Color electrophoretic display

By using electrophoretic media of light-scattering particles and non-light-scattering particles in the electrophoretic display, the problems of slow switching speed and insufficient color quality of full-color displays in the existing technology are solved, and fast switching and high color gamut display effects are achieved.

CN113795787BActive Publication Date: 2024-10-18E INK CORP
View PDF 145 Cites 0 Cited by

Patent Information

Application Number
CN202080033283.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-07
Publication Date
2024-10-18
Estimated Expiration
2040-05-07

AI Technical Summary

Technical Problem

Existing full-color electrophoretic displays have problems such as slow switching speed, high addressing voltage, or compromised color quality, making it difficult to achieve efficient full-color display.

Method used

An electrophoretic medium containing light-scattering particles and a variety of charged particles is used. The light-scattering particles and non-light-scattering particles have different colors. By adjusting the Zeta potential of the particles and the mass fraction of the polymer shell, fast switching and high color are achieved. Domain display.

Benefits of technology

Improved display switching times without sacrificing overall color gamut, enabling faster image transitions and high-quality color display.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113795787B_ABST
    Figure CN113795787B_ABST
Patent Text Reader

Abstract

An electrophoretic medium includes a fluid, a plurality of light scattering charged particles having a first polarity, and a first group of particles, a second group of particles, and a third group of particles, each group having a different color from each other. The first particles and the second particles may have a second polarity opposite to the first polarity, and the mobility of the third group of particles is less than half of the mobility of the light scattering particles, the first group of charged particles, and the second group of charged particles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Citation of Related Applications

[0002] This application claims priority to U.S. Patent Application No. 62 / 846,342, filed on May 10, 2019, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to a color electrophoretic display, and more particularly to an electrophoretic display capable of presenting more than two colors using a single layer of electrophoretic material including a plurality of color particles. Background Art

[0004] The term color as used herein includes black and white.White particles are generally of the light scattering type.

[0005] The term "gray state" is used herein in its conventional sense in the field of imaging, referring to a state between the two extreme optical states of a pixel, but does not necessarily mean a black-white transition between the two extreme states. For example, several patents and published applications of Iink Corporation referred to below describe electrophoretic displays in which the extreme states are white and dark blue, so that the intermediate gray state is actually light blue. In fact, as already mentioned, the change in optical state may not be a color change at all. The terms "black" and "white" may be used hereinafter to refer to the two extreme optical states of a display, and should be understood to generally include extreme optical states that are not strictly black and white, such as the white and dark blue states mentioned above.

[0006] The terms "bistable" and "bistable" are used herein in their conventional sense in the art to refer to a display including a display element having a first display state and a second display state, wherein at least one optical property of the first and second display states differs such that after any given element is driven to assume its first or second display state with an addressing pulse of finite duration, that state will persist after termination of the addressing pulse for a time at least several times (e.g., at least 4 times) the minimum duration of the addressing pulse required to change the state of the display element. It is shown in U.S. Pat. No. 7,170,670 that some particle-based electrophoretic displays supporting grayscale can be stable not only in their extreme black and white states, but also in their intermediate gray states, as well as some other types of electro-optical displays. Such types of displays are properly referred to as multistable rather than bistable, but for convenience, the term "bistable" will be used herein to cover both bistable and multistable displays.

[0007] The term "impulse", when used in reference to driving an electrophoretic display, is used herein to refer to the integral of the applied voltage with respect to time during the period of time that the display is driven.

[0008] Particles that absorb, scatter or reflect broadband or selected wavelengths of light are referred to herein as color or pigment particles. Various materials that absorb or reflect light other than pigments (which term means in a strict sense an insoluble color material) such as dyes or photonic crystals may also be used in the electrophoretic media and displays of the present invention.

[0009] Particle-based electrophoretic displays have been the subject of intensive research and development for many years. In such displays, a plurality of charged particles (sometimes referred to as pigment particles) move through a fluid under the influence of an electric field. Compared to liquid crystal displays, electrophoretic displays may have the following properties: good brightness and contrast, wide viewing angle, state bistability, and low power consumption. However, problems with the long-term image quality of these displays have prevented their widespread use. For example, the particles that make up electrophoretic displays tend to settle, resulting in insufficient service life for these displays.

[0010] As mentioned above, the electrophoretic medium requires the presence of a fluid. In most prior art electrophoretic media, the fluid is liquid, but the electrophoretic medium can be produced using a gaseous fluid; see, for example, Kitamura, T. et al., Electrical toner movement for electronic paper-like display, IDW Japan, 2001, Paper HCS1-1, and Yamaguchi, Y. et al., Toner display using insulative particles charged triboelectrically, IDW Japan, 2001, Paper AMD4-4. See also U.S. Patent Nos. 7,321,459 and 7,236,291. When such a gas-based electrophoretic medium is used in a direction that allows particle sedimentation, such as when used in a signboard where the medium is arranged in a vertical plane, such a gas-based electrophoretic medium appears to be susceptible to the same type of problems caused by particle sedimentation as a liquid-based electrophoretic medium. In fact, the particle settling problem is more severe in gas-based electrophoretic media than in liquid-based electrophoretic media because the lower viscosity of the gaseous suspending fluid compared to liquids allows for faster settling of the electrophoretic particles.

[0011] Numerous patents and applications assigned to or in the name of the Massachusetts Institute of Technology (MIT) and Ink Corp. describe various techniques for encapsulated electrophoretic and other electro-optical media. Such encapsulated media include a plurality of small capsules, each of which itself includes an inner phase containing electrophoretically mobile particles in a fluid medium and a capsule wall surrounding the inner phase. Typically, the capsules themselves are held in a polymer binder to form a coherent layer between two electrodes. The techniques described in these patents and applications include:

[0012] (a) electrophoretic particles, fluids, and fluid additives; see, e.g., U.S. Pat. Nos. 7,002,728 and 7,679,814;

[0013] (b) capsules, binders and encapsulation processes; see, e.g., U.S. Pat. Nos. 6,922,276 and 7,411,719;

[0014] (c) Films and subassemblies containing electro-optical materials; see, e.g., U.S. Patent Nos. 6,982,178 and 7,839,564;

[0015] (d) Backplanes, adhesive layers and other auxiliary layers and methods for use in displays; see, e.g., U.S. Pat. Nos. 7,116,318 and 7,535,624;

[0016] (e) Color formation and color adjustment; see, e.g., U.S. Patent Nos. 6,017,584; 6,664,944; 6,864,875; 7,075,502; 7,167,155; 7,667,684; 7,791,789; 7,839,564; 7,956,841; 8,040,594; 8,054,526; 8,098,418; 8,213,076 and 8,363,299; and U.S. Patent Application Publication Nos. 2004 / 0263947; 2007 / 0223079; 2008 / 0023332; 2008 / 0043 318; 2008 / 0048970; 2009 / 0004442; 2009 / 0225398; 2010 / 0103502; 2010 / 0156780; 2011 / 0164307; 2011 / 0195629; 2011 / 0310461; 2012 / 0008188; 2012 / 0019898; 2012 / 0075687; 2012 / 0081779; 2012 / 0134009; 2012 / 0182597; 2012 / 0212462; 2012 / 0157269; and 2012 / 0326957;

[0017] (f) Methods for driving displays; see, e.g., U.S. Patent Nos. 5,930,026; 6,445,489; 6,504,524; 6,512,354; 6,531,997; 6,753,999; 6,825,970; 6,900,851; 6,995,550; 7,012,600; 7,023,420; 7,034,783; 7,116,466; 7,119,772; 7,193,625; 7,202,847; 7,259,744; 7,30 4,787; 7,312,794; 7,327,511; 7,453,445; 7,492,339; 7,528,822; 7,545,358; 7,583,251; 7,602,374; 7,612,760; 7,679,599; 7,688,297; 7,729,039; 7,733,311; 7,733,335; 7,787,169; 7,952,557; 7,956,841; 7,999,787; 8,077,141; 8,12 and U.S. Patent Application Publication Nos. 2003 / 0102858; 2005 / 0122284; 2005 / 0253777; 2007 / 0091418; 2007 / 0103427; 2008 / 0024429; 2008 / 0024482 ; 2008 / 0136774; 2008 / 0291129; 2009 / 0174651; 2009 / 0179923; 2009 / 0195568; 2009 / 0322721; 2010 / 0220121; 2010 / 0265561; 2011 / 0193840; 2011 / 0193841; 2011 / 0199671; 2011 / 0285754; and 2013 / 0194250 (these patents and applications may be referred to hereinafter as MEDEOD (MEthods for Driving Electro-optic Displays) applications);

[0018] (g) Display applications; see, e.g., U.S. Patent Nos. 7,312,784 and 8,009,348; and

[0019] (h) Non-electrophoretic displays, such as described in U.S. Patent Nos. 6,241,921; 6,950,220; 7,420,549 and 8,319,759; and U.S. Patent Application Publication No. 2012 / 0293858.

[0020] Many of the aforementioned patents and applications recognize that the walls surrounding discrete microcapsules in an encapsulated electrophoretic medium can be replaced by a continuous phase, thereby producing a so-called polymer-dispersed electrophoretic display, wherein the electrophoretic medium includes a plurality of discrete droplets of an electrophoretic fluid and a continuous phase of a polymer material, and the discrete droplets of electrophoretic fluid within such a polymer-dispersed electrophoretic display can be considered to be capsules or microcapsules, even though there is no discrete capsule membrane associated with each individual droplet; see, e.g., U.S. Patent No. 6,866,760. Therefore, for the purposes of this application, such polymer-dispersed electrophoretic media are considered to be a subclass of encapsulated electrophoretic media.

[0021] A related type of electrophoretic display is the so-called microcell electrophoretic display. In a microcell electrophoretic display, the charged particles and fluid are not encapsulated in microcapsules, but are held in a plurality of cavities formed in a carrier medium (usually a polymer film). See, for example, U.S. Patent Nos. 6,672,921 and 6,788,449, both assigned to Sipix Imaging.

[0022] Although electrophoretic media are typically opaque (because, for example, in many electrophoretic media, the particles substantially block visible light from being transmitted through the display) and operate in a reflective mode, many electrophoretic displays can be made to operate in a so-called "shutter mode," in which one display state is substantially opaque and one display state is light-transmissive. See, for example, U.S. Patents Nos. 5,872,552, 6,130,774, 6,144,361, 6,172,798, 6,271,823, 6,225,971, and 6,184,856. Dielectrophoretic displays, which are similar to electrophoretic displays but rely on changes in electric field strength, can operate in a similar mode; see U.S. Patent No. 4,418,346. Other types of electro-optical displays can also operate in a shutter mode. Electro-optical media operating in a shutter mode can be used in a multilayer structure for a full-color display; in this structure, at least one layer adjacent to the viewing surface of the display is operated in a shutter mode to expose or hide a second layer further away from the viewing surface.

