Active material, battery and method for producing the same
By using silicon clathrate-type crystalline phase active material composed of Si and Al in lithium-ion batteries, combined with the void structure, the problem of large volume changes during charging and discharging of lithium-ion batteries is solved, and a more stable battery structure and lower energy consumption are achieved. Restrains pressure and improves battery performance.
Patent Information
- Application Number
- CN202110617432.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-05-28
AI Technical Summary
The volume of silicon used as the negative active material in existing lithium-ion batteries changes greatly during the charge and discharge process, resulting in an increase in structural stability and restraint pressure, which affects the performance of the battery.
A silicon clathrate type crystal phase containing at least Si and Al is used as the active material, and a silicon clathrate type I or type II crystal phase with a cage structure is constructed and voids are introduced inside the particles to reduce charge and discharge. The active material has a silicon clathrate type crystal phase and is obtained through heat treatment and acid treatment.
It effectively reduces the volume change of the battery during the charge and discharge process, reduces the restraint pressure, improves the structural stability and energy density of the battery, and reduces the dependence on the restraint fixture.
Smart Images

Figure CN113764649B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an active material, a battery, and a method for producing the same. Background Art
[0002] In recent years, the development of batteries has been in full swing. For example, in the automotive industry, the development of batteries used in electric vehicles or hybrid vehicles is advancing. In addition, Si is known as an active material used in batteries.
[0003] For example, Patent Document 1 discloses that, according to calculations, silicon inclusion compounds can be used as negative electrode active materials for lithium ion batteries. Specifically, as silicon inclusion compounds, Si 46 and Si 34 .
[0004] In addition, Patent Document 2 discloses an electrode active material, which contains an inclusion compound, wherein the inclusion compound includes a lattice and a guest substance contained in the lattice. Specifically, it is disclosed that the guest substance includes at least one selected from Ba, Ca, and Li, and the lattice includes at least one selected from Ga, Al, In, Ag, Au, Cu, Ni, and Co and at least one selected from Si and Sn.
[0005] Furthermore, Non-Patent Document 1 discloses a ternary silicon inclusion compound having a type I crystal phase.
[0006] Prior Art Literature
[0007] Patent Literature
[0008] Patent Document 1: U.S. Patent Application Publication No. 2012 / 0021283
[0009] Patent Document 2: International Publication No. 2014 / 050100
[0010] Non-patent literature
[0011] Non-patent document 1: Tiago FTCerqueira et al., "Prediction and Synthesis of aNon-Zintl Silicon Clathrate", Chem.Mater.2016, 28, 3711-3717 Summary of the invention
[0012] Si has a large theoretical capacity and is effective in increasing the energy density of batteries, but on the other hand, Si has a large volume change due to charge and discharge.
[0013] The present disclosure has been made in view of the above-mentioned actual situation, and a main object of the present disclosure is to provide an active material having a small volume change caused by charge and discharge.
[0014] In order to solve the above problems, the present disclosure provides an active material containing at least Si and Al, having a silicon clathrate-type crystal phase, wherein the ratio of the Al to the total of the Si and the Al is 0.1 atomic % or more and 1 atomic % or less.
[0015] According to the present disclosure, since the active material has a silicon inclusion compound type crystal phase, the volume change caused by charge and discharge can be reduced. In addition, the active material in the present disclosure contains Al in addition to Si, so the volume change caused by charge and discharge can be reduced.
[0016] In the above disclosure, the above active material may have voids inside the primary particles.
[0017] In the above disclosure, the void ratio of the voids may be 2% or more and 15% or less.
[0018] In the above disclosure, in the above active material, as the above silicon clathrate type crystal phase, a silicon clathrate II type crystal phase may be present.
[0019] In addition, the present disclosure provides a battery including a positive electrode layer, a negative electrode layer, and an electrolyte layer formed between the positive electrode layer and the negative electrode layer, wherein the negative electrode layer contains the above-mentioned active material.
[0020] According to the present disclosure, by using the above-mentioned active material, a battery with a small volume change due to charge and discharge can be produced.
[0021] In addition, the present disclosure provides a method for producing an active substance, comprising:
[0022] A step of preparing a Zintl compound, wherein the Zintl compound contains Na, Si and Al and has at least a Zintl phase, wherein the ratio of the Al to the total of the Si and the Al is less than 10 atomic %; a step of removing Na from the Zintl compound to form an intermediate having a silicon clathrate-type crystal phase; and a step of removing Al from the intermediate.
[0023] According to the present disclosure, by using a Zinter compound containing Al in addition to Na and Si, an active material having a small volume change due to charge and discharge can be obtained.
[0024] In the above disclosure, the preparation step may be a step of preparing the Zintl compound by heat-treating a raw material mixture containing a Na source, a Si source, and an Al source.
[0025] In addition, the present disclosure provides a method for manufacturing a battery, comprising: an active material manufacturing step of manufacturing an active material using the above-mentioned method for manufacturing an active material; and a negative electrode layer forming step of forming a negative electrode layer using the above-mentioned active material.
[0026] According to the present disclosure, by using the above-mentioned active material, a battery having a small volume change due to charge and discharge can be obtained.
[0027] In the present disclosure, an effect is achieved in that an active material having a small volume change due to charge and discharge can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a schematic three-dimensional diagram illustrating the crystal phase of Si.
[0029] Figure 2 This is a schematic cross-sectional view illustrating a battery in the present disclosure.
[0030] Figure 3 This is a flow chart illustrating the method for producing the active material in the present disclosure.
[0031] Figure 4 These are the results of XRD measurement of the intermediate and active material obtained in Example 2.
