An acid-catalyzed agent for stabilizing heavy metals in fly ash over a long period of time and a method of using the agent
Through three water washing and acid catalyst treatment, combined with mineral chemicals and extrusion granulation process, the pollution problem of heavy metals and chlorides in fly ash from domestic waste incineration has been solved, long-term stabilization and resource utilization of fly ash has been achieved, and the cost of filling has been reduced. Burial costs and sewage treatment problems.
Patent Information
- Application Number
- CN202110654320.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-11
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-06-11
AI Technical Summary
Heavy metals and chlorides enriched in fly ash from domestic waste incineration lead to secondary pollution. It is difficult to achieve complete harmlessness and resource utilization of fly ash with existing technology, and the high moisture content of filter cake after water washing has an impact on the stability of the kiln system. big.
Three water washing processes are used to remove soluble salts in fly ash, wastewater is treated through microfiltration and reverse osmosis, and acidic catalysts and mineral agents are combined to form long-term stable fly ash particles, reducing the risk of heavy metal leaching, and reducing the risk of heavy metal leaching through the extrusion granulation process. Moisture content.
It achieves long-term stabilization of heavy metals in fly ash, reduces the leaching concentration of heavy metals, reduces landfill costs, and solves the odor problems caused by desalination of sewage and decomposition of chelating agents after water washing, ensuring the long-term stability and stability of fly ash. Resource utilization.
Smart Images

Figure HDA0003113198530000011 
Figure HDA0003113198530000012
Abstract
Description
Technical Field
[0001] The invention belongs to the field of solid hazardous waste disposal and resource utilization, and specifically relates to an acid-catalyzed agent for stabilizing heavy metals in fly ash over a long period and a use method thereof, so as to achieve complete harmlessness of fly ash from the incineration of domestic waste. Background Art
[0002] Solid waste incineration has gradually become the main method for harmless treatment of solid waste in China due to its advantages of reduction, harmlessness and resource utilization. As of 2018, the daily treatment capacity of solid waste incineration is 6.247×10 5 t, and the annual incineration capacity is 2.28 × 10 8 t, after the incineration of garbage, the incineration fly ash will be equivalent to 2-5% of the original garbage mass, and the annual processing capacity of fly ash is 4.36~10.9× 10 6 t. However, secondary pollution will be generated during the incineration process, among which fly ash is rich in heavy metals and dioxins. In the "Technical Policy for the Prevention and Control of Hazardous Waste Pollution" promulgated in my country in 2001, fly ash from the incineration of domestic waste has been defined as hazardous waste (HW18). Fly ash from the incineration of domestic waste must be solidified and stabilized at the production site before it can be transported for safe landfill disposal. This means that the incineration fly ash must be disposed of in a standardized manner and meet the national standard "Pollution Control Standards for Domestic Waste Landfills" (GB16889-2008) before it can be disposed in domestic waste landfills.
[0003] Domestic waste contains abundant chlorine-containing organic matter (rubber, polyvinyl chloride, etc.) and inorganic matter (NaCl, KCl), which are mainly discharged in the form of hydrogen chloride during the treatment process, up to several hundred or even several thousand mg / L. The valence of chloride cations affects the corrosion rate of steel in concrete, and chlorine affects the migration and distribution of heavy metals and forms dioxins as one of the elements. It is well known that chlorides will corrode steel. Reducing the amount of chloride in fly ash can make fly ash a resource and then use it as a raw material in the construction industry.
[0004] The patent with publication number 101182144A adopts the method of water washing and cement kiln calcination to synergistically dispose of fly ash. However, the sewage generated during the water washing pretreatment process of this method is not desalted, and the salt content is high, which makes it difficult to meet the requirements of recycled water. Moreover, when the filter cake with high water content enters the kiln, the amount of admixture is small, which has an adverse effect on the raw material batching process and the stability of the kiln system. In the patent with publication number CN101817650A, a vacuum filter press device is used to vacuum filter the filter cake with high water content after water washing, and then enter the cement kiln for calcination. However, during the calcination process, a small amount of heavy metals will still be enriched in the fly ash, forming highly toxic fly ash. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an acid-catalyzed agent and a method for stabilizing heavy metals in fly ash for a long period of time. Specifically, it involves using a solid-liquid combined agent to stabilize various heavy metals in fly ash slurry after reducing the salt content, and at the same time, the fly ash particles obtained by extrusion granulation can be stored stably for a long time.
