Electrophotographic photoreceptor and image forming device having the same
By constructing a stacked photosensitive layer with oxytitanium phthalocyanine with specific X-ray diffraction spectrum, the light resistance and repeated power-on fatigue problems of electrophotographic photoreceptors under the requirements of high-speed, miniaturization and long-life, achieving stable image formation and prolong the life of the photoreceptor.
Patent Information
- Application Number
- CN202110548191.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-05-22
- Filing Date
- 2021-05-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-05-19
AI Technical Summary
Under the requirements of high-speed, miniaturization and long-life, the photoreceptor resistance and repeated power-on fatigue lead to image deterioration, and the material composite deterioration during the small-pathing process leads to a shortening of the photoreceptor life.
The oxytitanium phthalocyanine with a specific X-ray diffraction spectrum is used as the charge generation substance to construct a layered photosensitive layer with a specific spectral absorption spectrum, and the ultraviolet absorber is reduced or not added to improve the light resistance and stability of the photosensitive body.
It realizes the stability of maintaining image characteristics in high speed, miniaturization and long-term use, extends the life of the photoreceptor, and improves the printing resistance of the photoreceptor layer.
Smart Images

Figure CN113703295B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electrophotographic photoreceptor and an image forming device having the electrophotographic photoreceptor. More specifically, the present invention relates to an electrophotographic photoreceptor and an image forming device having the electrophotographic photoreceptor, wherein the electrophotographic photoreceptor has a photosensitive layer, the photosensitive layer contains oxytitanium phthalocyanine having a specific X-ray diffraction pattern as a charge generating material, and the photosensitive layer has a special spectral absorption spectrum. Background Art
[0002] Electrophotographic image forming apparatuses that form images using electrophotographic technology are often used in copying machines, printers, facsimile machines, and the like.
[0003] An electrophotographic photoreceptor (hereinafter also referred to as a “photoreceptor”) used in an electrophotographic process is composed of a substrate and a photosensitive layer containing a photoconductive material.
[0004] At present, research and development of photoreceptors having a photosensitive layer containing an organic photoconductive material as a main component (also referred to as "organic photoreceptors") are underway, and these materials currently constitute the mainstream of photoreceptors.
[0005] As organic photoreceptors, there are proposed a single-layer photosensitive layer structure in which a charge generating material and a charge transporting material (also called "charge moving material") are dispersed in a binder resin (also called "binder resin" or "binder resin") on a substrate (also called "conductive support"), and a laminated photosensitive layer structure in which a charge generating layer in which a charge generating material is dispersed in a binder resin and a charge transporting layer in which a charge transporting material is dispersed in a binder resin are laminated in sequence. Among them, the latter functional separation type photoreceptor has excellent electrophotographic characteristics and durability, has a high degree of freedom in material selection, and is easy to design various photoreceptor characteristics, and is widely used.
[0006] Among them, many schemes have been proposed for an organic photoreceptor composed of a charge generating layer and a charge transporting layer, wherein the charge generating layer is a layer in which a specific crystalline oxytitanium phthalocyanine is dispersed in a vapor-deposited film or a resin as a charge generating substance, and the charge transporting layer is a layer in which a low molecular weight organic compound is dispersed in a resin as a charge transporting substance.
[0007] Although organic photoreceptors have high sensitivity to long-wavelength light, low residual potential, high chargeability, and excellent electrostatic properties, they are unable to maintain these advantages due to repeated electrical fatigue.
[0008] In recent years, there has been an increasing demand for faster and smaller image forming apparatuses such as copy machines.
[0009] For example, as a means of increasing the speed, a tandem system in which image forming units such as photoreceptors, charging, exposure, development, cleaning, and neutralization are arranged is widely used for image forming elements for yellow, magenta, cyan, and black.
[0010] Therefore, in order to realize the miniaturization of the device, it is necessary to make each image forming unit itself compact, which requires the photoreceptor to be reduced in diameter. In the past, in order to extend the maintenance cycle of the photoreceptor, the photoreceptor was required to be enlarged in diameter, but by adopting the series connection method, it is necessary to reduce the diameter of the photoreceptor. In the case of reducing the diameter of the photoreceptor, repeated electrical fatigue is more serious than before, and there are many technical problems in extending the life (lifespan) of the photoreceptor. The cause of such deterioration is the result of the composite deterioration of various materials. Although it has not yet been identified, one of the reasons can be listed as insufficient light resistance of the photoreceptor.
[0011] The photoreceptor is exposed to light in normal use not only from the light source inside the copier. The photoreceptor is exposed to external light during maintenance such as replacing parts of peripheral components or when a paper jam occurs inside the machine. The light fatigue caused by these external lights is more damaging than the electrical fatigue inside the machine, and is the cause of image degradation. In addition, in the production process, careful attention is required under short-wavelength cut fluorescent lights to consider the degradation of the photoreceptor, which may also reduce productivity.
[0012] Various technologies have been proposed to address these issues.
[0013] Japanese Patent Application Laid-Open No. 10-048856 (Patent Document 1) and Japanese Patent Application Laid-Open No. 11-184108 (Patent Document 2) propose a technique of adding an ultraviolet absorber having a maximum absorption wavelength of 380 to 480 nm to a photosensitive layer.
[0014] Japanese Patent Application Laid-Open No. 2010-164639 (Patent Document 3) proposes a technique of adding an electron transport material (electron transport substance) having a maximum absorption wavelength of 300 to 370 nm and a specific structure having no absorption wavelength of 730 to 800 nm.
[0015] However, although both methods involve adding additives to the photosensitive layer, the magnitude of the effects is different, but the role of capturing charge transport remains the same.
[0016] Furthermore, the addition of a low molecular weight compound to the photosensitive layer may cause a problem of reduced printing durability even in a small amount.
[0017] As described above, the current situation is that image forming apparatuses such as copiers are still insufficient in meeting the requirements for higher speed, smaller size, smaller diameter of photoreceptors, and longer life.
[0018] Prior art literature
[0019] Patent Literature
[0020] Patent Document 1: Japanese Patent Application Publication No. 10-048856
[0021] Patent Document 2: Japanese Patent Application Publication No. 11-184108
[0022] Patent Document 3: Japanese Patent Application Publication No. 2010-164639 Summary of the invention
[0023] Technical Problems to be Solved by the Invention
[0024] Therefore, the object of the present invention is to provide an electronic photographic photoreceptor and an image forming device having the electronic photographic photoreceptor, wherein the electronic photographic photoreceptor uses a known crystalline form of oxytitanium phthalocyanine as a charge generating material, has excellent light resistance, does not reduce sensitivity during long-term repeated power-on fatigue during its service life, and can maintain stable image characteristics for a long time. Even with the high-speed, miniaturization, and small diameter of the photoreceptor, the printing resistance of the photosensitive layer will not be reduced, and images can be stably formed during long-term use.
[0025] Technical solutions for solving technical problems
[0026] The inventors of the present invention have conducted intensive research to solve the above-mentioned problems and have found that in a photosensitive body using oxytitanium phthalocyanine having a specific X-ray diffraction spectrum as a charge generating material, the photosensitive layer has a specific spectral absorption spectrum. Therefore, even if no ultraviolet absorber is added to the photosensitive layer or the amount of ultraviolet absorber added is reduced, the light resistance of the photosensitive body is significantly improved, and stable image characteristics can be maintained for a long time, thereby completing the present invention.
[0027] Thus, according to the present invention, at least a laminated photosensitive layer is provided, wherein a charge generating layer containing a charge generating material and a charge transporting layer containing a charge transporting material are laminated in this order on a substrate.
[0028] The charge generating substance is oxytitanium phthalocyanine having at least diffraction peaks at Bragg angles (2θ±0.2°) of 7.3°, 9.4°, 11.6°, 24.2°, and 27.3° in an X-ray diffraction spectrum using CuKα rays,
[0029] The laminated photosensitive layer is characterized in that it has a maximum absorption at a wavelength of 800 to 850 nm in a spectral absorption spectrum, and the absorbance (Abs) at a wavelength of 780 nm when the minimum absorbance at a wavelength of 400 to 800 nm is corrected as 0. 780nm ) and the absorbance at 860 nm (Abs 860nm ) ratio Abs 860nm / Abs 780nm It is 0.6 or more and 1.2 or less.
[0030] In addition, according to the present invention, an image forming device is provided, characterized in that it at least includes: the above-mentioned electronic photographic photoreceptor; a charging unit for charging the electronic photographic photoreceptor; an exposure unit for exposing the charged electronic photographic photoreceptor to form an electrostatic latent image; a developing unit for developing the electrostatic latent image formed by exposure to form a colorant image; a transfer unit for transferring the colorant image formed by development to a recording medium; a fixing unit for fixing the transferred colorant image on the recording medium to form an image; a cleaning unit for removing and recovering the colorant remaining on the electronic photographic photoreceptor; and a de-electrification unit for de-electrifying the surface charge remaining on the electronic photographic photoreceptor.
[0031] Beneficial Effects
[0032] According to the present invention, there can be provided an electronic photographic photoreceptor and an image forming device having the electronic photographic photoreceptor. The electronic photographic photoreceptor uses a known crystalline oxytitanium phthalocyanine as a charge generating material and has excellent light resistance. The sensitivity will not decrease during long-term repeated power-on fatigue during its service life and stable image characteristics can be maintained for a long time. The printing resistance of the photosensitive layer will not decrease even with high-speed, miniaturization, and smaller diameter of the photoreceptor, and images can be stably formed during long-term use.
[0033] The photoreceptor of the present invention can achieve the above-mentioned effects when any one of the following conditions (1) to (4) is satisfied.
[0034] (1) Ratio Abs 860nm / Abs 780nm It is greater than or equal to 0.75 and less than or equal to 1.
[0035] (2) Oxytitanium phthalocyanine has an average particle size D (50%) of 0.15 to 0.3 μm.
[0036] (3) The charge transport material is a trienamine dimer compound represented by the general formula (1) (described in detail in the section "charge transport layer") or a stilbene derivative represented by the general formula (2) (described in detail in the section "charge transport layer").