[0032] Figure 5 These are the results of SEM observation of the active material obtained in Example 2.
[0033] Figure 6 These are the results of SEM observation (cross section) of the active materials obtained in Examples 1 to 4 and Comparative Example 3.
[0034] Description of Reference Numerals
[0035] 1… Positive electrode layer
[0036] 2…Negative electrode layer
[0037] 3…Electrolyte layer
[0038] 4…Positive electrode collector
[0039] 5…Negative electrode collector
[0040] 10…Battery DETAILED DESCRIPTION
[0041] The active material, battery, and method for producing the same in the present disclosure are described in detail below.
[0042] A. Active substances
[0043] The active material in the present disclosure contains at least Si and Al and has a silicon clathrate type crystal phase, wherein the ratio of the Al to the total of the Si and the Al is 0.1 atomic % or more and 1 atomic % or less.
[0044] The active material in the present disclosure has a silicon inclusion compound type crystalline phase. In the silicon inclusion compound type crystalline phase, the skeleton atoms have a cage-type structure (cage), into which metal ions such as Li ions can enter. Even if the metal ions enter the cage, the expansion amount is small, so the volume change caused by charging and discharging is small. Examples of silicon inclusion compound type crystalline phases include silicon inclusion compound type I and type II crystalline phases.
[0045] In the crystalline phases of silicon inclusion type I and type II, such as Figure 1 As shown in (a) and (b), a polyhedron including pentagons or hexagons is formed by a plurality of Si elements. The polyhedron has a space inside that can accommodate metal ions such as Li ions. By filling the space with metal ions, the volume change caused by charge and discharge can be suppressed. In addition, since the silicon inclusion compound type I and type II crystalline phases have a space inside that can accommodate metal ions, they have the advantage of being easy to maintain the crystal structure even after repeated charge and discharge. In addition, in order to suppress the volume change caused by charge and discharge, especially in all-solid-state batteries, it is generally necessary to apply a high restraint pressure, but by using the active material disclosed in the present invention, it is possible to reduce the restraint pressure, and as a result, it is possible to suppress the size of the restraint fixture. On the other hand, conventional Si particles have a diamond-type crystalline phase. In the diamond-type crystalline phase, such as Figure 1 As shown in (c), a tetrahedron is formed by a plurality of Si elements. Since the tetrahedron has no space inside that can accommodate metal ions such as Li ions, the volume change caused by charge and discharge is large.
[0046] Thus, according to the present disclosure, since the active material has a silicon inclusion compound type crystalline phase, the volume change caused by charging and discharging can be reduced. Moreover, since the active material in the present disclosure contains Al in addition to Si, the volume change caused by charging and discharging can be reduced. It is speculated that the reason for this is because a part of Si constituting the cage of the silicon inclusion compound type crystalline phase is replaced by Al as a foreign element, and the cage becomes larger. In addition, as the cage becomes larger, the resistance during metal ion conduction becomes smaller. In addition, as described later, the active material in the present disclosure preferably has voids inside the primary particle. In this case, in addition to the silicon inclusion compound type crystalline phase, the voids also contribute to suppressing the volume change, and thus the volume change caused by charging and discharging can be further suppressed.
[0047] The active material in the present disclosure contains at least Si and Al. In the active material, as metal elements, only Si and Al may be contained, or other metal elements may be contained. As other metal elements, for example, Na may be mentioned. In addition, in the active material, as metal elements, only Si, Al and Na may be contained. The ratio of the total of Si and Al contained in the active material to all metal elements is, for example, 60 atomic % or more, 70 atomic % or more, or 80 atomic % or more.
[0048] In the active material, the ratio of Al to the total of Si and Al is usually 0.1 atomic % or more, and may be 0.2 atomic % or more. On the other hand, the ratio of Al to the total of Si and Al is usually 1 atomic % or less.
[0049] The composition of the active material in the present disclosure is not particularly limited, but preferably Na x (Si, Al) 136 (0≤x≤20). x may be 0 or greater than 0. On the other hand, x may be 10 or less or 5 or less. The composition of the active material can be determined by, for example, EDX, XRD, XRF, ICP, or atomic absorption spectrometry.
[0050] The active material in the present disclosure has a silicon inclusion compound type crystalline phase. The active material preferably has a silicon inclusion compound type crystalline phase as the main phase. The so-called "having a silicon inclusion compound type crystalline phase as the main phase" means that the peak belonging to the silicon inclusion compound type crystalline phase is the peak with the largest diffraction intensity among the peaks observed by X-ray diffraction measurement. The definition of "main phase" is the same in other crystalline phases. In addition, the silicon inclusion compound type crystalline phase has at least Si, but may also have Al. That is, a part of Si constituting the silicon inclusion compound type crystalline phase can be replaced by Al.
[0051] As the silicon inclusion compound type crystalline phase, for example, the silicon inclusion compound type I crystalline phase and the silicon inclusion compound type II crystalline phase can be cited. The active material in the present disclosure may contain the silicon inclusion compound type I crystalline phase as the main phase, or may contain the silicon inclusion compound type II crystalline phase as the main phase, but the latter is preferred. The reason is that the volume change caused by charge and discharge can be further reduced.
[0052] In addition, the active material in the present disclosure may (i) have a crystalline phase of silicon inclusion compound type I and not have a crystalline phase of silicon inclusion compound type II, (ii) may not have a crystalline phase of silicon inclusion compound type I and have a crystalline phase of silicon inclusion compound type II, or (iii) may have a crystalline phase of silicon inclusion compound type I and a crystalline phase of silicon inclusion compound type II. "Not having a crystalline phase" can be confirmed by not observing a peak of the crystalline phase in an X-ray diffraction measurement. The definition of "not having a crystalline phase" is the same for other crystalline phases.