[0006] The present invention provides a method and system for recycling waste incineration fly ash, which is characterized by comprising the following steps:
[0007] Step (1) is to use a conventional water washing process to remove soluble salt components such as chlorine, sodium and potassium in the fly ash, and then treat the wastewater generated after the water washing and reuse it;
[0008] The conventional water washing process described in step (1) is mainly carried out in three steps. The first step of water washing mainly involves water-cement ratio, stirring time and stirring rate. The water-cement ratio ranges from 2 to 100, the stirring time is 1 min to 2 h and the stirring rate is 10-500 r / min. Preferably, the water-cement ratio is 3 to 6, the stirring reaction time is 3-20 min and the stirring rate is 50 to 200 r / min. The suspension after the first step of water washing is allowed to stand and then subjected to coarse filtration treatment using a microfiltration membrane to obtain a salt-containing filtrate (1) and a fly ash slurry (1).
[0009] The second step of washing the fly ash slurry (1) mainly involves water-cement ratio, stirring time, and stirring rate, preferably a water-cement ratio of 2 to 5, a stirring reaction time of 1 to 15 minutes, and a stirring rate of 30 to 160 r / min. The suspension after the second step of washing is subjected to coarse filtration to obtain a salt-containing filtrate (2) and a fly ash slurry (2).
[0010] The third step of washing the fly ash slurry (2) mainly involves water-cement ratio, stirring time, and stirring rate, preferably a water-cement ratio of 2 to 4, a stirring reaction time of 1 to 10 minutes, and a stirring rate of 30 to 100 r / min. The third step of washing the suspension is subjected to a coarse filtration treatment to obtain a salt-containing filtrate (3) and a fly ash slurry (3).
[0011] The salt-containing filtrates (1), (2) and (3) are concentrated by a reverse osmosis membrane system.
[0012] Step (2) is to add the solid-liquid combination agent to the fly ash slurry (3) through an extrusion granulation device and mix them evenly, thereby reducing the water content of the system and granulating the fly ash slurry to reduce storage space;
[0013] The solid agent used in step (2) includes at least one mineral material such as fly ash, silica alumina powder, attapulgite, zircon powder, activated clay, wollastonite, bentonite, brucite, diatomaceous earth, talc, quartz sand, shell powder, titanium dioxide, volcanic ash, brucite, barite, zeolite, mullite powder, hydrotalcite, kaolin, ferrous sulfate, calcium sulfate, ferric sulfate, ferric chloride and palygorskite, and the added amount is 1-50% of the dry ash amount.
[0014] The solid agent used in step (2) is preferably palygorskite;
[0015] The liquid agent used in step (2) is a catalyst, which mainly includes at least one of citric acid, malic acid, tartaric acid, acetic acid, succinic acid and oxalic acid, and is prepared into a 30wt% solution;
[0016] The amount of the liquid agent used in step (2) is 1-20 wt% of the dry ash.
[0017] The microstructure of the fly ash treated in step (2) is a three-dimensional gelatinous structure, and the gelatinous structure can ensure the long-term stability of the treated fly ash;
[0018] The long-term stabilization period involved in step (2) is at least 1 year.
[0019] The storage environment involved in step (2) for stability for more than one year is outdoor storage, with a temperature of -10 to 35°C and a humidity of 35 to 95% with no quality inspection fluctuations.
