Resin composition, film and multilayer structure
By adding metal compounds to the resin composition and treating them under high humidity, the problem of insufficient gas barrier properties of the gas barrier film in the prior art under high humidity is solved, and excellent gas and oxygen barrier properties under high humidity are achieved. In food and pharmaceutical packaging materials.
Patent Information
- Application Number
- CN202080024889.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-27
- Filing Date
- 2020-03-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-03-27
AI Technical Summary
The existing gas barrier films have insufficient gas barrier properties under high humidity, especially oxygen barrier properties.
By increasing the metal compound in the resin composition, the average metal atom concentration near the film surface is increased, and the treatment is left to stand under high humidity to form an excellent gas barrier film.
It has achieved significant improvement in gas barrier properties and oxygen barrier properties under high humidity, and reduced oxygen permeability, which is suitable for packaging materials for food and medicine.
Smart Images

Figure GDA0003479668140000211 
Figure GDA0003479668140000241
Abstract
Description
Technical Field
[0001] The present invention relates to a resin composition, and more particularly, to a resin composition capable of obtaining a film having high gas barrier properties under high humidity. Background Art
[0002] Hydrophilic resins such as polyvinyl alcohol-based resins are excellent in strength, transparency, gas barrier properties, etc., and therefore are widely used as various packaging materials when formed into films, especially packaging materials for foods and pharmaceuticals that require suppression of oxygen degradation.
[0003] However, hydrophilic resins have a large number of hydroxyl groups and are therefore easily greatly affected by humidity, and their gas barrier properties are significantly reduced in a high humidity environment.
[0004] As a film with improved gas barrier properties, for example, Patent Document 1 discloses a material for a gas barrier film, which comprises water-insoluble inorganic fine particles having an average particle size of less than 500 nm and a water-soluble or water-dispersible polymer compound, wherein the water-insoluble inorganic fine particles are ionic crystals synthesized by reacting an inorganic compound or a salt thereof containing one or more selected from aluminum, silicon, zinc, zirconium, silver, and tin as an essential component, with one or more compounds selected from an organic acid, an inorganic acid, and a salt thereof.
[0005] In addition, Patent Document 2 discloses a gas barrier layer-forming composition comprising: a water-soluble polymer; at least one of a metal alkoxide, a hydrolyzate thereof, and tin chloride; and a general formula (R 1 Si(OR 2 )3)n(where R 1 is an organic functional group, R 2 The compound represented by CH3, C2H5, or C2H4OCH3).
[0006] Furthermore, Patent Document 3 discloses a method for producing a gas barrier laminate, which includes the following steps: a step of forming a coating film containing zinc ions, at least one of metal alkoxides and hydrolyzates thereof, and a water-soluble polymer on the surface of a substrate film or a laminate containing the same; and a step of drying the coating film to form a gas barrier layer on the above-mentioned surface.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2002-338821
[0010] Patent Document 2: Japanese Patent Application Publication No. 2016-221864
[0011] Patent Document 3: Japanese Patent Application Publication No. 2018-089567 Summary of the invention
[0012] Problem that the invention aims to solve
[0013] However, the gas barrier films disclosed in Patent Documents 1 to 3 above do not have sufficient gas barrier properties under high humidity, and further improvement has been sought.
[0014] Therefore, in this invention, under such background, a resin composition excellent in gas barrier properties under high humidity, in particular, oxygen barrier properties under high humidity is provided.
[0015] Solutions for solving problems
[0016] Therefore, the present inventors have found that a resin composition containing a hydrophilic resin and a metal compound, when formed into a film, has excellent gas barrier properties, particularly oxygen barrier properties, under high humidity by increasing the average metal atom concentration near the film surface.
[0017] The present inventors have also found that a resin composition containing a hydrophilic resin and a metal compound, when formed into a coating film, has excellent gas barrier properties even when exposed to high humidity for a long period of time.
[0018] That is, a first aspect of the present invention is a resin composition comprising a hydrophilic resin and a metal compound, wherein the resin composition satisfies the following formula (1) when formed into a film.
[0019] α1-β1≥1……(1)
[0020] The above α1 represents the average metal atomic concentration (%) within a depth range of 0 to 9 nm from the film surface, and the above β1 represents the average metal atomic concentration (%) within a depth range of 12 to 21 nm from the film surface.
[0021] A second gist of the present invention is a resin composition comprising a hydrophilic resin and a metal compound, and satisfies the following condition (A).
[0022] Condition (A):
[0023] The above-mentioned resin composition is made into a 10 wt% aqueous solution or aqueous dispersion, and the obtained cast film is left to stand for 1 week under the conditions of 23°C and 80% RH. When the contact angle (°) of water before treatment is set to α2 and the contact angle (°) of water after treatment is set to β2, the following formula (2) is satisfied.
[0024] (β2-α2)≥10……(2)
[0025] In addition, the third aspect of the present invention is a resin composition comprising a hydrophilic resin and a metal compound, wherein the resin composition is made into a film, and the oxygen permeability (cc·3μm / m 2 ·day·atm) satisfies the following formula (3).
[0026] Oxygen permeability (cc·3μm / m 2 ·day·atm)≤80……(3)
[0027] In addition, the fourth aspect of the present invention is a film containing the resin composition of the first aspect, the resin composition of the second aspect, or the resin composition of the third aspect, and the fifth aspect is a multilayer structure having at least one layer comprising the film of the fourth aspect.
[0028] Effects of the Invention
[0029] The resin composition of the first aspect is a resin composition comprising a hydrophilic resin and a metal compound, and when the resin composition is formed into a film, it satisfies the following formula (1).
[0030] α1-β1≥1……(1)
[0031] The above α1 represents the average metal atomic concentration (%) within a depth range of 0 to 9 nm from the film surface, and the above β1 represents the average metal atomic concentration (%) within a depth range of 12 to 21 nm from the film surface.
[0032] Therefore, when the resin composition is formed into a film, a film having excellent gas barrier properties, particularly oxygen barrier properties, under high humidity can be formed.
[0033] Furthermore, the resin composition according to the second aspect is a resin composition comprising a hydrophilic resin and a metal compound, and satisfies the following condition (A).
[0034] Condition (A):
[0035] The above-mentioned resin composition is made into a 10 wt% aqueous solution or aqueous dispersion, and the obtained cast film is left to stand for 1 week under the conditions of 23°C and 80% RH. When the contact angle (°) of water before treatment is set to α2 and the contact angle (°) of water after treatment is set to β2, the following formula (2) is satisfied.
[0036] (β2-α2)≥10……(2)
[0037] Therefore, when the resin composition is formed into a film, a film having excellent gas barrier properties, particularly oxygen barrier properties, under high humidity can be formed.