[0037] (4) A primer layer is provided between the substrate and the laminated photosensitive layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a diagram showing the spectral absorption spectrum of the photosensitive layer of the photoreceptor (Example 1) of the present invention.
[0039] Figure 2This is a schematic cross-sectional view showing the structure of the main part of the photoreceptor (laminated type photoreceptor) F01 of the present invention.
[0040] Figure 3 It is a schematic side view showing the configuration of a main part of the image forming apparatus 100 of the present invention.
[0041] Figure 4 3 is a diagram showing the X-ray diffraction spectrum pattern of oxytitanium phthalocyanine in Production Example 1. DETAILED DESCRIPTION
[0042] (1) Photoreceptor
[0043] The photoreceptor of the present invention comprises at least a laminated photosensitive layer, wherein a charge generating layer containing a charge generating material and a charge transporting layer containing a charge transporting material are laminated in this order on a substrate.
[0044] The charge generating substance is oxytitanium phthalocyanine having at least diffraction peaks at Bragg angles (2θ±0.2°) of 7.3°, 9.4°, 11.6°, 24.2°, and 27.3° in an X-ray diffraction spectrum using CuKα rays,
[0045] The laminated photosensitive layer is characterized in that it has a maximum absorption (λ) at a wavelength of 800 to 850 nm in a spectral absorption spectrum. max ), and the absorbance at a wavelength of 780 nm when the minimum absorbance in the wavelength range of 400 to 800 nm is taken as 0 for correction (Abs 780nm ) and the absorbance at 860 nm (Abs 860nm ) ratio Abs 860nm / Abs 780nm It is 0.6 or more and 1.2 or less.
[0046] When the photosensitive layer of the photoreceptor of the present invention has the above-mentioned spectral absorption spectrum, the λmax of the phthalocyanine dye has strong absorption on the long wavelength side, which indicates that the intermolecular interaction of the phthalocyanine dye is strong.
[0047] When the photosensitive layer is exposed to external light, an amount equivalent to the absorbed light energy is activated to an excited state. The more stable the excited state is, the greater the impact on the image. Therefore, it is considered how to form a structure that can quickly deactivate from the excited state to the ground state, but this will affect the light resistance of the photosensitive layer.
[0048] The photosensitive layer of the present invention has the above-mentioned spectral absorption spectrum, so that the charges that are exposed to external light and become excited move between the π-π bonds of the phthalocyanine dye and are easily and quickly deactivated in the ground state, resulting in a photosensitive layer with good light resistance.
[0049] That is, the photoreceptor of the present invention is characterized in that the laminated photosensitive layer provided on the substrate and containing specific oxytitanium phthalocyanine as a charge generating material has a specific spectral absorption spectrum.
[0050] First, oxytitanium phthalocyanine and a laminated photosensitive layer (hereinafter also referred to as a “photosensitive layer”) are described, and then a photoreceptor and an image forming apparatus including the photoreceptor are described.
[0051] <Oxytitanium phthalocyanine>
[0052] In the present invention, oxytitanium phthalocyanine used as a charge generating material has at least diffraction peaks at Bragg angles (2θ±0.2°) of 7.3°, 9.4°, 11.6°, 24.2°, and 27.3° in an X-ray diffraction spectrum using CuKα rays.
[0053] This oxytitanium phthalocyanine is represented by the following formula (A).
[0054] [Chemistry 1]
[0055]
[0056] Oxytitanium phthalocyanine represented by formula (A) can be produced by a known synthesis method described in, for example, Japanese Patent Application Laid-Open Nos. 6-293769, 2003-18534, and 7-271073, and "Phthalocyanine Compound" by Frank H. Moser and Arthur L. Thomas, Reinhold Publishing Corporation (New York), 1963.
[0057] The known synthesis methods may use titanium halides as starting materials or not, but the present inventors have confirmed that the excellent effects of the present invention can be obtained regardless of the starting materials and the method of synthesis, as long as the oxytitanium phthalocyanine has the above-mentioned X-ray diffraction spectrum characteristics. However, as described later, halogens such as chlorine contained in oxytitanium phthalocyanine may have an adverse effect on the charging performance of the photoreceptor, and oxytitanium phthalocyanine is preferably derived from a raw material that does not contain halogens such as chlorine.
[0058] The synthesis method is exemplified below. However, the following synthesis route is only an example and is not limited thereto.
[0059] Phthalonitrile and titanium alkoxide such as tetrabutoxytitanium are reacted in the presence of urea at a temperature of 150°C while stirring for at least 5 hours. After the reaction is completed, the generated oxytitanium phthalocyanine is filtered out. The obtained product is washed with solvents such as alcohols such as methanol, ethanol, n-propanol, butanol; chlorinated hydrocarbons such as dichloroethane and chloroform; ethers such as dimethyl ether, diethyl ether, tetrahydrofuran; ketones such as acetone and methyl ethyl ketone to obtain oxytitanium phthalocyanine. Since oxytitanium phthalocyanine is insoluble in these solvents, impurities attached to oxytitanium phthalocyanine are dissolved, so by repeated washing, the residual impurities can be reduced to the limit.
[0060] Alternatively, phthalonitrile and titanium tetrachloride may be heated and melted or reacted in a suitable solvent such as α-chloronaphthalene to synthesize dichlorotitanium phthalocyanine, which is then hydrolyzed with an alkali or water to obtain oxytitanium phthalocyanine.
[0061] Furthermore, isoindoline and tetraalkoxide titanium such as tetrabutoxytitanium are reacted by heating in a suitable solvent such as N-methylpyrrolidone to obtain oxytitanium phthalocyanine. The oxytitanium phthalocyanine may contain a phthalocyanine derivative in which the hydrogen atoms of the benzene ring of the phthalocyanine derivative are substituted with substituents such as chlorine, fluorine, nitro, cyano and sulfone.
[0062] By treating the thus obtained oxytitanium phthalocyanine with a water-immiscible organic solvent such as ethylene dichloride in the presence of water, crystalline oxytitanium phthalocyanine used as a charge generating material in the present invention can be obtained.
[0063] Examples of the treatment method (crystal conversion method) include a method of swelling oxytitanium phthalocyanine in water and treating it with an organic solvent, and a method of adding water to an organic solvent without swelling treatment and then throwing oxytitanium phthalocyanine powder therein.
[0064] As a method for swelling oxytitanium phthalocyanine in water, for example, oxytitanium phthalocyanine is dissolved in 10 to 30 times concentrated sulfuric acid, and when insoluble matter appears, it is removed by filtration, etc., and precipitated in cooled water. Then, the obtained oxytitanium phthalocyanine is filtered with ion exchange water, etc. to remove the acid, and the washing operation is repeated until it becomes neutral to obtain a wet cake (also called "wet paste").
[0065] When oxytitanium phthalocyanine is swollen in water, a known stirring and dispersing device such as a homomixer, a paint mixer, a ball mill, or a sand mill can be used.
[0066] In this way, amorphous oxytitanium phthalocyanine (low-crystalline oxytitanium phthalocyanine) can be converted into oxytitanium phthalocyanine crystals having a specific diffraction peak.
[0067] More specifically, the method for crystal conversion of oxytitanium phthalocyanine will be described.
[0068] Specifically, the target crystal form can be obtained by mixing and stirring the wet cake-like amorphous oxytitanium phthalocyanine (low-crystalline titanyl phthalocyanine) in the presence of water and an organic solvent without drying.
[0069] The organic solvent used here may be tetrahydrofuran alone, as long as the desired crystal form can be obtained, or it may be a mixed solvent selected from toluene, dichloromethane, carbon disulfide, o-dichlorobenzene and 1,1,2-trichloroethane.
[0070] Furthermore, the oxytitanium phthalocyanine of the present invention can also be obtained by grinding the amorphous oxytitanium phthalocyanine as a wet cake with sufficient stirring time or with mechanical strain.
[0071] As the apparatus for this treatment, in addition to a general stirring apparatus, a homogenizer, a dispersing mixer, a disperser, a stirrer, a ball mill, a sand mill, an attritor, an ultrasonic dispersing apparatus, etc. can also be listed. After the treatment, filtering is performed by a known method, and washing and separation are performed using methanol, ethanol or water, etc.
[0072] In the present invention, oxytitanium phthalocyanine used as the charge generating material preferably has an average particle size D (50%) of 0.15 to 0.3 μm.
[0073] For example, when dispersing the coating liquid for forming the charge generating layer described later, oxytitanium phthalocyanine is crushed (crushed), and when its average particle size is less than 0.15 μm, the generation efficiency of the carrier is reduced, and the sensitivity of the photoreceptor tends to deteriorate. In addition, since the occupancy ratio of the dye during dispersion is too high, coating defects are likely to occur during film formation, and it is difficult to generate stable charges during long-term use. On the other hand, if the average particle size exceeds 0.3 μm, the particle size distribution tends to deteriorate during long-term storage, and coating defects are likely to occur during film formation of the charge generating layer.
[0074] A more preferred average particle size of oxytitanium phthalocyanine is 0.18 to 0.28 μm.
[0075] The method for measuring the average particle size is described in detail in Examples.
[0076] <Photosensitive layer>
[0077] The photosensitive layer of the photoreceptor of the present invention has a maximum absorption (λ max ), and the absorbance at a wavelength of 780 nm (Abs 780nm ) and the absorbance at 860 nm (Abs 860nm ) ratio Abs 860nm / Abs 780nm It is 0.6 or more and 1.2 or less.
[0078] When the maximum absorption (λmax) is less than 800nm, the light resistance and the charge reduction due to repeated use may deteriorate. On the other hand, even if the maximum absorption (λmax) exceeds 850nm, the light resistance may be reduced, so it is best to fall within the prescribed range of the present invention.
[0079] The preferred wavelength of maximum absorption is 800 to 830 nm.
[0080] In addition, if the absorbance ratio is less than 0.6, the light resistance is particularly poor, and it is necessary to introduce an ultraviolet absorber into the charge transport layer (CTL). It is believed that this is because the maximum absorption (λmax) deviates to a low wavelength, the absorbance ratio becomes smaller, and thus the interaction between the oxytitanium phthalocyanines is weakened. In addition, when exposed to strong external light, the residual carriers generated in the charge generation layer when exposed to repeated electrical fatigue will not be deactivated and remain. On the contrary, if the absorbance ratio exceeds 1.2, the maximum absorption (λmax) shifts to a low wavelength, and the repeated VL (surface potential) rise will become larger.