[0053] The crystalline phase of silicon inclusion compound type I usually belongs to the space group (Pm-3n). The crystalline phase of silicon inclusion compound type I has typical peaks at 2θ=19.44°, 21.32°, 30.33°, 31.60°, 32.82°, 36.29°, 52.39°, and 55.49° in the X-ray diffraction measurement using CuKα rays. These peak positions can vary in the range of ±0.50°, in the range of ±0.30°, and in the range of ±0.10°.
[0054] The crystalline phase of silicon inclusion complex type II usually belongs to the space group (Fd-3m). The crystalline phase of silicon inclusion complex type II has typical peaks at 2θ=20.09°, 21.00°, 26.51°, 31.72°, 36.26°, and 53.01° in X-ray diffraction measurement using CuKα rays. These peak positions can vary in the range of ±0.50°, ±0.30°, and ±0.10°, respectively.
[0055] The lattice constant of the silicon inclusion compound type II crystal phase is, for example, The above can be On the other hand, the lattice constant of the silicon inclusion compound type II crystal phase is, for example, The lattice constant can be determined by performing XRD measurement on the active material and performing Rietveld analysis on the obtained XRD pattern.
[0056] In addition, the active material in the present disclosure may have a diamond-type Si crystalline phase or may not have a diamond-type Si crystalline phase. The diamond-type Si crystalline phase has typical peaks at 2θ=28.44°, 47.31°, 56.10°, 69.17°, and 76.37° in X-ray diffraction measurement using CuKα rays. These peak positions can vary in the range of ±0.50°, in the range of ±0.30°, and in the range of ±0.10°.
[0057] The peak intensity of the peak A at 2θ=31.72°±0.50° in the silicon clathrate II type crystal phase is defined as I A The peak intensity of peak B at 2θ=28.44°±0.50° in the diamond-type Si crystal phase is defined as I B I B / I A For example, it may be less than 1, may be 0.5 or less, or may be 0.3 or less.
[0058] In addition, the active material in the present disclosure preferably does not have a peak caused by a by-product described below. The details of the by-product are described in "C. Method for producing active material" described below.
[0059] The shape of the active material in the present disclosure may be, for example, a particle shape. The active material may be a primary particle or a secondary particle formed by agglomeration of primary particles. In either case, it is preferred that there be voids inside the primary particles. The void ratio of the voids may be, for example, greater than 2%, greater than 5%, or greater than 10%. On the other hand, the void ratio may be, for example, less than 40%, less than 20%, or less than 15%.
[0060] The porosity can be determined, for example, by the following steps. First, the electrode layer containing the active material is subjected to ion milling to obtain a cross-section. Then, the cross-section is observed using a SEM (scanning electron microscope) to obtain a photograph of the particles. The obtained photograph is binarized by strictly distinguishing between the silicon portion and the void portion using image analysis software. The areas of the silicon portion and the void portion are determined, and the porosity (%) is calculated by the following formula.
[0061] Void ratio (%) = 100 × (void area) / ((silicon area) + (void area))
[0062] Specific image analysis and calculation of void ratio can be performed as follows. As image analysis software, for example, Fiji ImageJ bundled with Java 1.8.0_172 (hereinafter referred to as Fiji) is used. The secondary electron image and the reflected electron image of the same field of view are synthesized to perform RGB color imaging. Moreover, in order to remove the noise of each pixel, the obtained RGB image is blurred using the function "Median (filter size (filter size) = 2)" in Fiji. Then, the function "Weka Machine Learning" in Fiji is used to designate any multiple areas in the image from which the above noise has been removed as silicon parts or void parts, respectively, and to create teaching data that strictly distinguishes between silicon parts and void parts. Moreover, based on the created teaching data, the silicon part and the void part are distinguished by machinery in Fiji, and the area ratio of the silicon part and the void part is calculated.
[0063] Regarding RGB color imaging, since both the secondary electron image and the reflected electron image are expressed in grayscale, for example, the brightness x in each pixel of the secondary electron image is assigned to a Red value, and similarly, the brightness y in the reflected electron image is assigned to a Green value. Thus, for example, RGB imaging is performed for each pixel according to R=x, G=y, and B=(x+y) / 2.
[0064] The detailed conditions in the above-mentioned "Weka Machine Learning" are shown below. As Training features (in machine learning, the numerical features of the image that the machine focuses on when creating teaching data), Gaussianblur, Hessian, Membrane projections, Mean, Maximum, Anisotropic diffusion, Sobelfilter, Difference of gaussians, Variance, Minimum, Median are selected. In addition, as other parameters, Membrane thickness is set to 3, Membrane patch size is set to 19, Minimum sigma is set to 1.0, and Maximum sigma is set to 16.0.
[0065] The average particle size of the primary particles is, for example, greater than 50 nm, may be greater than 100 nm, or may be greater than 150 nm. On the other hand, the average particle size of the primary particles is, for example, less than 3000 nm, may be less than 1500 nm, or may be less than 1000 nm. In addition, the average particle size of the secondary particles is, for example, greater than 1 μm, may be greater than 2 μm, or may be greater than 5 μm. On the other hand, the average particle size of the secondary particles is, for example, less than 60 μm, or may be less than 40 μm. Furthermore, the average particle size can be determined by, for example, SEM observation. The number of samples is preferably large, for example, greater than 20, may be greater than 50, or may be greater than 100.