[0038] The resin composition of the third aspect is a resin composition comprising a hydrophilic resin and a metal compound, wherein the resin composition is made into a film, and the oxygen permeability (cc·3μm / m 2 ·day·atm) satisfies the following formula (3).
[0039] Oxygen permeability (cc·3μm / m 2 ·day·atm)≤80……(3)
[0040] Therefore, when the resin composition is formed into a film, a film having excellent gas barrier properties, particularly oxygen barrier properties, under high humidity can be formed. DETAILED DESCRIPTION
[0041] Hereinafter, although the form for implementing this invention is demonstrated concretely, this invention is not limited to these.
[0042] The resin composition of the present invention contains a hydrophilic resin and a metal compound. Each component is described below.
[0043] 〔Hydrophilic resin〕
[0044] Specific examples of the hydrophilic resin include water-soluble resins such as vinyl alcohol resins, polysaccharides, acrylic resins, and polyether resins. The hydrophilic resins may be used alone or in combination of two or more.
[0045] In addition, the hydrophilic resin preferably has the following properties when formed into a film, for example.
[0046] That is, it is preferred that the area change rate of a 30 μm-thick film prepared using the hydrophilic resin and immersed in water at 25° C. for 2 hours is 105% or more. The area change rate can be calculated according to the following formula.
[0047] Area change rate (%) = film area after immersion / film area before immersion × 100
[0048] Hereinafter, specific hydrophilic resins will be described in detail.
[0049] [Vinyl alcohol resin]
[0050] The vinyl alcohol resins include resins generally known as ethylene-vinyl alcohol copolymer resins (ethylene content 20 to 60 mol%), and examples thereof include polyvinyl alcohol (hereinafter referred to as "PVA") resins.
[0051] The above-mentioned PVA-based resin is usually preferably an unmodified PVA-based resin, but a modified PVA-based resin may also be used.
[0052] The unmodified PVA resin can be generally produced by polymerizing a vinyl ester monomer and further saponifying the monomer.
[0053] The modified PVA-based resin can be produced by saponifying a polymer of a vinyl ester-based monomer and other unsaturated monomers, or by post-modifying an unmodified PVA resin.
[0054] Examples of the vinyl ester monomers include aliphatic vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl decanoate, vinyl laurate, vinyl stearate, vinyl versatate, and vinyl trifluoroacetate, and aromatic vinyl esters such as vinyl benzoate. Among them, aliphatic vinyl esters having 3 to 20 carbon atoms, more preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms are preferred, and vinyl acetate is particularly preferred. These are usually used alone, but a plurality of them may be used simultaneously as required.
[0055] Examples of the other unsaturated monomers include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid, or salts thereof or mono- or di-alkyl esters thereof; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as vinyl sulfonic acid, allyl sulfonic acid, and methyl allyl sulfonic acid, or salts thereof; alkyl vinyl ethers; N-acrylamidomethyltrimethylammonium chloride, allyltrimethylammonium chloride, dimethylallyl vinyl ketone, N-vinyl pyrrolidone, vinyl chloride; Vinylidene chloride, polyoxyethylene (meth) allyl ether, polyoxypropylene (meth) allyl ether and other polyoxyalkylene (meth) allyl ethers, polyoxyethylene (meth) acrylates, polyoxypropylene (meth) acrylates and other polyoxyalkylene (meth) acrylates, polyoxyethylene (meth) acrylamides, polyoxypropylene (meth) acrylamides and other polyoxyalkylene (meth) acrylamides, polyoxyethylene (1-(meth) acrylamide-1,1-dimethylpropyl) ester, polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene allylamine, polyoxyethylene vinylamine, polyoxypropylene vinylamine, etc. They can be used alone or in combination of two or more. It should be noted that, respectively, the above-mentioned "(meth) allyl" refers to allyl or methallyl, "(meth) acrylate" refers to acrylate or methacrylate, and "(meth) acrylic acid" refers to acrylic acid or methacrylic acid.
[0056] The PVA-based resin can be obtained by any of the known polymerization methods, saponification methods, and post-modification methods.
[0057] It should be noted that the introduction amount of the above-mentioned other unsaturated monomers and the modification amount based on post-modification can be appropriately set according to the type of monomer, usually 15 mol% or less, especially 10 mol% or less. If the introduction amount and the modification amount are too much, the crystallinity of the PVA-based resin tends to decrease and the gas barrier properties when made into a film tend to decrease.
[0058] The average saponification degree of the PVA resin is usually 70 to 100 mol%, preferably 80 to 100 mol%, particularly preferably 85 to 100 mol%, and further preferably 90 to 99.99 mol%. If the average saponification degree is less than 70 mol%, the oxygen permeability tends to increase under high humidity. It should be noted that the average saponification degree is measured in accordance with JIS K 6726.
[0059] The average polymerization degree of the PVA resin is usually 100 to 4000, preferably 200 to 3000, and particularly preferably 250 to 2500. If the average polymerization degree is too low, mechanical properties such as film strength tend to decrease, and if it is too high, operations such as difficulty in aqueous solution tend to become difficult. It should be noted that the average polymerization degree is measured in accordance with JIS K 6726.
[0060] Furthermore, as the above-mentioned PVA-based resin, two or more types different in modification type, modification amount, average saponification degree, average polymerization degree, etc. may be used in combination.
[0061] [Polysaccharides]
[0062] Examples of the polysaccharides include starch and cellulose.
[0063] Examples of the starch include natural starch such as corn starch and potato starch, etherified starch, esterified starch, cross-linked starch, grafted starch, roasted dextrin, enzyme-modified dextrin, α-starch, modified starch such as oxidized starch, and the like.
[0064] Examples of the cellulose include carboxymethyl cellulose, methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxypropyl methyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl cellulose, nitrocellulose, cationized cellulose, and metal salts thereof such as sodium salts.
[0065] [Acrylic resin]
[0066] Examples of the acrylic resin include polyacrylamide, polyacrylic acid, and metal salts thereof such as sodium salts.
[0067] [Polyether resin]
[0068] Examples of the polyether resin include polyethylene glycol and polypropylene glycol.
[0069] Among the above-mentioned hydrophilic resins, vinyl alcohol resins and polysaccharides are preferred from the perspective of excellent gas barrier properties under high humidity, especially oxygen barrier properties, PVA resins, modified starch (especially soluble starch), and hydroxypropyl methylcellulose are more preferred, and unmodified PVA resin is most preferred.
[0070] The hydrophilic resin is preferably the main component of the resin composition of the present invention, and the content of the hydrophilic resin is usually 80% by weight or more, preferably 90% by weight or more, and particularly preferably 95% by weight or more relative to the entire resin composition. The upper limit is usually 99.99% by weight.
[0071] The PVA resin is preferably the main component of the resin composition of the present invention, and the content of the PVA resin is usually 80% by weight or more, preferably 90% by weight or more, and particularly preferably 95% by weight or more relative to the resin composition as a whole. It should be noted that the upper limit is usually 99.99% by weight.