[0020] The present invention is based on the following principles :Soluble salts and heavy metals in fly ash are two major problems. The present invention optimizes the water washing process by three water washings to wash away a large amount of soluble components such as Na+, K+ and Cl- in fly ash, and then treats the wastewater by microfiltration and reverse osmosis after standing, and concentrates the salt for treatment. Regarding the heavy metals in fly ash, under the condition of high-efficiency acidic catalyst, the Si / Al structure in the mineral is depolymerized, and then in the process of re-gelation, based on the principle of charge balance, the heavy metal ions are fixed in it, and the adsorption of the mineral plays a synergistic role at the same time, thereby achieving the purpose of long-term stability.
[0021] The present invention has the following advantages and effects compared with the prior art :
[0022] (1) A large amount of soluble salts in fly ash can be removed by water washing, which provides the possibility for the long-term stability of fly ash in subsequent treatment.
[0023] (2) Develop a solid-liquid combined long-term stable chelating agent to treat fly ash, so as to ensure that the treated fly ash can be stored in the natural environment for a long time of more than one year without excessive leaching concentration of heavy metals;
[0024] (3) Develop an agent that can replace organic sulfur chelating agents, fundamentally solving the odor problem caused by the decomposition of chelating agents. This agent is completely colorless and odorless;
[0025] (4) The extrusion granulation process is used to reduce the bulk density of the fly ash after treatment, thus reducing the landfill treatment cost per ton. DETAILED DESCRIPTION
[0026] The following is a detailed description of an acid-catalyzed agent and method for stabilizing heavy metals in fly ash for a long period of time provided by the present invention in conjunction with specific embodiments, so as to achieve complete harmlessness and resource utilization of fly ash from the incineration of domestic waste.
[0027] The fly ash produced by the incineration of solid waste used is the fly ash produced by a domestic waste incineration power plant in Shenzhen, Guangdong.
[0028] Salt content test
[0029] Take the filtrate of M1g into a disposable plastic cup (M0), then put it in a 105℃ oven, dry it and weigh M2. Test its salt content: w% = (M2-M0) / M1*V x / m1*100%.
[0030] Leaching of fly ash chelates
[0031] Extraction method 1#: Use a pipette to transfer 17.25ml of glacial acetic acid and ultrapure water into a volumetric flask, dilute to 1L, and measure the pH value at about 2.6. According to the solid content, add the extract at a liquid-solid ratio of 20:1, put it into the tumbler and tumble it for 18 hours for extraction. During the first 4 hours, it needs to be deflated twice. Generally, 75g of solid is taken. Remove the sample from the tumbler, and use a full glass and 6μm microporous membrane filter sand core filter device to filter out 150ml of the extract in a plastic bottle under reduced pressure, and detect the concentration of various heavy metal ions. (HJ 300)
[0032] Heavy Metal Detection
[0033] The chelated fly ash was tested using the HJ 300-2007 leaching method. The heavy metal leaching concentration of the treated domestic waste incineration fly ash reached the national "Pollution Control Standard for Domestic Waste Landfills" GB 16889-2008. Enterprises must also refer to local emission standards for specific details.
[0034] Water washing example
[0035] The fly ash washing process is as follows:
[0036] (1) Water washing: First step: weigh m1 g of fly ash into a clean plastic measuring cup, add V1 mL of water, stir at a rate of r1 r / min, stir for t1 min, and test the salt content of the filtrate at the same time.
[0037] (2) After the first step of coarse filtration of the microfiltration membrane with water washing, V2 mL of water was added to the residue, the stirring rate was r2 r / min, the stirring time was t2 min, and the salt content of the filtrate was tested at the same time.
[0038] (3) After the second step of coarse filtration of the water-washed microfiltration membrane, add V3 mL of water, stir at a rate of r3 r / min, and stir for t3 min. At the same time, test the salt content of the filtrate.
[0039] The experimental data and results of the specific embodiments 1-9 of the washing are as follows Figure 1 As shown, according to the experimental results, it can be seen that the water-to-cement ratio of the first step water washing is 5, the stirring time is 5min and the stirring speed is 150r / min, the water-to-cement ratio of the second step water washing is 4, the stirring reaction time is 5min and the stirring speed is 150r / min, and the water-to-cement ratio of the second step water washing is 3, the stirring reaction time is 5min and the stirring speed is 150r / min.
