Method for manufacturing semiconductor substrate and semiconductor substrate

By forming an oxide semiconductor layer with a crystalline phase at high temperatures, the problems of undercutting and undercutting in the etching process of thin film transistors in the prior art are solved, and the stability and carrier mobility of the device are improved.

CN113838801BActive Publication Date: 2024-10-22BOE TECHNOLOGY GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010591840.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-24
Publication Date
2024-10-22
Estimated Expiration
2040-06-24

AI Technical Summary

Technical Problem

In the existing technology, it is difficult to form crystalline active layer materials at room temperature, which leads to easy undercutting and undercutting during the etching process, reducing the stability and yield of thin film transistors.

Method used

The physical vapor deposition process is used to form the first oxide semiconductor layer at a higher temperature, and the second oxide semiconductor layer is directly formed on it to form a channel stack of crystalline phases, reducing the existence of defective layers at the interface, thereby Avoid undercutting and drilling during etching.

Benefits of technology

It improves the stability and carrier mobility of thin film transistors, reduces defect formation during the etching process, and enhances the overall performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113838801B_ABST
    Figure CN113838801B_ABST
Patent Text Reader

Abstract

A method for manufacturing a semiconductor substrate and a semiconductor substrate. The manufacturing method comprises forming the first semiconductor layer at an interface on the substrate when the substrate is at a first temperature, wherein the material of the first semiconductor layer is a first oxide semiconductor material; directly forming the second semiconductor layer on the first semiconductor layer, wherein the material of the second semiconductor layer is a second oxide semiconductor material; the first semiconductor layer and the second semiconductor layer are patterned into a seed layer and a first channel layer, respectively, the first channel layer and the seed layer are both crystalline phase layers, wherein the first oxide semiconductor material and the second oxide semiconductor material can both be formed into a crystalline phase at a second temperature, the second temperature is less than or equal to 40°C, and the first temperature is greater than or equal to 100°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present disclosure relate to a method for manufacturing a semiconductor substrate and a semiconductor substrate. Background Art

[0002] Amorphous semiconductor materials are widely used in display technology driver devices. For example, amorphous silicon thin film transistors dominate the display semiconductor substrate backplane due to their simple process, good device uniformity and low temperature process. Oxide semiconductor thin film transistors with amorphous oxide semiconductors as channels, such as amorphous indium gallium zinc oxide (a-IGZO) and amorphous indium zinc oxide (a-IZO), are expected to replace amorphous silicon thin film transistors as mainstream display driver devices because of their high channel mobility, good large-area uniformity and visible light stability. Summary of the invention

[0003] At least some embodiments of the present disclosure provide a method for manufacturing a semiconductor substrate, comprising: providing a substrate; forming a semiconductor stack including a first semiconductor layer, a second semiconductor layer and a third semiconductor layer on the substrate by a physical vapor deposition process, comprising: when the substrate is at a first temperature, forming the first semiconductor layer at an interface on the substrate, wherein the material of the first semiconductor layer is a first oxide semiconductor material; directly forming the second semiconductor layer on the first semiconductor layer, wherein the material of the second semiconductor layer is a second oxide semiconductor material; and forming the third semiconductor layer, wherein the material of the third semiconductor layer is a third oxide semiconductor material; performing a composition process on the semiconductor stack so that the first semiconductor layer, the second semiconductor layer and the third semiconductor layer are patterned into a seed layer, a first channel layer and a second channel layer, respectively, wherein the seed layer, the first channel layer and the second channel layer constitute a channel stack; forming a gate and a gate insulating layer on the substrate; and forming a source and a drain on the substrate having the channel stack formed thereon, wherein the source and the drain are electrically connected to the channel stack. The second channel layer is located between the gate and the first channel layer, the first oxide semiconductor material is different from the third oxide semiconductor material, the first channel layer and the seed layer are both crystalline phase layers. The first oxide semiconductor material and the second oxide semiconductor material can both be formed into a crystalline phase at a second temperature, the second temperature is less than or equal to 40° C., and the first temperature is greater than or equal to 100° C.