[0066] The active material in the present disclosure is generally used in batteries. The active material in the present disclosure may be a negative electrode active material or a positive electrode active material, but the former is preferred. In the present disclosure, an electrode layer (negative electrode layer or positive electrode layer) having the above-mentioned active material and a battery having the electrode layer can also be provided. As a method for producing the active material, for example, the production method described in "C. Production method of active material" described later can be cited.
[0067] B.Battery
[0068] Figure 2 This is a schematic cross-sectional view illustrating a battery in the present disclosure. Figure 2 The battery 10 shown has: a positive electrode layer 1; a negative electrode layer 2; an electrolyte layer 3 formed between the positive electrode layer 1 and the negative electrode layer 2; a positive electrode collector 4 for collecting current from the positive electrode layer 1; and a negative electrode collector 5 for collecting current from the negative electrode layer 2. In the present disclosure, the negative electrode layer 2 contains the active material described in the above "A. Active material".
[0069] According to the present disclosure, by using the above-mentioned active material, a battery with a small volume change due to charge and discharge can be produced.
[0070] 1. Negative electrode layer
[0071] The negative electrode layer is a layer containing at least a negative electrode active material. Regarding the negative electrode active material, since it is the same as the content described in the above-mentioned "A. Active Material", it is omitted here. The proportion of the negative electrode active material in the negative electrode layer is, for example, more than 20 weight%, can be more than 30 weight%, or can be more than 40 weight%. If the proportion of the negative electrode active material is too small, there is a possibility that sufficient energy density cannot be obtained. On the other hand, the proportion of the negative electrode active material is, for example, less than 80 weight%, can be less than 70 weight%, or can be less than 60 weight%. If the proportion of the negative electrode active material is too much, there is a possibility that the ion conductivity and electronic conductivity in the negative electrode layer are relatively reduced.
[0072] The negative electrode layer may also contain at least one of an electrolyte, a conductive material and a binder as required. As an electrolyte, for example, the electrolyte described in "3. Electrolyte layer" described later can be cited. As a conductive material, for example, carbon materials, metal particles, and conductive polymers can be cited. As a carbon material, for example, acetylene black (AB), Ketjen black (KB) and other particulate carbon materials, carbon fibers, carbon nanotubes (CNT), carbon nanofibers (CNF) and other fibrous carbon materials can be cited. In addition, as a binder, for example, a rubber-based binder and a fluoride-based binder can be cited.
[0073] The thickness of the negative electrode layer is, for example, 0.1 μm or more and 1000 μm or less. The negative electrode layer in the present disclosure is generally used in batteries.
[0074] 2. Positive electrode layer
[0075] The positive electrode layer is a layer containing at least a positive electrode active material. In addition, the positive electrode layer may contain at least one of an electrolyte, a conductive material, and a binder as necessary.
[0076] Examples of the positive electrode active material include oxide active materials. Examples of the oxide active material include LiCoO2, LiMnO2, LiNiO2, LiVO2, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 and other rock salt layered active materials, LiMn2O4, Li4Ti5O 12 、Li(Ni 0.5 Mn 1.5 )O4 and other spinel active materials, LiFePO4, LiMnPO4, LiNiPO4, LiCoPO4 and other olivine active materials.
[0077] A coating containing a Li ion conductive oxide may also be formed on the surface of the oxide active material. The reason is that the reaction between the oxide active material and the solid electrolyte (particularly a sulfide solid electrolyte) can be suppressed. As a Li ion conductive oxide, for example, LiNbO3 can be cited. The thickness of the coating is, for example, greater than 1 nm and less than 30 nm. In addition, as a positive electrode active material, for example, Li2S can also be used.
[0078] The shape of the positive electrode active material can be, for example, a particle shape. The average particle size (D 50 ) is not particularly limited, and may be, for example, 10 nm or more, or 100 nm or more. On the other hand, the average particle size (D 50 ) is, for example, 50 μm or less, and may be 20 μm or less. The average particle size (D 50) can be calculated by measuring using, for example, a laser diffraction particle size distribution analyzer or a scanning electron microscope (SEM).
[0079] The electrolyte, conductive material, and binder used in the positive electrode layer are the same as those described in the above-mentioned “1. Negative electrode layer”, and thus are omitted here. The thickness of the positive electrode layer is, for example, 0.1 μm to 1000 μm.
[0080] 3. Electrolyte layer
[0081] The electrolyte layer is a layer formed between the positive electrode layer and the negative electrode layer, and contains at least an electrolyte. The electrolyte may be a solid electrolyte or a liquid electrolyte (electrolyte).
[0082] As solid electrolytes, inorganic solid electrolytes such as sulfide solid electrolytes, oxide solid electrolytes, nitride solid electrolytes, and halide solid electrolytes, and organic polymer electrolytes such as polymer electrolytes can be cited. As sulfide solid electrolytes, for example, solid electrolytes containing Li, X (X is at least one of P, As, Sb, Si, Ge, Sn, B, Al, Ga, and In) and S can be cited. In addition, the sulfide solid electrolyte may also contain at least one of O and halogen. As halogens, for example, F, Cl, Br, and I can be cited. The sulfide solid electrolyte can be glass (amorphous) or glass ceramics. As sulfide solid electrolytes, for example, Li2S-P2S5, LiI-Li2S-P2S5, LiI-LiBr-Li2S-P2S5, Li2S-SiS2, Li2S-GeS2, and Li2S-P2S5-GeS2 can be cited.