[0081] The absorbance ratio is preferably 0.75 or more and 1 or less.
[0082] The spectral absorption spectrum (absorbance) of the photosensitive layer can be controlled by adjusting the synthesis of the charge generating material and the dispensing conditions (dispersion method, dispersion time, medium diameter, medium amount, medium material) during dispersion of the charge generating layer forming coating liquid.
[0083] In the synthesis path of the charge generating material, it is important to reduce impurities as much as possible. For example, it is important to make the washing state of the deacidification process closer to pH 7.0 and reduce the sulfate ion concentration. When impurities remain in this process, it is difficult to adjust the maximum absorption (λmax) of the absorption spectrum to the long wavelength side. Due to the presence of impurities, the crystal structure becomes weak in interaction between phthalocyanines, which is important for maintaining stable electrical properties during long-term use.
[0084] In addition, the residual amount of impurities can be reduced by selecting the crystallization conditions and the crystallization solvent in the crystallization process of oxytitanium phthalocyanine. The crystallization solvent can strengthen the cleaning of impurities by adding toluene, but by adding a high boiling point solvent, the residual solvent in the crystal increases, which sometimes affects its characteristics. It is preferred to suppress impurities in the synthesis process and reduce residual solvent.
[0085] On the other hand, it is also possible to make adjustments based on the distributed allocation conditions.
[0086] The distribution is carried out using a pulverizing device with a spherical medium having a medium diameter of 0.1 to 3.0 mm, preferably 0.1 to 2.0 mm. When the medium diameter is greater than 2.0 mm, there is a tendency for the pulverizing efficiency to decrease. Therefore, the maximum absorption (λmax) cannot be adjusted within the prescribed range of the present invention, or the proportion of phthalocyanine is too large due to the extension of the dispersion time, which will not cause the disadvantages such as deterioration of characteristics, reduction of particle size, and the main cause of agglomerate formation.
[0087] In addition, the pulverization efficiency also changes due to the material of the medium, and the optimal conditions are affected by the phthalocyanine dye, so it is necessary to select the optimal dispersion conditions according to various materials. As long as the maximum absorption wavelength is within the specified range of the present invention, the adjustment from the synthesis process, the adjustment from the distribution conditions, etc. are not particularly limited, and the effect recorded in the present invention can be maintained.
[0088] <Electrophotographic Photoreceptor>
[0089] The photoreceptor of the present invention comprises at least a laminated photosensitive layer in which a charge generating layer containing a charge generating material and a charge transporting layer containing a charge transporting material are laminated in this order on a substrate.
[0090] The photoreceptor of the present invention will be described below using drawings, but the present invention is not limited thereto.
[0091] Figure 2 This is a schematic cross-sectional view showing the structure of the main part of the photoreceptor (laminated type photoreceptor) F01 of the present invention.
[0092] The laminated photoreceptor F01 includes a photosensitive layer in which an undercoat layer F21, a charge generating layer F22 containing a charge generating material, and a charge transporting layer F23 containing a charge transporting material are sequentially laminated on a substrate F1. In the figure, Fa indicates the surface of the photoreceptor.
[0093] <Base F1>
[0094] The substrate (also referred to as "conductive substrate" or "conductive support") has a function as an electrode of the photoreceptor and a function as a supporting member, and its constituent material is not particularly limited as long as it is a material used in the relevant technical field.
[0095] Specifically, metal materials such as aluminum, aluminum alloys, copper, zinc, stainless steel, and titanium, as well as polymer materials such as polyethylene terephthalate, nylon, and polystyrene, hard paper, and glass, which have been subjected to metal foil lamination, metal vapor deposition treatment, or vapor deposition or coating of a conductive polymer, tin oxide, indium oxide, and other conductive compounds, on the surface, can be cited. Among them, aluminum is preferred from the perspective of ease of processing, and aluminum alloys of JIS3003 series, JIS5000 series, and JIS6000 series are particularly preferred.
[0096] The shape of the conductive support is not limited to Figure 3 The cylindrical shape (drum shape) shown in the figure may also be a sheet shape, a column shape, an annular belt shape, etc.
[0097] In addition, the surface of the conductive support may be subjected to diffuse reflection treatments such as anodizing treatment, surface treatment using chemicals or hot water, coloring treatment, or roughening of the surface to prevent interference fringes caused by the laser, as required, without affecting the image quality.
[0098] <Base coating F21>
[0099] The photoreceptor of the present invention preferably includes an undercoat layer (also referred to as an "intermediate layer") between the substrate and the laminated photosensitive layer.
[0100] Generally, the undercoat layer covers the unevenness of the surface of the substrate and makes it uniform, improves the film-forming property of the laminated photosensitive layer, inhibits the peeling of the photosensitive layer from the conductive support, and improves the adhesion between the substrate and the photosensitive layer. Specifically, it can prevent the injection of charges from the substrate into the photosensitive layer, prevent the chargeability of the photosensitive layer from being reduced, and prevent the image from being fogged (so-called blackening).
[0101] The undercoat layer can be formed, for example, by dissolving or dispersing a binder resin in an appropriate solvent to prepare an undercoat layer coating liquid, applying the coating liquid to the surface of the substrate, and removing the organic solvent by drying.
[0102] Examples of the binder resin include acetal resins, polyamide resins, polyurethane resins, polyester resins, acrylic resins, epoxy resins, phenolic resins, melanin resins, polyurethane resins, etc. The binder resin is required to have the following properties: no dissolution or swelling in the solvent used when forming the photosensitive layer on the undercoat layer; excellent adhesion to the conductive support; flexibility, etc. Therefore, among the above-mentioned binder resins, polyamide resins are preferred, and polyamide resins containing alcohol-soluble nylon resins and piperazine compounds are particularly preferred.
[0103] Examples of the alcohol-soluble nylon resin include homopolymerized or copolymerized nylons such as nylon 6, nylon 66, nylon 610, nylon 11, and nylon 12, and chemically modified nylons such as N-alkoxymethyl-modified nylon.
[0104] Furthermore, a curing agent that crosslinks the binder resin may be used to form a cured film. As the curing agent, blocked isocyanate is preferred from the viewpoint of storage stability and electrical properties of the coating liquid.
[0105] Examples of the solvent include lower alcohols such as water, methanol, ethanol, n-propanol, isopropanol, n-butanol, 2-butanol, and isobutanol; ketones such as acetone, cyclohexanone, and 2-butanone; ethers such as tetrahydrofuran, dioxane, ethylene glycol, and diethyl ether; and halogenated hydrocarbons such as dichloromethane and vinyl chloride. These solvents can be selected from the solubility of the binder resin, the surface smoothness of the primer layer, and used alone or in combination of two or more.
[0106] Among these solvents, non-halogen organic solvents can also be preferably used in consideration of the global environment.
[0107] The coating liquid for forming the undercoat layer may contain metal oxide particles. The metal oxide particles can easily adjust the volume resistance value of the undercoat layer, can further suppress the injection of charges into the charge generating layer, and can maintain the electrical characteristics of the photoreceptor under various environments.
[0108] Examples of materials that can be used for the metal oxide particles include titanium oxide, aluminum oxide, aluminum hydroxide, and tin oxide.
[0109] The ratio (A / B) of the total mass A of the binder resin and the metal oxide particles to the mass B of the solvent in the undercoat layer-forming coating liquid is, for example, preferably about 1 / 99 to 30 / 70, particularly preferably about 2 / 98 to 40 / 60.
[0110] The ratio (C / D) of the mass C of the binder resin to the mass D of the metal oxide particles is, for example, preferably about 90 / 10 to 1 / 99, particularly preferably about 70 / 30 to 5 / 95.
[0111] The coating method of the undercoat layer coating liquid may be appropriately selected in consideration of the physical properties of the coating liquid, productivity, etc., and examples thereof include spray coating, bar coating, roll coating, knife coating, ring coating, and dip coating.
[0112] Among them, the dip coating method is to dip the substrate into a coating tank filled with a coating liquid and then lift it up at a constant speed or a gradually changing speed, so that a layer is formed on the surface of the substrate. The method is relatively simple and has advantages in productivity and cost, so it can be applied to the manufacture of photoreceptors. In the device used for the dip coating method, a coating liquid dispersing device represented by an ultrasonic generating device can also be provided in order to stabilize the dispersibility of the coating liquid.
[0113] The solvent in the coating film may be removed by natural drying or by forced removal of the solvent in the coating film by heating.
[0114] The temperature in such a drying step is not particularly limited as long as it is a temperature at which the used solvent can be removed, but is preferably about 50 to 140°C, and particularly preferably about 80 to 130°C.
[0115] When the drying temperature is lower than 50°C, the drying time becomes longer and the solvent may not evaporate sufficiently and remain in the photoreceptor layer. In addition, when the drying temperature exceeds about 140°C, the electrical properties of the photoreceptor deteriorate during repeated use and the obtained image may deteriorate.
[0116] Such temperature conditions are commonly used not only in the undercoat layer but also in the layer formation or other processing of the photosensitive layer described later.
[0117] The film thickness of the primer layer is not particularly limited, but is preferably 0.01 to 20 μm, more preferably 0.05 to 10 μm.
[0118] When the thickness of the primer layer is less than 0.01 μm, sometimes it is impossible to obtain sufficient effect of the blocking property of electron injection from the conductive substrate side and the countermeasure against interference fringes caused by light scattering. On the other hand, if the thickness of the primer layer exceeds 20 μm, the sensitivity change during continuous printing becomes large, and then the change of image density becomes large.
[0119] <Charge Generation Layer F22>
[0120] The charge generating layer in an electronic photographic device such as an image forming device has the function of generating charges by absorbing light irradiated from a light emitting device such as a semiconductor laser beam. It has a charge generating substance as a main component and may contain a binder resin or an additive as needed.