[0004] In some embodiments, the gate is located between the channel stack and the substrate, and the interface is a surface of the third semiconductor layer away from the substrate.

[0005] In some embodiments, the manufacturing method further includes: forming an insulating layer on the substrate, wherein the insulating layer is located between the first semiconductor layer and the substrate, the channel stack is located between the gate and the substrate, and the interface is a surface of the insulating layer away from the substrate.

[0006] In some embodiments, the channel stack has a bottom surface and a side surface facing the substrate, the bottom surface and the side surface are both planes, and a first angle between the bottom surface and the side surface is 20° to 70°.

[0007] In some embodiments, the channel stack has a bottom surface and a side surface facing the substrate, the side surface includes a first sub-side surface and a second sub-side surface, the bottom surface, the first sub-side surface and the second sub-side surface are all planes, a second angle between the bottom surface and the first sub-side surface is 50° to 80°, a third angle between the second sub-side surface and the bottom surface is 20° to 70°, and the second angle is different from the third angle.

[0008] In some embodiments, the third semiconductor layer is an amorphous layer.

[0009] In some embodiments, the electron mobility of the third semiconductor layer is greater than the electron mobility of the first semiconductor layer and the second semiconductor layer.

[0010] In some embodiments, the thickness of the second semiconductor layer is 4 to 8 times the thickness of the first semiconductor layer.

[0011] In some embodiments, the band gap Eg1 of the second channel layer, the band gap Eg2 of the seed layer, and the band gap Eg3 of the first channel layer satisfy: Eg1<Eg2≤Eg3;

[0012] The conduction band bottom energy level Ec1 of the second channel layer, the conduction band bottom energy level Ec2 of the seed layer and the conduction band bottom energy level Ec3 of the first channel layer satisfy: |Ec1|>|Ec2|≥|Ec3|;

[0013] A valence band top energy level Ec1 of the second channel layer, a valence band top energy level Ec2 of the seed layer, and a valence band top energy level Ec3 of the first channel layer satisfy: |Ev1|<|Ev2|≤|Ev3|.

[0014] In some embodiments, the seed layer has a thickness of 50 angstroms to 100 angstroms.

[0015] In some embodiments, the first temperature is greater than 120°C.

[0016] In some embodiments, the first oxide semiconductor material of the first semiconductor layer and the second oxide semiconductor material of the second semiconductor layer are the same, and the second semiconductor layer is formed at the second temperature.

[0017] In some embodiments, each of the first oxide semiconductor material and the second oxide semiconductor material includes two or more metal elements of In, Ga, Zn, and Sn.

[0018] In some embodiments, each of the first oxide semiconductor material and the second oxide semiconductor material is an IGZO material, wherein the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 7%-14%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 20%~40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 50%~70%.

[0019] In some embodiments, each of the first oxide semiconductor material and the second oxide semiconductor material is an IGZO material, wherein the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 35%-50%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 10%~40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 20%~40%.

[0020] In some embodiments, the third semiconductor layer includes a first semiconductor sublayer and a second semiconductor sublayer, the first semiconductor sublayer is between the gate and the second semiconductor sublayer, the first semiconductor sublayer is a crystalline phase layer, the second semiconductor sublayer is an amorphous phase layer, the gate is located between the channel stack and the substrate, and the interface is the surface of the second semiconductor sublayer away from the substrate.

[0021] In some embodiments, the third semiconductor layer further includes a third semiconductor sublayer, the third semiconductor sublayer is located between the gate and the first semiconductor sublayer, and the third semiconductor layer is a crystalline phase layer.

[0022] In some embodiments, for the same etching solution, a ratio of an etching rate of the third semiconductor layer to an etching rate of the second semiconductor layer is in a range of 0.2 to 5.