[0023] Packaged electrophoretic displays are generally not plagued by the aggregation and sedimentation failure modes of conventional electrophoretic devices and offer additional benefits, such as the ability to print or coat the display on a variety of flexible and rigid substrates. (The use of the term "printing" is intended to include all forms of printing and coating, including but not limited to: pre-metered coating such as patch die coating, slot or extrusion coating, slide or laminate coating, curtain coating; roll coating such as roller blade coating, forward and reverse roll coating; gravure coating; dip coating; spray coating; meniscus coating; spin coating; brush coating; air knife coating; screen printing process; electrostatic printing process; thermal printing process; inkjet printing process; electrophoretic deposition (see U.S. Patent No. 7,339,715); and other similar technologies.) Therefore, the resulting display can be flexible. In addition, because the display medium can be printed (using a variety of methods), the display itself can be inexpensively manufactured.

[0024] The aforementioned U.S. Patent No. 6,982,178 describes a method of assembling solid-state electro-optical displays (including packaged electrophoretic displays) that is well suited for mass production. In essence, the patent describes a so-called front plane laminate (FPL), which includes, in sequence, a light-transmitting conductive layer, a solid electro-optic medium layer in electrical contact with the conductive layer, an adhesive layer, and a release sheet. Typically, the light-transmitting conductive layer will be carried on a light-transmitting substrate, which is preferably flexible in the sense that the substrate can be manually wound on a drum of (for example) 10 inches (254 mm) in diameter without permanent deformation. The term "light-transmitting" is used in the patent and refers here to the fact that the layer designated thereby transmits sufficient light to enable an observer viewing through the layer to observe changes in the display state of the electro-optic medium, which is usually observed through the conductive layer and the adjacent substrate (if present); in the case where the electro-optic medium displays changes in reflectivity of invisible wavelengths, the term "light-transmitting" should of course be understood to refer to the transmission of the relevant invisible wavelengths. The substrate is typically a polymer film and typically has a thickness in the range of about 1 to about 25 mils (25-634 μm), preferably about 2 to about 10 mils (51-254 μm). Conveniently, the conductive layer is a thin metal layer or metal oxide layer such as aluminum or indium tin oxide (ITO), or can be a conductive polymer. Poly(ethylene terephthalate) (PET) films coated with aluminum or ITO are commercially available, such as aluminized Mylar (Mylar is a registered trademark) from DuPont of Wilmington, Delaware, and this commercial material can be used for the front plane laminate with good results.

[0025] Assembly of an electro-optical display using such a front plane laminate can be accomplished by removing the release sheet from the front plane laminate and contacting the adhesive layer with the backplane under conditions effective to cause the adhesive layer to adhere to the backplane, thereby securing the adhesive layer, electro-optical medium layer, and conductive layer to the backplane. This process is well suited to mass production because the front plane laminate can be mass produced, typically using roll-to-roll coating techniques, and then cut into sheets of any size required for a particular backplane.

[0026] U.S. Patent No. 7,561,324 describes a so-called double release sheet which is essentially a simplified version of the front plane laminate of the aforementioned U.S. Patent No. 6,982,178. One form of the double release sheet comprises a layer of a solid electro-optic medium sandwiched between two adhesive layers, one or both of which are covered by a release sheet. Another form of the double release sheet comprises a layer of a solid electro-optic medium sandwiched between two release sheets. Both forms of double release films are intended for use in a process generally similar to that of assembling an electro-optic display from the above-described front plane laminate, but involving two separate laminations; typically, in a first lamination, the double release sheet is laminated to the front electrode to form a front subassembly, and thereafter, in a second lamination, the front subassembly is laminated to the backplane to form the final display, although the order of the two laminations may be reversed as desired.

[0027] U.S. Patent No. 7,839,564 describes a so-called inverted front plane laminate, which is a variation of the front plane laminate described in the aforementioned U.S. Patent No. 6,982,178. The inverted front plane laminate includes, in sequence, at least one of a light-transmitting protective layer and a light-transmitting conductive layer, an adhesive layer, a solid electro-optic medium layer, and a release sheet. The inverted front plane laminate is used to form an electro-optic display having a laminated adhesive layer between the electro-optic layer and the front electrode or front substrate, and a second typically thin adhesive layer may or may not be present between the electro-optic layer and the backplane. Such an electro-optic display can combine good resolution with good low temperature performance.

[0028] As described above, the simplest prior art electrophoretic media essentially display only two colors. Such electrophoretic media use electrophoretic particles of one type having a first color in a colored fluid having a different second color (in this case, the first color is displayed when the particles are adjacent to the viewing surface of the display, and the second color is displayed when the particles are separated from the viewing surface), or electrophoretic particles of the first type and the second type having different first and second colors in a colorless fluid (in this case, the first color is displayed when the first type of particles are adjacent to the viewing surface of the display, and the second color is displayed when the second type of particles are adjacent to the viewing surface). Typically, the two colors are black and white. If a full-color display is desired, a color filter array can be placed on the viewing surface of a monochrome (black and white) display. Displays with color filter arrays rely on area sharing and color mixing to create color stimuli. The available display area is shared between three or four primary colors such as red / green / blue (RGB) or red / green / blue / white (RGBW), and the filters can be arranged in a one-dimensional (striped) or two-dimensional (2×2) repeating pattern. Other choices of primary colors or more than three primary colors are also known in the art. Three (in the case of an RGB display) or four (in the case of an RGBW display) sub-pixels are selected to be small enough so that at the desired viewing distance, they visually blend together into a single pixel with a uniform color stimulus ("color mixing"). The inherent drawback of area sharing is that the colorant is always present, and the color can only be modulated by switching the corresponding pixel of the underlying monochrome display to white or black (turning the corresponding primary color on or off). For example, in an ideal RGBW display, each of the red, green, blue and white primary colors occupies a quarter of the display area (a quarter of the sub-pixels), wherein the white sub-pixel is as bright as the monochrome display white below, and each of the color sub-pixels is no brighter than one-third of the monochrome display white. The brightness of the white shown by the display as a whole cannot be greater than half the brightness of the white sub-pixel (the white area of ​​the display is generated by displaying one white sub-pixel for every four sub-pixels, plus each color sub-pixel in color form is equivalent to one-third of the white sub-pixel, so that the contribution of the combined three color sub-pixels is no more than one white sub-pixel). In the case where the color pixels are switched to black, the brightness and saturation of the color are reduced by area sharing. Area sharing is particularly problematic when mixing yellow because it is brighter than any other color of equal brightness, and saturated yellow is almost as bright as white. Switching the blue pixels (a quarter of the display area) to black makes yellow too dark.

[0029] Multilayer stacked electrophoretic displays are known in the art; see, for example, J. Heikenfeld, P. Drzaic, JS Yeo and T. Koch, Journal of the SID, 19(2), 2011, pp. 129-156. In such displays, ambient light is passed through the image in each of the three primary colors in a subtractive manner, much like conventional color printing. U.S. Patent No. 6,727,873 describes a stacked electrophoretic display in which three layers of switchable cells are placed on a reflective background. Similar displays are known in which the color particles are moved laterally (see International Application No. WO 2008 / 065605) or isolated into micropits using a combination of vertical and lateral movement. In both cases, each layer is provided with electrodes for concentrating or dispersing the color particles on a pixel-by-pixel basis, so that each of the three layers requires a thin film transistor (TFT) (two of the three layers of the TFT must be substantially transparent) and a light-transmitting counter electrode. Such complex arrangements of electrodes are expensive to manufacture, and in the prior art it is difficult to provide a sufficiently transparent plane for the pixel electrodes, particularly when the white state of the display must be viewed through several layers of electrodes. Multilayer displays also suffer from parallax problems because the thickness of the display stack approaches or exceeds the pixel size.

[0030] U.S. Application Publication Nos. 2012 / 0008188 and 2012 / 0134009 describe a multicolor electrophoretic display having a single backplane that includes independently addressable pixel electrodes and a common light-transmitting front electrode. Multiple electrophoretic layers are arranged between the backplane and the front electrode. The displays described in these applications are capable of presenting any of the primary colors (red, green, blue, cyan, magenta, yellow, white, and black) at any pixel location. However, there are disadvantages to using multiple electrophoretic layers located between a single set of addressing electrodes. The electric field experienced by particles in a particular layer is lower than that of a single electrophoretic layer addressed with the same voltage. In addition, optical losses in the electrophoretic layer closest to the viewing surface (e.g., caused by light scattering or undesired absorption) may affect the appearance of the image formed in the electrophoretic layer below.

[0031] Attempts have been made to provide a full-color electrophoretic display using a single electrophoretic layer. For example, U.S. Patent Application Publication No. 2013 / 0208338 describes a color display including an electrophoretic fluid including one or two types of pigment particles dispersed in a transparent and colorless or colored solvent, the electrophoretic fluid being sandwiched between a common electrode and a plurality of drive electrodes. The drive electrodes are held at a specific distance to expose a background layer. U.S. Patent Application Publication No. 2014 / 0177031 describes a method for driving a display unit filled with an electrophoretic fluid including two types of charged particles carrying opposite charge polarities and having two contrasting colors. The two types of pigment particles are dispersed in a colored solvent or in a solvent in which uncharged or slightly charged colored particles are dispersed. The method includes driving the display unit to display the color of the solvent or the color of the uncharged or slightly charged colored particles by applying a drive voltage, wherein the drive voltage is about 1 to about 20% of the full drive voltage. U.S. Patent Application Publication Nos. 2014 / 0092465 and 2014 / 0092466 describe electrophoretic fluids and methods for driving electrophoretic displays. The fluid includes first, second, and third types of pigment particles, all of which are dispersed in a solvent or solvent mixture. The first and second types of pigment particles carry opposite charge polarities, and the third type of pigment particles have a charge level that is less than about 50% of the charge level of the first or second types. The three types of pigment particles have different levels of threshold voltage, or different levels of mobility, or both. None of these patent applications discloses a full-color display in the sense in which the term "full-color display" is used below.

