Method for recycling glass fiber reinforced plastics
By depolymerizing the polymer matrix of GRP and melting the glass-based components with combustion heat, the problems of quality degradation and difficulty in removing additives in glass fiber recycling are solved, achieving efficient and economical glass fiber recycling and reuse.
Patent Information
- Application Number
- CN202080027711.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-04-06
AI Technical Summary
It is difficult to effectively recycle glass fiber reinforced plastic (GRP) with existing technology, especially while maintaining material quality and reducing degradation. This results in a decrease in the quality of glass fiber during the recycling process and difficulty in removing additive degradation products, affecting the recycling of recycled materials. use.
By depolymerizing the polymer matrix of GRP, removing the pyrolysis products, and using the combustion heat of the remaining organic parts to melt the glass-based components and remove organic components and additives, efficient recycling and reuse of glass fibers can be achieved.
It achieves high-quality recycling of GRP, maintains the original characteristics of the material, and removes harmful additives and impurities. It is suitable for large-scale industrial-scale applications and is economically feasible.
Abstract
Description
Technical Field
[0001] The invention relates to a method for recycling glass-fiber-reinforced plastics, in particular plastics based on polyamide, polybutylene terephthalate or polyethylene terephthalate, to recover both the monomers of the polymer and the glass for the glass fibers. Background Art
[0002] Modern, highly resilient composite plastics are nowadays usually based on glass-fiber-reinforced thermoplastics, in particular polyamides or polyesters based on terephthalic acid. LANXESS Deutschland GmbH, Cologne, markets them under the trade name and Plastic pellets with chopped glass fiber reinforcement are sold under the trade name Continuous fiber reinforced semi-finished products / composites are sold. In the pelletized materials sold, the mass fraction of glass fiber reinforcement is typically in the range from 5 to 80% by weight.
[0003] Glass-based fillers and reinforcements, especially in the form of fibers, offer considerable improvements in strength, toughness and stiffness compared to plastic parts without fillers or reinforcements. This has led to the replacement of many metal-based structures with glass-reinforced plastics (GRP) in recent years, particularly in automotive manufacturing.
[0004] Additional heat-stabilizing additives now even make it possible to use GRP in areas that are subject to high thermal stresses, which would not be possible with pure polymers that have not been stabilized with these additives, particularly in the area of motor vehicle engine compartments.
[0005] Today, GRP-based components enable cost-effective lightweight construction throughout the transport sector. The weight reduction achieved in motor vehicles results in a significant reduction in energy consumption (fuel or electrical energy).
[0006] However, at the end of the use cycle (which ends in the case of motor vehicles with being sent to a car recycling plant), GRP-based components place very high demands on recycling operations, especially when the intention is to replace new materials consisting of the same substance. This applies all the more to GRP components, which must be highly modified for the intended application in order to avoid or reduce degradation during use. In the context of the present invention, degradation is understood to mean a deterioration in the level of mechanical properties, especially due to cleavage of the molecular chains of the (matrix) polymer.
[0007] Impurities also play an important role in the quality grade of GRP-based plastic recyclates. Mechanical recycling places particularly high demands on the plastic waste to be recycled when the recyclate is used to produce the same product or for other demanding applications. Mechanical recycling uses only physical methods. Physical methods include, for example, washing, drying, crushing, melting, compounding, melt filtering and regranulation. Of course, there are instances where plastic waste can be recycled into good quality recyclate via physical methods. The following prerequisites are usually required:
[0008] Components made of GRP must be collected in the same type of way, the level of contamination should be low, no significant polymer degradation should occur during the life cycle, and moreover only very little foreign matter should be absorbed by the polymer matrix during the entire life cycle, such as specialty oils and their additives, such as coolants in the case of engine and transmission oil pans for cars or trucks, or in the case of cooling circuit components such as coolant reservoirs. Such plastic-based recyclate materials can be reused to produce new components using conventional injection molding machines.
[0009] However, it has been found that only in very rare cases does mechanical recycling using purely physical methods produce a quality grade equivalent to the original new product.
[0010] The following are deteriorating aspects of GRP that promote degradation and thus hinder mechanical recycling, especially via purely physical methods:
[0011] - The high content of chopped glass fibers during compounding prevents the use of melt filters, especially if continuous cleaning and discharge of separated impurities plays a decisive role in improving the quality of the recyclate obtained in the mechanical recycling of unfilled thermoplastics.
[0012] - During compounding, preferably in the case where a conventional co-rotating twin screw extruder is typically used, the glass fibres are mechanically shortened, an effect which has a direct adverse effect on the strength and toughness of the GRP / compound / composite.
[0013] - Additives, in particular flame retardants or heat stabilizers, are subject to changes during the use cycle of GRP, in particular at high continuous use temperatures. However, degradation products of such additives remain in the mechanical recycling loop and therefore in the GRP recyclate.
[0014] Of course, there are various proposals to use physical methods to counteract degradation in the mechanical recycling of GRP. For example, the effect of reduced fiber length in the recyclate could be compensated by the subsequent addition of longer fibers. However, this approach is naturally not applicable to continuous fiber reinforced composites and is therefore limited to chopped glass fiber reinforced GRP.
[0015] However, polymer degradation can also be counteracted in various ways via targeted additions, in particular via chemically active chain extensions.