[0121] As the charge generating material, the above-mentioned oxytitanium phthalocyanine is used. Other charge generating materials known in the technical field can be used in combination within the range where the effect is not hindered. Since the properties of the photosensitive body of the present invention are improved in accordance with the content of oxytitanium phthalocyanine, the higher the content, the better, and it is preferred to contain at least 80%.
[0122] As a method for forming the charge generating layer, a method is preferably used in which a charge generating material is dispersed in a binder resin solution obtained by mixing a binder resin with a solvent by a conventionally known method, and the charge generating layer coating solution is applied onto the undercoat layer. This method is described below.
[0123] As other charge generating materials, there can be listed other metal phthalocyanines such as α-type, β-type, Y-type, amorphous oxytitanium phthalocyanine or gallium that are different from the above-mentioned oxytitanium phthalocyanine in crystal form, azo dyes such as monoazo dyes, disazo dyes and triazo dyes, indigo dyes such as indigo and thioindigo, perylene dyes such as perylene imide and perylene anhydride, polycyclic quinone dyes such as anthraquinone and pyrenequinone, metal phthalocyanines such as oxytitanium phthalocyanine and phthalocyanine dyes such as metal-free phthalocyanine, organic conductive materials such as squarylium pigments, pyrylium salts, thiopyrylium salts, triphenylmethane pigments, and inorganic photoconductive materials such as selenium and amorphous silicon, and the like. Materials with appropriate exposure sensitivity can be appropriately selected and used.
[0124] The binder resin is not particularly limited, and any binder resin used in the technical field and exemplified in the above-mentioned undercoat layer may be used. A binder resin having excellent compatibility with the charge generating material is preferred.
[0125] Specifically, polyester, polystyrene, polyurethane, phenolic resin, alkyd resin, melamine resin, epoxy resin, silicone resin, acrylic resin, methacrylic resin, polycarbonate, polyarylate, phenoxy resin, polyvinyl butyral (PVB), polyvinyl formal, and copolymer resins containing two or more repeating units of the repeating units constituting these resins, etc. can be cited. As copolymer resins, insulating resins such as vinyl chloride-vinyl acetate copolymer resins, vinyl chloride-vinyl acetate-maleic anhydride copolymer resins, and acrylonitrile-styrene copolymer resins, etc. can be cited. These binder resins can be used alone or in combination of two or more.
[0126] In the present invention, it is preferred that the binder resin is a resin obtained by an acetalization reaction of two or more aldehydes and polyvinyl alcohol, and has a weight average molecular weight of 60,000 to 200,000.
[0127] If the weight average molecular weight is less than 60,000, the dispersibility of the oxytitanium phthalocyanine of the present invention will be poor, and poor film forming properties will occur, and dispersion stability during long-term storage will be problematic. On the other hand, if the weight average molecular weight exceeds 200,000, the viscosity of the dispersion coating solution will increase, and the crystal system of the oxytitanium phthalocyanine will collapse.
[0128] A more preferred range of the weight average molecular weight is 80,000 or more and 120,000 or less.
[0129] The weight average molecular weight can be measured by a known method.
[0130] Examples of the solvent include halogenated hydrocarbons such as dichloromethane and dichloroethane; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; ethers such as tetrahydrofuran (THF) and dioxane; alkyl ethers of ethylene glycol such as 1,2-dimethoxyethane; aromatic hydrocarbons such as benzene, toluene, and xylene; aprotic polar solvents such as N,N-dimethylformamide and N,N-dimethylacetamide, etc. These solvents may be used alone or in combination of two or more.
[0131] Among these solvents, non-halogen organic solvents can also be preferably used in consideration of the global environment.
[0132] As with the primer layer, a disperser such as a paint stirrer, a ball mill, and a sand mill may be used to dissolve or disperse the charge generating material in the binder resin solution. In this case, it is preferred that the dispersion conditions are appropriately set so that impurities generated from the container and the components constituting the disperser due to wear and tear, etc., are not mixed into the coating solution.
[0133] The ratio (E / F) of the mass E of the charge generating material to the mass F of the binder resin is preferably, for example, approximately 80 / 20 to 55 / 45.
[0134] If the ratio (E / F) exceeds 80 / 20, that is, the mass E of the charge generating material becomes large, the charge generating material becomes excessive and the dispersion stability in the binder resin becomes poor. On the other hand, if the ratio (E / F) is less than 55 / 45, that is, the mass E of the charge generating material becomes small, the charge generating efficiency decreases and the sensitivity deteriorates.
[0135] A more preferable ratio is about 60 / 40 to 70 / 30.
[0136] The film thickness of the charge generating layer is not particularly limited, but is preferably 0.05 to 5 μm, and more preferably 0.1 to 1 μm.
[0137] When the thickness of the charge generating layer is less than 0.05 μm, the efficiency of light absorption decreases, and the sensitivity of the photoreceptor decreases. On the other hand, when the thickness of the charge generating layer exceeds 5 μm, the charge movement inside the charge generating layer becomes the rate-limiting stage of the process of eliminating the charge on the surface of the photosensitive layer, and the sensitivity of the photoreceptor decreases.
[0138] <Charge Transport Layer F23>
[0139] The charge transport layer has a surface that receives the charge generated by the charge generating material and transports it to the photoreceptor. Figure 2 The Fa) function contains a charge transport material and a binder resin, and contains additives as needed.
[0140] The charge transport material is not particularly limited, and any compound used in the technical field may be used.
[0141] Specifically, carbazole derivatives, pyrene derivatives, oxazole derivatives, oxadiazole derivatives, thiazole derivatives, thiadiazole derivatives, triazole derivatives, imidazole derivatives, imidazolinone derivatives, imidazoline derivatives, bisimidazoline derivatives, styryl compounds, hydrazone compounds, polycyclic aromatic compounds, indole derivatives, pyrazoline derivatives, oxazolinone derivatives, benzimidazole derivatives, quinazoline derivatives, benzofuran derivatives, acridine derivatives, phenazine derivatives, aminostilbene derivatives, triarylamine derivatives, phenylenediamine derivatives, stilbene derivatives, diphenylamine derivatives, dibenzoxazine derivatives, polymers having groups derived from these compounds on the main chain or side chain (poly-N-vinylcarbazole, poly-1-vinylpyrene, ethylcarbazole-formaldehyde resin, triphenylmethane polymer, poly-9-vinylanthracene polymer), polysilane, etc. These charge transport materials can be used alone or in combination of two or more.
[0142] Among these charge transport materials, the trienamine dimer compound represented by the general formula (1) and the stilbene derivative represented by the general formula (2) described below are particularly preferred.
[0143] The trienamine dimer compound is represented by the general formula (1):
[0144] [Chemistry 2]
[0145]
[0146] In the formula, Ar1 and Ar2 are the same or different, alkynyl groups which may have substituents or divalent groups derived from heterocyclic rings which may have substituents, Ar3 and Ar4 are the same or different, aryl groups which may have substituents or heterocyclic rings which may have substituents, R1 and R2 are the same or different, and are alkyl groups, m and n are integers of 1 to 4, a and b are the same or different, and are hydrogen atoms, halogen atoms, alkyl groups, fluoroalkyl groups, alkoxy groups or amino groups which may have substituents, and when m or n is 2 or more, two a or b bonded to adjacent positions are combined to form a methylenedioxy group, an ethylenedioxy group, a tetramethylene group or a butadienyl group.
[0147] Examples of the trienamine dimer compound of the general formula (1) include compounds described in Japanese Patent No. 4604083, and the compound can be synthesized by the method described in the patent publication.
[0148] Specifically, the trienamine dimer compound (trienamine-based compound) of the structural formula (a) used in the examples, in which Ar1 and Ar2 are p-phenylene, Ar3 and Ar4 are phenyl, R1 and R2 are hydrogen atoms, a and b are methyl groups, and the atomic numbers n and m are 1, can be cited.
[0149] The stilbene derivatives are represented by the general formula (2):
[0150] [Chemistry 3]
[0151]
[0152] In the formula, R 1 , R 2 , R 5 and R 6 are the same or different and are alkyl, alkoxy, aryl, aralkyl or halogen atoms, m, n, p and q are the same or different and are integers of 0 to 3, wherein R 1 and R 2 When they are the same group, m and n are different integers. 5 and R 6 When they are the same group, p and q are different integers, and R 3 and R 4 The same or different are a hydrogen atom or an alkyl group.
[0153] Examples of the stilbene derivatives of the general formula (2) include compounds described in Japanese Patent No. 3272257, and can be synthesized by the method described in the publication.
[0154] Specifically, R used in the examples can be cited. 1 , R 2 , R 5 and R 6 Methyl, R 3 and R 4 A stilbene derivative (stilbene compound) of the structural formula (b) wherein the atom is a hydrogen atom, the atomic numbers n and p are 1, and the atomic numbers m and q are 1.
[0155] For the substituent R of the general formula (2) 1 , R 2 , R 5 and R 6 Provide explanation.
[0156] Examples of the alkyl group include alkyl groups having 1 to 6 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, and n-hexyl.
[0157] Examples of the alkoxy group include alkoxy groups having 1 to 6 carbon atoms, such as a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, a tert-butoxy group, an n-pentyloxy group, and an n-hexyloxy group.
[0158] Examples of the aryl group include phenyl groups, naphthyl groups, anthryl groups, phenanthryl groups, fluorenyl groups, biphenyl groups, and o-terphenyl groups.
[0159] Examples of the aralkyl group include benzyl, phenethyl, diphenylmethyl, triphenylmethyl and other aralkyl groups.
[0160] Examples of the halogen atom include fluorine, chlorine, bromine, and iodine.
[0161] Substituent R 1 , R 2 , R 5 and R 6 When the number of atoms m, n, p and q is 2 or more, the substituents may be different from each other. For example, the substituent R 1 When the number of atoms m is 2, the same benzene ring may be substituted with different groups such as methyl and ethyl, or methyl and ethoxy.
[0162] As a substituent R of the general formula (1) 3 and R 4 Examples of the alkyl group include alkyl groups having 1 to 3 carbon atoms, such as methyl group, ethyl group, n-propyl group, isopropyl group, and the like.
[0163] As a method for forming the charge transport layer, it is preferred to disperse the charge transport material in a binder resin solution obtained by mixing a binder resin in a solvent by a conventionally known method, and then apply the charge transport layer coating solution on the charge generating layer. This method is described below.