[0032] U.S. Patent Application Publication No. 2007 / 0031031 describes an image processing device for processing image data to display an image on a display medium, wherein each pixel is capable of displaying white, black, and one other color. U.S. Patent Application Publication Nos. 2008 / 0151355; 2010 / 0188732 and 2011 / 0279885 describe color displays in which mobile particles move through a porous structure. U.S. Patent Application Publication Nos. 2008 / 0303779 and 2010 / 0020384 describe display media that include first particles, second particles, and third particles of different colors. The first particles and the second particles can form aggregates, and smaller third particles can move through pores left between the aggregated first particles and the second particles. U.S. Patent Application Publication No. 2011 / 0134506 describes a display device including an electrophoretic display element, the electrophoretic display element including: a plurality of types of particles encapsulated between a pair of substrates, at least one of the substrates being translucent and each of the corresponding plurality of types of particles having a charge of the same polarity, having different optical properties and being different in migration speed and / or electric field threshold for movement, a translucent display side electrode being arranged on the side of the substrate on which the translucent substrate is arranged, a first back side electrode being arranged on the side of the other substrate, facing the display side electrode, and a second back side electrode being arranged on the side of the other substrate, facing the display side electrode; and a voltage control unit that controls the voltage applied to the display side electrode, the first back side electrode, and the second back side electrode so that particles of the type having the fastest migration speed among the plurality of types of particles, or particles of the type having the lowest threshold among the plurality of types of particles, sequentially pass through each of the different types of particles, move to the first back side electrode or move to the second back side electrode, and then the particles moving to the first back side electrode move to the display side electrode. U.S. Patent Application Publication Nos. 2011 / 0175939; 2011 / 0298835; 2012 / 0327504 and 2012 / 0139966 describe color displays that rely on the aggregation of multiple particles and threshold voltage. U.S. Patent Application Publication No. 2013 / 0222884 describes electrophoretic particles that include: color particles that include a polymer containing a charged group and a colorant; and a branched silicone-based polymer that is attached to the color particles and includes a reactive monomer and at least one monomer selected from a specific set of monomers as a copolymerization component. U.S. Patent Application Publication No. 2013 / 0222885 describes a dispersion for an electrophoretic display, which includes a dispersion medium, a group of colored electrophoretic particles dispersed in the dispersion medium and migrating in an electric field, a group of non-electrophoretic particles that do not migrate and have a color different from that of the electrophoretic particle group, and a compound having a neutral polar group and a hydrophobic group, which is contained in the dispersion medium in a proportion of about 0.01 to about 1 mass % based on the entire dispersion.U.S. Patent Application Publication No. 2013 / 0222886 describes a dispersion for a display, including floating particles, which includes: core particles including a colorant and a hydrophilic resin; and a dispersion having 7.95 (J / cm2 and covering the surface of each of the core particles. 3 ) 1 / 2 or greater solubility parameter difference. U.S. Patent Application Publication Nos. 2013 / 0222887 and 2013 / 0222888 describe electrophoretic particles having a specified chemical composition. Finally, U.S. Patent Application Publication No. 2014 / 0104675 describes a particle dispersion including first color particles and second color particles that move in response to an electric field, and a dispersion medium, the second color particles having a larger diameter than the first color particles and a charging characteristic that is the same as the charging characteristic of the first color particles, wherein the ratio of the charge Cs of the first color particles to the charge Cl of the second color particles per unit area of ​​the display (Cs / Cl) is less than or equal to 5. Some of the aforementioned displays provide full color but at the expense of requiring a long and cumbersome addressing method.

[0033] U.S. Patent Application Publication Nos. 2012 / 0314273 and 2014 / 0002889 describe an electrophoretic device including a plurality of first and second electrophoretic particles contained in an insulating liquid, the first and second particles having different charging characteristics different from each other; the device also includes a porous layer, the porous layer being included in the insulating liquid and formed of a fiber structure. These patent applications are not full-color displays in the sense of the term "full-color display" used hereinafter.

[0034] See also US Patent Application Publication No. 2011 / 0134506 and US Patent No. 9,697,778, the latter describing a full color display using three different types of particles in a colored fluid, but the presence of the colored fluid limits the quality of the white state that can be achieved by the display.

[0035] In summary, the prior art is that full color displays usually involve compromises such as slow switching speeds (up to several seconds), high addressing voltages or compromises regarding color quality.Therefore, there is a need for improved full color electrophoretic displays. Summary of the invention

[0036] In a first aspect, a novel electrophoretic medium is provided, comprising: a fluid; a plurality of light scattering charged particles having a first polarity; and a first group of charged particles, a second group of charged particles, and a third group of charged particles, each group having a different color from each other, wherein the first particles and the second particles have a second polarity opposite to the first polarity, and the third particles are composite particles comprising a core pigment and a polymer shell, wherein: (a) the mass fraction of the polymer shell relative to the composite particles is at least 20 wt % to at most 50 wt %; and (b) the polymer shell comprises: (I) a first monomer unit derived from a first precursor of formula (1):

[0037] CH2=C(R 1a )C(O)R 2 (1)

[0039] Where: R 1a is –H or –CH3; R 2 Yes-OR 3 , –NHR 3 or -NR 3 2; R 3 It is C 1-6 Alkyl, C 1-6 Heteroalkyl, C 3-10 Cycloalkyl, C 3-10 Heterocycloalkyl, C 6-14 Aryl, C 5-14 heteroaryl or any combination thereof, each of which is optionally independently selected from R 4 The group is substituted one or more times; R 4 It is C 1-6 Alkyl, -OH, C 1-6 Alkoxy, -NH2, -NH(C 1-6 Alkyl), -N(C 1-6 Alkyl)2, C 1-6 Haloalkyl, or C 1-6 Haloalkoxy; (II) a second monomer unit derived from a second precursor of formula (2):

[0040] CH2=C(R 1b )C(O)R 5 (2)

[0042] Where: R 1b is –H or –CH3; R 5 Yes-OR 6 , –NHR 6 or -NR 6 2; R 6 It is C 1-6 Alkyl, C 1-6 Heteroalkyl, C3-10 Cycloalkyl, C 3-10 Heterocycloalkyl, C 6-14 Aryl, C 5-14 heteroaryl or any combination thereof, each of which is independently selected from R 7 The group is substituted one or more times; R 7 is halogen, -CN, -NO2, -S(O)- or -S(O)2-. In one embodiment, R 3 It is C 1-6 Alkyl, C 6-14 Aryl or any combination thereof, each of which is optionally independently selected from R 4 substituted one or more times by a group; and R 4 It is C 1-6 Alkyl or C 1-6 In another embodiment, R 2 Yes-OR 3 , and R 3 It is C 1-6 Alkyl or C 6-14 Aryl, C 6-14 Aryl is optionally independently selected from R 4 substituted one or more times by a group; and R 4 C 1-6 In another embodiment, R 6 It is C 1-6 Alkyl and R 7 is a halogen. Also provided is an embodiment wherein R 5 Yes-OR 6 , R 6 Is R 7 Replace at least three times C 1-6 Alkyl, and R 7Is -F. The first precursor may be selected from the group consisting of methyl methacrylate, methoxyphenyl methacrylate and N, N-diisopropylacrylamide. The second precursor may be trifluoroethyl methacrylate (TFEM). In the third particle, the mass fraction of the polymer shell relative to the composite particle may be at least 20wt% to a maximum of 50wt%. The mass fraction of the polymer shell relative to the composite particle may be measured by thermogravimetric analysis (TGA). The fluid may be a liquid having a dielectric constant less than or equal to 5. The electrophoretic medium may also include a charge control agent. Each color of the first group of charged particles, the second group of charged particles and the third group of charged particles may be independently selected from the group consisting of red, green, blue, magenta, cyan and yellow. At least two of the first charged particles, the second charged particles and the third charged particles may be non-light scattering. In one embodiment, the light scattering charged particles are white and the first group of particles, the second group of particles and the third group of particles are non-light scattering. In another embodiment, the light scattering charged particles are negatively charged, and the first group of particles and the second group of particles are positively charged. The fluid may have dissolved or dispersed therein a polymer having a number average molecular weight in excess of about 20,000 and which is substantially free of adsorbed particles.

[0043] In a second aspect, an electrophoretic medium is provided, comprising: a fluid; a plurality of light scattering charged particles having a first polarity; and a first group of charged particles, a second group of charged particles, and a third group of charged particles, each group having a different color from each other, wherein the first particles and the second particles have a second polarity opposite to the first polarity, and the magnitude of the electrophoretic mobility of the third group of particles is less than half the magnitude of the electrophoretic mobility of the light scattering particles, the first group of charged particles, and the second group of charged particles. The fluid may be a liquid having a dielectric constant less than or equal to 5. The electrophoretic medium may also include a charge control agent. The electrophoretic mobility may be measured based on the particle Zeta potential. In one embodiment, the third group of particles has a Zeta potential greater than or equal to -20 mV and less than or equal to 20 mV. The electrophoretic mobility may also be measured based on a particle charge-to-mass ratio or a particle dispersed conductivity measurement. In one embodiment, each color of the first group of charged particles, the second group of charged particles, and the third group of charged particles is independently selected from the group consisting of red, green, blue, magenta, cyan, and yellow. At least two of the first charged particles, the second charged particles, and the third charged particles can be non-light scattering. For example, the light scattering charged particles can be white, and the first group of particles, the second group of particles, and the third group of particles can be non-light scattering. In a non-limiting embodiment, the light scattering charged particles are negatively charged, and the first group of particles and the second group of particles are positively charged. A polymer having a number average molecular weight of more than about 20,000 and substantially non-absorbing particles may be dissolved or dispersed in the fluid.

[0044] In a third aspect, an electrophoretic medium is provided, comprising: a fluid; a plurality of light scattering charged particles having a first polarity; and a first group of charged particles, a second group of charged particles, and a third group of charged particles, each group having a different color from each other, wherein the first particles and the second particles have a second polarity opposite to the first polarity, and the third particles are composite particles comprising a core pigment and a polymer shell, wherein: (a) the mass fraction of the polymer shell relative to the composite particles is at least 20 wt % to at most 50 wt %; and (b) the polymer shell comprises: (I) a first monomer unit derived from a first precursor of formula (1):

[0045] CH2=C(R 1a )C(O)R 2 (1)

[0047] Where: R 1a is –H or –CH3; R 2 Yes-OR 3 , –NHR 3 or -NR 3 2; R 3 It is C 1-6 Alkyl, C 1-6 Heteroalkyl, C 3-10 Cycloalkyl, C 3-10 Heterocycloalkyl, C 6-14 Aryl, C 5-14 heteroaryl or any combination thereof, each of which is optionally independently selected from R 4 The group is substituted one or more times; R 4 It is C 1-6 Alkyl, -OH, C 1-6 Alkoxy, -NH2, -NH(C 1-6 Alkyl), -N(C 1-6 Alkyl)2, C 1-6 Haloalkyl, or C 1-6 (II) a second monomer unit derived from styrene, styrene optionally independently selected from C 1-6 Alkyl, C 1-6 Alkoxy, -NH(C 1-6 Alkyl), -N(C 1-6 alkyl) 2 and halogen groups are substituted one or more times. In one embodiment, R 3 It is C 1-6 Alkyl, C 6-14 Aryl or any combination thereof, each of which is optionally independently selected from R 4 substituted one or more times by a group; and R 4 It is C 1-6 Alkyl or C 1-6In another embodiment, R 2 Yes-OR 3 , and R 3 It is C 1-6 Alkyl or C 6-14 Aryl, C 6-14 Aryl is optionally independently selected from R 4 substituted one or more times by a group; and R 4 C 1-6 Alkoxy. In the third particle, the mass fraction of the polymer shell relative to the composite particle is at least 25wt% to at most 40wt%. The mass fraction of the polymer shell relative to the composite particle can be measured by thermogravimetric analysis (TGA). The fluid can be a liquid having a dielectric constant less than or equal to 5. The electrophoretic medium can also include a charge control agent. Each color of the first group of charged particles, the second group of charged particles, and the third group of charged particles is independently selected from the group consisting of red, green, blue, magenta, cyan, and yellow. At least two of the first charged particles, the second charged particles, and the third charged particles can be non-light scattering. In one embodiment, the light scattering charged particles are white and the first group of particles, the second group of particles, and the third group of particles are non-light scattering. In another non-limiting embodiment, the light scattering charged particles are negatively charged, and the first group of particles and the second group of particles are positively charged. A polymer having a number average molecular weight exceeding about 20,000 and substantially not absorbing particles may be dissolved or dispersed in the fluid.