[0072] 〔Metal compounds〕
[0073] The metal compound preferably has a structure in which specific structural units are layered at a specific interplanar spacing. For example, a metal complex can be mentioned that has a structure in which the metal complex is layered at a specific interplanar spacing.
[0074] Examples of the metal substance contained in the metal compound include Na, K, Ca, Mg, Si, Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, and Zn. These metal substances may be contained alone or in combination. Among them, Zn is preferred because of its excellent gas barrier properties, particularly oxygen barrier properties, under high humidity.
[0075] The above-mentioned metal compound is obtained, for example, from a compound having at least one metal selected from Na, K, Ca, Mg, Si, Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, and Zn (hereinafter referred to as a "metal-containing compound") and is obtained by the method described later.
[0076] More specifically, the structural unit of the metal compound includes a metal, a hydroxyl ligand, and an anionic ligand other than the hydroxyl ligand. Preferably, the structural unit includes a metal, a hydroxyl ligand, and an anionic ligand other than the hydroxyl ligand and is represented by the following chemical formula (4).
[0077] M a (OH) b A n- (2a-b) / n ……(4)
[0078] The above-mentioned M represents a metal substance, and A represents an anionic ligand other than a hydroxy ligand having a valence of n-. However, as A, O (oxo ligand) is excluded. n is an integer greater than 1, and a and b are numbers greater than 0, satisfying a / b=0.1 to 10.
[0079] In the above chemical formula (4), as the metal substance M, for example, Na, K, Ca, Mg, Si, Al, Ti, Cr, Mn, Fe, Co, Ni, Cu, Zn, etc. can be mentioned. These metal substances can be contained alone or in combination of two or more. Among them, from the perspective of excellent gas barrier properties under high humidity, especially oxygen barrier properties, Al, Si, Mg, Ni, Co, and Zn are preferred, Ni, Co, and Zn are particularly preferred, and Zn is particularly preferred.
[0080] In the above chemical formula (4), the anionic ligand A includes, for example, RO (alkoxy ligand), ROCO (carboxylic acid ligand), CO3, NO3, SO3, PO4, BO3, F, Br, Cl, etc. (R is an alkyl chain, C m H 2m+1 ; Chemical formulas such as m=1 to 20 are generally represented. Among them, as long as the effect of the present invention is not hindered, the alkyl chain may have a functional group such as an OH group). Among them, as anionic ligand A, O (oxy ligand) is excluded. These anionic ligands may be contained alone or in combination of two or more. Among them, from the viewpoint of interaction with hydrophilic resins, NO3, Cl, RO, and ROCO are preferred, ROCO is particularly preferred, and CH3OCO is particularly preferred.
[0081] The above-mentioned metal compound may contain water molecules.
[0082] In addition, the metal compound preferably has a main peak in X-ray diffraction at 2θ=2 to 15°, more preferably at 2θ=2 to 9°, and particularly preferably at 2θ=3 to 8°, when measured by wide-angle X-ray diffraction using CuKα rays.
[0083] It should be noted that the wide-angle X-ray diffraction was measured under the following conditions.
[0084] [Measurement conditions]
[0085] Equipment used: D8 DISCOVER (manufactured by Bruker Japan Co., Ltd.)
[0086] Detector: Two-dimensional detector VANTEC-500 (manufactured by Bruker Japan Co., Ltd.)
[0087] Voltage: 50kV
[0088] Current: 100mA
[0089] Camera length: 100mm
[0090] ·Measurement method: Reflection method
[0091] Cumulative time: 30 minutes
[0092] Wavelength: CuKα rays (Kα1 and Kα2 are not separated)
[0093] Detector position: 2θ = 10°
[0094] X-ray incident angle: θ = 0.3°
[0095] ·Conditions for 2θ direction one-dimensionalization: 2θ = 0 to 35°, azimuth angle (chi) = -95 to -85°
[0096] Azimuth direction one-dimensional: azimuth (chi) = -180 ~ 0°
[0097] When the azimuth direction is one-dimensionalized, the azimuth direction is one-dimensionalized within the range of 1.0° so that the peak with the strongest diffraction intensity is contained in the range of 2θ=2~15°. At this time, when a peak is observed in the range of -180~0° in the azimuth angle, it is judged that the diffraction peak is observed in the range of 2θ=2~15°. For example, when a diffraction peak is observed at 2θ=6.8°, when the azimuth direction is one-dimensionalized within the range of 2θ=6.0~7.0°, if a peak is observed in the range of azimuth angle=-180~0°, it can be judged that the diffraction peak is observed in the range of 2θ=2~15°.
[0098] From the perspective of interaction with the molecules of the hydrophilic resin and water molecules, the interlayer distance (distance between layers) of the metal compound is preferably 0.01 to 50 nm, more preferably 0.1 to 30 nm. The interlayer distance of the metal compound can be calculated by the Bragg formula based on the diffraction position of the strongest peak in the range of 2θ=2 to 15° when analyzed by X-ray diffraction.
[0099] The molecular weight of the layered structural unit peeled off from the metal compound is preferably 100 to 10,000, particularly preferably 200 to 2,000, from the viewpoint of the interaction of the hydrophilic resin at the molecular level.
[0100] Furthermore, the layered structural unit is preferably hydrophilic from the viewpoint of interaction with the molecules of the hydrophilic resin.
[0101] Furthermore, it is preferred that the layered structural unit does not decompose even when left to stand for 1000 hours in an environment of 20° C. and 90% RH.
[0102] Specific examples of the metal compound include layered compounds containing Zn as a metal substance. Among them, Zn-containing layered compounds represented by the chemical formula [Zn5(OH)8(CH3CO2)2·2H2O] are preferred from the perspective of excellent gas barrier properties under high humidity, especially excellent oxygen barrier properties.
[0103] In the present invention, it is presumed that the metal compound interacts with the hydrophilic resin to increase the polarity of the hydrophilic resin, thereby obtaining an effect of excellent gas barrier properties, particularly oxygen barrier properties, under high humidity.
[0104] The metal conversion content of the metal compound in the resin composition of the present invention is usually 0.01 to 20 parts by weight, preferably 0.01 to 10 parts by weight, more preferably 0.1 to 8 parts by weight, and particularly preferably 0.2 to 4 parts by weight, relative to 100 parts by weight of the hydrophilic resin. In addition, the metal conversion content of the metal compound in the resin composition of the present invention is usually 0.01 to 20% by weight, preferably 0.01 to 10% by weight, more preferably 0.1 to 8% by weight, and particularly preferably 0.2 to 4% by weight, relative to the resin composition. If the content of the metal compound is too small, there is a tendency for the gas barrier properties, especially the oxygen barrier properties, to be reduced under high humidity. If the content of the metal compound is too high, there is a tendency for the transparency to be reduced due to whitening when formed into a film or the like.
