A graphene composite copper sulfide / nickel sulfide catalytic material and its preparation method and application
Through the preparation of graphene composite copper sulfide/nickel sulfide catalytic materials, the problem of slow catalytic kinetics of precious metal catalysts in ORR and AOR is solved, and high-efficiency and low-cost catalytic performance is achieved, which is suitable for zinc-air batteries and ethanol electrolysis. Pool application.
Patent Information
- Application Number
- CN202110877877.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-07-29
AI Technical Summary
Existing precious metal catalysts have slow catalytic kinetics in oxygen reduction reaction (ORR) and alcohol oxidation reaction (AOR), and their industrial application is limited due to the high cost, easy poisoning and poor cycle stability of precious metals.
Using graphene composite copper sulfide/nickel sulfide catalytic material, through controlled hydrothermal method and sulfidation calcination under argon atmosphere, the synergistic effect of strong interfacial coupling and sulfur vacancies was adjusted to prepare a bifunctional catalyst with excellent catalytic performance.
It achieves efficient catalytic performance for oxygen reduction and alcohol oxidation reactions, demonstrates fast charge and discharge performance and high cycle stability, and reduces the energy barrier of the catalytic reaction, making it suitable for market promotion.
Smart Images

Figure CN113659151B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanomaterials and electrochemical catalytic oxygen reduction and alcohol oxidation, and in particular to a graphene composite copper sulfide / nickel sulfide catalytic material and a preparation method and application thereof. Background Art
[0002] Against the backdrop of the continuous consumption of fossil fuels and increasingly prominent environmental issues, renewable, green, and efficient energy storage and conversion technologies such as direct alkaline fuel cells, proton exchange membrane fuel cells, and hydrogen electrolysis have attracted widespread attention. Promising technologies such as metal-air batteries and water electrolysis hydrogen production devices involve oxygen reduction reaction (ORR) and alcohol oxidation reaction (AOR). Especially in the ORR process at the cathode, the high O=O bond energy (498 kJ / mol) and the complex multi-step four-electron reaction pathway make its catalytic kinetics sluggish, which greatly limits the overall efficiency of the fuel cell and the energy / power output.
[0003] At present, platinum group metal-based materials with high catalytic activity, such as platinum, palladium and their alloys, are generally considered to be the most advanced ORR catalysts. At the same time, platinum and palladium-based precious metals are also widely used to catalyze the AOR process due to their strong dehydrogenation and CC bond cleavage capabilities. However, precious metal elements have the characteristics of low abundance, high price, easy poisoning, and poor cycle stability, which greatly hinder their industrial application.
[0004] Therefore, the development of efficient, low-cost, and durable non-noble metal-based bifunctional ORR / AOR catalysts is urgently needed. Summary of the invention
[0005] In view of this, the present invention aims to propose a graphene composite copper sulfide / nickel sulfide catalytic material and its preparation method and application, so as to replace precious metal catalysts with the characteristics of high price, easy poisoning and poor cycle stability.
[0006] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0007] A method for preparing a graphene composite copper sulfide / nickel sulfide catalytic material comprises the following steps:
[0008] S1. preparing graphene oxide dispersion;
[0009] S2, dissolving copper nitrate, nickel nitrate and urea in deionized water, stirring evenly, adding the graphene dispersion, and mixing evenly to form a mixed solution;
[0010] S3, placing the mixed solution in a polytetrafluoroethylene reactor for hydrothermal reaction, cooling to room temperature, washing with deionized water and ethanol by centrifugation, and drying to obtain a precursor powder;
[0011] S4. Place the precursor powder and sulfur powder in a porcelain boat, and calcine under an argon atmosphere to obtain a graphene composite copper sulfide / nickel sulfide catalytic material.
[0012] Optionally, in step S2, the molar ratio of the copper nitrate to the nickel nitrate is in the range of 1:6 to 6:1, and the ratio of the total molar number of the copper nitrate and the nickel nitrate to the molar number of the urea is in the range of 3:10.
[0013] Optionally, the reaction temperature of the hydrothermal reaction in step S3 is in the range of 120° C. to 180° C., and the reaction time is in the range of 3 h to 24 h.
[0014] Optionally, in step S4, the mass ratio of the precursor powder to the sulfur powder is in the range of 1:1 to 1:15.