[0164] The binder resin is not particularly limited, and any resin having adhesive properties used in the technical field can be used. A resin having excellent compatibility with the charge transporting material is preferred.
[0165] Specifically, there can be mentioned vinyl polymer resins such as polymethyl methacrylate, polystyrene, and polyvinyl chloride, and their copolymer resins, and resins such as polycarbonate, polyester, polyester carbonate, polysulfone, phenoxy resin, epoxy resin, silicone resin, polyarylate, polyamide, polyether, polyurethane, polyacrylamide, phenolic resin, and polyphenylene ether, and thermosetting resins formed by partially crosslinking these resins, etc. These binder resins can be used alone or in combination of two or more.
[0166] Among them, the volume resistance value of polystyrene, polycarbonate, polyarylate and polyphenylene ether is 10 13 Ω or more, and has excellent electrical insulation, film forming properties, potential characteristics, etc., and is therefore preferred, and polycarbonate is particularly preferred.
[0167] Examples of the solvent include aromatic hydrocarbons such as benzene, toluene, xylene, and monochlorobenzene; halogenated hydrocarbons such as dichloromethane and dichloroethane; ethers such as tetrahydrofuran, dioxane, and dimethoxymethyl ether; and aprotic polar solvents such as N,N-dimethylformamide. In addition, a solvent such as alcohol, acetonitrile, or methyl ethyl ketone may be further added as needed. These solvents may be used alone or in combination of two or more.
[0168] Among these solvents, non-halogen organic solvents can also be preferably used in consideration of the global environment.
[0169] The charge transport layer may contain additives within a range not hindering the effects of the present invention.
[0170] Examples of the additive include ultraviolet absorbers for improving light resistance, and specific examples include perinone dyes used in Examples.
[0171] However, adding an additive to the charge transport layer forms a trap for charge transport and adversely affects the properties of the photoreceptor. The amount of additive added is about 1 to 10 parts by mass based on the charge transport material.
[0172] The ratio (G / H) of the mass G of the charge transport material to the mass H of the binder resin is preferably, for example, approximately 10 / 12 to 10 / 30.
[0173] The film thickness of the charge transport layer is not particularly limited, but is preferably about 5 to 50 μm, more preferably about 10 to 40 μm.
[0174] If the film thickness of the charge transport layer is less than 5 μm, the charge retention capability of the photoreceptor surface is reduced. On the other hand, if the film thickness of the charge transport layer exceeds 50 μm, the resolution of the photoreceptor is reduced.
[0175] (2) Image Forming Apparatus 100
[0176] The image forming device of the present invention includes at least: the photosensitive body of the present invention; a charging unit for charging the photosensitive body; an exposure unit for exposing the charged photosensitive body to form an electrostatic latent image; a developing unit for developing the electrostatic latent image formed by exposure to form a colorant image (visualization); a transfer unit for transferring the colorant image formed by development to a recording medium; a fixing unit for fixing the transferred colorant image on the recording medium to form an image; a cleaning unit for removing and recovering the colorant remaining on the photosensitive body; and a de-staticizing unit for de-staticizing the surface charge remaining on the photosensitive body.
[0177] Hereinafter, the image forming apparatus and its operation according to the present invention will be described based on the drawings, but the present invention is not limited to the following description.
[0178] Figure 3 It is a schematic side view showing the configuration of a main part of the image forming apparatus 100 of the present invention.
[0179] Figure 3 The image forming device (laser printer) 100 includes a photosensitive body 1 (equivalent to Figure 2 The image forming apparatus comprises an image forming unit (F01), an exposure unit (semiconductor laser) 31, a charging unit (charger) 32, a developing unit (developer) 33, a transfer unit (transfer charger) 34, a conveying belt (not shown), a fixing unit (fixer) 35, and a cleaning unit (cleaner) 36. Reference numeral 51 indicates a recording medium (recording paper or transfer paper).
[0180] The photoreceptor 1 is rotatably supported by the main body of the image forming apparatus 100, and is driven by a driving unit (not shown) to rotate around a rotation axis 44 in the direction of arrow 41. The driving unit is composed of, for example, a motor and a reduction gear, and transmits its driving force to a conductive support body constituting the core of the photoreceptor 1, thereby driving the photoreceptor 1 to rotate at a predetermined peripheral speed. The charging unit (charger) 32, the exposure unit 31, the developing unit (developer) 33, the transfer unit (transfer charger) 34, and the cleaning unit (cleaner) 36 are arranged in this order along the outer peripheral surface of the photoreceptor 1 from the upstream side to the downstream side of the rotation direction of the photoreceptor 1 indicated by the arrow mark 41.
[0181] The charger 32 is a device for charging the outer peripheral surface (equivalent to Figure 2 The photosensitive member F01 is charged uniformly at a predetermined potential by a charging unit. Examples of the charging unit include a non-contact charging method such as a corona charging method of a charging charger and a contact charging method such as a charging roller or a charging brush.
[0182] The exposure unit 31 includes a semiconductor laser as a light source, and exposes the outer peripheral surface of the charged photoreceptor 1 corresponding to the image information by irradiating the laser beam output from the light source to the surface of the photoreceptor 1 between the charger 32 and the developer 33. The light is repeatedly scanned along the extension direction of the rotation axis 44 of the photoreceptor 1 as the main scanning direction, so that an image is formed and an electrostatic latent image is sequentially formed on the surface of the photoreceptor 1. That is, the charge amount of the photoreceptor 1 uniformly charged by the charger 32 is different due to the irradiation and non-irradiation of the laser beam, thereby forming an electrostatic latent image.
[0183] The developer 33 is a developing unit that develops the electrostatic latent image formed on the surface of the photosensitive body 1 by exposure using a developer (colorant), and comprises: a developing roller 33a, which is arranged to face the photosensitive body 1 and supplies colorant to the outer peripheral surface of the photosensitive body 1; and a housing 33b, which supports the developing roller 33a so that it can rotate around a rotation axis parallel to the rotation axis 44 of the photosensitive body 1 and contains a developer containing colorant in its internal space.
[0184] The transfer charger 34 is a transfer unit that transfers the toner image formed as a visible image on the outer peripheral surface of the photoreceptor 1 by development, through a transport unit (not shown), from the direction of arrow 42 to the transfer paper 51, which is a recording medium provided between the photoreceptor 1 and the transfer charger 34. The transfer charger 34 is, for example, a contact transfer unit, which includes a charging unit, and transfers the toner image to the transfer paper 51 by providing a charge having a polarity opposite to that of the toner to the transfer paper 51.
[0185] The cleaner 36 is a cleaning unit that removes and recovers the toner remaining on the outer peripheral surface of the photoreceptor 1 after the transfer operation performed by the transfer charger 34, and the cleaner 36 includes a cleaning blade 36a that peels off the toner remaining on the outer peripheral surface of the photoreceptor 1, and a recovery housing 36b that contains the toner peeled off by the cleaning blade 36a. In addition, the cleaner 36 is provided together with a de-static lamp (not shown).
[0186] In addition, in the image forming apparatus 100, a fixing device 35 is provided on the downstream side of the transfer paper 51 passing between the photosensitive body 1 and the transfer charger 34. The fixing device 35 is a fixing unit that fixes the transferred image. The fixing device 35 includes a heating roller 35a having a heating unit (not shown) and a pressure roller 35b that is disposed opposite to the pressure roller 35a and is pressed against the heating roller 35a to form a contact portion.
[0187] Reference numeral 37 denotes a separation unit for separating the transfer paper from the photosensitive body, and reference numeral 38 denotes a housing for housing the above-mentioned units of the image forming apparatus.
[0188] The image forming operation by the image forming apparatus 100 is performed as follows.
[0189] First, when the photoreceptor 1 is driven to rotate in the direction of arrow 41 by the driving unit, the surface of the photoreceptor 1 is uniformly charged to a predetermined positive potential by the charger 32 arranged upstream of the imaging point of the light from the exposure unit 31 in the rotation direction of the photoreceptor 1.
[0190] Next, light corresponding to image information is irradiated from exposure unit 31 onto the surface of photoreceptor 1. The surface charge of the irradiated portion of photoreceptor 1 is removed by the exposure, and a difference is created between the surface potential of the irradiated portion and the surface potential of the non-irradiated portion, thereby forming an electrostatic latent image.
[0191] The developer 33 is provided downstream of the light imaging point of the exposure unit 31 in the rotation direction of the photoreceptor 1 , and toner is supplied to the surface of the photoreceptor 1 on which the electrostatic latent image is formed, to develop the electrostatic latent image and form a toner image.
[0192] In synchronization with the exposure of the photoreceptor 1, the transfer paper 51 is fed between the photoreceptor 1 and the transfer charger 34. The transfer charger 34 provides the fed transfer paper 51 with charges of opposite polarity to the toner, and the toner image formed on the surface of the photoreceptor 1 is transferred onto the transfer paper 51.
[0193] The transfer paper 51 to which the toner image is transferred is conveyed to the fixing device 35 by the conveying unit, and is heated and pressed when passing through the contact portion between the heating roller 35a and the pressure roller 35b of the fixing device 35, so that the toner image is fixed to the transfer paper 51 to form a stable image. The transfer paper 51 to which the image is formed is discharged to the outside of the image forming apparatus 100 by the conveying unit.
[0194] On the other hand, after the transfer charger 34 transfers the toner image, the toner remaining on the surface of the photoreceptor 1 is peeled off and recovered from the surface of the photoreceptor 1 by the cleaner 36. The charge on the surface of the photoreceptor 1 from which the toner is removed is removed by the light from the charge removal lamp, and the electrostatic latent image on the surface of the photoreceptor 1 disappears. Then, the photoreceptor 1 is further driven to rotate, and a series of actions starting from charging are repeated, thereby continuously forming an image.
[0195] The image forming apparatus 100 described above is a black-and-white image forming apparatus (printer), and may be, for example, a color image forming apparatus of an intermediate transfer method capable of forming a color image. Specifically, it may be a so-called tandem full-color image forming apparatus in which a plurality of electrophotographic photosensitive bodies each having a toner image formed thereon are arranged in parallel in a predetermined direction (for example, the horizontal direction H or the substantially horizontal direction H). In addition, the image forming apparatus 100 may also be another color image forming apparatus, a copier, a multifunction machine, or a facsimile machine.