[0023] At least some embodiments of the present disclosure provide a semiconductor substrate, including: a substrate substrate; and

[0024] A thin film transistor on a substrate, wherein the thin film transistor includes a gate, a gate insulating layer, a channel stack and a source and drain electrically connected to the channel stack, and the channel stack includes: a seed layer of a first oxide semiconductor material, a first channel layer of a second oxide semiconductor material and a second channel layer of a third oxide semiconductor material. The second channel layer is located between the gate and the first channel layer, the second oxide semiconductor material is different from the third oxide semiconductor material, the first channel layer and the seed layer are both crystalline phase layers, the first oxide semiconductor material and the second oxide semiconductor material are both materials that can form a crystalline phase at a second temperature, and the second temperature is less than or equal to 40°C. The semiconductor substrate also includes an interface on the substrate, the distance between the surface of the first channel layer facing the substrate and the interface is less than or equal to 100 angstroms, and the seed layer is located between the interface and the surface of the first channel layer facing the substrate.

[0025] In some embodiments, the gate is located between the channel stack and the substrate, and the interface is a surface of the second channel layer away from the substrate.

[0026] In some embodiments, the semiconductor substrate further includes: an insulating layer on the base substrate, wherein the insulating layer is located between the seed layer and the base substrate, the channel stack is located between the gate and the base substrate, and the interface is a surface of the insulating layer away from the base substrate.

[0027] In some embodiments, the channel stack has a bottom surface and a side surface facing the substrate, the bottom surface and the side surface are both planes, and a first angle between the bottom surface and the side surface is 20° to 70°.

[0028] In some embodiments, the channel stack has a bottom surface and a side surface facing the substrate, the side surface includes a first sub-side surface and a second sub-side surface, the bottom surface, the first sub-side surface and the second sub-side surface are all planes, a second angle between the bottom surface and the first sub-side surface is 50° to 80°, a third angle between the second sub-side surface and the bottom surface is 20° to 70°, and the second angle is different from the third angle.

[0029] In some embodiments, the second channel layer is an amorphous phase layer.

[0030] In some embodiments, the electron mobility of the second channel layer is greater than the electron mobility of the seed layer and the first channel layer.

[0031] In some embodiments, the thickness of the first channel layer is 4 to 8 times the thickness of the seed layer.

[0032] In some embodiments, the band gap Eg1 of the second channel layer, the band gap Eg2 of the seed layer, and the band gap Eg3 of the first channel layer satisfy: Eg1<Eg2≤Eg3;

[0033] The conduction band bottom energy level Ec1 of the second channel layer, the conduction band bottom energy level Ec2 of the seed layer and the conduction band bottom energy level Ec3 of the first channel layer satisfy: |Ec1|>|Ec2|≥|Ec3|;

[0034] A valence band top energy level Ec1 of the second channel layer, a valence band top energy level Ec2 of the seed layer, and a valence band top energy level Ec3 of the first channel layer satisfy: |Ev1|<|Ev2|≤|Ev3|.

[0035] In some embodiments, the seed layer has a thickness of 50 angstroms to 100 angstroms.

[0036] In some embodiments, the first oxide semiconductor material is the same as the second oxide semiconductor material.

[0037] In some embodiments, each of the first oxide semiconductor material and the second oxide semiconductor material includes two or more metal elements of In, Ga, Zn, and Sn.

[0038] In some embodiments, the first oxide semiconductor material is an IGZO material, wherein the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 7%-14%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 20%-40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 50%-70%.

[0039] In some embodiments, the first oxide semiconductor material is an IGZO material, wherein the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 35%-50%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 10%-40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 20%-40%.

[0040] In some embodiments, the second channel layer includes a first channel sublayer and a second channel sublayer, the first channel sublayer is between the gate and the second channel sublayer, the first channel sublayer is a crystalline phase layer, the second channel sublayer is an amorphous phase layer, the gate is located between the channel stack and the substrate, and the interface is a surface of the second channel sublayer away from the substrate.