[0015] Optionally, the calcination temperature in step S4 is in the range of 300° C. to 500° C., the calcination time is in the range of 2 h to 3 h, and the heating rate of the sintering furnace is in the range of 2° C. / min to 10° C. / min.
[0016] Another object of the present invention is to provide a graphene composite copper sulfide / nickel sulfide catalytic material, which is prepared by the above-mentioned preparation method of the graphene composite copper sulfide / nickel sulfide catalytic material.
[0017] Optionally, the morphology of the graphene composite copper sulfide / nickel sulfide catalytic material is bimetallic copper-nickel sulfide nanoparticles loaded on graphene sheets, and the particle size of the nanoparticles is in the range of 22 nm to 24 nm.
[0018] The third object of the present invention is to provide an application of the graphene composite copper sulfide / nickel sulfide catalytic material as described above in the fields of zinc-air batteries, ethanol electrolysis cells and water splitting catalysis.
[0019] The fourth object of the present invention is to provide a self-driving energy system, using the above-mentioned graphene composite copper sulfide / nickel sulfide catalytic material, and the specific assembly method includes:
[0020] 1) After the graphene composite copper sulfide / nickel sulfide catalyst material and conductive carbon black are uniformly mixed, isopropanol, deionized water and a binder are added, and ultrasonic dispersion is performed to obtain a cathode catalyst ink, and the cathode catalyst ink is drop-coated on a conductive carbon cloth and dried to obtain a catalytic electrode;
[0021] 2) Assembling a zinc-air battery using a zinc sheet as an anode and a mixed solution of potassium hydroxide and zinc acetate as an electrolyte;
[0022] 3) Using the catalytic electrode as an electrolysis anode to construct an ethanol electrolysis cell, and using the zinc-air battery to drive the ethanol electrolysis cell to achieve simultaneous preparation of hydrogen and acetate.
[0023] Optionally, in step 2), the molar ratio of the potassium hydroxide to the zinc acetate in the electrolyte is in the range of 2:0.1 to 4:0.1.
[0024] Compared with the prior art, the graphene composite copper sulfide / nickel sulfide catalytic material provided by the present invention and its preparation method and application have the following advantages:
[0025] (1) The present invention adopts a controllable hydrothermal method and subsequent sulfurization calcination in an argon atmosphere, and obtains a graphene composite copper sulfide / nickel sulfide catalytic material by changing the amount of sulfur powder, the molar ratio of the two metals, the calcination temperature, the gas flow rate, the heating rate, etc. The synergistic effect between the strong interface coupling and the sulfur vacancies can effectively regulate the electronic structure, promote the adsorption behavior of oxygen intermediates, and further reduce the energy barrier of the catalytic reaction, showing excellent and efficient dual-functional catalytic performance of oxygen reduction and alcohol oxidation.
[0026] (2) The graphene composite copper sulfide / nickel sulfide catalytic material prepared by the present invention is applied to zinc-air batteries, and exhibits excellent fast charge and discharge performance, high specific capacity and cycle stability in terms of electrochemical performance.
[0027] (3) The reaction conditions of the present invention are mild and the equipment requirements are low, which is conducive to market promotion. In addition, the assembled zinc-air battery is used to drive the alcohol molecular electrolysis cell to construct a self-driven energy conversion system, which can simultaneously achieve the efficient preparation of hydrogen and acetate. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 is the XRD pattern of the graphene composite copper sulfide / nickel sulfide catalytic material described in Example 1 of the present invention;
[0030] Figure 2 is a SEM image of the graphene composite copper sulfide / nickel sulfide catalytic material described in Example 1 of the present invention;
[0031] Figure 3 is a TEM image of the graphene composite copper sulfide / nickel sulfide catalytic material described in Example 1 of the present invention;
[0032] Figure 4 Schematic diagram of the synthesis of the graphene composite copper sulfide / nickel sulfide catalytic material according to an embodiment of the present invention;
[0033] Figure 5 This is a graph characterizing the ORR performance of the graphene composite copper nickel sulfide / nickel sulfide catalytic material described in Example 1 of the present invention under 1 mol / L KOH;
[0034] Figure 6 It is a graph characterizing the electrical performance of a zinc-air battery assembled with the graphene composite copper nickel sulfide / nickel sulfide catalytic material described in Example 1 of the present invention;
[0035] Figure 7 It is a characterization spectrum of the AOR performance of the graphene composite copper nickel sulfide / nickel sulfide catalytic material in Example 1 of the present invention in a 1 mol / L KOH+1 mol / L ethanol mixed electrolyte;
[0036] Figure 8 This is a characterization spectrum of the graphene composite copper nickel sulfide / nickel sulfide catalytic material described in Example 1 of the present invention applied to the electro-oxidation reaction of organic alcohols. DETAILED DESCRIPTION
[0037] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0038] In the description of the present invention, it should be noted that the terms "first" and "second" mentioned in the embodiments of the present invention are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. The "within the range of..." described in this embodiment includes both end values, such as "within the range of 1 to 100", including the values of 1 and 100.