[0016] However, it must be noted that degradation is a fundamental problem in the mechanical recycling of GRP and it is not possible to run GRP repeatedly through a use-recycling loop without significant effects on the quality and product properties, in particular toughness, strength, stiffness, creep, heat resistance, etc.
[0017] As mentioned, recompounding reduces the fiber length. It is also generally not possible to directly remove the chopped glass fibers from the (matrix) polymer which is highly viscous in the molten state and thereby separate the fibers from the polymer matrix.
[0018] The high cost and complexity of separating the fibers from the matrix, optionally subjecting them to further cleaning, and preparing them for use as recyclate fibers must also ultimately be compared to the low cost of new glass fibers.
[0019] All three reasons explain why glass fibres from post-consumer GRP materials have hitherto only been rarely recovered and reused as filler or reinforcement.
[0020] WO 2017 007965A1 describes a method for depolymerizing unreinforced polyethylene terephthalate to obtain terephthalic acid and ethylene glycol therefrom. For this purpose, the polymer is added to a mixture of a nonpolar solvent that swells the polymer and an agent that cleaves the ester functions and depolymerized. WO 2017 007965A1 does not specify the recovery of fillers or reinforcing agents, in particular glass fibers.
[0021] EP 3 023 478 A2 discloses a method which enables the recycling of fibers, in particular in the case of carbon fiber composite plastics. The method comprises firstly pyrolyzing the polymer matrix of the composite plastic in a main reactor at 400° C. to 600° C. The remaining fiber residues and soot residues are washed, whereby the fibers absorb water. The wet residue is subsequently returned to the main reactor, where the fibers are cleaned under oxidative conditions at 350° C. to 400° C. The pyrolysis products formed in the first step during the pyrolysis are not subjected to material recovery but are transferred to a second reactor, where the toxic pyrolysis products are neutralized at up to 15 000° C. using a thermal plasma.
[0022] JP 2000034363 A describes a method for depolymerizing chopped glass fiber reinforced polyamide 6 composite plastics, wherein the polymer matrix is first depolymerized at a temperature of around 280° C. and then the entire reaction mixture is added to water and the caprolactam obtained by depolymerization, i.e. the monomer building block of polyamide 6, is dissolved in the water. Due to the significantly lower viscosity of aqueous caprolactam solutions, often only 1-100 mPa·s, the glass fibers can be removed from the continuous aqueous phase and washed.
[0023] The shortcoming of the method of JP 2000034363 A is the distillation of energy consumption to obtain high-purity caprolactam from the dilute caprolactam aqueous solution. In addition, the reuse of the glass fiber separated and washed in JP 2000034363 A is not without problems. Due to the shortening of fiber length during processing, the glass fiber removed and washed from JP 2000034363 A no longer reaches the same reinforcing effect as using new glass fiber. In addition, composite plastics contain a large amount of additives that stay on the fiber and can not be washed off with water completely nowadays. Under these circumstances, the method according to JP 2000034363 A does not provide high-quality recycled fiber yet.
[0024] Finally, for optimal function, glass-based reinforcing fibers require that the glass fiber surface has good compatibility with the polymer matrix, which is typically achieved via a customized surface coating (also referred to as size). Applying a suitable size to the dry, reclaimed glass fiber agglomerates obtained as per JP2000034363 A has proven to be impossible. The fiber agglomerates treated with aqueous size cannot be separated and in a feedable form after drying. In any case, the quality of new glass fibers cannot be obtained using the method described in JP 2000034363A.
[0025] JP 2000037726 A also describes a method for removing glass fibers (here chopped glass fibers) when recycling composite plastics based on polyamide 6 (PA6). JP 2000037726 A includes first depolymerizing the PA6 polymer matrix and thereby separating it from the glass fibers. JP 2000037726 A also describes that it is also possible in principle to recycle the glass fibers by converting the residual components of the PA6 used as the matrix polymer remaining on the fibers into gaseous components at the end of the depolymerization by heating to 400° C.-700° C. by pyrolytic decomposition. The temperature required for the pyrolysis must be provided to the method from an external source. JP 2000037726 A finally describes the option of subsequently heating the fibers "cleaned" in this way to a temperature above their melting temperature. This energy for melting the glass fibers must also be provided by an external source.
[0026] Neither JP 2000034363 A nor JP 2000037726 A deals with the fundamental problem of additives additionally used in plastics, their degradation products or their removal from wash water or pyrolysis products. The latter is however necessary in order to prevent these often environmentally disturbing substances from entering the environment.
[0027] Problems to be solved by the present invention
[0028] Starting from the prior art described above, the problem addressed by the present invention is to provide a method for recycling GRP, preferably based on polyamide 6, based on polybutylene terephthalate (PBT) and based on polyethylene terephthalate (PET), without using (wash) water to clean the glass fibers, by which the glass fibers can be recovered not only in their monomeric form (matrix) polymer but also in the form of glass suitable for glass fiber production and processed in the polymerization process / glass fiber production process to polymer / glass fibers of virgin quality. At the same time, the additives should be discharged efficiently from the recycling circuit without adverse effects on the environment and the method should be sufficiently economical and viable for large industrial scale application.