[0041] In some embodiments, the second channel layer further includes a third channel sublayer, the third channel sublayer is located between the gate and the first channel sublayer, and the third channel layer is a crystalline phase layer.

[0042] In some embodiments, for the same etching solution, a ratio of an etching rate of the second channel layer to an etching rate of the first channel layer is in a range of 0.2 to 5. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments or related technical descriptions will be briefly introduced below. Obviously, the drawings in the following description only relate to some embodiments of the present disclosure and are not limitations of the present disclosure.

[0044] Figure 1 A flow chart of a method for manufacturing a semiconductor substrate according to at least one embodiment of the present disclosure is shown.

[0045] Figures 2A to 2H A schematic diagram of a substrate structure corresponding to each step in a method for manufacturing a semiconductor substrate according to an embodiment of the present disclosure is shown.

[0046] FIG. 3A to FIG. 3D Graphs showing the XRD analysis results of sample substrates 1 to 4.

[0047] 4A to 4D TEM images and FFT-converted diffraction patterns of each semiconductor layer in the semiconductor stack in the embodiment of the present disclosure and a comparative semiconductor layer.

[0048] Figure 5A A scanning electron microscope photograph showing a thin film transistor in a semiconductor substrate according to an embodiment of the present disclosure; Figure 5B A scanning electron microscope photograph showing a channel stack of a thin film transistor in a semiconductor substrate according to an embodiment of the present disclosure when the photoresist thereon is not removed when the channel stack is formed by using a first etching solution; Figure 5C A scanning electron microscope photograph showing a channel stack of a thin film transistor in a semiconductor substrate according to an embodiment of the present disclosure when the photoresist thereon is not removed when the channel stack is formed by using a second etching solution; Figure 5D FIG. 1 is a graph showing IV characteristic test results of a thin film transistor in an embodiment of the present disclosure.

[0049] Fig. 6A and 6B Schematic diagrams of the structures of a semiconductor substrate having a semiconductor stack and a channel stack formed thereon according to an example of an embodiment of the present disclosure are respectively shown; Figure 6C and 6DSchematic diagrams of structures of a semiconductor substrate having a semiconductor stack and a channel stack formed thereon according to another example of an embodiment of the present disclosure are respectively shown.

[0050] Figures 7A to 7H A schematic diagram of a substrate structure corresponding to each step in a method for manufacturing a semiconductor substrate according to another embodiment of the present disclosure is shown.

[0051] Fig. 8A A schematic diagram showing the formation of drilling and undercutting in the patterning process in the related art; Figure 8B A scanning electron microscope photograph of a channel stack in the related art is shown; Figure 8C This is a graph showing IV characteristic test results of a thin film transistor with drilling and undercutting in a stacked channel in the related art. DETAILED DESCRIPTION

[0052] The technical solutions in the embodiments of the present disclosure will be clearly and completely described below in conjunction with the accompanying drawings. With reference to the non-limiting exemplary embodiments shown in the accompanying drawings and described in detail in the following description, the exemplary embodiments of the present disclosure and their various features and advantageous details are more fully described. It should be noted that the features shown in the figures are not necessarily drawn to scale. The description of known materials, components and process technologies is omitted so as not to obscure the exemplary embodiments of the present disclosure. The examples are intended only to facilitate the understanding of the implementation of the exemplary embodiments of the present disclosure, and to further enable those skilled in the art to implement the exemplary embodiments. Therefore, the examples should not be understood as limiting the scope of the exemplary embodiments of the present disclosure.

[0053] Unless otherwise defined, the technical or scientific terms used herein shall have the usual meanings understood by persons of ordinary skill in the field to which the present disclosure belongs. The words "first", "second" and similar terms used in the present disclosure do not indicate any order, quantity or importance, but are only used to distinguish different components. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly. In addition, in the present disclosure, a certain numerical point and the upper and lower numerical points of a certain numerical range include all numerical points within the deviation range of ±5% of the corresponding numerical point.