[0039] In the description of the embodiments of the present application, the term "some specific embodiments" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same implementation or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0040] Combination Figure 4 As shown, an embodiment of the present invention provides a method for preparing a graphene composite copper sulfide / nickel sulfide catalytic material, comprising the following steps:
[0041] S1. preparing graphene oxide dispersion;
[0042] S2, dissolving copper nitrate, nickel nitrate and urea in deionized water, stirring evenly, adding graphene dispersion, and mixing evenly to form a mixed solution;
[0043] S3, placing the mixed solution in a polytetrafluoroethylene reactor for hydrothermal reaction, cooling to room temperature, washing with deionized water and ethanol by centrifugation, and drying to obtain a precursor powder;
[0044] S4. Place the precursor powder and sulfur powder in two porcelain boats respectively, and calcine them under an argon atmosphere to obtain a graphene composite copper sulfide / nickel sulfide catalytic material.
[0045] Specifically, in step S1, the graphene oxide dispersion can be prepared by conventional methods. In the present invention, the modified Hummer's method is used to prepare graphite oxide powder, and then the above-mentioned graphite oxide powder is weighed and dispersed in water to prepare a graphite oxide solution with a concentration of 8 mg / mL, and a uniformly dispersed graphene oxide dispersion is prepared by an ultrasonic exfoliation method.
[0046] It is understandable that graphene not only has better electrical and thermal conductivity, but the numerous oxygen-containing groups and defects on its surface not only bring many chemically active sites, but also provide anchoring sites for metal ions; in addition, graphene can play the role of structural support and conductive channel in the catalyst system, greatly improving the directional separation and transmission efficiency of charges in the catalytic system.
[0047] Transition metal-based materials, such as metal sulfides, generally exhibit superior intrinsic conductivity and intrinsic activity compared to metal oxides due to the difference in electronegativity and atomic radius between oxygen and sulfur atoms, as well as sulfur vacancies as an anion defect that effectively regulates catalytic activity. Thanks to the synergistic catalytic effect of the bimetallic active centers, bimetallic sulfides often show better catalytic performance than single metal sulfides.
[0048] Therefore, the inventors innovatively constructed a bimetallic copper-nickel sulfide heterojunction anchored on graphene with rich interfaces and sulfur vacancies as an efficient bifunctional catalyst for ORR / AOR. A controllable hydrothermal method and subsequent sulfurization calcination in an argon atmosphere were used to obtain a graphene composite copper sulfide / nickel sulfide catalytic material by changing the amount of sulfur powder, the molar ratio of the bimetallic, the calcination temperature, the gas flow rate, the heating rate, etc. The synergistic effect between its strong interface coupling and sulfur vacancies can effectively regulate the electronic structure, promote the adsorption behavior of oxygen intermediates, and further reduce the energy barrier of the catalytic reaction, showing excellent and efficient oxygen reduction and alcohol oxidation ORR / AOR bifunctional catalytic performance.
[0049] Specifically, in step S2, the molar ratio of copper nitrate Cu(NO3)2·3H2O, nickel nitrate Ni(NO3)2·6H2O and urea is in the range of 0.2:0.2:1 to 0.3:0.3:1. Further, the amount of Cu(NO3)2·3H2O substance is 0.60-2.40mmol, the amount of Ni(NO3)2·6H2O substance is 0.60-2.40mmol, the amount of urea substance is 3-8mmol, and the volume of deionized water is 15-39mL.
[0050] In step S3, the reaction temperature of the hydrothermal reaction of the mixed solution in the polytetrafluoroethylene reactor is in the range of 120°C to 180°C, and the reaction time is in the range of 3h to 24h. After the reaction is terminated and the reaction temperature is naturally cooled to room temperature, the obtained product is centrifuged on a centrifuge with a rotation speed of 4000r / min for 5min, and the product is washed with deionized water and ethanol for multiple times, and the product after centrifugal washing and separation is dried at 60°C for 24h to finally obtain a phase precursor powder.