[0029] It has surprisingly been found that, in contrast to the teaching of the above-mentioned prior art, it is possible to produce glass fibers of virgin quality from post-consumer GRP materials, in particular from glass fiber reinforced thermoplastics based on PA6, PET or PBT, while also removing by depolymerization a large part of the polymer matrix which can be reconstructed to give the same original polymer. Summary of the invention
[0030] The solution to this problem and therefore the subject of the present invention is a method for recycling GRP by:
[0031] a) depolymerizing up to 80% by weight of the polymer matrix of the GRP, removing the pyrolysis products resulting from the polymer matrix and enriching the remaining residue in a mixture of glass-based components, residual matrix, monomers, pyrolysis products and components that are problematic for recycling, and
[0032] b) utilizing the organic fraction remaining in the residue at the end of process step a) as energy source by using its combustion heat to heat and melt the glass-based component and simultaneously removing the organic constituents by conversion into gaseous combustion products.
[0033] Therefore, in process step a), the polymer matrix / its cleavage products are not quantitatively removed from the glass fibers.
[0034] According to the invention, "problematic components" are in particular impurities and additives for the originally intended use of the GRP.
[0035] According to the invention, the components which are problematic for the recycling of GRP are preferably functional additives, in particular UV stabilizers, heat stabilizers, gamma stabilizers, antistatic agents, elastomer modifiers, flow promoters, mold release agents, flame retardants, emulsifiers, nucleating agents, plasticizers, lubricants, dyes, pigments or additives for increasing conductivity. These and further additives are described, for example, in Müller, Kunststoff-Additive [Plastic Additives], 3rd edition, Hanser-Verlag, Munich, Vienna, 1989 and Plastics Additives Handbook [Plastic Additives Handbook], 5th edition, Hanser-Verlag, Munich, 2001. In the context of the present invention, impurities are preferably degradation products of additives and impurities, in particular dust, soil, iron oxides in the form of rust or foreign substances which have penetrated into the polymer matrix or adhered thereto.
[0036] The method according to the invention therefore consists of two separate processes, in which the components originally used for producing the GRP are separated into monomers and cleavage products on the one hand and into a glass melt on the other hand.
[0037] The method according to the invention also makes it possible to remove components that are problematic for recycling, in particular impurities, and thus to produce a recyclate having the characteristics of a new material.
[0038] The process according to the invention is characterized in that when the (matrix) polymer on which the GRP is based is resynthesized from monomers produced as cracking products, no substantial impairment of the product quality of the polymer occurs even through repeated use-recycling cycles. In the process according to the invention, the polymer matrix / to be recycled (matrix) polymer is recycled to an extent of more than 50% by weight to about 80% by weight.
[0039] For the sake of clarity, it should be noted that the scope of the present invention encompasses all reported definitions and parameters in any desired combination in a general sense or within a preferred range. This applies not only to material parameters but also to any form of use and method as described in the context of the present invention. Unless otherwise noted, the standards cited should be understood to mean the version valid on the application date. Unless otherwise noted, the reported percentages are weight percentages. In the context of the present invention, the term (matrix) polymer and polymer matrix have the same definition, wherein the focus / emphasis of the term polymer matrix is on the matrix and in the term (matrix) polymer, the emphasis is on the polymer.
[0040] According to Kunststoffe.de, "Begriffsdefinitionen für das werkstofflicheRecycling", excerpted from W.Hellerich, G.Harsch, E.Baur, Werkstoff-Führer Kunststoffe 10 / 2010, page 55:
[0041] https: / / www.kunststoffe.de / themen / basics / recycling / werkstoffliches-recycling / artikel / begriffsdefinitionen-fuer-das-werkstoffliche-recycling-1001597.html
[0042] Recyclate is an umbrella term that refers to molded material / processed plastics with defined properties. In many cases, recyclate is mixed with new material. Recyclate has undergone a manufacturing process in its history. Masterbatches or blends produced from two or more plastics by processing (i.e., by a manufacturing process) are not considered recyclates.
[0043] The invention preferably relates to a process in which the GRP to be used in process step a) is heated and, optionally after addition of a catalyst or a depolymerization-promoting auxiliary, the polymer matrix of the GRP is subjected to cleavage in the absence of air.
[0044] The invention therefore relates to a process in which, during or after process step a), the cleavage products and / or added auxiliaries, in particular the hydrolysis or solvolysis liquid, are distilled off by reduced pressure.
[0045] The invention preferably relates to a process for recycling GRP, wherein in process step a) at least 50% by weight of the polymer matrix is depolymerized.
[0046] The present invention particularly preferably relates to a process for recycling GRP, wherein in process step a) at least 50% by weight and at most 80% by weight of the polymer matrix are depolymerized.
[0047] In the case in which method step b) is not carried out in a furnace for glass production, method step b) is followed by a further method step c) of removing the glass melt for further processing.
[0048] Method step a)
[0049] The depolymerization in process step a) is preferably carried out with the addition of auxiliaries or catalysts to promote the depolymerization. Preferred catalysts that promote the depolymerization of the (matrix) polymer are bases or acids or their salts. Inorganic bases or inorganic acids or their salts are particularly preferred. Very particular preference is given to using calcium hydroxide, calcium carbonate, sodium carbonate, potassium carbonate or phosphoric acid. These catalysts that promote the depolymerization of the (matrix) polymer are used in a concentration ranging from 0.1% to 20% by weight, preferably in a concentration ranging from 0.5% to 10% by weight, particularly preferably in a concentration ranging from 1% to 7% by weight, in each case based on the total polymer matrix introduced in process step a).