[0083] The electrolyte preferably contains a supporting electrolyte and a solvent. As the supporting electrolyte (lithium salt) of the electrolyte with lithium ion conductivity, inorganic lithium salts such as LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(FSO2)2, LiC(CF3SO2)3 and other organic lithium salts can be cited. As the solvent used for the electrolyte, cyclic esters (cyclic carbonates) such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC), dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (EMC) and other chain esters (chain carbonates) can be cited. The electrolyte preferably contains two or more solvents.
[0084] The thickness of the electrolyte layer is, for example, 0.1 μm or more and 1000 μm or less.
[0085] 4. Other components
[0086] The battery in the present disclosure preferably has a positive electrode current collector for collecting the positive electrode layer, and a negative electrode current collector for collecting the negative electrode layer. As the material of the positive electrode current collector, for example, SUS, aluminum, nickel, iron, titanium and carbon can be listed. On the other hand, as the material of the negative electrode current collector, for example, SUS, copper, nickel and carbon can be listed.
[0087] The battery in the present disclosure may also have a confining jig that applies confining pressure to the positive electrode layer, the electrolyte layer, and the negative electrode layer along the thickness direction. In particular, when the electrolyte layer is a solid electrolyte layer, in order to form a good ion conduction path and an electron conduction path, it is preferred to apply confining pressure. The confining pressure is, for example, more than 0.1 MPa, more than 1 MPa, or more than 5 MPa. On the other hand, the confining pressure is, for example, less than 100 MPa, less than 50 MPa, or less than 20 MPa.
[0088] 5. Battery
[0089] The type of battery in the present disclosure is not particularly limited, but typically, it is a lithium-ion battery. In addition, the battery in the present disclosure may be a liquid battery containing an electrolyte as an electrolyte layer, or may be an all-solid battery having a solid electrolyte layer as an electrolyte layer. In addition, the battery in the present disclosure may be a primary battery or a secondary battery, but among them, a secondary battery is preferred. The reason is that it can be repeatedly charged and discharged, for example, it is useful as a vehicle-mounted battery.
[0090] The battery in the present disclosure may be a single cell or a stacked battery. The stacked battery may be a monopolar stacked battery (a stacked battery connected in parallel) or a bipolar stacked battery (a stacked battery connected in series). Examples of the shape of the battery include a coin-shaped, stacked, cylindrical, and square shape.
[0091] C. Method for producing active substances
[0092] Figure 3 is a flow chart illustrating a method for producing an active material in the present disclosure. Figure 3 In the manufacturing method shown, first, a Zintel compound is prepared (preparation step), wherein the Zintel compound contains Na, Si and Al, has at least a Zintel phase, and the ratio of Al to the total of Si and Al is less than 10 atomic %. Next, Na is removed from the Zintel compound to form an intermediate having a silicon inclusion compound type crystal phase (Na removal step). Next, Al is removed from the intermediate (Al removal step). Thus, an active material having a silicon inclusion compound type crystal phase and having voids inside the primary particle is obtained.
[0093] According to the present disclosure, by using a Zinter compound containing Al in addition to Na and Si, an active material having a small volume change due to charge and discharge can be obtained.
[0094] 1. Preparation process
[0095] The preparation step in the present disclosure is a step of preparing a Zinter compound containing Na, Si, and Al, having at least a Zinter phase, wherein the ratio of the Al to the total of the Si and the Al is less than 10 atomic %.
[0096] The Zintel compound contains at least Na, Si and Al. In the Zintel compound, as metal elements, only Na, Si and Al may be contained, or other metal elements may be contained. The total ratio of Na, Si and Al contained in the Zintel compound to all metal elements is, for example, 70 atomic % or more, 80 atomic % or more, or 90 atomic % or more.
[0097] In the Zintel compound, the ratio of Al to the total of Si and Al is, for example, 0.1 atomic % or more, 0.5 atomic % or more, or 1 atomic % or more. On the other hand, the ratio of Al to the total of Si and Al is usually less than 10 atomic %, or less than 8 atomic %. The composition of the Zintel compound is not particularly limited, but preferably Na z (Si, Al) 136 This composition (121≤z≤151) indicates that z may be 126 or more, or 131 or more. On the other hand, z may be 141 or less.
[0098] The Zintl compound has a Zintl phase. The Zintl phase has typical peaks at 2θ=16.10°, 16.56°, 17.64°, 20.16°, 27.96°, 33.60°, 35.68°, 40.22°, and 41.14° in X-ray diffraction measurement using CuKα rays. These peak positions can vary in the range of ±0.50° and can vary in the range of ±0.30°. The Zintl compound preferably has a Zintl phase as the main phase. The Zintl compound may or may not have a crystalline phase of a silicon inclusion compound type I. In addition, the Zintl compound may or may not have a crystalline phase of a silicon inclusion compound type II.
[0099] The intermediate may have a Zinter phase containing Na, Si and Al, and a byproduct containing at least Al. The Zinter phase preferably contains Na, Si and Al. A typical Zinter phase is composed of Na and Si, but it is presumed that if a part of Si is replaced by Al, it becomes easy to obtain a desired silicon inclusion compound type crystal phase (a silicon inclusion compound type crystal phase in which a part of Si is replaced by Al).
[0100] The by-product contains at least Al. The by-product preferably has peaks at 2θ=34.8° and 36.0° in X-ray diffraction measurement using CuKα rays. These peak positions can vary within the range of ±0.3° and can vary within the range of ±0.1°. The by-product may also contain at least one of Na and O in addition to Al.
[0101] The Zintl compound can be obtained by heat treating a raw material mixture containing a Na source, a Si source, and an Al source. As the Na source, for example, a simple substance of Na and an alloy with Na as the main component can be cited. As the Si source, for example, a simple substance of Si and an alloy with Si as the main component can be cited. As the Al source, for example, a simple substance of Al, an alloy with Al as the main component, and an Al oxide can be cited. As the Al oxide, for example, Al2O3 can be cited.