[0105] In addition, when the resin composition contains a plurality of metal compounds having different metal substances, the total amount of all the metal compounds contained in the resin composition is taken as the content.
[0106] In addition, the content of the above-mentioned metal compound can be determined by a standard addition method using ICP-MS.
[0107] The above-mentioned metal compound can be obtained, for example, by the following methods: method (I) of reacting the metal-containing compound in the presence of a base; method (II) of heating the metal-containing compound and reacting it.
[0108] Examples of the metal-containing compound used in the above methods include organic acid metal salts and inorganic metal salts.
[0109] As the organic acid constituting the above-mentioned organic acid metal salt, for example, monocarboxylic acids such as acetic acid, dicarboxylic acids such as succinic acid, oxalic acid, tartaric acid, citric acid, tribasic or higher carboxylic acids such as ethylenediaminetetraacetic acid, etc. can be enumerated. They can be used alone or in combination of two or more. In addition, the organic acid metal salt can be a hydrate or an anhydride.
[0110] As the organic acid metal salt, monovalent carboxylic acid metal salts are preferred, and metal acetate is particularly preferred, and zinc acetate or its hydrate is particularly preferred, from the viewpoint of excellent gas barrier properties, particularly oxygen barrier properties, under high humidity.
[0111] As the above-mentioned inorganic metal salt, for example, fluoride, chloride, bromide, iodide, oxo acid salt etc. of metal can be enumerated. They can be used alone or in combination of two or more. In addition, the inorganic metal salt can be a hydrate or anhydride.
[0112] As the inorganic metal salt, metal chlorides and oxoacid salts are preferred, and zinc chloride, zinc nitrate, or hydrates thereof are particularly preferred, from the viewpoint of excellent gas barrier properties, particularly oxygen barrier properties, under high humidity.
[0113] Each method is described in detail below.
[0114] [Method (I)]
[0115] The above method (I) is a method of reacting a metal-containing compound in the presence of a base.
[0116] Examples of the base used in the method (I) include hydroxides of alkali metals or alkaline earth metals, etc. Among them, hydroxides of alkali metals are preferred, and sodium hydroxide is particularly preferred, because of their excellent reactivity with the metal-containing compound.
[0117] In the reaction between the metal-containing compound and the base, the metal-containing compound and the base can usually be mixed in a solution and reacted.
[0118] The method of mixing the metal-containing compound with the base is not particularly limited, and examples thereof include the following methods: a method of mixing a solution in which the metal-containing compound is dissolved in a solvent with a solution in which the base is dissolved in a solvent; a method of mixing a slurry in which the metal-containing compound is dispersed with a solution in which the base is dissolved in a solvent; etc. Among them, from the perspective of reaction efficiency, a method of mixing a solution in which the metal-containing compound is dissolved in a solvent with a solution in which the base is dissolved in a solvent is preferred. Furthermore, when an organic acid metal salt is used as the metal-containing compound, a method of adding a solution in which the organic acid metal salt is dissolved in a solvent to a solution in which the base is dissolved in a solvent and mixing the solution is preferred, and when an inorganic metal salt is used, a method of adding a solution in which the base is dissolved in a solvent to a solution in which the inorganic metal salt is dissolved in a solvent and mixing the solution is preferred.
[0119] The solvent for dissolving the metal-containing compound and the base is not particularly limited as long as it can dissolve the metal-containing compound and the base, and examples thereof include water, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol and other lower alcohols having 1 to 5 carbon atoms. These can be used alone or in combination of two or more. Among them, water is preferred from the perspective of easy post-treatment.
[0120] The concentration of the metal-containing compound in the solution in which the metal-containing compound is dissolved is usually 0.5 to 3 mol / L, preferably 1 to 2 mol / L.
[0121] In addition, the concentration of the alkali in the solution containing the alkali dissolved in the solvent is usually 0.01 to 100 mol / L, preferably 0.1 to 30 mol / L, and particularly preferably 1 to 10 mol / L. If the concentration of the metal-containing compound and the alkali is too low than the above range, the reaction tends to be insufficient. In addition, if the concentration of the metal-containing compound and the alkali is too high than the above range, side reactions tend to occur.
[0122] The molar ratio of the metal-containing compound to the base (metal-containing compound:base) is usually 0.5:2 to 2:0.5, preferably 0.8:1.5 to 1.5:0.8, particularly preferably 0.9:1.2 to 1:1. If the molar ratio is outside the above range, the reaction tends to proceed insufficiently.
[0123] In addition, the pH when the metal-containing compound is reacted with the base is usually 4 to 9, preferably 5 to 8. When the pH is too low below the above range, the reaction tends to be insufficient. Moreover, when the pH is too high above the above range, the metal compound generated by the reaction tends to decompose. It should be noted that the pH is adjusted by adjusting the amount of the solution in which the metal-containing compound is dissolved and the amount of the solution in which the base is dissolved.
[0124] The reaction temperature in the above reaction is usually 15 to 60° C., preferably 20 to 40° C. If the reaction temperature is too low, the reaction tends to not proceed sufficiently, while if the reaction temperature is too high, the metal-containing compound decomposes due to heat, and the target metal compound tends not to be obtained.
[0125] The reaction time is usually 0.5 to 5 hours, preferably 1 to 3 hours, and the reaction can be carried out under normal pressure.
[0126] After the above reaction, a metal compound is obtained as a precipitate. The obtained metal compound may be used directly, but it is preferably used after being purified by washing, pulverization or the like.
[0127] [Method (II)]
[0128] The above method (II) is a method of heating and reacting a metal-containing compound.
[0129] The above-mentioned method (II) is usually carried out by heating the solution in which the metal-containing compound is dissolved while stirring.
[0130] As the solvent in which the metal-containing compound is dissolved, the solvents listed in the above method (I) can be used. Among them, water and alcohols are preferred, and water is particularly preferred.
[0131] As the heating conditions, the solution may be heated at a temperature of generally 20 to 100° C., preferably 50 to 95° C., and particularly preferably 70 to 90° C. If the reaction temperature is too low, the reaction tends to not proceed sufficiently, and if the reaction temperature is too high, the metal-containing compound decomposes due to heat, and the target metal compound tends not to be obtained.
[0132] The reaction time is usually 0.1 to 100 hours, preferably 0.5 to 30 hours, particularly preferably 1 to 10 hours, and the reaction can be carried out under normal pressure.
[0133] After the above reaction, a metal compound is obtained as a precipitate. The obtained metal compound may be used directly, or may be used after being purified by washing, pulverization or the like.