[0050] The polymer matrix of the GRP to be used in the process according to the invention preferably contains essentially at least one polymer from the following group: polyamide 6 (PA6), polyamide 66 (PA66), polyethylene terephthalate (PET), polybutylene terephthalate (PBT) or a copolymer of PET and PBT. Essentially preferably is to be understood as meaning an extent of at least 70% by weight, based on the polymer matrix introduced in process step a).
[0051] The polymer matrix of the GRP to be used in the method according to the invention preferably contains essentially polyamide 6 (PA6), polyamide 66 (PA66), polybutylene terephthalate (PBT) or a copolymer of PBT and PET.
[0052] The polymer matrix of the GRP to be used in the method according to the invention preferably contains essentially polyamide 6 (PA6) or polyamide 66 (PA66).
[0053] The polymer matrix of the GRP to be used in the method according to the invention preferably contains essentially polybutylene terephthalate (PBT) or a copolymer of PBT and PET.
[0054] In the case of PA6, ε-caprolactam is obtained in process step a) as a depolymerization product. The depolymerization in process step a) preferably enables recovery from the PA6 of 50 to 80% by weight of the ε-caprolactam originally used for its production.
[0055] In the context of the studies leading to the present invention, it was found that at the beginning of the depolymerization of GRP based on glass fiber reinforced PA6 carried out in process step a), high decomposition rates were achieved and few foreign substances were observed in the cleavage products. According to the invention, the preferred cleavage product in the depolymerization of PA6 carried out in process step a) is ε-caprolactam. Potassium carbonate or sodium carbonate particularly leads to high yields of ε-caprolactam.
[0056] Before being used for depolymerization, the GRP components to be used in process step a) are preferably collected in a similar manner and also used in a similar manner in process step a). Similar means that the plastics to be processed are identical in terms of their base polymers but differ from one another in specific properties, such as flame retardant additives. See: Kunststoffe.de, "Begriffsdefinitionen für das werkstoffliche Recycling", from W. Hellerich, G. Harsch, E. Baur, Werkstoff-Führer Kunststoffe 10 / 2010, page 55:
[0057] https:
[0058] / / www.kunststoffe.de / themen / basics / recycling / werkstoffliches-recycling / ar tikel / begriffsdefinitionen-fuer-das-werkstoffliche-recycling-1001597.html
[0059] The GRP fraction to be used in process step a) is particularly preferably collected in the same manner before being used for depolymerization and also used in the same manner in process step a), so that the cleavage product removed in process step a) does not need to be subjected to any expensive and inconvenient treatment.
[0060] In the context of the present invention, the same type is understood to mean that plastics of the same grade according to DIN EN ISO 11469 / VDA 260, optionally from different raw material producers, are processed. See: Kunststoffe.de, "Begriffsdefinitionen für das werkstoffliche Recycling", from W. Hellerich, G. Harsch, E. Baur, Werkstoff-Führer Kunststoffe 10 / 2010, page 55:
[0061] https:
[0062] / / www.kunststoffe.de / themen / basics / recycling / werkstoffliches-recycling / ar tikel / begriffsdefinitionen-fuer-das-werkstoffliche-recycling-1001597.html
[0063] Before use in the depolymerization, the GRP component to be used in process step a) is preferably first subjected to cleaning in order to prevent adhering impurities from being introduced into the pyrolysis in process step a).
[0064] Before being used for depolymerization, the GRP component to be used in method step a) is preferably comminuted into small pieces to simplify / accelerate the handling, transportability and depolymerization of the (matrix) polymer. In the context of the present invention, comminution is representative of any crushing process, in particular a mechanical crushing process. The crushing process arranged upstream of method step a) according to the present invention has been scientifically studied, for example in the project Recycling von Polymeren aus Schredderfraktionen, project partner UNISENSOR Sensorsysteme GmbH in Karlsruhe. DE 10 2014 111 871 B1 from this project relates to a device and a corresponding method for separating one or more material fractions from at least one material flow of a free-flowing matrix material, preferably from a block of recyclable plastic. The contents of DE 10 2014 111 871 B1 are fully incorporated into the present application.
[0065] In a further preferred variant, before the deagglomeration in process step a), the comminuted fraction is ground to provide particles with a particle size of less than <10 mm, particularly preferably <5 mm. The term ground material used in this context, which is obtained by grinding plastics, particularly preferably has different and irregular particle sizes (in the range from 2 to 5 mm) and may contain dust fractions. In this regard, see: Kunststoffe.de, "Begriffsdefinitionen für daswerkstoffliche Recycling", from W. Hellerich, G. Harsch, E. Baur, Werkstoff-Führer Kunststoffe 10 / 2010, page 55:
[0066] https:
[0067] / / www.kunststoffe.de / themen / basics / recycling / werkstoffliches-recycling / ar tikel / begriffsdefinitionen-fuer-das-werkstoffliche-recycling-1001597.html
[0068] In a further preferred variant, before the deagglomeration in process step a), the comminuted fraction is ground to provide a powder having a particle size of less than <1 mm and the powder is mixed with at least one deagglomeration-promoting auxiliary and / or catalyst.