[0102] In the raw material mixture, the ratio of Na to the total of Si and Al is not particularly limited, and Na is, for example, 0.8 mole parts or more, or 1 mole parts or more relative to 1 mole part of the total of Si and Al. On the other hand, Na is, for example, 1.5 mole parts or less, or 1.3 mole parts or less relative to 1 mole part of the total of Si and Al. In addition, in the raw material mixture, the ratio of Al to the total of Si and Al is, for example, 0.1 atomic % or more, or 0.5 atomic % or more, or 1 atomic % or more. On the other hand, in the raw material mixture, the ratio of Al to the total of Si and Al is, for example, less than 10 atomic % or less, or 8 atomic % or less.
[0103] The heat treatment temperature is, for example, 500° C. to 1000° C. In addition, the heat treatment time is, for example, 1 hour to 50 hours. In particular, the heat treatment is preferably performed at about 700° C. (for example, 650° C. to 750° C.) and for about 20 hours (for example, 15 hours to 25 hours).
[0104] 2. Na removal process
[0105] The Na removal step in the present disclosure is a step of removing the Na from the Zintl compound to form an intermediate having a silicon clathrate-type crystal phase.
[0106] As a method for removing Na from the Zintel compound, for example, heat treatment can be cited. The heat treatment temperature is, for example, above 280°C, and can be above 300°C. On the other hand, the heat treatment temperature is, for example, below 500°C. The heat treatment time is, for example, above 1 hour and below 50 hours. The heat treatment can be carried out in a normal pressure atmosphere or in a reduced pressure atmosphere. In the latter case, the pressure during the heat treatment is, for example, below 10Pa, below 1Pa, or below 0.1Pa. In addition, the heat treatment can also be carried out in an inert atmosphere such as an Ar atmosphere.
[0107] The intermediate has a silicon inclusion compound type crystalline phase. The intermediate preferably has a silicon inclusion compound type crystalline phase as the main phase. The intermediate may contain a silicon inclusion compound type I crystalline phase as the main phase, or may contain a silicon inclusion compound type II crystalline phase as the main phase, but the latter is preferred. The reason is that the volume change caused by charge and discharge can be further reduced.
[0108] In addition, the intermediate may (i) have a crystalline phase of silicon inclusion compound type I and not have a crystalline phase of silicon inclusion compound type II, (ii) may not have a crystalline phase of silicon inclusion compound type I and have a crystalline phase of silicon inclusion compound type II, or (iii) may have a crystalline phase of silicon inclusion compound type I and a crystalline phase of silicon inclusion compound type II. The composition of the intermediate is not particularly limited, but preferably Na y (Si, Al) 136 (0≤y≤24). y may be 0 or greater than 0. On the other hand, y may be 20 or less or 10 or less.
[0109] 3. Al removal process
[0110] The Al removal step in the present disclosure is a step of removing the Al from the intermediate. "Al removal" also includes the removal of compounds containing Al (such as the above-mentioned byproducts). By removing Al, an active material having voids inside the primary particle can be obtained.
[0111] As a method for removing Al from the intermediate, for example, acid treatment can be cited. Acid treatment is, for example, a treatment in which an acid solution is brought into contact with the intermediate. The acid solution contains, for example, an acid and a solvent. As the acid used for the acid solution, for example, hydrochloric acid, sulfuric acid, acetic acid, formic acid, propionic acid, oxalic acid, and hydrofluoric acid can be cited. The solvent used for the acid solution can be water or an organic solvent. In addition, the acid concentration (normality) in the acid solution is not particularly limited, for example, it is greater than 0.5N and less than 3N. Furthermore, the acid itself can be used instead of the acid solution without dilution with a solvent.
[0112] 4. Active substances
[0113] The active material obtained by each of the above steps has a silicon inclusion compound type crystal phase. In addition, the above active material preferably contains at least Si and Al, and the ratio of Al to the total of Si and Al is within a specified range. Furthermore, the above active material preferably has voids inside the primary particle. Regarding the preferred embodiment of the active material, the contents described in the above "A. Active material" can be appropriately cited.
[0114] D. Battery manufacturing method
[0115] The present disclosure provides a method for manufacturing a battery, comprising: an active material manufacturing step of manufacturing an active material using the above-mentioned method for manufacturing an active material; and a negative electrode layer forming step of forming a negative electrode layer using the above-mentioned active material.
[0116] According to the present disclosure, by using the above-mentioned active material, a battery with a small volume change due to charge and discharge can be obtained. The active material production process is the same as that described in the above-mentioned "C. Active material production method".
[0117] In the negative electrode layer forming step, the above-mentioned active material is used to form the negative electrode layer. The method for forming the negative electrode layer is not particularly limited, and a known method can be used. For example, by applying a slurry containing at least an active material to a negative electrode collector and drying it, a negative electrode layer formed on the negative electrode collector can be obtained. Regarding the preferred mode of the obtained negative electrode layer, the contents described in the above-mentioned "B. Battery 1. Negative Electrode Layer" can be appropriately cited.
[0118] The method for forming the battery is not particularly limited, and a known method can be used. The method for manufacturing the battery in the present disclosure may also have, in addition to the active material manufacturing process and the negative electrode layer forming process, a positive electrode layer forming process for forming a positive electrode layer, an electrolyte layer forming process for forming an electrolyte layer, and a configuration process for sequentially configuring the positive electrode layer, the electrolyte layer, and the negative electrode layer. The preferred embodiment of the obtained battery can be appropriately cited in the above-mentioned "B. Battery".