[0054] In oxide semiconductor thin film transistors, a layer of oxide that blocks etching liquid corrosion can be added to the top of the channel layer as an etching barrier layer to reduce the corrosion of the underlying oxide by the etching liquid during the source and drain etching process, thereby reducing back channel defects and improving the stability and mobility of the transistor. For example, adding a layer of oxide etching barrier layer can reduce back channel etching defects and improve device stability.

[0055] Due to material limitations, existing active layer materials cannot crystallize at room temperature and can only crystallize in a high temperature environment (high temperature and high oxygen can form microcrystallization). The inventors of this application have discovered that metal oxide semiconductor materials with a specific element ratio can form a crystalline phase layer at room temperature, and the crystalline phase layer formed at room temperature will have a mismatch area (i.e., a defect layer) at the growth interface.

[0056] In the related art, in the case where the channel layer includes two oxide semiconductor layers L1 and L2, if a crystalline oxide semiconductor layer L2 is formed on the oxide semiconductor layer L1 at room temperature, the material of the oxide semiconductor layer L2 is a room temperature crystallizable material, and a defect layer Ls is easily generated at the interface thereof due to lattice mismatch. The defect layer Ls is easily etched along the interface between the two oxide semiconductor layers due to a relatively fast etching rate, so that the etching liquid is easily drilled along the interface between the two oxide semiconductor layers, thereby forming drilling and undercutting during the patterning process, see Fig. 8A and Figure 8B If the drilling and undercutting are formed, the etching solution will etch the overlap between the source and drain S / D and the channel stack during the subsequent source and drain etching process, causing the source and drain to be disconnected (see Fig. 8A In addition, in the case where the oxide semiconductor layer L2 is directly formed on the insulating layer at room temperature, the material of the oxide semiconductor layer L2 is a room temperature crystallizable material, and a defective layer is easily generated at the interface between the insulating layer and the oxide semiconductor layer L2 due to lattice mismatch. The defective layer is easily etched by the etching solution along the interface between the oxide semiconductor layer and the insulating layer due to the high etching rate, thereby forming an undercut during the patterning process. Figure 7C Also shown in the figure is the IV characteristic test result of the thin film transistor with drilling and undercut in the stacked channel in the related art. Figure 8C It can be seen that the IV characteristics of the thin film transistor in the related art in the off state fluctuate significantly, which is due to the adverse effects of drilling and undercutting on the side of the channel stack during the etching process.

[0057] At least one embodiment of the present disclosure provides a method for manufacturing a semiconductor substrate, comprising: providing a substrate substrate; forming a semiconductor stack including a first semiconductor layer, a second semiconductor layer and a third semiconductor layer on the substrate substrate by a physical vapor deposition process, comprising: when the substrate substrate is at a first temperature, forming the first semiconductor layer at an interface on the substrate substrate, wherein the material of the first semiconductor layer is a first oxide semiconductor material; directly forming the second semiconductor layer on the first semiconductor layer, wherein the material of the second semiconductor layer is a second oxide semiconductor material; and forming the third semiconductor layer, wherein the material of the third semiconductor layer is a third oxide semiconductor material; performing a composition process on the semiconductor stack so that the first semiconductor layer, the second semiconductor layer and the third semiconductor layer are The three semiconductor layers are patterned into a seed layer, a first channel layer and a second channel layer, respectively, wherein the seed layer, the first channel layer and the second channel layer constitute a channel stack; a gate and a gate insulating layer are formed on the substrate; and a source and a drain are formed on the substrate having the channel stack, and the source and the drain are electrically connected to the channel stack, wherein the second channel layer is located between the gate and the first channel layer, the first oxide semiconductor material is different from the third oxide semiconductor material, the first channel layer and the seed layer are both crystalline phase layers, wherein the first oxide semiconductor material and the second oxide semiconductor material can both form a crystalline phase at a second temperature, the second temperature is less than or equal to 40°C, and the first temperature is greater than or equal to 100°C.