[0069] In one embodiment, if necessary, the fraction obtained by comminution (comminuted fraction) can be subjected to further treatment before being used for depolymerization in process step a). It may be preferred to use additional process steps to remove the metal components adhering to the (matrix) polymer and to recover them separately. In this case, magnetic separators or inductive separators are preferably used.
[0070] The at least one depolymerization-promoting catalyst and / or auxiliary is preferably selected such that these undergo residue-free combustion in process step b) to provide energy or can remain as inorganic constituents in the glass components and ultimately in the recycled glass without having a significant effect on the glass quality.
[0071] It is preferred when at least 20% by weight of the original polymer matrix remains as organic residues in process step a). This remaining at least 20% by weight of the polymer matrix is used in process step b) to melt the glass-based component, preferably the glass fibers, via a combustion process and the resulting combustion heat.
[0072] It is preferred when this simultaneously releases glass-based components from organic impurities. It is preferred when a GRP component based on an easily and rapidly depolymerizable polymer is used in process step a). In the context of the present invention, preferred easily and rapidly depolymerizable polymers are polybutylene terephthalate (PBT), polyethylene terephthalate (PET) or polyamide 6 (PA6).
[0073] In the case of a PA6-based GRP fraction, the depolymerization is preferably carried out by heating at temperatures <350° C. in the absence of oxygen, particularly preferably in the presence of at least one basic catalyst; in this case, the depolymerization can be referred to as pyrolysis.
[0074] In the case of GRP based on PBT to be recycled, the depolymerization in process step a) is preferably carried out in the presence of water as depolymerization-promoting auxiliary. The depolymerization of GRP based on PBT is preferably carried out at a temperature in the range from 240° C. to 350° C. This forms terephthalic acid and 1,4-butanediol / tetrahydrofuran, the dehydration product thereof. The depolymerization can likewise be carried out in the presence of alcohols as auxiliary agents in a solvolytic manner, which leads to the formation of the corresponding esters.
[0075] In the case of PET based GRP to be recycled, the depolymerization is preferably carried out in the presence of water and / or alcohol at a temperature exceeding 280°C.
[0076] Preferably and in one embodiment, the cleavage products of the GRP (matrix) polymer produced in process step a) by cleavage of the polymer chains are provided (preferably after any necessary purification, in particular by distillation) to a subsequent repolymerization to produce a recyclate plastic having the characteristics of a new material. The repolymerization of the cleavage products makes it possible, in particular after additional purification of these cleavage products, referred to as monomers, to reproduce the same polymer / same plastic, in particular to produce new GRP based on recyclate. This process variant is preferably used in the case where the GRP (matrix) polymer contains only a few monomers and ideally only one monomer, and the monomer or monomers obtained are separable and purifiable by methods established on a large industrial scale, preferably by distillation or rectification.
[0077] GRPs which are particularly preferred for treatment by the process according to the invention are those which are based on PA6 as (matrix) polymer, which in turn is based on ε-caprolactam as monomer.
[0078] Optionally or in a preferred embodiment, the monomers / cracked products produced in process step a) are sent to a large-scale industrial-scale processing plant and purified together with monomers conventionally produced by petrochemical methods before repolymerization to produce recyclate plastics. Here too, preferred large-scale industrial-scale processing plants are distillation plants or rectification plants.
[0079] Preferably and in a further embodiment, part of the monomers / cleavage products of the GRP (matrix) polymer produced in method step a) by cleavage of the polymer chains is also used as additional fuel for the combustion operation in method step b). This method variant is preferably used in cases where the GRP (matrix) polymer consists of at least two different monomers or the polymer matrix consists of a blend of at least two different plastics or there are no post-consumer plastics of the same type as feed stream. Feed stream is an established term in process engineering. This refers to the flow of reactants (feed) into the process, in the present case the process according to the invention for recycling GRP.
[0080] Depolymerization, which is preferably understood to mean hydrolysis, solvolysis or pyrolysis / thermolysis, depending on the type of underlying (matrix) polymer, can be carried out in different process engineering apparatuses.
[0081] After adding suitable auxiliaries / catalysts, in particular basic catalysts, the GRP to be used according to the invention, in particular based on polyamide, is preferably directly heated (pyrolysis / thermolysis) in the absence of oxygen, preferably under a nitrogen atmosphere. This is preferably done using batch reactors which, by staggered start-up in time, can provide material for the second process step b) in a quasi-continuous manner.
[0082] In the case where the (matrix) polymer, in particular PBT or PET, is depolymerized in process step a) via superheated steam or using alcohols, preference is given to using an autoclave. After the exposure time, the volatile components are distilled off, preferably under reduced pressure, and the remaining residue is transferred to process step b).
[0083] Method step b)
[0084] Process step b) is preferably carried out in a rotary kiln - see U. Richers, Thermische Behandlung von in Forschungszentrum Karlsruhe GmbH, Karlsruhe, 1995.