[0040] Stabilization Example
[0041] Comparative experiment 1
[0042] After the fly ash slurry is granulated and dehydrated, the granulated fly ash 1# is weighed into a clean plastic measuring cup to test the moisture content. Without adding any chelating agent, the leaching experiment is directly carried out using the leaching agent 1#.
[0043] Example 10
[0044] Through the dosing device, palygorskite is added to the fly ash slurry after three water washings, and the addition ratio is 100g of dry ash, 5g of palygorskite and 3g of 30wt% citric acid solution, and then enters the extrusion granulation filter device to stabilize the heavy metals in the fly ash slurry and reduce the water content of the fly ash slurry. The granulated fly ash is placed for 1 day for leaching experiment and the heavy metal leaching concentration is detected.
[0045] Embodiment 11
[0046] Through the dosing device, palygorskite is added to the fly ash slurry after three water washings, and the addition ratio is 100g of dry ash, 5g of fly ash and 3g of 30wt% citric acid solution, and then enters the extrusion granulation filter device to stabilize the heavy metals in the fly ash slurry and reduce the water content of the fly ash slurry. The granulated fly ash is placed for 1 day for leaching experiment and the heavy metal leaching concentration is detected.
[0047] Example 12
[0048] Through the dosing device, palygorskite is added to the fly ash slurry after three water washings, and the addition ratio is 100g of dry ash, 5g of attapulgite and 3g of 30wt% citric acid solution, and then enters the extrusion granulation filter device to stabilize the heavy metals in the fly ash slurry and reduce the water content of the fly ash slurry. The granulated fly ash is placed for 1 day for leaching experiment and the heavy metal leaching concentration is detected.
[0049] Embodiment 13
[0050] Through the dosing device, palygorskite is added to the fly ash slurry after three water washings, and the addition ratio is 100g of dry ash, 8g of palygorskite and 3g of 30wt% citric acid solution, and then enters the extrusion granulation filter device to stabilize the heavy metals in the fly ash slurry and reduce the water content of the fly ash slurry. The granulated fly ash is placed for 1 day for leaching experiment and the heavy metal leaching concentration is detected.
[0051] Embodiment 14
[0052] Through the dosing device, palygorskite is added to the fly ash slurry after three water washings, and the addition ratio is 100g of dry ash, 8g of palygorskite and 5g of 30wt% acetic acid solution, and then enters the extrusion granulation filter device to stabilize the heavy metals in the fly ash slurry and reduce the water content of the fly ash slurry. The granulated fly ash is placed for 1 day for leaching experiment and the heavy metal leaching concentration is detected.
[0053] Embodiment 15
[0054] Through the dosing device, palygorskite is added to the fly ash slurry after three water washings, and the addition ratio is 100g of dry ash, 8g of palygorskite and 3g of 30wt% citric acid solution, and then enters the extrusion granulation filter device to stabilize the heavy metals in the fly ash slurry and reduce the water content of the fly ash slurry. After the granulated fly ash is placed for 6 months, the leaching experiment is carried out to detect the heavy metal leaching concentration.
[0055] Example 16
[0056] Through the dosing device, palygorskite is added to the fly ash slurry after three water washings, and the addition ratio is 100g of dry ash, 8g of palygorskite and 3g of 30wt% citric acid solution, and then enters the extrusion granulation device to stabilize the heavy metals in the fly ash slurry and reduce the water content of the fly ash slurry. After the granulated fly ash is placed for 12 months, the leaching experiment is carried out to detect the heavy metal leaching concentration. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1It is a summary diagram of the experimental data and results of water washing examples 1-9#.
[0058] Figure 2 This is a summary chart of the results of comparison experiment 1# and curing experiments 10-16#.