[0048] The electrophoretic medium of the present invention may be in any of the forms discussed above. Thus, the electrophoretic medium may be unencapsulated, encapsulated in discrete capsules surrounded by a capsule wall, or in the form of a polymer dispersion or micro-unit medium.

[0049] The invention extends to a front plane laminate, a double release sheet, an inverted front plane laminate or an electrophoretic display comprising the electrophoretic medium of the invention. The display of the invention may be used in any application in which prior art electro-optical displays are used. Thus, for example, the display may be used in an electronic book reader, a portable computer, a tablet computer, a cellular phone, a smart card, a sign, a watch, a shelf label and a flash drive.

[0050] These and other aspects of the invention will be apparent in view of the following description. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 is a schematic diagram of a pigment particle having a copolymer attached to its surface.

[0052] Figure 2 is a graph of predicted and measured zeta potentials for a variety of different composite pigment particles according to various embodiments of the present invention.

[0053] Figure 3 One waveform for driving a display sample including a dispersion according to various embodiments of the present invention is shown.

[0054] Figure 4 Another waveform for driving a display sample including a dispersion according to various embodiments of the present invention is shown.

[0055] Figure 5 It is shown that by applying Figure 3 FIG. 1 is a graph of waveforms obtained for cyan quality as a function of the zeta potential of pigments included in displays made according to various embodiments of the present invention.

[0056] Figure 6 It is shown that by applying Figure 4 Graph of the total color gamut obtained with the waveform as a function of the zeta potential of the pigments included in displays made according to various embodiments of the present invention.

[0057] Figure 7 is a diagram showing that for a display manufactured according to various embodiments of the present invention, by applying Figure 3 The cyan quality obtained by applying the waveform Figure 4 A graph of the total color gamut obtained with the waveform.

[0058] 8 is a schematic cross-sectional view showing the positions of respective particles in the electrophoretic medium when black, white, subtractive three primary colors, and additive three primary colors are displayed.

[0059] Fig. 9 Includes Table 2. DETAILED DESCRIPTION

[0060] definition

[0061] Unless otherwise provided herein, the following terms and phrases have the meanings as shown below. The present disclosure may employ other terms and phrases that are not clearly defined herein. Such other terms and phrases should have the meanings that they would have for a person of ordinary skill in the art within the context of the present disclosure. In some cases, a term or phrase may be defined as a singular or plural form. In this case, it should be understood that any singular term may include its plural counterpart, and vice versa, unless explicitly stated otherwise.

[0062] As used herein, the singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise. For example, reference to "a substituent" includes a single substituent as well as two or more substituents, etc.

[0063] As used herein, "for example," "for example," "such as," or "including" are intended to introduce examples that further illustrate a more general subject matter. Unless explicitly stated otherwise, such examples are provided merely as an aid to understanding the embodiments shown in the present disclosure and are not meant to be limiting in any way. These phrases also do not indicate any kind of preference for the disclosed embodiments.

[0064] As used herein, the term "polymer" refers to a polymeric compound prepared by polymerizing monomers, whether the same or two or more types. Thus, the generic name "polymer" is intended to encompass the term "homopolymer" and the term "interpolymer" as defined below. Trace amounts of impurities may be incorporated into and / or within the polymer structure.

[0065] As used herein, the term "interpolymer" refers to a polymer prepared by polymerizing at least two different monomers. The general name "interpolymer" includes copolymers (used to refer to polymers prepared from two different types of monomers) and polymers prepared from more than two different types of monomers. Thus, "polymers derived from one or more monomers" refers to homopolymers when the monomer is one, copolymers when the monomer is two, and other types of interpolymers when the monomer is three or more.

[0066] The terms "monomeric unit", "monomeric unit", "monomer residue" or "monomer residue" are understood to mean the residue resulting from the polymerization of the corresponding monomer. For example, a polymer derived from the polymerization of styrene monomers will provide polymer segments comprising repeating styrene monomer units, i.e.,

[0067] “—CH(C6H5)CH2—”.

[0068] As used herein, the term "functional group" refers to a linked collection of atoms or a single atom within a molecular entity, wherein a molecular entity is any structurally or isotopically distinct atom, molecule, ion, ion pair, free radical, radical ion, complex, conformer, etc., that is identifiable as an individually distinguishable entity. Unless otherwise indicated, describing a group as "formed" by a particular chemical transformation does not mean that the chemical transformation involves making the molecular entity containing the group.

[0069] As used herein, the various functional groups represented will be understood to have a point of attachment at the functional group with a hyphen or dash (-) or an asterisk (*). In other words, in the case of -CH2CH2CH3, it will be understood that the point of attachment is the leftmost CH2 group. If a group is recited without an asterisk or dash, the point of attachment is represented by the ordinary and common meaning of the listed group.

[0070] As used herein, polyatomic divalent functional groups are read from left to right. For example, if the specification or claims record ADE and D is defined as -OC(O)-, then replacing D with the resulting group is: A-OC(O)-E rather than AC(O)OE.

[0071] As used herein, the term "alkyl" refers to a straight or branched chain saturated hydrocarbon having from 1 to 30 carbon atoms, which may be optionally substituted, with multiple degrees of substitution permitted as further described herein. As used herein, examples of "alkyl" include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, sec-butyl, tert-butyl, isopentyl, n-pentyl, neopentyl, n-hexyl, and 2-ethylhexyl. The number of carbon atoms in an alkyl group is indicated by the phrase "C x-y "Alkyl" means an alkyl group as defined herein containing from x to y (including endpoints) carbon atoms. Thus, "C 1-6 "Alkyl" means an alkyl chain having 1 to 6 carbon atoms, and includes, for example, but is not limited to methyl, ethyl, n-propyl, isopropyl, isobutyl, n-butyl, sec-butyl, tert-butyl, isopentyl, n-pentyl, neopentyl and n-hexyl. In some cases, the "alkyl" group can be divalent, in which case the group can alternatively be referred to as an "alkylene" group. In addition, in some cases, one or more carbon atoms in the alkyl or alkylene group can be replaced by a heteroatom (e.g., where feasible, selected from nitrogen, oxygen or sulfur, including nitrogen oxides, sulfur oxides and sulfur dioxide), and are referred to as "heteroalkyl" or "heteroalkylene" groups.

[0072] As used herein, "cycloalkyl" refers to a 3 to 24-membered cyclic hydrocarbon ring, which may be optionally substituted as further described herein, and multiple degrees of substitution are allowed. Such "cycloalkyl" groups are monocyclic or polycyclic. As used herein, the term "cycloalkyl" does not include ring systems containing aromatic rings, but does include ring systems that may have one or more degrees of unsaturation. As used herein, examples of "cycloalkyl" groups include, but are not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, 1-norbornyl, 2-norbornyl, 7-norbornyl, 1-adamantyl, and 2-adamantyl. In some cases, a "cycloalkyl" group may be divalent, in which case the group may alternatively be referred to as a "cycloalkylene" group. In addition, in some cases, one or more carbon atoms in a cycloalkyl or cycloalkylene group may be replaced by a heteroatom (e.g., where feasible, selected from nitrogen, oxygen, or sulfur, including nitrogen oxides, sulfur oxides, and sulfur dioxide), and are referred to as a "heterocycloalkyl" or "heterocycloalkylene" group.

[0073] As used herein, "aryl" refers to a 6-30-membered cyclic aromatic hydrocarbon, which may be optionally substituted as further described herein, and multiple degrees of substitution are allowed. Examples of "aryl" used herein include, but are not limited to, phenyl and naphthyl. As used herein, the term "aryl" also includes a ring system in which a phenyl or naphthyl is optionally fused to one to three non-aromatic, saturated or unsaturated carbocyclic rings. For example, "aryl" will include a ring system such as indene, which may be attached to an aromatic or non-aromatic ring. In some cases, an "aryl" group may be divalent, in which case the group may alternatively be referred to as an "arylene" group. In addition, as used herein, "arylalkyl" refers to an alkyl substituent (as defined above) further substituted by one or more (e.g., one to three) aryl groups (as defined herein). Similarly, "alkylaryl" refers to an aryl substituent, which is further substituted by one or more (e.g., one to five) alkyl groups.

[0074] As used herein, the term "heteroaryl" refers to a 5- to 30-membered monocyclic or polycyclic ring system that contains at least one aromatic ring and further contains one or more heteroatoms. Such "heteroaryl" groups may be optionally substituted as further described herein, and multiple degrees of substitution are allowed. In a polycyclic "heteroaryl" group containing at least one aromatic ring and at least one non-aromatic ring, the aromatic ring does not need to contain heteroatoms. Thus, for example, as used herein, "heteroaryl" will include indolyl. In addition, the attachment point can be any ring within the ring system, regardless of whether the ring containing the attachment point is aromatic or contains heteroatoms. Thus, for example, as used herein, "heteroaryl" will include indol-1-yl, indol-3-yl, and indol-5-yl. Where feasible, examples of heteroatoms include nitrogen, oxygen, or sulfur atoms, including nitrogen oxides, sulfur oxides, and sulfur dioxide. As used herein, examples of "heteroaryl" groups include, but are not limited to, furanyl, thienyl, pyrrolyl, oxazolyl, thiazolyl, imidazolyl, isoxazolyl, isothiazolyl, 1,2,4-triazolyl, pyrazolyl, pyridinyl, pyridazinyl, pyrimidinyl, indolyl, isoindolyl, benzo[b]thienyl, benzimidazolyl, benzothiazolyl, pteridinyl, and phenazinyl, wherein attachment can occur at any point on the ring as long as attachment is chemically feasible. Thus, for example, "thiazolyl" refers to thiazol-2-yl, thiazol-4-yl, and thiazol-5-yl. In some cases, a "heteroaryl" group may be divalent, in which case the group may alternatively be referred to as a "heteroarylene" group. In addition, as used herein, "heteroarylalkyl" refers to an alkyl substituent (as defined above) that is further substituted with one or more (e.g., one to three) heteroaryl groups (as defined herein). Similarly, "alkylheteroaryl" refers to an aryl substituent that is further substituted with one or more (eg, one to five) alkyl groups.