[0085] It is preferred when, in process step a), not more than 20% by weight of the original (matrix) polymer remains as organic residues, which are supplied to process step b) together with the glass-based component. This organic residue is burned in process step b), wherein the heat of combustion initially heats and ultimately melts the glass-based component. Process step b) is preferably carried out at a temperature in the range from 1300° C. + / - 300° C.
[0086] By burning the remaining organic material, impurities, additives and decomposition products remaining on the glass-based component are removed at the same time. Preferably, the organic impurities, additives and decomposition products are oxidized to CO2 and water.
[0087] It is preferred when all the energy used for process step b) is generated by the combustion of the organic materials / residues and the glass-based components introduced into process step b).
[0088] However, in one embodiment, it is preferred to use conventional gas burners to provide additional energy in method step b). In a preferred embodiment, these are provided with a gaseous fuel based on C1-C4-hydrocarbons as combustion fuel. Preferably natural gas or biogas is used for this purpose.
[0089] The additional energy supply in process step b) should preferably be used when the heat of combustion of the organic materials / residues or of the polymers still present in the organic residues is insufficient to reach the melting temperature of the glass-based component and / or to exceed the usual residence time of the glass-based component in the molten state until further processing.
[0090] The combustion of the organic materials / residues in process step b) is preferably carried out by supplying air, an air-oxygen mixture or pure oxygen.
[0091] Process step b) is preferably carried out directly in the melting zone of the glass fiber production plant, wherein the organic material / organic residue is combusted using additionally introduced air / oxygen. The residue obtained in process step a) is fed as a side stream of the main feed stream of the inorganic glass raw material mixture into the melting zone of the furnace of the glass fiber production plant or optionally after crushing, in particular comminution, is provided as a solid to the furnace of the glass fiber production plant. The solid feed can be carried out separately or mixed with the main feed stream of the glass raw material mixture.
[0092] It is likewise preferred if method step b) is carried out in the vicinity of the glass fiber production plant and the glass melt produced by method step b) is combined directly with the glass melt of the glass fiber production plant.
[0093] In the case where the glass-based component of the GRP is glass fibers, the combustion operation in method step b) also produces impurities on the surface of the glass fibers or the sizing agent to be oxidized and discharged (preferably in the form of CO 2 ) via the combustion gases.
[0094] Impurities or decomposition products from the polymer matrix of the GRP used which could not be oxidized to CO 2 in process step b) are preferably discharged via the combustion gases.
[0095] Impurities, additives or their decomposition products can form pollutants in process step b). These are preferably supplied together with the combustion gases produced to exhaust gas purification, where the pollutants are intercepted in order to comply with legislative emission regulations.
[0096] In particular, in the case where the combustion of the (matrix) polymer containing residues of bromine- or phosphorus-containing additives is carried out in process step b), in principle toxic by-products which are undesirable for humans and the environment may form and are therefore present in the combustion gases. However, as a result of modern exhaust gas purification, these can nowadays be easily separated from the exhaust gases so that these substances do not enter the environment and the legislative emission regulations are met. The German Federal Emission Control Act (law on protection against harmful environmental influences from air pollution, noise, vibrations and similar events) stipulates, in particular, in its latest version of April 12, 2019 (BGB1 I p. 432) the environmental law_ It is an important branch of the Regulations and is concerned with the practice of protecting humans, animals, plants, soil, water, atmosphere and cultural assets from the harm and discharge of unmeasurable substances.
[0097] In one method variant of method step b), the organic (matrix) polymer adhering to the glass-based component, preferably the glass fibers, is initially pyrolyzed at elevated temperature and the heat of combustion of the carbonized residues adhering to the glass component / glass fibers is then used together with the heat of combustion of the pyrolysis gases and / or pyrolysis oil produced to melt the glass component / glass fibers.
[0098] It is particularly preferred to introduce the pyrolysis gases produced in process step b) at another point in the melting operation in the process according to the invention. It is also preferred to directly mix the pyrolysis gases with the natural gas preferably used for the melting operation in process step b). This process variant makes it possible to provide sufficient combustion heat in process step b) even after complete depolymerization of the (matrix) polymer in process step a) to melt the glass-based component, preferably the glass fibers, and to maintain them at melting temperature until further processing.
[0099] In the case where method step b) is carried out directly and immediately in the melting zone of the glass fiber production plant, it is preferred to introduce customary glass fiber additives, in particular SiO2, Al2O3, MgO, B2O3, CaO, into the glass / matrix residue composition resulting from method step a).
[0100] Method step c)
[0101] If method step b) is not carried out in a glass production furnace or in the immediate vicinity thereof, removal of the glass melt for subsequent further processing takes place in method step c).
[0102] It is preferred when the glass melt produced in process step c) is supplied to the production of glass fibers or to the production of glass powder or glass spheres. It is particularly preferred when the glass component produced in process step c) is supplied to a conventionally operated furnace for the production of glass fibers so that it can then be used for respinning into glass fibers.
[0103] Since almost all impurities are concentrated in the organic residue at the end of method step a) and are discharged in method step b) via a subsequent combustion process in the form of combustion gases and are thus removed from the glass component, the method according to the invention enables the production of high-quality glass melts, from which high-quality glass recyclates, in particular in the form of glass fibers, ground glass or glass powder, can be produced in further processing steps.