[0051] In step S4, the precursor powder and sulfur powder are placed in a quartz boat, and then the quartz boat is placed in a tube furnace, and argon gas is introduced into the tube furnace, and then the tube furnace is heated to 300°C-550°C at a heating rate of 2°C / min-10°C / min, and then calcined in an argon atmosphere at a temperature of 300°C-550°C for 2h-10h, and then naturally cooled to room temperature to obtain a graphene composite copper sulfide / nickel sulfide catalytic material.
[0052] Wherein, the mass ratio of the precursor powder to the sulfur powder is in the range of 1:1 to 1:15.
[0053] The preparation method provided by the embodiment of the present invention has simple process operation, mild reaction conditions, low equipment requirements, low raw material prices, and is suitable for large-scale industrial production.
[0054] Another embodiment of the present invention provides a graphene composite copper sulfide / nickel sulfide catalytic material, which is prepared by the above-mentioned preparation method of the graphene composite copper sulfide / nickel sulfide catalytic material.
[0055] The graphene composite copper sulfide / nickel sulfide catalytic material uses graphene sheets as a matrix, and copper sulfide and nickel sulfide nanoparticles are directly grown on the matrix. That is, the morphology of the graphene composite copper sulfide / nickel sulfide catalytic material is bimetallic copper nickel sulfide nanoparticles loaded on the graphene sheets, and the particle size of the nanoparticles is in the range of 22nm to 24nm.
[0056] Another embodiment of the present invention provides an application of the graphene composite copper sulfide / nickel sulfide catalytic material as described above in the fields of zinc-air batteries, ethanol electrolysis cells, and water splitting catalysis.
[0057] The graphene composite copper sulfide / nickel sulfide catalytic material prepared by the present invention has the advantages of uniform size and good dispersibility. It is applied to zinc-air batteries and shows excellent fast charge and discharge performance, high specific capacity and cycle stability in terms of electrochemical performance. In addition, it can also be applied to other organic alcohol molecule electrooxidation reactions, such as methanol, ethylene glycol, isopropanol, 1,2-propylene glycol, glycerol and benzyl alcohol, etc., showing multifunctional catalytic activity for the electrooxidation of organic alcohol molecules. By introducing easily oxidized organic small molecules into the electrolyte, the oxygen evolution reaction of water decomposition can be replaced by ethanol oxidation reaction, and high-value organic products (acetate) can be prepared at the same time.
[0058] Another embodiment of the present invention provides a self-driving energy system, which uses the above-mentioned graphene composite copper sulfide / nickel sulfide catalytic material, and the specific assembly method includes:
[0059] 1) After the graphene composite copper sulfide / nickel sulfide catalyst material and the conductive carbon black are uniformly mixed, isopropyl alcohol, deionized water and a binder are added, and the cathode catalyst ink is obtained by ultrasonic dispersion, and the cathode catalyst ink is drop-coated on the conductive carbon cloth and dried to obtain a catalytic electrode;
[0060] 2) Assembling a zinc-air battery using a zinc sheet as an anode and a mixed solution of potassium hydroxide KOH and zinc acetate Zn(Ac)2 as an electrolyte;
[0061] 3) A catalytic electrode is used as an electrolytic anode to construct an ethanol electrolytic cell, and a zinc-air battery is used to drive the ethanol electrolytic cell to achieve the simultaneous preparation of hydrogen and acetate.
[0062] Preferably, in step 1), 3-10 mg of graphene composite copper sulfide / nickel sulfide catalyst material, 3-10 mg of conductive carbon black, 500-800 μL of isopropanol, 50-450 μL of deionized water, and 50-100 μL of Nafion binder are added, and the ultrasonic dispersion time is 1-1.2 h. A volume of 100-600 μL of cathode catalyst ink is drop-coated on the conductive carbon cloth.
[0063] Step 2) In the electrolyte, the molar ratio of potassium hydroxide to zinc actinide is in the range of 2:0.1 to 4:0.1, that is, the electrolyte includes 4-6M KOH and 0.1-0.3M Zn(Ac)2.