[0119] The above embodiments are merely examples, and any solution having substantially the same structure and achieving the same function and effect as the technical concept described in the claims of the present disclosure is included in the technical scope of the present disclosure.
[0120] Example
[0121] [Example 1]
[0122] (Synthesis of active substances)
[0123] Si simple substance (purity 99%, with Si oxide film on the surface), Al simple substance and Na simple substance (purity 99.5%) were mixed so as to have a molar ratio (atomic ratio) of Si simple substance: Al simple substance: Na simple substance = 0.995: 0.005: 1.1. In the obtained mixture, the ratio of Al to the total of Si and Al was 0.5 atomic%. Then, the obtained mixture was put into a boron nitride crucible, sealed in an Ar atmosphere, and heated at 700°C for 20 hours to synthesize a Zintel compound (blocky) containing Na, Si and Al. The obtained Zintel compound was crushed and heated at 340°C for 20 hours under vacuum (about 0.1 Pa) to remove Na and obtain an intermediate. The obtained intermediate was treated with dilute hydrochloric acid (1N) for 10 minutes to remove Al (byproduct containing Al) and obtain an active material.
[0124] (Production of negative electrode)
[0125] The dispersion medium (butyl butyrate), the binder (butyl butyrate solution in which 5% by weight of polyvinylidene fluoride is dissolved), the above-mentioned active material, the solid electrolyte (Li2S-P2S5 glass ceramic), and the conductive material (VGCF (vapor-phase carbon fiber)) are placed in a polypropylene container, and oscillated for 3 minutes with an oscillator (TTM-1 manufactured by Shibata Science Co., Ltd.), and then stirred for 30 seconds with an ultrasonic dispersion device to prepare a negative electrode layer slurry. The negative electrode layer slurry is applied to the negative electrode collector (copper foil) by a doctor blade method using an applicator, and then dried on a hot plate adjusted to 100°C for 30 minutes. Thus, a negative electrode having a negative electrode layer and a negative electrode collector is obtained.
[0126] (Production of positive electrode)
[0127] The dispersion medium (butyl butyrate), the binder (butyl butyrate solution in which 5 wt% polyvinylidene fluoride was dissolved), the positive electrode active material (LiNi coated with lithium niobate) and the 1 / 3 Co 1 / 3 Mn 1 / 3 O2), solid electrolyte (Li2S-P2S5 glass ceramic), conductive material (VGCF (vapor-phase carbon fiber)) were placed in a polypropylene container, oscillated for 3 minutes with an oscillator (TTM-1 manufactured by Shibata Science Co., Ltd.), and then stirred for 30 seconds with an ultrasonic dispersion device to prepare a positive electrode layer slurry. The positive electrode layer slurry was applied to the positive electrode collector (aluminum foil) using a doctor blade method using an applicator, and then dried on a hot plate adjusted to 100°C for 30 minutes. Thus, a positive electrode having a positive electrode layer and a positive electrode collector was obtained.
[0128] (Fabrication of Solid Electrolyte Layer)
[0129] The dispersion medium (heptane), the binder (heptane solution in which 5 wt% of butadiene rubber is dissolved), and the solid electrolyte (Li2S-P2S5 glass ceramic containing lithium iodide) are placed in a polypropylene container and stirred for 30 seconds using an ultrasonic dispersion device. Then, the polypropylene container is vibrated with an oscillator for 30 minutes to prepare a slurry for a solid electrolyte layer. The slurry for the solid electrolyte layer is applied to an aluminum foil as a substrate using an applicator by a doctor blade method, and then dried on a hot plate heated to 100°C for 30 minutes, thereby preparing a solid electrolyte layer on the substrate.
[0130] (Production of Evaluation Batteries)
[0131] The negative electrode, the solid electrolyte layer, and the positive electrode were stacked in this order, and the obtained stack was pressed under the conditions of 130° C., 200 MPa, and 3 minutes to obtain a battery for evaluation.
[0132] [Examples 2 to 4]
[0133] Active materials and evaluation batteries were obtained in the same manner as in Example 1, except that the ratio of Al to the total of Si and Al (Al input amount) was changed to 1 atomic % (Example 2), 3 atomic % (Example 3), and 5 atomic % (Example 4).
[0134] [Comparative Example 1]
[0135] An active material and an evaluation battery were obtained in the same manner as in Example 1 except that Al single substance was not used.
[0136] [Comparative Example 2]
[0137] An active material and an evaluation battery were obtained in the same manner as in Example 2 except that the acid treatment was not performed.
[0138] [Comparative Example 3]
[0139] An active material and an evaluation battery were obtained in the same manner as in Example 1 except that the ratio of Al to the total of Si and Al (Al input amount) was changed to 10 atomic %.
[0140] [evaluate]
[0141] (XRD measurement)
[0142] X-ray diffraction (XRD) measurement using CuKα rays was performed on the active materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3. The active materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were all confirmed to have a silicon inclusion compound II-type crystalline phase as the main phase. In addition, the XRD pattern of the silicon inclusion compound II-type crystalline phase was subjected to Rietveld analysis to determine the lattice constant. Moreover, the lattice constant of Comparative Example 1 was used as a reference to determine the relative values of the lattice constants of Examples 1 to 4 and Comparative Examples 2 and 3, and the results are shown in Table 1.