[0134] Generally, metal compounds refer to, for example, metal salts, metal oxides, metal complexes, metal elements or alloys, but the metal compounds obtained by the above methods are metal layer compounds having a layered structure with a specific interplanar spacing having the layered structural units shown in the above chemical formula (4). Therefore, when hydrophilic resin molecules and water molecules exist around the metal compound, the layers of the metal compound are peeled off, and the fine layered structural units after the peeling interact with the hydrophilic resin at the molecular level, and it is estimated that excellent gas barrier properties, especially oxygen barrier properties, can be obtained.
[0135] [Other ingredients]
[0136] In the resin composition of the present invention, within the scope of not hindering the effect of the present invention, it can contain: the compounding agent usually mixed in the resin composition, for example, heat stabilizer, antioxidant, antistatic agent, coloring agent, ultraviolet absorber, lubricant, plasticizer, light stabilizer, surfactant, antibacterial agent, desiccant, anti-blocking agent, flame retardant, crosslinking agent, curing agent, foaming agent, crystal nucleating agent, antifogging agent, biodegradable additive, silane coupling agent, oxygen absorbent etc. They can be used alone or in combination of two or more.
[0137] The resin composition of the present invention can be obtained by mixing, for example, a hydrophilic resin, a metal compound, and other components as necessary.
[0138] The resin composition of the present invention can also be obtained by, for example, mixing a hydrophilic resin, a metal-containing compound, and a solvent and heating and stirring the mixture. In the above method, the metal-containing compound reacts in the solvent to undergo structural changes, thereby generating a metal compound.
[0139] The amount of the metal-containing compound is usually 0.01 to 20 parts by weight, preferably 0.01 to 10 parts by weight, more preferably 0.1 to 8 parts by weight, particularly preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the hydrophilic resin in terms of metal.
[0140] The solvent is not particularly limited as long as it can dissolve the hydrophilic resin, and water is usually used. In order to shorten the drying time after film formation, lower alcohols having 1 to 5 carbon atoms, such as methanol, ethanol, propanol, n-butanol, isopropanol, etc., can be used within the range in which the hydrophilic resin can be dissolved.
[0141] The amount of the solvent blended is usually 100 to 9900 parts by weight, preferably 400 to 1900 parts by weight, based on 100 parts by weight of the hydrophilic resin.
[0142] The order of mixing the hydrophilic resin, the metal-containing compound and the solvent is not particularly limited, and they may be mixed all at once or sequentially. However, from the viewpoint of reactivity, it is preferred to mix the hydrophilic resin and the metal-containing compound in a solvent.
[0143] The heating temperature is usually 20 to 100° C., preferably 40 to 95° C., and particularly preferably 80 to 95° C. If the heating temperature is too low, the hydrophilic resin tends not to be completely dissolved, and if the heating temperature is too high, the metal-containing compound tends to decompose.
[0144] The reaction time is usually 0.5 to 5 hours, preferably 1 to 4 hours, and particularly preferably 2 to 3 hours. If the reaction time is too short, the reaction tends to be insufficient, and even if the reaction time is too long, the reaction yield does not improve and the economic efficiency tends to decrease.
[0145] In addition, the pressure during heating may be carried out at normal pressure.
[0146] <Resin composition>
[0147] The resin composition according to one embodiment of the present invention contains a hydrophilic resin and a metal compound, and satisfies the following formula (1) when formed into a thin film.
[0148] α1-β1≥1……(1)
[0149] In the above formula (1), "α1" represents the average metal atom concentration (%) within a depth range of 0 to 9 nm from the surface of the film, and the above "β1" represents the average metal atom concentration (%) within a depth range of 12 to 21 nm from the surface of the film.
[0150] In the resin composition of one embodiment of the present invention, the difference α1-β1 must be 1 or more, preferably 2 or more, and more preferably 3 or more. If α1-β1 is less than 1, the gas barrier properties under high humidity decrease. The upper limit of α1-β1 is usually 50.
[0151] The above average metal atom concentration is measured using an X-ray optical electron spectrometer under the following measurement conditions.
[0152] [X-ray optical electron spectrometer measurement conditions]
[0153] · Equipment used: JPS-9030 (manufactured by JEOL Ltd.)
[0154] Excitation X-ray source: non-monochromatic AlKa, power: 12kV, 25mA (300W)
[0155] Analyzer mode CAE mode (constant energy resolution mode)
[0156] Resolution EP: 50 energy levels 1eV
[0157] EP: 30 energy level 0.2eV
[0158] ·Analysis area φ6mm
[0159] The metal element in the average metal atom concentration measured by the X-ray optical electron spectrometer is preferably derived from the metal compound.
[0160] In one embodiment of the present invention, the average metal atom concentration near the surface of the film when the film is formed is increased, so that the gas barrier property under high humidity, especially the oxygen barrier property, is excellent. In order to obtain such a resin composition, for example, a method of leaving the resin composition at high humidity can be cited, among which a method of leaving the film containing the resin composition at high humidity is preferred.
[0161] Furthermore, the resin composition according to one embodiment of the present invention contains a hydrophilic resin and a metal compound, and satisfies the following condition (A).
[0162] Condition (A):
[0163] The above-mentioned resin composition is made into a 10% aqueous solution or aqueous dispersion, and the obtained cast film is left to stand for 1 week under the conditions of 23°C and 80% RH. When the contact angle (°) of water before treatment is set to α2 and the contact angle (°) of water after treatment is set to β2, the following formula (2) is satisfied.
[0164] (β2-α2)≥10……(2)
[0165] From the perspective of excellent gas barrier properties under high humidity, especially oxygen barrier properties, the difference (β2-α2) between the contact angle of water after the above treatment and the contact angle of water before the treatment is 10 or more, preferably 15 or more, and more preferably 20 or more. The contact angle of the above water is as follows: Under the conditions of 23°C and 50% RH, 2 μL of purified water is dropped on the above cast film to form a water drop, and the contact angle between the water drop and the surface of the cast film is measured 10 times using a contact angle meter (DropMaster 500: manufactured by KYOWAINTERFACE SCIENCE) as the average value.
[0166] In addition, from the viewpoint of excellent gas barrier properties, particularly oxygen barrier properties, under high humidity, the contact angle of water after the treatment is usually 60° or more, preferably 70° or more, particularly preferably 75° or more.
[0167] In addition, a resin composition according to one embodiment of the present invention comprises a hydrophilic resin and a metal compound, and when the resin composition is made into a film, the oxygen permeability (cc·3 μm / m 2 ·day·atm) satisfies the following formula (3).