[0196] [Example]
[0197] Hereinafter, the present invention will be specifically described by means of Production Examples, Comparative Production Examples, Examples, and Comparative Examples. However, the present invention is not limited to the following Examples unless it exceeds the gist of the present invention.
[0198] As described below, in Examples 1 to 6, 8 to 10 and Comparative Examples 1 to 6, the charge generating coating liquids prepared in Manufacturing Examples 1 to 6 and Comparative Manufacturing Examples 1 to 3 were prepared as charge generating materials, and the coating liquid for forming an undercoat layer, the coating liquid for forming a charge generating layer and the coating liquid for forming a charge transporting layer were sequentially coated on a substrate to prepare a coating film in which an undercoat layer F21, a charge generating layer F22 and a charge transporting layer F23 were sequentially stacked on a substrate F1. Figure 2 The laminated photoreceptor F01.
[0199] In Example 7, a laminated photoreceptor was prepared in the same manner as in Example 1 except that the undercoat layer F21 was not formed.
[0200] <Synthesis of Oxytitanium Phthalocyanine>
[0201] (Production Example 1)
[0202] 30 parts of 1,3-diiminoisoindoline and 210 parts of sulfolane were mixed, heated and stirred at 180°C under a nitrogen stream, and 21 parts of titanium tetrabutoxide were added dropwise. After the addition was completed, the mixture was kept at 180°C and stirred for 6 hours to react. After the reaction was completed, the mixture was cooled and filtered, and the powder of the obtained precipitate was washed with chloroform, then carefully washed with methanol, and then washed several times with hot water at 85°C, and then dried to obtain crude oxytitanium phthalocyanine.
[0203] 5 parts of the obtained crude oxytitanium phthalocyanine washed with hot water were stirred in 100 parts of sulfuric acid at 3 to 5°C, gradually dissolved, and filtered. When the reaction temperature exceeded 5°C, phthalocyanine might decompose, so the temperature was strictly controlled to be 5°C or less.
[0204] The obtained sulfuric acid solution was stirred in 3500 parts of ice water and dripped in small amounts at a time. During this period, the temperature of the ice water was always controlled below 5°C. The precipitated crystals were filtered and then repeatedly suspended and washed with a cleaning liquid to obtain a wet cake of the target oxytitanium phthalocyanine. The pH measurement result of the washing liquid, 6.8, confirmed that the deacidification washing was completed.
[0205] 150 parts of tetrahydrofuran were added to the obtained wet cake, and the mixture was stirred at 2200 rpm by a homogenizer at room temperature. After 1 hour, the mixture was immediately filtered under reduced pressure. The crystals obtained on the filter were washed with tetrahydrofuran to obtain 9 parts of tetrahydrofuran wet cake. The mixture was dried under reduced pressure (5 mmHg) and 70°C for two days to obtain 8 parts of oxytitanium phthalocyanine crystals. Furthermore, the obtained 3 g of oxytitanium phthalocyanine crystals were crystallized again by tetrahydrofuran and dried under reduced pressure to obtain the oxytitanium phthalocyanine crystals of Manufacturing Example 1.
[0206] As a charge generating material, 3 parts by mass of the obtained oxytitanium phthalocyanine and 2 parts by mass of polyvinyl butyral (PVB) resin (manufactured by Sekisui Chemical Co., Ltd., trade name: BX-1) as a binder resin were added to 32 parts by mass of cyclohexanone and 128 parts by mass of methyl ethyl ketone, and glass beads (manufactured by As-one Co., Ltd., trade name: BZ-1, bead diameter: 1 mm) were used as a medium. A paint mixer was used to perform a dispersion treatment for 0.5 hours to prepare 20 g of a coating liquid for forming a charge generating layer.
[0207] The X-ray diffraction spectrum of the dried product of the charge generating layer forming coating solution was measured under the following conditions using the following apparatus: The X-ray diffraction spectrum of the dried product of the coating solution corresponds to the X-ray diffraction spectrum of the contained oxytitanium phthalocyanine.
[0208] X-ray diffraction device: manufactured by Rigaku Corporation, model: ATX-G (for thin film structure evaluation)
[0209] X-ray source:
[0210] Voltage: 50kV
[0211] Current: 300mA
[0212] Start angle: 5.0 degrees
[0213] Stop angle: 30.0 degrees
[0214] Step angle: 0.02 degrees
[0215] Measuring time: 5 degrees / min
[0216] Measurement method: θ / 2θ scanning method
[0217] Figure 4 : is a graph showing the X-ray diffraction spectrum pattern of oxytitanium phthalocyanine in Production Example 1, from which it is confirmed that there are diffraction peaks at Bragg angles of 7.3°, 9.4°, 11.6°, 24.2°, and 27.3°. The X-ray diffraction spectrum pattern of oxytitanium phthalocyanine was measured similarly below.
[0218] The average particle size D (50%) of oxytitanium phthalocyanine in the obtained charge generating layer-forming coating liquid was measured using a laser diffraction particle size distribution measuring apparatus (manufactured by Nikkiso Co., Ltd. (currently Microtrac-BEL Co., Ltd.), model: Microtrac MT-3000II).
[0219] As a result, it was found that the average particle size D (50%) of oxytitanium phthalocyanine in Production Example 1 was 0.26 μm. The average particle size D (50%) of oxytitanium phthalocyanine was measured in the same manner below.
[0220] (Production Example 2)
[0221] 40 g of phthalonitrile, 18 g of titanium tetrachloride and 500 ml of α-chloronaphthalene were heated and stirred at 200-250° C. for 3 hours under a nitrogen atmosphere, cooled to 100-130° C., filtered while hot, and washed with 200 ml of α-chloronaphthalene heated to 100° C. to obtain a crude dichlorotitanium phthalocyanine product. The obtained crude product was washed with 200 ml of α-chloronaphthalene at room temperature and then with 200 ml of methanol, and then further suspended and washed in 500 ml of methanol for 5 times, and then washed several times with hot water, and then dried to obtain a crude oxytitanium phthalocyanine.
[0222] 5 parts of the obtained crude oxytitanium phthalocyanine washed with hot water were stirred in 100 parts of sulfuric acid at 3 to 5°C, gradually dissolved, and filtered. When the reaction temperature exceeded 5°C, phthalocyanine might decompose, so the temperature was strictly controlled to be below 5°C.
[0223] The obtained sulfuric acid solution was stirred in 3500 parts of ice water and dripped in small amounts at a time. During this period, the temperature of the ice water was always controlled below 5°C. The precipitated crystals were filtered and then repeatedly suspended and washed with a cleaning liquid to obtain a wet cake of the target oxytitanium phthalocyanine. The pH measurement result of the washing liquid, 6.9, confirmed that the deacidification washing was completed.
[0224] Tetrahydrofuran was added as a crystallization solvent to the obtained wet cake, and the mixture was stirred at 2200 rpm for 1 hour at room temperature by a homomixer, and then filtered. After washing with methanol, oxytitanium phthalocyanine was obtained. Furthermore, a second crystallization treatment was performed again using a mixed solvent of THF: toluene = 5:5, and the mixture was dried under reduced pressure to obtain the oxytitanium phthalocyanine crystal of Production Example 2.
[0225] A coating liquid for forming a charge generating layer of Production Example 2 was prepared in the same manner as in Production Example 1 except that the oxytitanium phthalocyanine crystal of Production Example 2 was used instead of the oxytitanium phthalocyanine crystal of Production Example 1.
[0226] The X-ray diffraction spectrum of the dried product of the charge generation layer-forming coating liquid obtained in the same manner as in Production Example 1 was measured, and it was confirmed that the spectrum had the diffraction peaks specified in the present invention.
[0227] (Production Example 3)
[0228] In Manufacturing Example 2, when preparing the coating liquid for forming a charge generating layer, 20 g of the coating liquid for forming a charge generating layer was prepared in the same manner as in Manufacturing Example 2, except that glass beads (manufactured by As-one Co., Ltd., trade name: BZ-01, bead diameter: 0.1 mm) were used as the dispersion medium and dispersed using a paint stirrer for 0.75 hours.
[0229] The X-ray diffraction spectrum of the dried product of the charge generation layer-forming coating liquid obtained in the same manner as in Production Example 1 was measured, and it was confirmed that the spectrum had the diffraction peaks specified in the present invention.
[0230] (Production Example 4)
[0231] In Production Example 1, 20 g of a charge generating layer forming coating liquid was prepared in the same manner as in Production Example 1 except that glass beads (manufactured by As-one Co., Ltd., trade name: BZ-01, bead diameter: 0.1 mm) were used for dispersion.
[0232] The X-ray diffraction spectrum of the dried product of the charge generation layer-forming coating liquid obtained in the same manner as in Production Example 1 was measured, and it was confirmed that the spectrum had the diffraction peaks specified in the present invention.
[0233] (Production Example 5)
[0234] In Manufacturing Example 2, when preparing the coating liquid for forming a charge generating layer, polyvinyl butyral (PVB) resin (manufactured by Sekisui Chemical Co., Ltd., trade name: BM-2) was used as the binder resin, and 20 g of the coating liquid for forming a charge generating layer was prepared in the same manner as in Manufacturing Example 2, except that the mixture was dispersed by a paint stirrer for 0.5 hours.
[0235] The X-ray diffraction spectrum of the dried product of the charge generation layer-forming coating liquid obtained in the same manner as in Production Example 1 was measured, and it was confirmed that the spectrum had the diffraction peaks specified in the present invention.
[0236] (Production Example 6)
[0237] In Manufacturing Example 1, when preparing the coating liquid for forming a charge generating layer, 20 g of the coating liquid for forming a charge generating layer was prepared in the same manner as in Manufacturing Example 1, except that glass beads (manufactured by As-one Co., Ltd., trade name: BZ-1, bead diameter: 0.1 mm) were used as the dispersion medium and dispersed using a paint stirrer for 0.75 hours.