[0143] In addition, as a representative result, the XRD patterns of the intermediate (before acid treatment) and the active material (after acid treatment) obtained in Example 2 are shown in FIG. Figure 4 .like Figure 4 As shown in (a), it was confirmed that the intermediate before the acid treatment had a silicon inclusion compound II type crystal phase as the main phase, and had peaks derived from by-products at 2θ=34.8° and 36.0°. Figure 4 As shown in (b), it was confirmed that the active material after acid treatment also had a silicon inclusion compound II type crystalline phase as the main phase, similarly to the intermediate. On the other hand, the active material after acid treatment was different from the intermediate in that the peak derived from the by-product disappeared. That is, it was confirmed that the by-product was removed by the acid treatment.
[0144] (SEM-EDX measurement)
[0145] The active materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to SEM-EDX (scanning electron microscope-energy dispersive X-ray spectroscopy) measurement. As a representative result, the SEM image of the active material obtained in Example 2 is shown in FIG. Figure 5 .like Figure 5 As shown, it was confirmed that the active material obtained in Example 2 was porous. In addition, the results of EDX confirmed that Al and Na were uniformly dispersed. In addition, O was detected in a ratio greater than Al and less than Na. In addition, the ratio of Al to the total of Si and Al was found to be 0.2 atomic %. In addition, SEM-EDX measurement was performed on the intermediate, and the results suggested that the by-product contained Na, Al and O.
[0146] The active materials obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were subjected to SEM observation of particle cross sections. The results of Examples 1 to 4 and Comparative Example 3 (results of adding Al and performing acid treatment) are shown in FIG. Figure 6 .like Figure 6 As shown in Table 1, voids are formed inside the primary particles. In addition, the SEM images were analyzed to determine the porosity. The results are shown in Table 1.
[0147] (Measurement of the increase in restraint pressure)
[0148] The evaluation batteries obtained in Examples 1 to 4 and Comparative Examples 1 to 3 were charged and the increase in restraint pressure was measured. Specifically, the evaluation batteries were restrained at a pressure of 5 MPa using a restraint fixture capable of measuring the restraint pressure using a force sensor, placed in a desiccator, and charged to a voltage of 4.55 V at a constant current of 0.1 C. The restraint pressure at 4.55 V was measured to determine the increase in restraint pressure from the state before charging. The results are shown in Table 1. The results of the increase in restraint pressure in Table 1 are relative values when the results of Comparative Example 1 are set to 1.
[0149] Table 1
[0150]
[0151] As shown in Table 1, it was confirmed that Examples 1 to 4 had a smaller increase in the restraint pressure than Comparative Examples 1 to 3. In addition, the following points were confirmed. First, regarding the lattice constant, it was confirmed that Examples 1 to 4 had a larger lattice constant than Comparative Example 1. It is speculated that the reason for the increase in the lattice constant is that part of Si is replaced by Al as a foreign element. Through this replacement, the cage of the silicon inclusion compound type crystal phase becomes larger (the density as an active material becomes lower), and as a result, it is speculated that even if Li is filled, the increase in restraint pressure can be suppressed.
[0152] Secondly, in Examples 1 to 4, by-products were removed by acid treatment, and voids were formed inside the primary particles. Thus, it is inferred that in Examples 1 to 4, by forming voids inside the primary particles, even if Li is filled, the increase in the restraint pressure can be suppressed. On the other hand, in Comparative Example 1, since Al is not added, no voids are formed inside the primary particles.
[0153] In Comparative Example 2, since no acid treatment was performed, no voids were formed inside the primary particles. It is speculated that since no acid treatment was performed in Comparative Example 2, byproducts remained in the active material, and the effect of suppressing the increase in restraint pressure was not obtained. In addition, it is speculated that the remaining byproducts became resistance, hindering the Li ion path, resulting in an increase in resistance.
[0154] In Comparative Example 3, the increase in restraint pressure is greater than that in Comparative Example 1. This is presumably because a large amount of Al is input, and thus a large amount of by-products are generated, making it difficult to maintain a silicon inclusion type crystal phase after the acid treatment.
Claims
1. An active substance, Contains at least Si and Al, A silicon inclusion compound II type crystalline phase is present as a main phase. The active material has voids inside the primary particles. The ratio of the Al to the total of the Si and the Al is 0.1 atomic % or more and 1 atomic % or less.
2. The active substance according to claim 1, The void ratio of the voids is 2% or more and 15% or less.
3. A battery comprising a positive electrode layer, a negative electrode layer, and an electrolyte layer formed between the positive electrode layer and the negative electrode layer, The negative electrode layer contains the active material according to claim 1 or 2.
4. A method for producing the active material according to claim 1 or 2, comprising: A step of preparing a Zinter compound, wherein the Zinter compound contains Na, Si and Al, has at least a Zinter phase, and the ratio of the Al to the total of the Si and the Al is less than 10 atomic %; A step of removing Na from the Zintir compound to form an intermediate having a silicon inclusion compound type crystal phase; and and an Al removing step of removing the Al from the intermediate.
5. The method for producing an active material according to claim 4, The preparation step is a step of preparing the Zintl compound by heat-treating a raw material mixture containing a Na source, a Si source, and an Al source.
6. A method for manufacturing a battery, comprising: An active material production process of producing an active material using the method for producing an active material according to claim 4 or 5; and A negative electrode layer forming step of forming a negative electrode layer using the active material.
Citation Information
Patent Citations
Silicon Clathrate Anodes For Lithium-Ion Batteries
US20120021283A1
Electrode active material, method for manufacturing electrode active material, electrode, cell, and method for using clathrate compound
WO2014050100A1
Negative electrode active material for lithium secondary battery, its manufacturing method, and lithium secondary battery
JP2004214054A
Active material, battery and method for producing active material
US20200176768A1