[0064] The present invention utilizes the excellent and efficient ORR / AOR performance of the graphene-composite copper nickel sulfide / nickel sulfide catalytic material, drives the alcohol molecule electrolysis cell through the assembled zinc-air battery, and constructs a self-driven energy conversion system, which can simultaneously realize the efficient preparation of hydrogen and acetate, saves costs to a certain extent, and is conducive to large-scale application.
[0065] On the basis of the above-mentioned embodiments, the present invention is further described below in combination with the preparation method of the graphene composite copper sulfide / nickel sulfide catalytic material. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. The experimental methods in the following examples where specific conditions are not specified are usually based on the conditions recommended by the manufacturer. Unless otherwise specified, percentages and parts are calculated by mass.
[0066] Example 1
[0067] This embodiment provides a method for preparing a graphene composite copper sulfide / nickel sulfide catalytic material, comprising the following steps:
[0068] 1) preparing a graphene oxide (GO) dispersion with a concentration of 8 mg / mL by a modified Hummers method;
[0069] 2) Weigh 1mmol Cu(NO3)2, 2mmol Ni(NO3)2 and 6mmol urea and dissolve them in 30mL deionized water, stir for 20 minutes, take 0.8mL GO dispersion, add it dropwise into the solution, and stir for 20 minutes to form a mixed solution;
[0070] 3) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined reactor, reacted in an oven at 160° C. for 6 h, and the precipitate was taken out after cooling to room temperature, washed three times by centrifugation with deionized water and ethanol, and then dried in an oven at 60° C. for 12 h to obtain a precursor powder;
[0071] 4) 100 mg of precursor powder and 500 mg of sulfur powder were placed in two porcelain boats respectively, calcined at 350° C. in an argon atmosphere for 2 h with a heating rate of 2° C. / min, and taken out after natural cooling to obtain a graphene composite copper sulfide / nickel sulfide catalytic material, which was labeled Cu1Ni2-S / G.
[0072] The Cu1Ni2-S / G prepared in Example 1 was used as a sample, and its structure was determined by X-ray diffractometer. The results are as follows: Figure 1 As shown, the peaks at 44.9° and 53.4° correspond to the (220) and (311) planes of NiS2 (JCPDF card number 089-7142), respectively, and the peaks at 29.3°, 32.8° and 48.0° correspond to the (102), (006) and (110) planes of CuS (JCPDF card number 079-2321), respectively, confirming that the sulfide phase is a composite of copper sulfide and nickel sulfide.
[0073] Figure 2 This is the SEM image of Cu1Ni2-S / G. Figure 2 It can be clearly seen that the nanoparticles are riveted to the graphene sheets.
[0074] Furthermore, by Figure 3 The transmission electron microscope TEM image shown can further confirm that the graphene flakes are uniformly loaded with metal sulfide nanoparticles with an average size of 24 nanometers, which is a zero-dimensional / two-dimensional heterostructure.
[0075] From the above tests, it can be seen that the formation process of the graphene composite copper sulfide / nickel sulfide catalytic material provided by the present invention is to first load the copper nickel basic carbonate precursor (Cu1Ni2-pre / G) on the reduced graphene oxide, and then in situ calcinate it under an argon atmosphere, which has rich heterogeneous interfaces and sulfur vacancy structures.
[0076] The Cu1Ni2-S / G prepared in Example 1 was used to form a three-electrode test system, and the oxygen reduction and alcohol oxidation performance were tested by the Chenhua CHI760E workstation. The specific method was as follows: a rotating disk electrode loaded with graphene composite copper sulfide / nickel sulfide catalytic material, a platinum black electrode and a saturated calomel electrode were used as the working electrode, counter electrode and reference electrode, respectively, to form a three-electrode test system.
[0077] Figure 5 The ORR performance of the Cu1Ni2-S / G three-electrode test system under 1 mol / L KOH. Figure 5 AE are the linear scanning voltammetry curves at different speeds at a scan rate of 5 mV / s, H2O2 yield and electron transfer number, SCN - Linear sweep voltammetry curves of poisoning test, methanol tolerance and stability test graphs.