[0104] In the preferred case of depolymerization / pyrolysis of the polymer matrix in process step a) to an extent of not more than 80% by weight of the original GRP matrix, sufficient organic material remains on the glass component, the combustion of which provides sufficient combustion heat to melt the glass-based components of the GRP, preferably the glass fibers, and to provide them for mechanical recycling. With not more than 20% by weight of organic material remaining from the original (matrix) polymer, impurities, additives and decomposition products remaining on the glass-based components are oxidized to CO2 during the combustion process and removed thereby. DETAILED DESCRIPTION
[0105] In particular, the present invention relates to a method for recycling GRP, the method comprising:
[0106] a) depolymerizing up to 80% by weight of the polymer matrix of the GRP, removing the pyrolysis products resulting from the polymer matrix and enriching the remaining residue in a mixture of glass-based components, residual matrix, monomers, pyrolysis products and components that are problematic for recycling, and
[0107] b) utilizing the organic fraction remaining in the residue at the end of process step a) as energy source by using its combustion heat to heat and melt the glass-based component and simultaneously removing the organic constituents by conversion into gaseous combustion products, provided that the polymer matrix is based on polyamide 6 (PA6), on polyamide 66 (PA66), on polybutylene terephthalate (PBT) or on a copolymer of PBT and PET.
[0108] The present invention additionally relates to a method for recycling GRP by:
[0109] a) depolymerizing up to 80% by weight of the polymer matrix of the GRP, removing the pyrolysis products resulting from the polymer matrix and enriching the remaining residue in a mixture of glass-based components, residual matrix, monomers, pyrolysis products and components that are problematic for recycling, and
[0110] b) utilizing the organic fraction remaining in the residue at the end of process step a) as energy source by using its combustion heat to heat and melt the glass-based component and simultaneously removing the organic constituents by conversion into gaseous combustion products, provided that the polymer matrix is based on polyamide 6 (PA6) or on polyamide 66 (PA66), in particular PA6.
[0111] In particular, the present invention also relates to a method for recycling GRP, the method comprising:
[0112] a) depolymerizing up to 80% by weight of the polymer matrix of the GRP, removing the pyrolysis products resulting from the polymer matrix and enriching the remaining residue in a mixture of glass-based components, residual matrix, monomers, pyrolysis products and components that are problematic for recycling, and
[0113] b) utilizing the organic fraction remaining in the residue at the end of process step a) as energy source by using its combustion heat to heat and melt the glass-based component and simultaneously removing the organic constituents by conversion into gaseous combustion products, provided that the polymer matrix is based on polybutylene terephthalate (PBT) or on a copolymer of PBT and PET.
[0114] In particular, the present invention also relates to a method for recycling GRP, the method comprising:
[0115] a) depolymerizing up to 80% by weight of the polymer matrix of the GRP, removing the pyrolysis products resulting from the polymer matrix and enriching the remaining residue in a mixture of glass-based components, residual matrix, monomers, pyrolysis products and components that are problematic for recycling, and
[0116] b) utilizing the organic fraction remaining in the residue at the end of process step a) as energy source by using its combustion heat to heat and melt the glass-based component and simultaneously removing the organic components by conversion into gaseous combustion products, and
[0117] c) Separation of the glass melt for further processing
[0118] A prerequisite is that the polymer matrix is based on polyamide 6 (PA6), on polyamide 66 (PA66), on polybutylene terephthalate (PBT) or on a copolymer of PBT and PET.
[0119] The present invention further relates to a method for recycling GRP, the method comprising:
[0120] a) depolymerizing up to 80% by weight of the polymer matrix of the GRP, removing the pyrolysis products resulting from the polymer matrix and enriching the remaining residue in a mixture of glass-based components, residual matrix, monomers, pyrolysis products and components that are problematic for recycling, and
[0121] b) utilizing the organic fraction remaining in the residue at the end of process step a) as energy source by using its combustion heat to heat and melt the glass-based component and simultaneously removing the organic components by conversion into gaseous combustion products, and
[0122] c) Separation of the glass melt for further processing
[0123] A prerequisite is that the polymer matrix is based on polyamide 6 (PA6) or on polyamide 66 (PA66), in particular PA6.
[0124] The present invention particularly finally relates to a method for recycling GRP, which method is:
[0125] a) depolymerizing up to 80% by weight of the polymer matrix of the GRP, removing the pyrolysis products resulting from the polymer matrix and enriching the remaining residue in a mixture of glass-based components, residual matrix, monomers, pyrolysis products and components that are problematic for recycling, and
[0126] b) utilizing the organic fraction remaining in the residue at the end of process step a) as energy source by using its combustion heat to heat and melt the glass-based component and simultaneously removing the organic components by conversion into gaseous combustion products, and
[0127] c) Separation of the glass melt for further processing
[0128] A prerequisite is that the polymer matrix is based on polybutylene terephthalate (PBT) or on a copolymer of PBT and PET.
[0129] Examples
[0130] 150g of The pulverized GRP made of BKV30H2.0 was melted in a 500 mL round-bottom flask in a metal bath (T=320° C.) in a glass apparatus with KPG stirrer (blade stirrer and torque measurement). 5% potassium carbonate, based on the post-consumer plastic, was added as a finely powdered depolymerization catalyst.