[0168] Oxygen permeability (cc·3μm / m 2 ·day·atm)≤80……(3)
[0169] The oxygen permeability is preferably 80cc·3μm / m 2 ·day·atm or less, more preferably 70cc·3μm / m 2 ·day·atm or less, more preferably 55cc·3μm / m 2 ·day·atm or less, more preferably 40cc·3μm / m 2 ·day·atm or less, more preferably 35cc·3μm / m 2 ·day·atm or less, more preferably 30cc·3μm / m 2 ·day·atm or less, more preferably 25cc·3μm / m 2 ·day·atm or less, more preferably 20cc·3μm / m 2 ·day·atm or less, particularly preferably 10cc·3μm / m 2It should be noted that the above oxygen permeability is measured under an environment of 23°C and 80% RH, and the lower limit of the oxygen permeability is usually 0cc·3μm / m 2 ·day·atm. The above oxygen permeability can be obtained using an oxygen permeability measuring device.
[0170] <Film containing resin composition>
[0171] The film containing the resin composition of the present invention is obtained by forming a composition containing the above-mentioned resin composition into a film, and is preferably obtained by forming the above-mentioned resin composition into a film.
[0172] As a method for forming the above-mentioned film, for example, the following methods can be cited: a method using a solution or dispersion (coating liquid) of the resin composition of the present invention; a method of melt-molding a pellet-shaped composition containing the resin composition of the present invention using an extruder; etc. Among them, the method using a solution or dispersion (coating liquid) of the resin composition is preferred. In addition, the solid content concentration when using the above-mentioned coating liquid is usually 0.5 to 30% by weight, preferably 5 to 20% by weight.
[0173] The coating solution may be prepared by, for example, a method of simultaneously adding all components to a solvent and mixing them; a method of adding other components to a solution in which a part of the components is dissolved in a solvent and mixing them; etc. Among them, a method of adding other components to a solution in which a hydrophilic resin is dissolved in a solvent and mixing them is preferred from the perspective of workability.
[0174] In the method for obtaining the metal compound, it is also preferred to dissolve the hydrophilic resin in a solvent before reacting the metal-containing compound. From the viewpoint of workability, it is particularly preferred to obtain the metal compound by the method (II) above.
[0175] As the solvent, the solvents listed above for the metal compounds can be used, and among them, water is preferred.
[0176] As the film forming method, for example, a known method such as a method based on a casting method such as a melt extrusion method, an endless belt method, a drum method, and a coating method can be adopted. Among them, a method based on a casting method is preferred, and a method based on a coating method is particularly preferred.
[0177] Examples of the coating method include known methods such as bar coating, roll coating, die coating, gravure coating, comma coating, and screen printing.
[0178] After coating, the film can be dried by, for example, heating at 60 to 105° C. for 0.5 to 10 minutes to obtain a film made of the resin composition. The film can be stretched by uniaxial stretching, biaxial stretching or the like as required.
[0179] The above-mentioned film may form a single-layer film or a multilayer structure. The above-mentioned multilayer structure preferably has at least one layer comprising the above-mentioned film. In addition, the above-mentioned multilayer structure may be laminated with the film after film formation or with a substrate film formed from other substrate resins.
[0180] The thickness of the film containing the resin composition of the present invention is usually 0.1 to 200 μm, preferably 0.2 to 100 μm, and particularly preferably 0.3 to 50 μm. It should be noted that when the film after the film formation is a multilayer structure, the value obtained by summing up the thickness of all films containing the resin composition is taken as the thickness of the film.
[0181] Examples of the base resin include linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, high-density polyethylene, polyethylene resins such as ethylene-propylene (block and random) copolymers, ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers, polybutylene, polypentene, polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain), and (unmodified) polyolefin resins such as these. The broad sense polyolefin resins, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylate copolymers, polyester resins, polyamide resins (also comprising copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, chlorinated polyethylene, chlorinated polypropylene and other halogenated polyolefins, aromatic or aliphatic polyketones etc. of modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft modification with unsaturated carboxylic acids or their esters of hydrocarbons. They can be used alone or in combination of more than two kinds. In addition, the substrate film formed by these substrate resins can be subjected to surface treatments such as corona treatment.
[0182] As described above, by allowing the film containing the resin composition of the present invention to stand at high humidity, the film satisfies the above formula (1) and formula (2). Therefore, the film has excellent gas barrier properties, especially oxygen barrier properties, under high humidity. The principle of obtaining this effect is unclear, but it is speculated that this is because the molecules of the hydrophilic resin are plasticized by standing at high humidity, and the metal compound dispersed in the film interacts with the hydrophilic resin or is locally present on the surface of the film.
[0183] In the present invention, high humidity means 20±5° C. and 90±10% RH.
[0184] The standing time is usually 70 hours or more, preferably 100 hours or more, and more preferably 150 hours or more. The upper limit of the standing time is usually 1000 hours.
[0185] The transparency of the film containing the resin composition of the present invention is very excellent, and its transparency is particularly excellent than that of the film containing inorganic layered compounds and fillers. Specifically, the haze of the film containing the resin composition of the present invention is preferably 1% or less, more preferably 0.6% or less, further more preferably 0.3% or less, and particularly preferably 0.2% or less. It should be noted that the above haze is a HAZE value measured according to the standard of JIS K7361-1. For example, 10 test pieces of 50mm×50mm are cut out from the film and measured with a haze meter (NDH-4000 manufactured by Nippon Denshoku Co., Ltd.), and the average value of the 10 pieces is taken as the haze (%).
[0186] The resin composition of the present invention and a film containing the resin composition are useful as a packaging material, and can be particularly suitably used as a packaging material for foods, medicines, and the like.
[0187] Example
[0188] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited to the description of the Examples unless the gist of the present invention is exceeded.
[0189] In addition, "part" and "%" in the examples are by weight unless otherwise specified.
[0190] <<First embodiment>>
[0191] Prior to the first embodiment, the following hydrophilic resin was prepared.
[0192] 〔Hydrophilic resin〕
[0193] [PVA-based resin]
[0194] PVA (1) (unmodified PVA resin, average degree of polymerization 300, average degree of saponification 99 mol%)
[0195] [Polysaccharides]
[0196] Hydroxypropyl methylcellulose (HPMC) (Mitsubishi Chemical Foods Corporation, HYPROMELLOSE AW-4)
[0197] <Example 1-1>
[0198] 100 parts of PVA (1) and 1 part of Zn(CH3COO)2·2H2O as a metal-containing compound were added to 900 parts of water, and the mixture was heated and stirred at 90°C for 3 hours to prepare a resin composition (coating liquid). The obtained coating liquid was applied to the corona-treated surface of a PET substrate having a thickness of 38 μm and corona-treated using a wire rod #18, and dried at 80°C for 5 minutes to obtain a two-layer film having a film layer of 2.2 μm thick formed of the resin composition laminated on the PET substrate. The obtained film was allowed to stand for 200 hours under humidity conditioning conditions of 23°C and 80% RH to prepare a film.