[0078] from Figure 5 It can be seen that Cu1Ni2-S / G has a positive starting potential (0.91V) and half-wave potential (0.77V) with a limiting current of 5.57mA / cm 2 The ring-disk test showed that its H2O2% yield was very low and the electron transfer number was close to 4, indicating that its oxygen reduction reaction was close to a 4-electron transfer path. - The metal active site poisoning experiment showed that the metal site was the main active site. After adding methanol during the ORR process, Cu1Ni2-S / G still maintained a stable current density, showing better methanol tolerance than Pt / C. At the same time, the current retention rate was as high as 91% after 20 hours of stability test, which was significantly better than the precious metal Pt / C catalyst.
[0079] Figure 6 This is a graph characterizing the electrical performance of a zinc-air battery assembled with the graphene composite copper nickel sulfide / nickel sulfide catalytic material Cu1Ni2-S / G described in Example 1. Figure 6AF are schematic diagram of flow zinc-air battery, open circuit voltage stability diagram, discharge curve and power curve, discharge specific capacity, rate stability and charge and discharge stability test.
[0080] from Figure 6 It can be seen that the maximum discharge power of zinc-air battery can reach 127.1mW / cm 2 , excellent noble metal Pt / C catalyst (126.9mW / cm 2 ). The current rate performance is excellent and shows good reversibility. At 10mA / cm 2 At the discharge current density, its specific capacity is 814.3mAh / g Zn , the corresponding energy density is as high as 952.7Wh / kg. When Cu1Ni2-S / G and Ni3Fe1-LDH materials form a mixed catalyst, the assembled zinc-air battery shows excellent cycle stability.
[0081] Figure 7 This is a graph characterizing the AOR performance of Cu1Ni2-S / G prepared in Example 1 of the present invention in a 1 mol / L KOH+1 mol / L ethanol mixed electrolyte. Figure 7 AF are the linear scanning voltammetry curve at a scanning rate of 5 mV / s, Tafel slope, mass activity comparison bar graph, linear scanning voltammetry curve after normalization of electrochemical active surface area, nuclear magnetic resonance hydrogen spectrum, and stability test spectrum.
[0082] from Figure 7 It can be seen that compared with Cu1Ni2-S, Cu-S and Ni-S, Cu1Ni2-S / G shows a lower overpotential at 10 mA / cm -2 Under the current density, an ultra-low reaction potential (1.37V vs. RHE) can be obtained, and its mass activity (1.45V vs. RHE) is as high as 637.1mA / mg. At the same time, the Faradaic efficiency of acetate generation can reach 96%, and it shows excellent stability.
[0083] Figure 8 It is a characterization spectrum of applying Cu1Ni2-S / G to the electro-oxidation reaction of organic alcohols. The Cu1Ni2-S / G catalyst prepared in Example 1 can be extended to the electro-oxidation reaction of other organic alcohol molecules, such as methanol, ethylene glycol, isopropanol, 1,2-propylene glycol, glycerol and benzyl alcohol, showing multifunctional catalytic activity for the electro-oxidation of organic alcohol molecules.
[0084] Example 2
[0085] This embodiment provides a method for preparing a Cu1Ni2-S material, comprising the following steps:
[0086] 1) Weigh 1mmol Cu(NO3)2, 2mmol Ni(NO3)2 and 6mmol urea and dissolve them in 30mL deionized water and stir for 20 minutes;
[0087] 2) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined reactor, and reacted in a 160°C oven for 6 h. After cooling to room temperature, the precipitate was taken out, washed three times by centrifugation with deionized water and ethanol, and then dried in a 60°C oven for 12 h.
[0088] 3) Weigh 100 mg of the precursor powder prepared above and 500 mg of sulfur powder, place them in two porcelain boats respectively, calcine them at 350°C in an argon atmosphere for 2 h with a heating rate of 2°C / min, take them out after natural cooling, and obtain copper sulfide / nickel sulfide material, which is marked as Cu1Ni2-S.
[0089] The Cu1Ni2-S prepared in Example 2 was used to form a three-electrode test system, and a linear sweep voltammetry test was performed in a 0.1 mol / L KOH solution at a scan rate of 5 mV / s. The results showed that the starting potential, half-wave potential, and limiting diffusion current were 0.88 V, 0.76 V, and 4.99 mA / cm, respectively. 2 In the mixed electrolyte of 1mol / L KOH+1mol / L ethanol, its mass activity is 365.7mA / mg.