[0058] At least another embodiment of the present disclosure provides a semiconductor substrate, comprising: a substrate; and a thin film transistor on the substrate, wherein the thin film transistor comprises a gate, a gate insulating layer, a channel stack and a source and drain electrically connected to the channel stack, the channel stack comprises: a seed layer of a first oxide semiconductor material, a first channel layer of a second oxide semiconductor material and a second channel layer of a third oxide semiconductor material, wherein the second channel layer is located between the gate and the first channel layer, the second oxide semiconductor material is different from the third oxide semiconductor material, the first channel layer and the seed layer are both crystalline phase layers, the first oxide semiconductor material and the second oxide semiconductor material are both materials that can be formed into a crystalline phase at a second temperature, the second temperature is less than or equal to 40°C, wherein the semiconductor substrate also comprises an interface on the substrate, the distance between the surface of the first channel layer facing the substrate and the interface is less than or equal to 100 angstroms, and the seed layer is located between the interface and the surface of the first channel layer facing the substrate. Here, the interface on the substrate does not specifically refer to the surface of the substrate itself, but can also refer to the surface between two different material layers formed on the substrate that are in contact with each other. The different material layers include insulating layers and semiconducting layers.

[0059] In the above-mentioned embodiments of the present disclosure, since a first semiconductor layer is formed on the interface with a first oxide semiconductor material that can form a crystalline phase at a lower second temperature (for example, room temperature or lower temperature) at a higher first temperature, and then a second semiconductor layer of a crystalline phase is formed directly on the first semiconductor layer, the defective layer existing in the case of forming the second semiconductor layer directly on the interface at room temperature is eliminated or the thickness of the defective layer is effectively reduced, thereby avoiding undercutting and drilling in the subsequent etching process of the oxide semiconductor stack.

[0060] Figure 1 A flow chart of a method for manufacturing a semiconductor substrate according to at least one embodiment of the present disclosure is shown.

[0061] See also Figure 1 , a method for manufacturing a semiconductor substrate according to at least one embodiment of the present disclosure comprises the following steps:

[0062] S110: providing a substrate;

[0063] S120: forming a semiconductor stack including a first semiconductor layer, a second semiconductor layer and a third semiconductor layer on a substrate by a physical vapor deposition process;

[0064] S130: performing a patterning process on the semiconductor stack, so that the first semiconductor layer, the second semiconductor layer and the third semiconductor layer are patterned into a seed layer, a first channel layer and a second channel layer, respectively, wherein the seed layer, the first channel layer and the second channel layer constitute a channel stack;

[0065] S140: forming a gate and a gate insulating layer on the substrate;

[0066] S150: forming a source and a drain on the substrate having the channel stack.

[0067] In the method for manufacturing a semiconductor substrate of at least one embodiment of the present disclosure, the execution order of steps S110 to S150 is not limited. Depending on the structure to be formed (for example, whether the thin film transistor on the substrate is a top gate structure or a bottom gate structure), the execution order of steps S110 to S150 can be adjusted accordingly. In addition, the method for manufacturing a semiconductor substrate of at least one embodiment of the present disclosure may also include the steps of forming other layers and corresponding pixel structures. The method for manufacturing a semiconductor substrate of at least one embodiment of the present disclosure will be described in detail below in conjunction with the accompanying drawings. The embodiments of the present disclosure are not limited to the specific examples described.

[0068] Figures 2A to 2H A schematic diagram of a substrate structure corresponding to each step in a method for manufacturing a semiconductor substrate 100 according to an embodiment of the present disclosure is shown.

[0069] See also Figure 2A , a base substrate 110 is provided, and a gate 170 and a gate insulating layer 160 are formed on the base substrate 110. The base substrate 110 may be a rigid substrate or a flexible substrate. For example, the material of the base substrate 110 may be glass, polyimide, polycarbonate, polyethylene, polyacrylate, or polyethylene terephthalate, etc. The gate insulating layer 160 may be formed as a single layer of silicon nitride (SiNx) or silicon oxide (SiO2) or a stacked layer of silicon nitride (SiNx) and silicon oxide (SiO2).