[0199] <Example 1-2>
[0200] In Example 1-1, the amount of added Zn(CH3COO)2·2H2O was changed to 0.3 parts in metal conversion relative to 100 parts of PVA (1) so that the thickness of the film layer formed by the resin composition was 3 μm. Apart from this, the film was prepared using the same method as in Example 1-1 and under the same humidity control conditions.
[0201] <Example 1-3>
[0202] In Example 1-1, a thin film was produced by the same method as in Example 1-1, and under the same humidity control conditions, except that the thickness of the thin film layer formed of the resin composition was 0.4 μm.
[0203] <Example 1-4>
[0204] In Example 1-1, a film was prepared by the same method as in Example 1-1 and under the same humidity control conditions, except that PVA (1) was changed to HPMC and the thickness of the film layer formed of the resin composition was 1.7 μm.
[0205] <Example 1-5>
[0206] In Example 1-1, the amount of added Zn(CH3COO)2·2H2O was changed to 10 parts in metal conversion relative to 100 parts of PVA (1) so that the thickness of the film layer formed by the resin composition was 3 μm. Apart from this, the film was prepared using the same method as in Example 1-1 and under the same humidity control conditions.
[0207] <Comparative Example 1-1>
[0208] In Example 1-1, a film was produced by the same method as in Example 1-1 except that the thickness of the film layer formed of the resin composition was 3.5 μm and the humidity of the film was not regulated.
[0209] 〔Wide-angle X-ray diffraction (XRD) measurement〕
[0210] The thin films of Examples 1-1 to 1-5 and Comparative Example 1-1 obtained above were subjected to wide-angle X-ray diffraction (XRD) measurement under the following conditions.
[0211] [Measurement conditions]
[0212] Equipment used: D8 DISCOVER (manufactured by Bruker Japan Co., Ltd.)
[0213] Voltage: 50kV
[0214] Current: 100mA
[0215] Camera length: 150mm
[0216] Measurement method: Reflection method
[0217] Cumulative time: 20 minutes
[0218] The results of the measurement showed that the main peaks were detected at 2θ=6.8°, 13.5°, and 20.2° in the diffraction spectra of the films of Examples 1-1 to 1-5. These peaks were consistent with the Zn-containing layered compounds described in Inorg.Chem.2013, 52, 95-102, and therefore, the metal compounds contained in the films of Examples 1-1 to 1-5 were identified as Zn-containing layered compounds [Zn5(OH)8(CH3CO2)2·2H2O].
[0219] In addition, when the films of Examples 1-1 to 1-5 were measured by wide-angle X-ray diffraction, the interlayer distance was calculated using the Bragg formula based on the diffraction position of 2θ=6.8° where the peak intensity was the strongest. As a result, the above-mentioned Zn-containing layered compound [Zn5(OH)8(CH3CO2)2·2H2O] was a layered compound with an interlayer distance of 1.3 nm.
[0220] On the other hand, in the thin film of Comparative Example 1-1, the main peak detected in the thin films of Examples 1-1 to 1-5 was not detected.
[0221] <Measurement by X-ray photoelectron spectroscopy>
[0222] For the films of Examples 1-1 to 1-5 and Comparative Example 1-1 obtained above, the average Zn atomic concentration (%) in the range of 0 to 9 nm from the surface depth of the thin film layer formed by the resin composition, and the average Zn atomic concentration (%) in the range of 12 to 21 nm from the surface depth of the above-mentioned thin film layer were measured using an X-ray photoelectron spectrometer.
[0223] The measurement conditions are as follows.
[0224] [Measurement conditions]
[0225] · Equipment used: JPS-9030 (manufactured by JEOL Ltd.)
[0226] Excitation X-ray source: non-monochromatic AlKa, power: 12kV, 25mA (300W)
[0227] Analyzer mode CAE mode (constant energy resolution mode)
[0228] Resolution EP: 50 energy levels 1eV
[0229] EP: 30 energy level 0.2eV
[0230] ·Analysis area φ6mm
[0231] 〔Oxygen barrier properties〕
[0232] Only the film layer formed of the resin composition was peeled off from the films of Examples 1-1 to 1-5 and Comparative Example 1-1 obtained above, and the oxygen permeability of the film was measured at 23°C and 80% RH using an oxygen permeability measuring device (OX-TRAN100A, manufactured by MOCON).
[0233] [Table 1]
[0234]
[0235] ※1: Hydroxypropyl methylcellulose
[0236] ※2: Content relative to 100 parts by weight of hydrophilic resin
[0237] As can be seen from Table 1 above, the oxygen permeability of the resin composition film layer of the films of Examples 1-1 to 1-5 is 80 cc·3 μm / m 2 ·day·atm or less, and the oxygen barrier property is excellent. In addition, the oxygen permeability of the resin composition film layer of the film of Comparative Example 1-1 when measured under the above conditions exceeds 100cc·3μm / m 2 ·day·atm, poor oxygen barrier properties.
[0238] Furthermore, the resin composition film layers of the films of Examples 1-1 to 1-5, which contained a hydrophilic resin and a metal compound and had α1-β1 of 1 or more, were excellent in oxygen barrier properties under high humidity.
[0239] On the other hand, the film of Comparative Example 1-1 in which α1-β1 was less than 1 had poor oxygen barrier properties under high humidity in the resin composition film layer.
[0240] <<Second embodiment>>
[0241] Prior to the second embodiment, the following hydrophilic resin was prepared.
[0242] 〔Hydrophilic resin〕
[0243] [PVA-based resin]
[0244] PVA (2-1) (unmodified PVA resin, average degree of polymerization 300, average degree of saponification 99 mol%)
[0245] ·PVA (2-2) (modified PVA resin, average degree of polymerization 450, average degree of saponification 98 mol%)
[0246] PVA (2-3) (unmodified PVA resin, average degree of polymerization 400, average degree of saponification 88 mol%)
[0247] [Polysaccharides]
[0248] · Starch (water-soluble starch, manufactured by Fujifilm Wako Pure Chemical Corporation, starch (soluble))
[0249] · Hydroxypropyl methylcellulose (Mitsubishi Chemical Foods Corporation, HYPROMELLOSE AW-4)
[0250] <Example 2-1>
[0251] 100 parts of PVA (2-1) and 1 part of Zn acetate in terms of metal were added to 900 parts of water, and the mixture was heated to 90°C while being stirred to dissolve. After that, the mixture was stirred for 3 hours while being maintained at 90°C, and then cooled to room temperature (23°C) to prepare a solution of a resin composition. The obtained solution of the resin composition was adjusted to a solid content concentration of 10% with water, and then film-formed by a casting method, and dried in a hot air dryer at 120°C for 5 minutes to obtain a resin composition film (thickness 3 μm).
[0252] Furthermore, the resin composition film was laminated to a thickness of 30 μm or more, and wide-angle X-ray diffraction was performed according to the above method. As a result, a diffraction peak was observed at 2θ=6.2°.