[0090] Example 3
[0091] This embodiment provides a method for preparing a Ni-S material, comprising the following steps:
[0092] 1) Weigh 3mmol Ni(NO3)2 and 6mmol urea and dissolve them in 30mL deionized water, stirring continuously for 20 minutes;
[0093] 2) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined reactor, and reacted in a 160°C oven for 6 h. After cooling to room temperature, the precipitate was taken out, washed three times by centrifugation with deionized water and ethanol, and then dried in a 60°C oven for 12 h.
[0094] 3) Weigh 100 mg of the precursor powder prepared above and 500 mg of sulfur powder, place them in two porcelain boats respectively, calcine them at 350°C in an argon atmosphere for 2 h with a heating rate of 2°C / min, take them out after natural cooling, and obtain nickel sulfide material, which is marked as Ni-S.
[0095] The Ni-S prepared in Example 3 was used to form a three-electrode test system, and a linear sweep voltammetry test was performed in a 0.1 mol / L KOH solution at a scan rate of 5 mV / s. The results showed that the starting potential, half-wave potential and limiting diffusion current were 0.86 V, 0.74 V and 4.63 mA / cm, respectively. 2 In the mixed electrolyte of 1mol / L KOH+1mol / L ethanol, its mass activity is 277.2mA / mg.
[0096] Example 4
[0097] This embodiment provides a method for preparing a Cu-S material, comprising the following steps:
[0098] 1) Weigh 3mmol Cu(NO3)2 and 6mmol urea and dissolve them in 30mL deionized water, stirring continuously for 20 minutes;
[0099] 2) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined reactor, and reacted in a 160°C oven for 6 h. After cooling to room temperature, the precipitate was taken out, washed three times by centrifugation with deionized water and ethanol, and then dried in a 60°C oven for 12 h.
[0100] 3) Weigh 100 mg of the precursor powder prepared above and 500 mg of sulfur powder, place them in two porcelain boats respectively, calcine them at 350°C in an argon atmosphere for 2 h with a heating rate of 2°C / min, take them out after natural cooling, and obtain copper sulfide material, which is marked as Cu-S.
[0101] The Cu-S prepared in Example 4 was used to form a three-electrode test system, and a linear sweep voltammetry test was performed in a 0.1 mol / L KOH solution at a scan rate of 5 mV / s. The results showed that the starting potential, half-wave potential and limiting diffusion current were 0.85 V, 0.65 V and 5.33 mA / cm, respectively. 2 In the mixed electrolyte of 1mol / L KOH+1mol / L ethanol, its mass activity is 5.2mA / mg.
[0102] Example 5
[0103] This embodiment provides a method for preparing Cu4Ni1-S, comprising the following steps:
[0104] 1) Weigh 2.4mmol Cu(NO3)2, 0.6mmol Ni(NO3)2 and 6mmol urea and dissolve them in 36mL deionized water, and stir for 20 minutes;
[0105] 2) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined reactor, and reacted in a 160°C oven for 6 h. After cooling to room temperature, the precipitate was taken out, washed three times by centrifugation with deionized water and ethanol, and then dried in a 60°C oven for 12 h.
[0106] 3) Weigh 100 mg of the precursor powder prepared above and 500 mg of sulfur powder, place them in two porcelain boats respectively, calcine them at 350°C in an argon atmosphere for 2 h with a heating rate of 2°C / min, take them out after natural cooling, and obtain a copper sulfide / nickel sulfide material, which is marked as Cu4Ni1-S.
[0107] The Cu4Ni1-S prepared in Example 5 was used to form a three-electrode test system, and a linear sweep voltammetry test was performed in a 0.1 mol / L KOH solution at a scan rate of 5 mV / s. The results showed that the starting potential, half-wave potential and limiting diffusion current were 0.85 V, 0.74 V and 5.31 mA / cm, respectively. 2 .
[0108] Example 6
[0109] This embodiment provides a method for preparing Cu1Ni4-S, comprising the following steps:
[0110] 1) Weigh 0.6mmol Cu(NO3)2, 2.4mmol Ni(NO3)2 and 6mmol urea and dissolve them in 36mL deionized water, and stir for 20 minutes;
[0111] 2) The mixed solution was transferred to a 50 mL polytetrafluoroethylene-lined reactor, and reacted in a 160°C oven for 6 h. After cooling to room temperature, the precipitate was taken out, washed three times by centrifugation with deionized water and ethanol, and then dried in a 60°C oven for 12 h.