[0070] See also Figures 2B to 2D A semiconductor stack 140 is formed on the gate insulating layer 160 by a physical vapor deposition process, such as a sputtering process. The semiconductor stack 140 includes a semiconductor layer 141 , a semiconductor layer 142 , and a semiconductor layer 143 .

[0071] Here, the materials of the semiconductor layer 142 and the semiconductor layer 143 are both indium gallium zinc oxide (IGZO, where I represents the indium element (In), G represents the gallium element (Ga), Z represents the zinc element (Zn), and O represents the oxygen element) as an example for explanation. For example, the metal oxide semiconductor of each of the semiconductor layer 142 and the semiconductor layer 143 contains two or more metal elements of In, Ga, Zn, and Sn. The embodiments of the present disclosure are not limited to this. In other embodiments, the materials of the semiconductor layer 142 and the semiconductor layer 143 may also be In-Sn-Zn-O materials or In-Al-Sn-Zn-O materials.

[0072] Here, the semiconductor stack 140 includes a three-layer structure of a semiconductor layer 141, a semiconductor layer 142, and a semiconductor layer 143 as an example for explanation. The embodiments of the present disclosure are not limited to this. In other embodiments, the semiconductor stack 140 may also include other semiconductor layers, so it can be a 4-layer or more layer structure, as long as it includes the semiconductor layer 141, the semiconductor layer 142, and the semiconductor layer 143 in a prescribed order. In other embodiments, there may be no obvious interface between the semiconductor layer 142 and the semiconductor layer 143, that is, the semiconductor layer 142 and the semiconductor layer 143 are substantially connected as a continuous layer. In this case, the semiconductor stack 140 may also be a two-layer structure.

[0073] Here, the sputtering process usually bombards the surface of a solid target material with particles (ions, neutral atoms or molecules) of a certain energy, so that atoms or molecules on the surface of the solid target material are separated from the target material and fall on the surface of the substrate with a certain energy to form a film on the substrate.

[0074] See also Figure 2B , a semiconductor layer 141 is deposited on the gate insulating layer 160. Here, the deposition temperature of the semiconductor layer 141 is not limited. The material of the semiconductor layer 141 is an oxide semiconductor material. For example, the material of the semiconductor layer 141 is deposited at a lower second temperature (e.g., room temperature of 0°C to 40°C or lower) to form an amorphous phase layer. It should be noted that the temperature here refers to the temperature at the substrate in the physical vapor deposition process.

[0075] For example, the oxide semiconductor material of the semiconductor layer 141 is, for example, IGZO (111), IGZO (423), IGZO (136), IGZO (432), IGZO (312), IGZO (513), IGZO (534), IGZO (713), IGZO (514), IGZYO, IGTO, ITZO, IZO, ITO, etc. Here, the numerical value in the brackets represents the ratio of the number of atoms of the three elements In, Ga and Zn in this material. For example, IGZO (423) means that in this material, the ratio of the number of atoms of the three elements In, Ga and Zn is 4:2:3. Preferably, the oxide semiconductor material of the semiconductor layer 141 is a material with high mobility. For example, the oxide semiconductor material of the semiconductor layer 141 is IGZO (423), which has a narrow band gap (2.5-2.7 eV) and a high carrier concentration (1×10 16 -9×10 16 ) and the carrier Hall mobility is high (15-25cm 2 / V·s).

[0076] The embodiments of the present disclosure do not limit the crystal morphology and oxide semiconductor material of the semiconductor layer 141. For example, in another embodiment, the semiconductor layer 141 may be a crystalline phase layer. The material of the semiconductor layer 141 may be other metal oxide semiconductor materials not mentioned above.