[0253] <Example 2-2>
[0254] In Example 2-1, except that PVA (2-1) was changed to PVA (2-2) and the amount of Zn acetate added was 5 parts in terms of metal, a resin composition film (thickness 3 μm) was obtained in the same manner as in Example 2-1. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, a diffraction peak was observed at 2θ = 6.2°.
[0255] <Example 2-3>
[0256] In Example 2-2, except that the amount of Zn acetate added was 10 parts in terms of metal, a resin composition film (3 μm in thickness) was obtained in the same manner as in Example 2-2. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, a diffraction peak was observed at 2θ=6.2°.
[0257] <Example 2-4>
[0258] In Example 2-1, except that PVA (2-1) was changed to hydroxypropylmethylcellulose, a resin composition film (thickness 3 μm) was obtained in the same manner as in Example 2-1. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, a diffraction peak was observed at 2θ=6.2°.
[0259] <Example 2-5>
[0260] In Example 2-1, except that PVA (2-1) was changed to starch, a resin composition film (thickness 3 μm) was obtained in the same manner as in Example 2-1. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, a diffraction peak was observed at 2θ=6.2°.
[0261] <Example 2-6>
[0262] In Example 2-1, except that PVA (2-1) was changed to PVA (2-3), a resin composition film (thickness 3 μm) was obtained in the same manner as in Example 2-1. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, a diffraction peak was observed at 2θ=6.2°.
[0263] <Comparative Example 2-1>
[0264] A thin film of PVA (2-1) (3 μm in thickness) was obtained in the same manner as in Example 2-1 except that Zn acetate was not added. Wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, no diffraction peak was observed at 2θ=2 to 15°.
[0265] <Comparative Example 2-2>
[0266] In Example 2-2, a thin film of PVA (2-2) (thickness 3 μm) was obtained in the same manner as in Example 2-2 except that Zn acetate was not added. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, no diffraction peak was observed at 2θ=2 to 15°.
[0267] <Comparative Example 2-3>
[0268] In Example 2-4, a hydroxypropylmethylcellulose film (thickness 3 μm) was obtained in the same manner as in Example 2-4 except that Zn acetate was not added. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, no diffraction peak was observed at 2θ=2 to 15°.
[0269] <Comparative Example 2-4>
[0270] In Example 2-5, a starch film (thickness 3 μm) was obtained in the same manner as in Example 2-5 except that Zn acetate was not added. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, no diffraction peak was observed at 2θ=2 to 15°.
[0271] <Comparative Example 2-5>
[0272] In Example 2-6, a thin film of PVA (2-3) (thickness 3 μm) was obtained in the same manner as in Example 2-6 except that Zn acetate was not added. In addition, wide-angle X-ray diffraction was performed in the same manner as in Example 2-1. As a result, no diffraction peak was observed at 2θ=2 to 15°.
[0273] [Contact angle measurement]
[0274] For the films of Examples 2-1 to 2-6 and Comparative Examples 2-1 to 2-5 obtained above, 2 μL of purified water was dripped onto the films at 23°C and 50% RH to form water drops. The contact angle between the water drop and the film surface was measured 10 times using a contact angle meter (DropMaster 500: manufactured by KYOWA INTERFACESCIENCE Co., Ltd.), and the average value was taken as the contact angle of water before treatment (α2). In addition, the contact angle of water (β2) after these films were left to stand for 1 week under high humidity conditions of 23°C and 80% RH was measured in the same manner as above. The results are shown in Table 2 described below.
[0275] 〔Oxygen barrier properties〕
[0276] The oxygen permeability of the films of Examples 2-1 to 2-6 and Comparative Examples 2-1 to 2-5 left to stand for one week under the high humidity conditions was measured using an oxygen permeability measuring apparatus (OX-TRAN100A, manufactured by MOCON) at 23°C and 80% RH.
[0277] [Table 2]
[0278] ※1 HPMC: Hydroxypropyl methylcellulose
[0279] ※2Content relative to 100 parts of hydrophilic resin
[0280] As can be seen from Table 2 above, the films of the resin compositions of Examples 2-1 to 2-6, which contain a hydrophilic resin and a metal compound and in which the difference between the contact angle (β2) of water after long-term treatment at high humidity and the contact angle (α2) of water before treatment is 10 or more, have excellent oxygen barrier properties at high humidity.
[0281] On the other hand, the films of Comparative Examples 2-1 to 2-5, in which the difference between the water contact angles (β2) and (α2) was less than 10, all had poor oxygen barrier properties.
[0282] The above embodiments show specific aspects of the present invention, but the above embodiments are merely examples and are not to be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to be within the scope of the present invention.
[0283] Industrial Applicability
[0284] The resin composition of the present invention is excellent in gas barrier properties, particularly oxygen barrier properties, under high humidity and is therefore useful as a packaging material, and can be particularly suitably used as a packaging material for foods, pharmaceuticals, and the like.
Claims
1. A resin composition, characterized in that The invention comprises a hydrophilic resin and a metal compound, wherein the metal compound is a layered compound containing Zn as a metal substance, and the metal conversion content of the metal compound is 0.01 to 20% by weight relative to the resin composition. When the resin composition is made into a film, it satisfies the following formula (1): α1-β1≥1……(1) The α1% represents the average metal atomic concentration within a range of 0 to 9 nm in depth from the film surface, and the β1% represents the average metal atomic concentration within a range of 12 to 21 nm in depth from the film surface.
2. A resin composition, characterized in that The invention comprises a hydrophilic resin and a metal compound, wherein the metal compound is a layered compound containing Zn as a metal substance, and the metal conversion content of the metal compound is 0.01 to 20% by weight relative to the resin composition. The resin composition satisfies the following condition A: Condition A: The resin composition is made into a 10 wt % aqueous solution or aqueous dispersion, and the obtained cast film is left to stand for 1 week under the conditions of 23° C. and 80% RH. When the contact angle of water before treatment is set to α2 and the contact angle of water after treatment is set to β2, the following formula (2) is satisfied, wherein the unit of the water contact angle is °, (β2-α2)≥10……(2)。 3. A resin composition, characterized in that The invention comprises a hydrophilic resin and a metal compound, wherein the metal compound is a layered compound containing Zn as a metal substance, and the metal conversion content of the metal compound is 0.01 to 20% by weight relative to the resin composition. When the resin composition is made into a film, the oxygen permeability under 23°C and 80% RH environment satisfies the following formula (3), and the unit of the oxygen permeability is cc·3μm / m 2 ·day·atm, Oxygen permeability ≤80……(3).
4. A film, characterized in that: A resin composition comprising the resin composition according to any one of claims 1 to 3.
5. A multilayer structure, characterized in that: The invention has a plurality of layers, and at least one layer comprises the film according to claim 4.