[0238] The X-ray diffraction spectrum of the dried product of the charge generation layer-forming coating liquid obtained in the same manner as in Production Example 1 was measured, and it was confirmed that the spectrum had the diffraction peaks specified in the present invention.
[0239] (Comparative Manufacturing Example 1)
[0240] 40 g of phthalonitrile, 18 g of titanium tetrachloride and 500 ml of α-chloronaphthalene were heated and stirred at 200-250° C. for 3 hours under a nitrogen atmosphere, cooled to 100-130° C., filtered while hot, and washed with 200 ml of α-chloronaphthalene heated to 100° C. to obtain a crude dichlorotitanium phthalocyanine product. The obtained crude product was washed with 200 ml of α-chloronaphthalene at room temperature and then with 200 ml of methanol, and then further suspended and washed in 500 ml of methanol for 5 times, and then washed several times with hot water, and then dried to obtain a crude oxytitanium phthalocyanine.
[0241] 5 parts of the obtained crude oxytitanium phthalocyanine washed with hot water were stirred in 100 parts of sulfuric acid at 3 to 5°C, gradually dissolved, and filtered. When the reaction temperature exceeded 5°C, phthalocyanine might decompose, so the temperature was strictly controlled to be below 5°C.
[0242] The obtained sulfuric acid solution was stirred in 3500 parts of ice water and dripped in small amounts at a time. During this period, the temperature of the ice water was always controlled below 5°C. The precipitated crystals were filtered and then repeatedly suspended and washed with a cleaning liquid to obtain a wet cake of the target oxytitanium phthalocyanine. The pH measurement result of the washing liquid, 6.2, confirmed that the deacidification washing was completed.
[0243] Tetrahydrofuran was added as a crystallization solvent to the obtained wet cake, and the mixture was stirred at 2200 rpm for 1 hour at room temperature by a homomixer, and then filtered. After washing with methanol, oxytitanium phthalocyanine was obtained. Furthermore, a second crystallization treatment was performed again using a mixed solvent of THF: toluene = 9:1, and the mixture was dried under reduced pressure to obtain oxytitanium phthalocyanine crystals of Comparative Production Example 1.
[0244] A charge generating layer-forming coating liquid of Comparative Production Example 1 was prepared in the same manner as in Production Example 1 except that the oxytitanium phthalocyanine crystal of Comparative Production Example 1 was used instead of the oxytitanium phthalocyanine crystal of Production Example 1.
[0245] The X-ray diffraction spectrum of the dried product of the charge generation layer-forming coating liquid obtained in the same manner as in Production Example 1 was measured, and it was confirmed that the spectrum had the diffraction peaks specified in the present invention.
[0246] (Comparative Manufacturing Example 2)
[0247] In Comparative Production Example 1, 20 g of the charge generating layer forming coating liquid was prepared in the same manner as in Comparative Production Example 1 except that glass beads (manufactured by As-one Co., Ltd., trade name: BZ-1, bead diameter: 0.1 mm) were used for dispersion.
[0248] The X-ray diffraction spectrum of the dried product of the charge generation layer-forming coating liquid obtained in the same manner as in Production Example 1 was measured, and it was confirmed that the spectrum had the diffraction peaks specified in the present invention.
[0249] (Comparative Manufacturing Example 3)
[0250] In Manufacturing Example 5, when preparing the coating liquid for forming a charge generating layer, 20 g of the coating liquid for forming a charge generating layer was prepared in the same manner as in Manufacturing Example 5, except that glass beads (manufactured by As-one Co., Ltd., trade name: BZ-2, bead diameter: 0.2 mm) were used as the dispersion medium and dispersed using a paint stirrer for 1.0 hour.
[0251] The X-ray diffraction spectrum of the dried product of the charge generation layer-forming coating liquid obtained in the same manner as in Production Example 1 was measured, and it was confirmed that the spectrum had the diffraction peaks specified in the present invention.
[0252] (Example 1)
[0253] (Formation of Primer Layer)
[0254] 3 parts by mass of titanium oxide (manufactured by Showa Denko K.K., trade name: TS-043) and 2 parts by mass of copolyamide (nylon) (manufactured by Toray Industries, Ltd., trade name: CM8000) were added to 25 parts by mass of methanol, and dispersed for 8 hours using a paint stirrer (disperser) to prepare 3 kg of a coating liquid for forming a primer layer. Next, by a dip coating method, specifically, the obtained coating liquid was filled in a coating tank, and an aluminum drum-shaped substrate having a diameter of 30 mm and a length of 357 mm was immersed in the coating liquid, then pulled up and dried to form a primer layer having a film thickness of 1.0 μm.
[0255] (Formation of Charge Generation Layer)
[0256] In the same manner as the formation of the undercoat layer, the coating liquid for forming a charge generating layer obtained in Production Example 1 was applied to the surface of the undercoat layer by dip coating. Specifically, the coating tank was filled with the obtained coating liquid for forming a charge generating layer, and the drum-shaped substrate having the undercoat layer was immersed in the coating liquid, then lifted up and dried naturally to form a charge generating layer with a film thickness of 0.2 μm.
[0257] (Formation of Charge Transport Layer)
[0258] As a charge transport material, 10 parts by mass of a triphenylamine compound (TPD) represented by the following structural formula (a) (manufactured by Tokyo Chemical Industry Co., Ltd., trade name: D2448), [Chemical 4]
[0259]
[0260] 104 parts by mass of tetrahydrofuran were added to 20 parts by mass of Z-type polycarbonate (manufactured by Teijin Chemicals Ltd., trade name: TS2020) as a binder resin, and the mixture was stirred and mixed to prepare 3 kg of a coating liquid for forming a charge transport layer.
[0261] Next, the coating liquid for forming the charge transport layer is applied to the surface of the charge generating layer by dip coating in the same manner as the formation of the primer layer. Specifically, the coating liquid for forming the charge transport layer is filled in the coating tank, and the drum-shaped substrate on which the charge generating layer is formed is immersed in the coating liquid, then pulled up and dried at 130° C. for 1 hour to form a charge transport layer with a film thickness of 25 μm.
[0262] So, made Figure 2 The photoreceptor F1 is shown.
[0263] The photosensitive layer of the obtained photoreceptor was peeled off, and its light absorption spectrum was measured in the wavelength range of 400 to 900 nm using an ultraviolet visible spectrophotometer (UV-VIS SPECTROPHOTOMETER, model: UV-2450, manufactured by Shimadzu Corporation).
[0264] The obtained absorption spectrum is shown in Figure 1 .
[0265] According to the spectral absorption spectrum, the maximum absorption is at a wavelength of 833 nm, and when the minimum absorbance in the wavelengths of 400 to 800 nm is corrected as 0, the ratio of the absorbance at a wavelength of 780 nm to the absorbance at a wavelength of 860 nm is 0.99.
[0266] (Examples 2 to 6)
[0267] Photoreceptors F1 of Examples 2 to 6 were prepared in the same manner as in Example 1 except that the charge generating layer-forming coating liquids obtained in Production Examples 2 to 6 were used as the charge generating layer-forming coating liquids.
[0268] (Example 7)
[0269] A photoreceptor F1 of Example 7 was prepared in the same manner as in Example 1 except that no undercoat layer was formed on the aluminum drum-shaped substrate.
[0270] (Example 8)
[0271] Photoreceptor F1 of Example 8 was prepared in the same manner as in Example 4 except that 1 part by mass of an ultraviolet absorber (perinone dye, CIsolvent Orange, manufactured by Kiwa Chemical Industry Co., Ltd., product name: Orange HG) was added to the charge transport layer-forming coating liquid.
[0272] (Example 9)
[0273] As the charge transport material of the charge transport layer, in addition to using the following structural formula (b): [Chemical 5]
[0274]
[0275] Photoreceptor F1 of Example 9 was prepared in the same manner as in Example 2 except for the stilbene compound shown.
[0276] The compound represented by formula (b) was previously synthesized by the method described in Japanese Patent No. 3272257.
[0277] (Example 10)
[0278] As the charge transport material of the charge transport layer, in addition to using the following structural formula (c):
[0279] [Chemistry 6]
[0280]
[0281] Photoreceptor F1 of Example 10 was prepared in the same manner as in Example 2 except for the use of the butadiene-based compound (1,1-bis(p-diethylphenyl)-4,4-biphenyl-1,3-butadiene, manufactured by Takasago Chemical Co., Ltd., product name: T-405).
[0282] (Comparative Examples 1-2)
[0283] Photoreceptors F1 of Comparative Examples 1 and 2 were prepared in the same manner as in Example 1 except that the charge generating layer-forming coating liquids obtained in Comparative Production Examples 1 and 2 were used as the charge generating layer-forming coating liquids.
[0284] (Comparative Example 3)
[0285] Photoreceptor F1 of Comparative Example 3 was prepared in the same manner as in Comparative Example 1 except that 1 part by mass of an ultraviolet absorber (perinone dye, CIsolvent Orange, manufactured by Kiwa Chemical Industries, Ltd., product name: Orange HG) was added to the charge transport layer-forming coating liquid.
[0286] (Comparative Example 4)
[0287] Photoreceptor F1 of Comparative Example 4 was prepared in the same manner as in Comparative Example 1 except that 3 parts by mass of an ultraviolet absorber (perinone dye, CIsolventOrange, manufactured by Kiwa Chemical Industries, Ltd., product name: OrangeHG) was added to the charge transport layer-forming coating liquid.
[0288] (Comparative Example 5)
[0289] Photoreceptor F1 of Comparative Example 5 was prepared in the same manner as in Comparative Example 1 except that a butadiene compound represented by structural formula (c) (Takasago Chemical Industries, Ltd., product name: T-405) was used as the charge transport material of the charge transport layer.
[0290] (Comparative Example 6)
[0291] A photoreceptor F1 of Comparative Example 6 was prepared in the same manner as in Example 1 except that the charge generating layer forming coating liquid obtained in Comparative Production Example 3 was used as the charge generating layer forming coating liquid.
[0292] [evaluate]
[0293] The photoreceptors F01 prepared in Examples 1 to 10 and Comparative Examples 1 to 5 were evaluated in the following items using a test copying machine obtained by modifying a digital copying machine (manufactured by Sharp Corporation, trade name: MX-2600).