[0112] 3) Weigh 100 mg of the precursor powder prepared above and 500 mg of sulfur powder, place them in two porcelain boats respectively, calcine them at 350°C in argon atmosphere for 2 h with a heating rate of 2°C / min, take them out after natural cooling, and obtain a copper sulfide / nickel sulfide material, which is marked as Cu1Ni4-S.
[0113] The Cu1Ni4-S prepared in Example 6 was used to form a three-electrode test system, and a linear sweep voltammetry test was performed in a 0.1 mol / L KOH solution at a scan rate of 5 mV / s. The results showed that the starting potential, half-wave potential, and limiting diffusion current were 0.86 V, 0.75 V, and 4.25 mA / cm, respectively. 2 .
[0114] In summary, by adjusting the molar ratio of copper and nickel metals, the ORR catalytic activity of copper-nickel sulfide can be effectively optimized, including performance indicators such as the onset potential, half-wave potential and limiting diffusion current.
[0115] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a graphene composite copper sulfide / nickel sulfide catalytic material, characterized in that: The following steps are involved: S1. preparing graphene oxide dispersion; S2, dissolving copper nitrate, nickel nitrate and urea in deionized water, stirring evenly, adding the graphene dispersion, and mixing evenly to form a mixed solution; S3, placing the mixed solution in a polytetrafluoroethylene reactor for hydrothermal reaction, cooling to room temperature, washing with deionized water and ethanol by centrifugation, and drying to obtain a precursor powder; S4. Place the precursor powder and sulfur powder in two porcelain boats respectively, and calcine them under an argon atmosphere to obtain a graphene composite copper sulfide / nickel sulfide catalytic material.
2. The preparation method according to claim 1, characterized in that: In step S2, the molar ratio of the copper nitrate to the nickel nitrate is in the range of 1:6 to 6:1, and the ratio of the total molar number of the copper nitrate and the nickel nitrate to the molar number of the urea is in the range of 3:
10.
3. The preparation method according to claim 2, characterized in that: The reaction temperature of the hydrothermal reaction in step S3 is in the range of 120° C. to 180° C., and the reaction time is in the range of 3 h to 24 h.
4. The preparation method according to any one of claims 1 to 3, characterized in that In step S4, the mass ratio of the precursor powder to the sulfur powder is in the range of 1:1 to 1:
15.
5. The preparation method according to claim 4, characterized in that: The calcination temperature in step S4 is in the range of 300° C. to 500° C., the calcination time is in the range of 2 h to 3 h, and the heating rate of the sintering furnace is in the range of 2° C. / min to 10° C. / min.
6. A graphene composite copper sulfide / nickel sulfide catalytic material, characterized in that: The material is prepared by the method for preparing the graphene composite copper sulfide / nickel sulfide catalytic material according to any one of claims 1 to 5.
7. The graphene composite copper sulfide / nickel sulfide catalytic material according to claim 6, characterized in that: The morphology of the graphene composite copper sulfide / nickel sulfide catalytic material is that bimetallic copper-nickel sulfide nanoparticles are loaded on graphene sheets, and the particle size of the nanoparticles is in the range of 22nm to 24nm.
8. An application of the graphene composite copper sulfide / nickel sulfide catalytic material as claimed in claim 6 or 7 in the fields of zinc-air batteries, ethanol electrolysis cells and water splitting catalysis.
9. A self-driving energy system, characterized in that: Using the graphene composite copper sulfide / nickel sulfide catalytic material according to claim 6 or 7, the specific assembly method includes: 1) After the graphene composite copper sulfide / nickel sulfide catalyst material and conductive carbon black are uniformly mixed, isopropanol, deionized water and a binder are added, and ultrasonic dispersion is performed to obtain a cathode catalyst ink, and the cathode catalyst ink is drop-coated on a conductive carbon cloth and dried to obtain a catalytic electrode; 2) Assembling a zinc-air battery using a zinc sheet as an anode and a mixed solution of potassium hydroxide and zinc acetate as an electrolyte; 3) Using the catalytic electrode as an electrolysis anode to construct an ethanol electrolysis cell, and using the zinc-air battery to drive the ethanol electrolysis cell to achieve simultaneous preparation of hydrogen and acetate.
10. The self-driving energy system according to claim 9, characterized in that: Step 2) In the electrolyte, the molar ratio of the potassium hydroxide to the zinc acetate is in the range of 2:0.1 to 4:0.1.