[0075] As used herein, "alkoxy" refers to -OR, wherein R is an alkyl group (as defined above). The number of carbon atoms in the alkyl group is represented by the phrase "Cx-y alkoxy", which refers to an alkoxy group having an alkyl group containing x to y (including endpoints) carbon atoms as defined herein.

[0076] As used herein, "halogen" or "halo" refers to fluorine, chlorine, bromine and / or iodine. In some embodiments, the term refers to fluorine and / or chlorine. As used herein, "haloalkyl" or "haloalkoxy" refers to an alkyl or alkoxy group substituted with one or more halogen atoms, respectively. The term "perfluoroalkyl" or "perfluoroalkoxy" refers to an alkyl and alkoxy group, respectively, in which each available hydrogen is replaced by fluorine.

[0077] In some cases, the present disclosure may relate to "a combination" or "combinations" of specific groups, which means that two or more of the aforementioned groups can be combined to form a new group. For example, the phrase "R is an alkylene group, an arylene group, or a combination thereof" means that R can be a group containing both an alkylene group and an arylene group, such as -(alkylene)-(arylene)-, -(arylene)-(alkylene)-, -(alkylene)(arylene)(alkylene)-, etc.

[0078] As used herein, "substituted" means that one or more hydrogens of a designated moiety are replaced by the named substituent(s), and unless otherwise indicated, multiple degrees of substitution are permitted provided that the substitution results in a stable or chemically feasible compound. A stable compound or a chemically feasible compound is one whose chemical structure is not substantially altered when maintained at a temperature of about -80°C to about +40°C for at least one week in the absence of moisture or other chemically reactive conditions, or a compound that retains its integrity long enough for electrophoretic applications. As used herein, the phrase "substituted with one or more..." or "substituted one or more times..." refers to the number of substituents, which is equal to one to the maximum number of substituents possible based on the number of available bonding sites, provided that the above-mentioned conditions of stability and chemical feasibility are met.

[0079] As used herein, "optionally" means that the event described subsequently may or may not occur. In some embodiments, the optional event does not occur. In some other embodiments, the optional event does occur one or more times.

[0080] As used herein, "comprising" or "including" or "containing" or "comprising" refers to an open group, meaning that the group may include additional components in addition to those explicitly listed. For example, the phrase "comprising A" means that A must be present, but other components may also be present. The terms "comprising", "having" and "comprising" and their grammatical variations have the same meaning. In contrast, "consisting of" or "composed of" or "consisting of" refers to a closed group. For example, the phrase "consisting of A" means that A and only A are present.

[0081] As used herein, "or" is to be given its broadest reasonable interpretation and is not limited to an "either-or" construction. Thus, the phrase "comprising A or B" means that A may be present and B may not be present, or B may be present and A may not be present, or both A and B may be present. Furthermore, for example, if A defines a class that may have multiple components (e.g., A1 and A2), one or more components of the class may be present at the same time.

[0082] As used herein, "wt%" is an abbreviation for the mass percentage of a given component of an item. It is a way of expressing the composition of a mixture or product in a dimensionless dimension; mole fraction (mole percent, mol%) and volume fraction (vol%) are other ways.

[0083] Detailed description

[0084] As described above, the present invention provides, in one aspect, an electrophoretic medium comprising a light scattering particle (typically white) and three other particles that typically provide subtractive primary colors. When the mobility of one of the particles of the subtractive primary colors (e.g., measured according to Zeta potential) is less than or equal to half the mobility of the other particles in the electrophoretic medium, improved switching times can be achieved without sacrificing the overall color gamut.

[0085] The three particles providing the subtractive primary colors may be substantially non-light scattering ("SNLS"). The use of SNLS particles allows the mixing of colors and provides more color results than can be achieved using the same number of scattering particles. The aforementioned US2012 / 0327504 uses particles with subtractive primary colors, but requires two different voltage thresholds for independent addressing of non-white particles (i.e., using three positive voltages and three negative voltages to address the display). These thresholds must be sufficiently separated to avoid crosstalk, and the separation requires the use of high addressing voltages for some colors. In addition, addressing the colored particles using the highest threshold also moves all other colored particles, and these other particles must then be switched to their desired positions with a lower voltage. This step-by-step color addressing mechanism produces flickering of undesirable colors and long transition times. Specific embodiments of the present invention do not require the use of such a step-by-step waveform, and addressing of all colors can be achieved using only two positive voltages and two negative voltages (i.e., only five different voltages are required in the display, two positive voltages, two negative voltages and zero, but in other embodiments, more different voltages may preferably be used to address the display).

[0086] FIG. 8 of the accompanying drawings is a schematic cross-sectional view showing the positions of individual particles in the electrophoretic medium of the color display described in U.S. Pat. No. 9,921,451 when displaying black, white, subtractive primary colors, and additive primary colors. In FIG. 8 , it is assumed that the viewing surface of the display is at the top (as shown), that is, the user observes the display from this direction and the light is incident from this direction. As previously mentioned, in a preferred embodiment, only one of the four particles used in the electrophoretic medium of the present invention substantially scatters light, and in FIG. 8 , the particle is assumed to be a white pigment. Basically, the white light scattering particles form a white reflector against which any particles above the white particles are observed (as shown in FIG. 8 ). Light entering the viewing surface of the display passes through these particles, reflects from the white particles, returns through these particles and is presented from the display. Thus, the particles above the white particles can absorb various colors, and the colors that appear to the user are generated by the combination of particles above the white particles. Any particles arranged below the white particles (from the user's perspective behind) are masked by the white particles and do not affect the displayed color. Since the second, third and fourth particles are substantially non-light scattering, their order or arrangement relative to each other is unimportant, but their order or arrangement relative to the white (light scattering) particles is critical for the reasons already stated.

[0087] More specifically, when cyan, magenta, and yellow particles are below white particles (case [A] in FIG8 ), there are no particles above the white particles, and the pixel simply displays white. When a single particle is above a white particle, the color of the single particle is displayed, showing yellow, magenta, and cyan in cases [B], [D], and [F], respectively, in FIG8 . When two particles are above a white particle, the displayed color is a combination of the colors of the two particles; in FIG8 , in case [C], the magenta and yellow particles display red, in case [E], the cyan and magenta particles display blue, and in case [G], the yellow and cyan particles display green. Finally, when all three color particles are above white particles (case [H] in FIG8 ), all incident light is absorbed by the particles of the subtractive primary colors, and the pixel displays black.

[0088] It is possible that a subtractive primary color can be presented by particles that scatter light, so that the display will include two types of light scattering particles, one of which is white and the other is colored. However, in this case, the position of the colored light scattering particles with respect to the other colored particles covering the white particles will be important. For example, when presenting black (when all three colored particles are located above the white particles), the colored scattering particles cannot be located above the colored non-scattering particles (otherwise, they will be partially or completely hidden behind the scattering particles, and the presented color will be the color of the colored scattering particles, rather than black).

[0089] If more than one type of colored particles scatters light, black will not be easily rendered.

[0090] FIG. 8 shows an idealized situation in which the color is uncontaminated (i.e., the white light scattering particles completely mask any particles located behind the white particles). In practice, masking with white particles may be imperfect, so that there may be some small amount of absorption of light by particles that would ideally be completely masked. Such contamination will typically reduce both the brightness and chromaticity of the color presented. In the electrophoretic medium of the present invention, such color contamination should be minimized to a degree that the color formed is commensurate with the industrial standard for color reproduction. A particularly preferred standard is SNAP (Standard for Newspaper Advertisement Production), which specifies L*, a*, and b* values ​​for each of the eight primary colors referred to above. (Hereinafter, "primary colors" will be used to refer to eight colors: black, white, subtractive primary colors, and additive primary colors, as shown in FIG. 8 .)

[0091] Methods for electrophoretically arranging a plurality of differently colored particles in "layers" as shown in FIG. 8 have been described in the prior art. The simplest of these methods involves causing pigments having different electrophoretic mobilities to "race"; see, for example, U.S. Patent No. 8,040,594. This racing is more complex than initially appreciated because the movement of the charged pigments themselves changes the electric field experienced locally within the electrophoretic fluid. For example, as positively charged particles move toward the cathode and negatively charged particles move toward the anode, their charges screen the electric field experienced by charged particles intermediate the two electrodes. It is conceivable that while the electrophoresis of the present invention involves pigment racing, this is not the only phenomenon that results in the arrangement of the particles shown in FIG. 8.

[0092] In color displays, as described in U.S. Pat. No. 9,921,451, one of the color pigments has the same charge polarity as the white pigment (usually negatively charged). Negatively charged color pigments and white pigments move in the same direction in an electric field, so the generation of pure white and yellow states requires some means to selectively delay or enhance the movement of one of these pigments relative to the other. In practice, complex waveforms are used to ensure that the white pigment covers the negatively charged color pigment to a degree exceeding the uncontaminated white state for the observer. Such complex waveforms may not allow a rapid transition from another color to the white state. For example, for some displays, this transition may last for about 5-10 seconds. In the case where white and yellow are negatively charged and cyan and magenta are positively charged and cyan pigments form weaker aggregations with yellow than magenta pigments, cyan must be formed from the previous white state, followed by a second stage of bringing the cyan pigment to the viewing surface, as described in U.S. Pat. No. 9,921,451. Therefore, it takes a longer update time to form cyan from another color than to form a white state. However, in many applications of full color electrophoretic displays, it is preferred to have much shorter image transitions, on the order of three seconds or less.

[0093] As mentioned above, it has now been found that switching times can be improved when the mobility of one of the particles of the subtractive primary colors is less than or equal to half the mobility of the other particles in the electrophoretic medium. In broad terms, the mobility can be expressed as where ν is the electrophoretic velocity, is the applied electric field. The measured value of the mobility of the colored particles can be obtained in one of a variety of ways. Although the mobility can be measured directly, it may not be simple for non-polar media. For example, the mobility can be calculated by the measured value of the Zeta potential ζ or the charge-to-mass ratio Q / M of the particles, or by the measured value of the difference between the conductivity λ of the dispersion and the conductivity λ0 of its slurry. Morrison, ID and Tarnawskyj, CJ, Langmuir 1991, 7, 2358 discuss the relationship between mobility and Zeta potential, charge-to-mass ratio and conductivity.

[0094] In one example, the electrophoretic medium may include a solvent with a low dielectric constant, a white pigment with a silane surface treatment and a polymer coating and a Zeta potential of <-60mV, a first color pigment containing a polymer coating and a Zeta potential of>30mV, a second color pigment that may or may not contain a polymer coating and a Zeta potential of>20mV (the polymer coating provides a smaller spatial stability than the polymer coating on the first color pigment and the third color pigment), and a third color particle with a Zeta potential in the range of -20mV to +20mV. More generally, a formulation according to various embodiments of the present invention may include a white scattering pigment containing a polymer coating and having a first polarity, two color pigments having a second polarity opposite to the first polarity (at least one of the two pigments has a polymer coating), and a third color pigment containing a polymer coating, wherein the mobility of the third color pigment is less than half of the mobility of any other pigment. The polymer coating of the third color pigment is preferably insoluble in the electrophoretic solvent, but can be removed by a solvent with a greater polarity. In some formulations, the white pigment, the two color pigments having a second polarity, and the third color pigment all contain a polymer coating. Each coating may have a composition different from all other coatings. Alternatively, two or more pigments may have the same coating.