[0059] according to Figure 1 According to the experimental results in , the soluble salt content in the fly ash can be washed out to the maximum extent by optimizing the water-cement ratio, stirring rate, and stirring time of the three water washings. Comparing the different experimental conditions and experimental results of Example 1-9#, the stirring rate is controlled at 150r / min, the stirring time is 5min, the first water-cement ratio is 5, the second water-cement ratio is 4, and the third water-cement ratio is 3. 16.8% of the soluble salt content can be washed out from the original ash. Reasonable adjustment of the water-cement ratio of the three water washings can not only ensure the washing out of the soluble salt, but also reasonably control the amount of water used.
[0060] according to Figure 2 From the experimental results in the experiment, it can be seen that the leaching concentrations of Zn\Pb\Cu\Cd in the raw ash seriously exceeded the standard by comparing with experiment 1#. Different palygorskite, fly ash and attapulgite were used for stabilization research in experiments 10#, 11# and 12# respectively. From the leaching concentration data of Zn\Pb\Cu\Cd, palygorskite has the best effect. From the data of 10# and 13#, by increasing the dosage of palygorskite, the leaching concentration of Pb\Cu\Cd can be reduced by an order of magnitude, and the effect is significant. From the data of 13# and 14#, the catalytic effect of lemon acid is better than that of acetic acid. From the data of 13#, 15# and 16#, after three water washings, under the catalytic conditions of citric acid, the heavy metals in palygorskite-solidified fly ash can achieve a stable effect for at least one year.
[0061] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the formula and preparation process of the present invention may be subject to various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for acid-catalyzed long-term stabilization of heavy metals in fly ash, characterized in that: The following steps are involved: The soluble salt components such as chlorine, sodium and potassium in the fly ash are removed by water washing. The water washing process is mainly divided into three steps: in the first step of water washing, the water-to-cement ratio ranges from 2 to 100, the stirring time is 1 min to 2 h, and the stirring rate is 10-500 r / min. After the first step of water washing, the suspension is allowed to stand and then subjected to coarse filtration with a microfiltration membrane to obtain a salt-containing filtrate and a fly ash slurry. In the second step of water washing, the water-to-cement ratio ranges from 2 to 5, and the stirring time is 1-15 min. , the stirring rate is 30-160r / min, the suspension after the second step of water washing is subjected to coarse filtration treatment to obtain salt-containing filtrate 2 and fly ash slurry 2, the water-cement ratio of the third step of water washing fly ash slurry 2 is 2-4, the stirring time is 1-10min, the stirring rate is 30-100r / min, the suspension after the third step of water washing is subjected to coarse filtration treatment to obtain salt-containing filtrate 3 and fly ash slurry 3, and the salt-containing filtrate 1, the salt-containing filtrate 2 and the salt-containing filtrate 3 are concentrated by a reverse osmosis membrane system; The solid-liquid combination agent is added to the fly ash slurry 3 through an extrusion granulation device and mixed evenly, thereby reducing the water content of the system, and at the same time, the fly ash slurry is granulated to reduce the storage space; the solid agent includes fly ash, silica aluminum powder, attapulgite, zircon powder, activated clay, wollastonite, bentonite, brucite, diatomaceous earth, talc, quartz sand, shell powder, titanium dioxide, volcanic ash, brucite, barite, zeolite, mullite powder, hydrotalcite, kaolin, ferrous sulfate, calcium sulfate, ferric sulfate, ferric chloride and palygorskite, and the addition amount is 1-50% of the dry ash amount; the liquid agent is a catalyst, mainly including at least one agent of citric acid, malic acid, tartaric acid, acetic acid, succinic acid and oxalic acid, which is prepared into a 30wt% solution; the addition amount of the liquid agent is 1-20wt% of the dry ash amount.
2. The method for acid-catalyzed long-term stabilization of heavy metals in fly ash according to claim 1, characterized in that: The fly ash involved is the fly ash generated by the incineration of domestic waste.
3. The method for acid-catalyzed long-term stabilization of heavy metals in fly ash according to claim 1, characterized in that: The long-term stable placement time is at least 1 year.