer having the columnar crystal structure has a dense point structure, and a grain size of the columnar crystal structure of the metal layer is 30 nm to 100 nm; and An oxide layer is disposed on the surface of the metal layer, and the oxide layer is one of copper oxide or chromium oxide. 2 . The packaging mold according to claim 1 , wherein a thickness of the oxide layer is 100 nm to 1 μm. 3 . The encapsulation mold according to claim 1 , wherein the coating layer has a thickness of 2 μm to 10 μm. 4 . The packaging mold according to claim 1 , wherein the crystal structure of the columnar crystal structure of the metal layer is a cubic crystal system, and the crystal structure belongs to a body-centered cubic structure.
5. A method for preparing a packaging mold, comprising the following steps: Providing a packaging film substrate; A metal layer having a columnar crystal structure is formed on the surface of the packaging film substrate by a magnetron sputtering process, and the metal layer comprises one of copper or chromium, wherein the surface of the metal layer having the columnar crystal structure has a dense point structure, and the grain size of the columnar crystal structure of the metal layer is 30nm to 100nm; and The packaging mold is placed in an oxygen-containing environment to form an oxide layer on the surface of the metal layer, wherein the oxide layer is one of copper oxide or chromium oxide. 6 . The method for preparing a packaging mold according to claim 5 , wherein the bias voltage used in the magnetron sputtering process is 30 V to 100 V, and the target power is 5 Kw to 15 Kw. 7 . The method for preparing a packaging mold according to claim 5 , wherein the gas pressure of the closed chamber furnace in the magnetron sputtering process is 0.1 Pa to 1 Pa, and the sputtering deposition time is 40 minutes to 120 minutes. 8 . The method for preparing a packaging mold according to claim 5 , wherein the temperature in the oxygen-containing environment is 75° C. to 90° C.
9. The method for preparing a packaging mold according to any one of claims 5 to 8, wherein after the step of providing the packaging film substrate and before the step of forming the metal layer, the method further comprises cleaning the surface of the packaging film substrate with argon ions, wherein the argon ion cleaning step comprises the following steps: Argon gas is introduced into a closed chamber furnace, and a bias voltage of 100V to 800V is applied to clean the surface of the packaging film substrate.