[0294] [Evaluation 1]
[0295] The photosensitive body (drum) to be evaluated was wrapped in light-shielding paper, a 10 mm x 30 mm window was opened on the light-shielding paper, and the image was exposed to a fluorescent lamp with an illumination of 400 Lux for 0.5 hours, and then half-tone printing was performed using a test copier. The images before and after light exposure were compared and evaluated together with the print results before light exposure.
[0296] The obtained results were visually judged according to the following criteria.
[0297] VG: Unable to confirm the impact on the image.
[0298] G: Only the ID (Image Density) of the exposed part increases slightly, but the impact is minor and there is no problem in actual use.
[0299] B: The impact caused by the exposed part is clear and cannot be used in practice
[0300] [Evaluation 2]
[0301] A photosensitive body (drum) to be evaluated is set in a test copier, and the process of charging, exposure, and de-charging is repeated 600,000 times in a low-humidity (NL) environment (temperature 25°C / relative humidity 10%). The initial charged potential and the charged potential after electrical fatigue are measured, and the differences ΔV0 are used as indicators of charge reduction in the low-humidity environment.
[0302] The obtained results were judged according to the following criteria.
[0303] VG: Very good (0≤ΔV0<60)
[0304] G: Good (60≤ΔV0<80)
[0305] NB: slightly better (80≤ΔV0<100)
[0306] B: Not good (100≤ΔV0)
[0307] [Evaluation 3]
[0308] A photosensitive body (drum) to be evaluated is set in a test copier, and the process of charging, exposure, and de-charging is repeated 600,000 times in a high-humidity (NH) environment (temperature 25°C / relative humidity 85%). The initial sensitivity potential and the sensitivity potential after electrical fatigue are measured, and the surface potential difference ΔVL is measured.
[0309] The obtained results were judged according to the following criteria.
[0310] VG: Very good (0≤|ΔVL|<30)
[0311] G: Good (30≤|ΔVL|<60)
[0312] NB: slightly better (60≤|ΔVL|<75)
[0313] B: Not good (75≤|ΔVL|)
[0314] [Overall evaluation]
[0315] Based on the determination results of evaluations 1 to 4, comprehensive determination was performed according to the following criteria.
[0316] VG: All VGs with ratings 1 to 4
[0317] G: No B was judged in the judgments of evaluations 1 to 4
[0318] B: In the evaluations 1 to 4, there is a B
[0319] The obtained evaluation results are shown in Table 1 together with the main constituent materials of the photoreceptor and their physical properties.
[0320] [Table 1]
[0321]
[0322] *:Titanium Tetrabutoxide
[0323] **: Ultraviolet absorber (the amount added is the mass ratio to the charge transport material)
[0324] From Table 1, we can see the following.
[0325] (1) According to the results of Evaluation 1, the light resistance of the photoreceptor having a charge generating layer (Examples 1 to 10) is significantly improved compared with the existing photoreceptors (Comparative Examples 1 to 6), and the charge generating layer contains oxytitanium phthalocyanine as the charge generating material that satisfies the requirements of the spectral absorption spectrum of the present invention.
[0326] (2) In addition, the absorbance ratio Abs of the spectral absorption spectrum of oxytitanium phthalocyanine is satisfied. 860nm / Abs 780nm The photosensitive members satisfying the requirement of 0.75 or more and 1 or less (Examples 1, 3, and 6) have a further improved light resistance than the photosensitive members not satisfying the requirement (Examples 2, 4, and 5).
[0327] (3) According to the results of Evaluation 2, the photoreceptor having an undercoat layer between the aluminum substrate and the charge generating layer (Example 1) and the photoreceptor having no undercoat layer (Example 7) can more effectively reduce ΔV0 in a low humidity environment.
[0328] (4) According to the results of Evaluation 3, the photoreceptor satisfying the requirement that the average particle size D (50%) of oxytitanium phthalocyanine is 0.15 to 0.3 μm (Example 1) can suppress ΔVL under a high humidity environment compared with the photoreceptors not satisfying this requirement (Examples 5 and 6).
[0329] (5) Even if the absorbance ratio Abs does not satisfy the spectral absorption spectrum of oxytitanium phthalocyanine 860nm / Abs 780nm In the photoreceptor having the requirement of 0.75 or more and 1 or less (Example 4), the light resistance can also be improved by using an additive (ultraviolet absorber) for improving light resistance in the charge transport layer (Example 8)
[0330] However, since an additive is added to the charge transport layer to form a trap for charge transport, ΔVL in a high humidity environment deteriorates, and therefore the party that satisfies the above-mentioned requirement of the absorbance ratio of the spectral absorption spectrum can maintain stable image characteristics for a long time. (6) As a charge transport material, the photoreceptor using the trienamine dimer compound represented by the general formula (1) (Example 2) and the photoreceptor using the stilbene derivative of the general formula (2) (Example 9) are superior in the effect of reducing ΔV0 in a low humidity environment and the effect of suppressing ΔVL in a high humidity environment, as compared with the photoreceptor using a compound as a conventional charge transport material (Example 10), and a tendency of slightly poor light resistance can be seen (this tendency can also be confirmed in the comparison between Comparative Example 1 and Comparative Example 5).
[0331] However, as in (5) above, by using oxytitanium phthalocyanine having an absorbance in a more preferred range in the spectral absorption spectrum, it is possible to provide a photoreceptor having sufficiently improved light resistance, extremely good ΔV0 and ΔVL, and stable image characteristics for a long period of time.
[0332] The present invention is not limited to the above-described embodiments, and can be implemented in various other ways. Therefore, the embodiments involved are only examples in all aspects and should not be understood in a restrictive manner. The scope of the present invention is the scope shown in the claims, and there is no limitation in the text of the specification. Further, deformation and changes belonging to the equivalent scope of the claims are within the scope of the present invention.
[0333] Description of Reference Numerals
[0334] F01 laminated electrophotographic photoreceptor
[0335] F1 substrate (conductive support)
[0336] F21 base coating (middle layer)
[0337] F22 Charge generation layer
[0338] F23 Charge transport layer
[0339] Fa photoreceptor surface
[0340] 31 exposure unit (semiconductor laser)
[0341] 32 live unit (live device)
[0342] 33 developing unit (developer)
[0343] 33a Development roller
[0344] 33b Housing
[0345] 34 transfer unit (transfer charger)
[0346] 35 Fusing unit (fuser)
[0347] 35a Heating roller
[0348] 35b pressure roller
[0349] 36 cleaning unit (cleaner)
[0350] 36a Cleaning scraper
[0351] 36b Recovery housing
[0352] 37 Separation unit
[0353] 38 Case
[0354] 41, 42 Arrow
[0355] 44 Rotation axis
[0356] 51 Recording medium (recording paper or transfer paper)
[0357] 100 Image forming device (laser printer)
Claims
1. An electrophotographic photoreceptor, characterized in that: The electrophotographic photoreceptor comprises at least a laminated photosensitive layer, wherein a charge generating layer containing a charge generating material and a charge transporting layer containing a charge transporting material are laminated in sequence on a substrate. The charge generating material is oxytitanium phthalocyanine having at least diffraction peaks at Bragg angles 2θ±0.2° of 7.3°, 9.4°, 11.6°, 24.2° and 27.3° in an X-ray diffraction spectrum using CuKα rays, The laminated photosensitive layer has a maximum absorption λ at a wavelength of 800 to 850 nm in the spectral absorption spectrum. max , and the absorbance Abs at a wavelength of 780 nm when the minimum absorbance in the wavelength range of 400 to 800 nm is taken as 0 for correction 780nm Absorbance at 860 nm 860nm Ratio Abs 860nm / Abs 780nm is 0.6 or more and 1.2 or less, The charge transport material is a trienamine dimer compound represented by the general formula (1): [Chemistry 1] In the formula, Ar1 and Ar2 are the same or different and are alkynyl groups which may have a substituent or a divalent group derived from a heterocyclic ring which may have a substituent, Ar3 and Ar4 are the same or different and are aryl groups which may have a substituent or a heterocyclic group which may have a substituent, R1 and R2 are the same or different and are hydrogen atoms or alkyl groups, m and n are integers of 1 to 4, a and b are the same or different and are hydrogen atoms, halogen atoms, alkyl groups, fluoroalkyl groups, alkoxy groups or amino groups which may have a substituent, and when m or n is 2 or more, two a or b bonded to adjacent positions are combined to form a methylenedioxy group, an ethylenedioxy group, a tetramethylene group or a butadienyl group, The charge transport material may be a stilbene derivative represented by the general formula (2): [Chemistry 2] In the formula, R 1 , R 2 , R 5 and R 6 are the same or different and are alkyl, alkoxy, aryl, aralkyl or halogen atoms, m, n, p and q are the same or different and are integers from 0 to 3, wherein R 1 and R 2 When they are the same group, m and n are different integers. 5 and R 6 When they are the same group, p and q are different integers, and R 3 and R 4 are the same or different and are a hydrogen atom or an alkyl group.
2. The electrophotographic photoreceptor according to claim 1, wherein The ratio Abs 860nm / Abs 780nm It is greater than or equal to 0.75 and less than or equal to 1.
3. The electrophotographic photoreceptor according to claim 1, wherein The oxytitanium phthalocyanine has an average particle size D50% of 0.15 to 0.3 μm.
4. The electrophotographic photoreceptor according to any one of claims 1 to 3, characterized in that: An undercoat layer is provided between the substrate and the laminated photosensitive layer.
5. An image forming device, characterized in that: At least comprising: the electrophotographic photoreceptor according to any one of claims 1 to 4; a charging unit for charging the electrophotographic photoreceptor; an exposure unit for exposing the charged electrophotographic photoreceptor to form an electrostatic latent image; a developing unit for developing the electrostatic latent image formed by the exposure to form a toner image; and a transfer unit for transferring the toner image formed by the development to a recording medium; A fixing unit that fixes the transferred toner image on the recording medium to form an image; a cleaning unit that removes and recovers the toner remaining on the electrophotographic photoreceptor; and a charge removal unit that removes the surface charge remaining on the electrophotographic photoreceptor.