[0095] Assuming that the core pigments comprising the particles are approximately the same size, and assuming that the Zeta potential of each uncoated particle is approximately the same, the size of the Zeta potential of the composite particles depends on the polymer shell surrounding each core pigment. According to a method for manufacturing pigment particles contained in an electrophoretic medium according to various embodiments of the present invention, a polymer coating can be provided on the core pigment particles using a dispersion polymerization operation. In a preferred method, a dispersion of core pigment particles is provided in a solution of appropriate monomers in a solvent that also contains a polymerization initiator. Homopolymers formed by at least one monomer are soluble in the solvent, while homopolymers formed by at least another monomer are insoluble at a sufficiently high molecular weight. When copolymers are produced as the polymerization of the monomer mixture proceeds, the polymer begins to deposit on the core pigment particles and becomes insoluble in the solvent as its molecular weight increases. However, there is a sufficient amount of more soluble monomers to provide a copolymer portion that is soluble in the solvent. These segments provide steric stability for the coated core pigment particles.

[0096] Figure 1 A schematic diagram of a polymer coated pigment particle is provided in . A core pigment particle 102 is modified with a smaller polymer particle 104 containing a solvent soluble segment 106. As more polymer particles are deposited on the core particle, its surface is gradually covered. Without wishing to be bound by theory, a simple model of the process will now be described. Many assumptions are made in this model; however, the model has some value in helping to understand various embodiments of the present invention.

[0097] If it is assumed that polymer particles 104 attach to the surface of the modified pigment particle 102 at random locations and that polymer particles do not spread over the particle surface once attached, the probability that an additional polymer particle will hit a portion of the core pigment particle 102 that is not already covered by polymer depends on the amount of polymer already present. This yields an expression for the proportion P of the surface of the pigment particle that is covered by polymer of the following type:

[0098] P=1–exp(-kQ) (1)

[0099] where Q is the relative mass of the polymer particles added to the pigment particles and k is a constant that depends on the radii of the polymer and pigment particles and their relative densities.

[0100] If we further assume that the Zeta potential of the modified particle is the surface area average Zeta potential of the uncovered pigment surface and the polymer, and that the Zeta potential of the polymer is the mass ratio average of the Zeta potentials of the pure polymer made from each constituent monomer, then the Zeta potential of the composite particle is given by:

[0101]

[0102] Where m i is the relative mass of monomer i in the polymer comprising the polymer particle, ζ i is the zeta potential of a particle made of pure polymer made from monomer i, and ζ pig is the Zeta potential of the unmodified pigment particle. Equation (2) allows a rough prediction of the Zeta potential of a particular composite particle given its composition.

[0103] Figure 2 A comparison between the predicted and measured Zeta potentials of a number of different composite pigment particles of the invention is shown, all of which are derivatives of the same base pigment particle (Pigment Yellow 155). Note that in the preparation of pigment particles (such as the embodiment described in detail in Example 1 below), only about one-third of the mass of the monomer added to the polymerization reaction is actually deposited on the surface of the isolated pigment particles. As a result, the composition of the deposited polymer is not necessarily the same as the composition of the monomer added to the reaction vessel. Therefore, the Zeta potential estimated by equation (2) is only an approximation.

[0104] Generally, monomers used to prepare particles incorporated into electrophoretic media according to various embodiments of the present invention should be soluble in the polymerization solvent. At least one monomer should form a polymer that becomes insoluble as polymerization proceeds.

[0105] Monomers that impart a more positive charge to the product polymer include esters and amides of ethylene acid, such as those of formula (1):

[0106] CH2=C(R 1a )C(O)R 2 Formula (1)

[0107] Functional group R 1a Typically -H or -CH3. In one embodiment, the group R 2 With the formula -OR 3 , forming acrylate or methacrylate. 2 With the formula –NHR 3 When the monomer is acrylamide. Also included are those wherein R 2 With the formula -NR 3 2, in which case the monomer is N,N-diacrylamide. In a non-limiting embodiment, the group R 3 Can be C 1-6 Alkyl, C 1-6 Heteroalkyl, C 3-10 Cycloalkyl, C 3-10 Heterocycloalkyl, C 6-14 Aryl, C 5-14 In addition, the group R 3can be independently selected from R 4 In a representative embodiment, R 4 Can be C 1-6 Alkyl, -OH, C 1-6 Alkoxy, -NH2, -NH(C 1-6 Alkyl), -N(C 1-6 Alkyl)2, C 1-6 Haloalkyl, or C 1-6 Representative individual monomers of formula (1) include methyl methacrylate (MMA), methoxyphenyl methacrylate and N,N-diisopropylacrylamide.

[0108] Monomers that impart more negative charge include styrene and substituted styrenes. Non-limiting examples of substituted styrenes include styrenes independently selected from C 1-6 Alkyl, C 1-6 Alkoxy, -NH(C 1-6 Alkyl), -N(C 1-6 Another class of monomers that introduce more negative charge is provided by molecules of formula (2):

[0109] CH2=C(R 1b )C(O)R 5 Formula (2)

[0110] Functional group R 1b Typically -H or -CH3. In one embodiment, the group R 5 With the formula -OR 6 , forming acrylate or methacrylate. 5 With the formula –NHR 6 When the monomer is acrylamide. Also included are those wherein R 5 With the formula -NR 6 2, the monomer is N,N-diacrylamide. In a non-limiting embodiment, the group R 6 Can be C 1-6 Alkyl, C 1-6 Heteroalkyl, C 3-10 Cycloalkyl, C 3-10 Heterocycloalkyl, C 6-14 Aryl, C 5-14 In addition, the group R 6 are independently selected from R 7 In a representative embodiment, R 7is halogen, -CN, -NO2, -S(O)- or -S(O)2-. Representative single monomers of formula (2) include fluorinated or partially fluorinated esters of ethylene acid, such as trifluoromethyl, difluoromethyl, monofluoromethyl, pentafluoroethyl, tetrafluoroethyl, trifluoroethyl, difluoroethyl, monofluoroethyl acrylate or methacrylate. In an exemplary embodiment, the monomer of formula (2) is trifluoroethyl methacrylate (TFEM).

[0111] The monomer providing a soluble homopolymer may be a derivative of polydimethylsiloxane (PDMS), such as acrylate-terminated polydimethylsiloxane, or a long-chain or branched acrylate, such as lauryl methacrylate or 2-ethylhexyl-1-methacrylate.

[0112] As described above, in a preferred embodiment of the present invention, a group of composite particles in the electrophoretic medium has a Zeta potential in the range of -20 mV to +20 mV. As is known in the art, a group of pigment particles will generally exhibit a range of mobilities depending on the distribution of particles within the group. Therefore, the Zeta potential value represents the average value of the mobility of the entire collection of particles.

[0113] The extent of the polymer shell is conveniently assessed by thermogravimetric analysis (TGA), a technique in which the temperature of a dried sample of the particles is increased and the mass loss due to pyrolysis is measured as a function of temperature. Conditions can be found under which the polymer coating is lost but the core pigment is retained (these conditions depend on the exact core pigment particles used). By using TGA, the mass proportion of the polymer particles, i.e. the mass fraction of the polymer shell in the composite particle, can be measured and this can be converted to a volume fraction using the known densities of the core pigment and the polymer attached to the core pigment.

[0114] A method for estimating the polymer coverage of the above-mentioned pigment particles by weight analysis is also provided in Example 2 below. The coverage can be adjusted by changing the mass ratio of monomers and particles in the reaction mixture used to prepare the composite pigment particles. According to an exemplary embodiment, the mass fraction of the polymer shell in the composite particles is at least 25wt% to a maximum of 75wt%. In a further embodiment, the mass fraction is at least 25wt% to a maximum of 70wt%, at least 25wt% to a maximum of 60wt%, at least 25wt% to a maximum of 50wt%, or at least 25wt% to a maximum of 40wt%. In a further embodiment, the mass fraction is at least 20wt% to a maximum of 70wt%, at least 20wt% to a maximum of 60wt%, at least 20wt% to a maximum of 50wt%, or at least 20wt% to a maximum of 40wt%.

[0115] A wide variety of forms can be used for the core pigment: spheres, needles or otherwise anisometric, aggregates of smaller particles (i.e., "grape clusters"), composite particles comprising small pigment particles or dyes dispersed in a binder, etc., as is known in the art. The polymer shell can be a covalently bonded polymer made by modification processes or chemical adsorption known in the art, or can be physically adsorbed onto the particle surface.

[0116] In this analysis, it is assumed that the polymer shell uniformly encapsulates the entire surface of the core pigment. However, this is difficult to ensure. (See, for example, the aforementioned U.S. Patent Nos. 6,822,782, Figure 6 , and the related descriptions at columns 16-17.) The method of polymer attachment may favor one side of the crystalline core pigment over another, and some areas of the core pigment may be covered with polymer, while other areas are not covered or are minimally covered with polymer. Moreover, particularly when grafting techniques are used to attach the polymer to the pigment surface, the growth of the polymer may be patchy, leaving large areas of the core pigment uncovered even if the mass of grafted polymer is large.

[0117] As already mentioned, in a preferred embodiment, the present invention requires the use of light scattering particles that are usually white, and three kinds of substantially non-light scattering particles. Of course, there are no complete light scattering particles or complete non-light scattering particles, and the minimum degree of light scattering of the light scattering of the light scattering particles used in the electrophoresis of the present invention and the maximum permissible degree of light scattering allowed in the substantially non-light scattering particles can vary slightly according to the following factors, such as the exact pigment used, their color and the ability of the user or application to allow a slight deviation from the ideal desired color. The scattering and absorption characteristics of the pigment can be evaluated by measuring the diffuse reflectance of the sample of the pigment dispersed in the suitable matrix or liquid under white and black backgrounds. The results from these measurements can be explained according to multiple models known in the art, for example, one-dimensional Kubelka-Munk processing. In the present invention, it is preferred that when the pigment is approximately isotropically distributed in a layer of 1 μm including the pigment and the liquid having a refractive index less than 1.55 with a volume of 15%, the white pigment presents a diffuse reflectance of at least 5% measured on a black background at 550nm. Under the same conditions, the yellow, magenta and cyan pigments preferably exhibit a diffuse reflectance of less than 2.5% measured on a black background at 650, 550 and 450 nm, respectively. (The wavelengths selected for the above measurements for the yellow, magenta and cyan pigments correspond to the spectral regions where these pigments have minimum absorption.) Color pigments that meet these criteria are referred to below as "non-scattering" or "substantially non-light scattering".