[0131] The melting process was carried out statically and only periodically stirred (approximately every 5 minutes), about 2 to 3 turns. After about 40 minutes, the melting of 150 g of pulverized GRP was completed.
[0132] Under slow stirring at 12 revolutions per minute (rpm), the internal pressure was reduced in 50 mbar steps to 20 to 30 mbar, and considerable foam development was observed.
[0133] The polyamide 6 starting material caprolactam was converted into a gaseous state and the entire apparatus was continuously heated using a hot air blower so that this monomer, which has a melting point of 68° C., did not become solid and cause blockage in the apparatus.
[0134] The following fractions of caprolactam shown in Table 1 were obtained:
[0135] Table 1
[0136] Flask Duration (min) Amount (g) 1 32 43.14 2 25 40.34 3 44 39.42 sum 101 82.90 Yield 79%
[0137] Caprolactam fractions 1 to 3 were analyzed by gas chromatography. The purity decreased from fraction 1 to fraction 3 but in each case proved to be suitable for repolymerization by hydrolytic polymerization. The caprolactam proportion in these fractions was more than 99.5% by weight.
[0138] The residue remaining after depolymerization was divided into portions and transferred into glass boats, which were surrounded by pure oxygen in a muffle furnace, ignited using a Bunsen burner and burned without adding further heat.
[0139] At the end of the combustion process, the glass residue was separated off, dried at 115° C. and homogenized in accordance with DIN 52331. These samples were then subjected to ICP-OES analysis.
[0140] In addition to the measured CuO concentration (which is due to the use of In addition to the thermal stability of the grade Compared to the glass fibers used in BKV30H2.0, there are no significant deviations in the glass composition of the glass residue.
Claims
1. A method for recycling glass fiber reinforced plastics, characterized in that: a) depolymerizing at least 50% and up to 80% by weight of the polymer matrix of the glass fiber reinforced plastic, removing the pyrolysis products resulting from the depolymerization of the polymer matrix and enriching the remaining residue in a mixture of glass-based components, residual matrix, monomers, pyrolysis products and components problematic for recycling, wherein the components problematic for recycling include UV stabilizers, heat stabilizers, gamma stabilizers, antistatic agents, elastomer modifiers, flow promoters, mold release agents, flame retardants, emulsifiers, nucleating agents, plasticizers, lubricants, dyes, pigments or additives for increasing conductivity, b) utilizing the organic fraction remaining in the remaining residue at the end of process step a) as an energy source by using its combustion heat to heat and melt the glass-based components in the remaining residue, generating a glass melt and simultaneously removing the organic components in the remaining residue by conversion into gaseous combustion products, and c) separating the glass melt for further processing, Provided that the pyrolysis product is ε-caprolactam and the recyclate plastic is polyamide 6, the glass-fiber-reinforced plastic to be used in process step a) is heated and, after addition of additives, subjected to pyrolytic pyrolysis in the absence of air.
2. The method according to claim 1, characterized in that The components of the glass-fiber-reinforced plastic to be used in process step a) are collected beforehand in a similar manner and used in a similar manner in process step a).
3. The method according to claim 1 or 2, characterized in that The components of the glass-fiber-reinforced plastic to be used in process step a) are collected beforehand in the same manner and used in the same manner in process step a).
4. The method according to claim 1 or 2, characterized in that: Prior to use in the deagglomeration, the components of the glass-fiber-reinforced plastic to be used in process step a) are comminuted into small pieces.
5. The method according to claim 1 or 2, characterized in that: Prior to the depolymerization, the glass-fiber-reinforced plastic to be used in process step a) is subjected to cleaning.
6. The method according to claim 1 or 2, characterized in that: During or after process step a), the cleavage products are distilled off under reduced pressure.
7. The method according to claim 1 or 2, characterized in that: The cleavage products of the glass fiber reinforced plastic matrix polymer produced in process step a) by cleavage of the polymer chains are supplied to subsequent repolymerization to produce a recyclate plastic having the characteristics of a new material.
8. The method according to claim 1 or 2, characterized in that: The cleavage products of the glass-fiber-reinforced plastic matrix polymer produced in process step a) by cleavage of the polymer chains are also used at least partially as fuel for the combustion operation in process step b).
9. The method according to claim 1 or 2, characterized in that: With the remaining at least 20% by weight of organic material, impurities, additives and decomposition products remaining on the glass components are removed from the glass reinforcement / glass melt during the combustion process in process step b).
10. The method according to claim 9, characterized in that With a remaining amount of at least 20% by weight of organic material, impurities, additives and decomposition products remaining on the glass component are converted into CO2 by oxidation.
11. The method according to claim 1 or 2, characterized in that: In process step b) additional energy is provided.
12. The method according to claim 11, characterized in that Additional energy is provided by means of a gas burner.
13. The method according to claim 1 or 2, characterized in that: The depolymerization is carried out in the presence of at least one basic catalyst at a temperature of <350°C.
Citation Information
Patent Citations
A process for recycling composite materials and a system for treating waste gases
EP3023478A2
Recycling of nylon 6 products
JP2000034363A
Polyethylene terephthalate depolymerization
WO2017007965A1
Method for recycling thermoplastic resin products
JP2000037726A