[0118] Table 1 below shows the diffuse reflectance of preferred yellow, magenta, cyan and white pigments (Y1, M1, C1 and W1, described in more detail below) used in the electrophoretic medium of the present invention, as well as the ratio of their absorption coefficient and scattering coefficient based on the Kubelka-Munk analysis of these materials dispersed in a polyisobutylene matrix.

[0119] Table 1

[0120]

[0121] The core pigment used in the white particles is typically a high refractive index metal oxide such as titanium dioxide, which is well known in the field of electrophoretic displays. The core pigments used to provide the subtractive primary colors, cyan, magenta and yellow, include but are not limited to the following.

[0122] Suitable yellow core pigments include CI Pigment Yellow 1, 3, 12, 13, 14, 16, 17, 73, 74, 81, 83, 97, 111, 120, 126, 137, 139, 150, 151, 155, 174, 175, 176, 180, 181, 191, 194, 213 and 214. Preferred yellow core pigments include CI Pigment Yellow 139, 155 and 180.

[0123] Suitable magenta core pigments include CI Pigment Red 12, 14, 48:2, 48:3, 48:4, 57:1, 112, 122, 146, 147, 176, 184, 185, 209, 257 and 262; and CI Pigment Violet 19 and 32. A preferred magenta core pigment is CI Pigment Red 122.

[0124] Suitable cyan core pigments include CI Pigment Blue 15:1, 15:2, 15:3, 15:4 and 79; and CI Solvent Blue 70.

[0125] The display device can be constructed using the electrophoretic fluid of the present invention in several ways known in the prior art. The electrophoretic fluid can be encapsulated in a microcapsule or incorporated into a microcell structure that is subsequently sealed with a polymer layer. The microcapsule or microcell layer can be coated or embossed on a plastic substrate or film that carries a transparent coating of a conductive material. The assembly can be laminated to a backplane that carries pixel electrodes using a conductive adhesive.

[0126] Example

[0127] Examples will now be given, but by way of illustration only, to illustrate details of preferred electrophoretic media of the present invention and processes for driving these preferred electrophoretic media.

[0128] Example 1 - Preparation of yellow pigment

[0129] Step 1: Preparation of the mill base.

[0130] A mixture of Pigment Yellow 155 (available from Clariant as Ink Jet Yellow 4GC, 1670 g) and isopar-E (9440 g) was charged to a storage tank. The mixture was circulated through a LabStar horizontal agitator bead mill (Netzsch Premier Technologies) equipped with 0.7 to 1.2 mm spherical grinding media (ceria-stabilized zirconium oxide, available from Jyoti, 1840 g). Grinding was performed at an agitator speed of 1000 rpm, with a run time equivalent to 375 minutes / kg of pigment.

[0131] Step 2: Aggregation.

[0132] The millbase prepared as described above (183.18 g, based on an assayed pigment content of 13.67% or 25.04 g) was charged to a 250 ml polypropylene bottle, sonicated for 75 minutes, and then transferred to a 500 ml three-necked round bottom flask equipped with a mechanical stirrer, a rubber septum, and a subsurface nitrogen delivery tube. A wash with Isopar E (27 mL) was added. The suspension was rapidly stirred under nitrogen sparge for 15 minutes, at which time a mixture of a monomethacryloxypropyl-terminated polydimethylsiloxane macromonomer (12.90 g) with a molecular weight of approximately 10,000 available from Gelest as MCR-M22, methyl methacrylate (8.40 g), and trifluoroethyl methacrylate (2.70 g) was added, along with additional Isopar E wash (5 mL).

[0133] The mixture was stirred and heated in an oil bath under continuous nitrogen sparge and reached 55°C after one hour. At this point the nitrogen delivery was changed to above the surface, a thermometer was introduced into the flask and a solution of azobisisobutyronitrile (92 mg) in ethyl acetate (0.72 g) was added via syringe. After a further 75 minutes the batch temperature was 66°C. After a further 15.5 hours the temperature was 63°C and the heating bath was removed. Stirring was continued until the temperature dropped to 40°C at which point the batch was diluted with Isopar E (60 mL) and stirred while slowly cooling to 33°C. At this point the contents were transferred to two 250 mL polypropylene bottles while washing with enough Isopar E to bring the total dispersed volume to 500 mL. The batch was centrifuged at 3500 rpm for 30 minutes. A sample of the supernatant was retained. The solid was suspended in Isopar E to a total volume of 250 mL and tumbled for 4 hours then centrifuged at 3440 rpm for 30 minutes. The supernatant was discarded and the solid resuspended in Isopar E. E to a total volume of 250 mL and centrifuged again for 30 minutes. This process was repeated 3 more times (5 centrifuges in total). The wet cake at the end of the process was suspended in hexane to 250 mL and centrifuged at 3500 rpm for 30 minutes. The solid was air-dried for 3 days and then placed in a vacuum oven at 50° C. for 24 hours to provide a yellow solid weighing 34.42 g.

[0134] Step 3: Dispersion of composite pigments.

[0135] To a 125 mL polypropylene bottle was added the dry pigment (10.00 g) prepared as described above and Isopar E (40.00 g). Over the course of six days, the mixture was subjected to eight 90-minute ultrasonic baths during which the mixture was rotated on a roller mill. The resulting dispersion was filtered through a 200 micron fabric mesh to provide a mobile dispersion and leave no residual solids. The weighed sample was dried overnight in a convection oven at 170° F., leaving a residual solid weight of 20.26%.

[0136] Example 2 - Estimation of mass fraction relative to the weight of composite particles

[0137] Add the pigment to be tested (0.5899g), tetrahydrofuran (7.05g) and a small magnetic stirring bar to the scintillation bottle. The bottle is capped and placed on a stirrer / heating plate, and heated and stirred. The 250mL glass jar is inverted on the bottle to prevent airflow from entering and provide safety protection when the bottle bursts. The temperature of the heating plate is adjusted so that the batch temperature is 60°C (measured regularly using a pyrometer). Heating is stopped after two hours, and the contents continue to stir for another two hours, and then transferred to a 15mL Nalgene centrifugal cone together with about 2ml of THF washings. The dispersion is centrifuged at 3070rpm for 30 minutes. The supernatant is transferred to a scintillation bottle with a tare weight of 14.0412g and placed in a convection oven at 170°F overnight. THF (6.5g) is added to the centrifugal precipitate the next day. The cone is capped, shaken and ultrasonicated to achieve dispersion, and then centrifuged at 3070rpm for 30 minutes. The supernatant was added to the bottle containing the residue of the first supernatant, and the solution was again dried in a convection oven at 170°F overnight. The pellet after centrifugation was air dried overnight, and then both components were vacuum dried at 70°C for 8 hours. The gross weight of the bottle plus the contents was 14.1873 g, representing a net weight of 0.1461 g polymer (24.77% of the original sample weight). The residual pigment dried in the centrifuge cone was transferred to a scintillation vial, giving a net weight of 0.4532 g (76.83% of the original sample weight), so the mass balance was 101.60%.

[0138] Table 2 Fig. 9 ) show the physical properties of pigments prepared and analyzed as described above in Examples 1 and 2. The particle sizes quoted are measured in solution, where the polymer shell (if present) is swollen by solvent.

[0139] Example 3 - Measurement of electro-optical properties of formulations

[0140] Step 1: Preparation of exemplary electrophoretic fluids

[0141] Fluid (i): A white particle dispersion similar to that described in Part A of Example 12 of U.S. Pat. No. 9,921,451 (15.53 g) was combined with a cyan particle dispersion similar to that prepared as described in Example 7 of U.S. Pat. No. 9,921,451 (1.93 g), a magenta particle dispersion similar to that prepared as described in Example 5 of U.S. Pat. No. 9,921,451 (2.29 g), a yellow pigment dispersion similar to that described in Step 3 of Example 1 above (2.30 g), a surfactant similar to Solsperse 19000 available from The Lubrizol Company of Wickliffe, Ohio (1.16 g of a 50% w / w solution in Isopar E), and a polyisobutylene having a molecular weight of 850,000 (1.06 g of a 15% w / w solution in Isopar E). The resulting mixture was thoroughly mixed overnight and sonicated for 90 minutes to produce an electrophoretic fluid.

[0142] Step 2: Preparation of display device

[0143] An array of microcells imprinted onto a polyethylene terephthalate film having a transparent conductor (indium tin oxide, ITO) coating is filled with an electrophoretic fluid prepared as described in step 1 above. The microcells are hexagonal in shape, with a depth of 14 or 17 microns measured from side to side and a width of 130 microns. Excess electrophoretic fluid is removed from the microcells with a scraper and they are sealed with a composite polymer coating as described in U.S. Patent No. 9,759,978. The assembly is laminated to a glass backplane having an ITO electrode using a doped thermal adhesive having a thickness of 3 μm, substantially as described in U.S. Patent No. 7,012,735, to produce a display device.

[0144] The device was electro-optically tested in a manner similar to that described in Section D of Example 11 of U.S. Patent 9,921,451. Figure 3 and Figure 4 The waveforms used are shown in FIG. Figure 3 The waveform is similar to that in U.S. Patent 9,921,451 Figure 7 The waveform shown in B is used to produce cyan. Figure 3 The voltages shown in refer to the voltage of the backplane of the device relative to the front plane (viewing surface).

[0145] In applying Figure 3The reflected spectrum of the display device is measured following the waveform of the wavelength of light recorded. The recorded optical density is converted into "analytical density": that is, the contribution to the observed absorption spectrum of each individual color pigment. The analytical density is determined after baseline correction to compensate for optical losses in the display device. The quality of the cyan color is then estimated as the analytical density corresponding to the light absorption of the cyan pigment minus the larger of the analytical densities corresponding to the light absorption of the magenta and yellow pigments. The larger this value, the more ideal the cyan color is considered to be.

[0146] Figure 4 The waveform (again showing the voltage applied to the backplane relative to the frontplane) is intended to probe the total color gamut (i.e., the volume of all colors addressable by the device). The waveform consists of "dipoles," pairs of pulses of opposite polarity, whose duration and amplitude are systematically varied, as shown by the dark envelope in the figure. The voltages explored were + / - 3.5, 6.1, 9.4, 13.4, 18.2, 23.7, and 30 V, with pulse length durations of 50, 80, 120, 190, and 300 milliseconds. For each voltage pair (+,-), each pulse duration pair was visited once. This was done in such a way that the pulse duration pair in one dipole had exactly one value changed in the next dipole, and that value was adjacent in the ordered list of pulse duration values. The voltages were explored in a similar manner. In this way, the changes in the waveform are as smooth as possible, because consecutive dipoles are as similar to each other as possible. The reflectance spectrum is obtained throughout the waveform (not only at its end) and converted to CIEL*a*b* units. The color space (in ΔE) was plotted in 3D color space. 3 The volume of the convex hull surrounding this point cloud in units of is considered to be the total color gamut available for that particular display device.

[0147] Figure 5 and Figure 6 The Zeta potential of the yellow pigment is shown as a function of the Figure 3 The cyan quality obtained by applying the waveform Figure 4 The total color gamut obtained from the waveform of . As mentioned above, the point corresponding to the zeta potential of -55 mV is from the non-functionalized control yellow pigment.

[0148] from Figure 5 As can be seen in the graph, excellent cyan quality scores can be achieved when the magnitude of the zeta potential of the yellow pigment is below about 20 mV. The cyan quality scores are also higher using the thinner microcup (14 micron) compared to the thicker microcup (17 micron). When the magnitude of the zeta potential of the yellow pigment is above about 20 mV, the cyan quality scores are very poor using the thicker microcup.

[0149] Without wishing to be bound by theory, it is believed that the improved cyan quality scores achieved using yellow pigments made according to embodiments of the present invention are due to their low mobility. When the yellow pigment is positively charged and has high mobility, its properties are very similar to those of the cyan pigment. Therefore, it is difficult to distinguish the two colors with any applied waveform. On the other hand, when the yellow pigment is negatively charged and has high mobility, it becomes difficult to separate from the white pigment, at least in the case of a short applied waveform.

[0150] from Figure 6 It is obvious that when using long waveforms (such as Figure 4 When using positively charged yellow pigments with high mobility, the color gamut may decrease slightly. Figure 7 Shown without sacrificing use Figure 4 The total color gamut of the waveform is measured using Figure 3 A fast waveform can achieve a high cyan quality score.

[0151] It will be apparent to those skilled in the art that various changes and modifications may be made to the specific embodiments of the invention described above without departing from the scope of the invention.Therefore, the entire foregoing description should be interpreted in an illustrative rather than a limiting sense.

[0152] The electrophoretic media of the present application may include any additives used in conventional electrophoretic media as described, for example, in the above-mentioned E Ink and MIT patents and applications. Thus, for example, the electrophoretic media of the present application will typically include at least one charge control agent (CCA) to control the charge on the various particles, and a polymer having a number average molecular weight of more than about 20,000 and substantially non-absorbent particles may be dissolved or dispersed in the fluid to improve the bistability of the display, such as described in U.S. Pat. No. 7,170,670.

[0153] All of the above patents and patent application publications are incorporated herein by reference in their entirety. If there is any inconsistency between the contents of the present application and any patents and applications incorporated herein by reference, the contents of the present application shall control to the extent necessary to resolve such inconsistency.

Claims

1. An electrophoretic medium, comprising: fluid; a plurality of light scattering charged particles having a first polarity; as well as a first group of charged particles, a second group of charged particles, and a third group of charged particles, each group having a different color from each other, wherein the first group of charged particles and the second group of charged particles have a second polarity opposite to the first polarity, and The third group of charged particles are composite particles comprising a core pigment and a polymer shell, wherein: (a) the mass fraction of the polymer shell relative to the composite particle is at least 20 wt% and at most 50 wt%; and (b) The polymer shell comprises: (I) a first monomer unit derived from a first precursor of formula (1): CH2=C(R 1a )C(O)R 2 (1) Where: R 1a is –H or –CH3; R 2 Yes-OR 3 , –NHR 3 or -NR 3 2; R 3 It is C 1-6 Alkyl, C 1-6 Heteroalkyl, C 3-10 Cycloalkyl, C 3-10 Heterocycloalkyl, C 6-14 Aryl, C 5-14 heteroaryl or any combination thereof, each of which is optionally independently selected from R 4 The group is substituted one or more times; R 4 It is C 1-6 Alkyl, -OH, C 1-6 Alkoxy, -NH2, -NH(C 1-6 Alkyl), -N(C 1-6 Alkyl)2, C 1-6 Haloalkyl or C 1-6 haloalkoxy; and (II) a second monomer unit derived from a second precursor of formula (2): CH2=C(R 1b )C(O)R 5 (2) Where: R 1b is –H or –CH3; R 5 Yes-OR 6 , –NHR 6 or -NR 6 2; R 6 It is C 1-6 Alkyl, C 1-6 Heteroalkyl, C 3-10 Cycloalkyl, C 3-10 Heterocycloalkyl, C 6-14 Aryl, C 5-14 heteroaryl or any combination thereof, each of which is independently selected from R 7 The group is substituted one or more times; R 7 is halogen, -CN, -NO2, -S(O)- or -S(O)2-, And the magnitude of the electrophoretic mobility of the third group of charged particles is less than half the magnitude of the electrophoretic mobility of the light scattering charged particles, the first group of charged particles, and the second group of charged particles.

2. The electrophoretic medium according to claim 1, wherein: R 3 It is C 1-6 Alkyl, C 6-14 Aryl or any combination thereof, each of which is optionally independently selected from R 4 substituted one or more times by a group; and R 4 It is C 1-6 Alkyl or C 1-6 Alkoxy.

3. The electrophoretic medium according to claim 1, wherein: R 2 Yes-OR 3 , and R 3 It is C 1-6 Alkyl or C 6-14 Aryl, the C 6-14 Aryl is optionally independently selected from R 4 substituted one or more times by a group; and R 4 C 1-6 Alkoxy.

4. The electrophoretic medium according to claim 1, wherein: R 6 It is C 1-6 Alkyl and R 7 It's a halogen.

5. The electrophoretic medium according to claim 1, wherein: R 5 Yes-OR 6 , R 6 Is R 7 Replace at least three times C 1-6 Alkyl, and R 7 Yes -F.

6. The electrophoretic medium according to claim 1, wherein: The first precursor is selected from the group consisting of methyl methacrylate, methoxyphenyl methacrylate and N,N-diisopropylacrylamide.

7. The electrophoretic medium according to claim 1, wherein: The second precursor is trifluoroethyl methacrylate.

8. A front plane laminate, a double release sheet, an inverted front plane laminate or an electrophoretic display comprising the electrophoretic medium according to claim 1.

9. An electronic book reader, a portable computer, a tablet computer, a cellular phone, a smart card, a sign, a watch, a shelf label or a flash drive comprising the electrophoretic display according to claim 8.

10. An electrophoretic medium, comprising: fluid; a plurality of light scattering charged particles having a first polarity; as well as a first group of charged particles, a second group of charged particles, and a third group of charged particles, each group having a different color from each other, Wherein, the first group of charged particles and the second group of charged particles have a second polarity opposite to the first polarity, and the electrophoretic mobility of the third group of charged particles is less than half of the electrophoretic mobility of the light scattering charged particles, the first group of charged particles and the second group of charged particles.

11. The electrophoretic medium according to claim 10, wherein: The electrophoretic mobility is measured based on the particle zeta potential.

12. The electrophoretic medium according to claim 11, wherein: The third group of charged particles has a Zeta potential greater than or equal to -20 mV and less than or equal to 20 mV.

13. The electrophoretic medium according to claim 10, wherein: Electrophoretic mobility is measured based on the charge-to-mass ratio of the particles.

14. The electrophoretic medium according to claim 10, wherein: Electrophoretic mobility is measured based on the conductivity measurements of the particle dispersion.

15. A front plane laminate, a double release sheet, an inverted front plane laminate or an electrophoretic display comprising the electrophoretic medium according to claim 10.

16. An electronic book reader, a portable computer, a tablet computer, a cellular phone, a smart card, a sign, a watch, a shelf label or a flash drive comprising the electrophoretic display according to claim 15.

17. An electrophoretic medium, comprising: fluid; a plurality of light scattering charged particles having a first polarity; as well as a first group of charged particles, a second group of charged particles, and a third group of charged particles, each group having a different color from each other, wherein the first group of charged particles and the second group of charged particles have a second polarity opposite to the first polarity, and The third group of charged particles are composite particles comprising a core pigment and a polymer shell, wherein: (a) the mass fraction of the polymer shell relative to the composite particle is at least 20 wt % and at most 50 wt %; and (b) The polymer shell comprises: (I) a first monomer unit derived from a first precursor of formula (1): CH2=C(R 1a )C(O)R 2 (1) Where: R 1a is –H or –CH3; R 2 Yes-OR 3 , –NHR 3 or -NR 3 2; R 3 It is C 1-6 Alkyl, C 1-6 Heteroalkyl, C 3-10 Cycloalkyl, C 3-10 Heterocycloalkyl, C 6-14 Aryl, C 5-14 heteroaryl or any combination thereof, each of which is optionally independently selected from R 4 The group is substituted one or more times; R 4 It is C 1-6 Alkyl, -OH, C 1-6 Alkoxy, -NH2, -NH(C 1-6 Alkyl), -N(C 1-6 Alkyl)2, C 1-6 Haloalkyl or C 1-6 haloalkoxy; and (II) a second monomer unit derived from styrene, wherein the styrene is optionally independently selected from C 1-6 Alkyl, C 1-6 Alkoxy, -NH(C 1-6 Alkyl), -N(C 1-6 alkyl)2 and halogen groups are substituted one or more times, And the magnitude of the electrophoretic mobility of the third group of charged particles is less than half the magnitude of the electrophoretic mobility of the light scattering charged particles, the first group of charged particles, and the second group of charged particles.

18. The electrophoretic medium according to claim 17, wherein: R 3 It is C 1-6 Alkyl, C 6-14 Aryl or any combination thereof, each of which is optionally independently selected from R 4 substituted one or more times by a group; and R 4 It is C 1-6 Alkyl or C 1-6 Alkoxy.

19. The electrophoretic medium according to claim 17, wherein: R 2 Yes-OR 3 , and R 3 It is C 1-6 Alkyl or C 6-14 Aryl, the C 6-14 Aryl is optionally independently selected from R 4 substituted one or more times by a group; and R 4 C 1-6 Alkoxy.

20. The electrophoretic medium according to claim 17, wherein: In the third group of charged particles, the mass fraction of the polymer shell relative to the composite particles is at least 25 wt % and at most 40 wt %.

21. The electrophoretic medium according to claim 17, wherein: The mass fraction of the polymer shell relative to the composite particles is measured by thermogravimetric analysis (TGA).

22. A front plane laminate, double release sheet, inverted front plane laminate or electrophoretic display comprising the electrophoretic medium of claim 17.

23. An electronic book reader, a portable computer, a tablet computer, a cellular phone, a smart card, a sign, a watch, a shelf label or a flash drive comprising the electrophoretic display according to claim 22.

Citation Information

Patent Citations

  • Method and apparatus for determining properties of an electrophoretic display

    US20030102858A1

  • Full color reflective display with multichromatic sub-pixels

    US20040263947A1

  • Electro-optic displays, and methods for driving same

    US20050122284A1

  • Tiled displays and methods for driving same

    US20050253777A1

  • Image processing device and image processing method

    US20070031031A1