[0077] Next, see Figure 2C , at a higher first temperature, a semiconductor layer 142 is deposited on an upper surface (interface) 111 of the semiconductor layer 141 away from the substrate 110. Here, the interface refers to a surface where two different material layers are in contact with each other. The upper surface 111 is the interface between the semiconductor layer 141 and the atmosphere in the deposition chamber before the semiconductor layer 142 is formed, and is the interface between the semiconductor layer 141 and the semiconductor layer 142 after the semiconductor layer 142 is formed. The first temperature is greater than or equal to 100°C. Preferably, the first temperature is greater than or equal to 120°C. In one example, the first temperature is at least 60°C higher than the second temperature.

[0078] The material of the semiconductor layer 142 is an oxide semiconductor material different from that of the semiconductor layer 141. Here, the two materials being the same means that the two materials not only contain the same type and number of elements, but also the same proportion of each element in all elements (here, the corresponding proportion is allowed to have an error of less than 5% due to process accuracy). Therefore, the two materials being different means that the two materials contain different types of elements or different numbers of elements or different proportions of each element in all elements.

[0079] For example, the oxide semiconductor material of the semiconductor layer 142 is an oxide semiconductor material that can form a crystalline phase at a second temperature (e.g., room temperature). Here, the position of the crystalline phase formed by the oxide semiconductor material at the second temperature is not limited. As long as the oxide semiconductor material can form a crystalline phase within a sufficient thickness range (e.g., 500 angstroms), it can be considered as an oxide semiconductor material that can form a crystalline phase at the second temperature. Since the first temperature is at least 60°C higher than the second temperature, for an oxide semiconductor material that can form a crystalline phase at room temperature or lower, a first temperature greater than or equal to 100°C can effectively promote its rapid crystallization at the growth interface and thereby effectively reduce the defect layer at the interface.

[0080] For example, the material of the semiconductor layer 142 can be a metal oxide semiconductor material containing two or more metal elements of In, Ga, Zn, and Sn, such as IGZO (136), IGZO (423), IGZO (132), IGZO (243), IGZO (153), IGO, ITZO, etc.

[0081] In an example of an indium gallium zinc oxide material that can be crystallized at room temperature, the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 7%-14%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 20%-40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 50%-70%. The indium gallium zinc oxide material can form a crystalline phase layer at room temperature by a physical vapor deposition process (the oxygen partial pressure is preferably between 0% and 50% (O2 / Ar+O2)). In another example of an indium gallium zinc oxide material that is crystallizable at room temperature, the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 35%-50%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 10%-40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 20%-40%. The indium gallium zinc oxide material can form a crystalline phase layer at around 25°C by a physical vapor deposition process (the oxygen partial pressure is preferably greater than 50%).

[0082] For example, the oxide semiconductor material of the semiconductor layer 142 is a Zn-rich IGZO material. For example, in the Zn-rich IGZO material, the ratio of the number of Zn atoms to the sum of the number of In, Ga and Zn atoms is greater than or equal to 60%. For example, the material of the semiconductor layer 142 is IGZO (136), which has a wide band gap (2.9 to 3.3 eV) and a low carrier concentration (1×10 14 -5×10 15). The IGZO (136) of the semiconductor layer 142 can be formed into a crystalline state (for example, a C-axis crystal (CAAC) crystal type) at room temperature. In the present embodiment, the crystalline semiconductor layer 142 is formed by sputtering deposition at a temperature greater than 100°C to reduce or eliminate a possible defect layer at the interface 111. For example, the conduction band bottom energy level of the IGZO (136) crystalline phase layer of the semiconductor layer 142 is higher than the conduction band bottom energy level of the IGZO (423) amorphous phase layer of the semiconductor layer 141, and the valence band top energy level of the IGZO (136) crystalline phase layer of the semiconductor layer 142 is lower than the valence band top energy level of the IGZO (423) amorphous phase layer of the semiconductor layer 141.

[0083] Here, the thickness of the semiconductor layer 142 of the crystalline phase is, for example, 50 to 100 angstroms. If an X-ray diffraction test is performed on the semiconductor layer 142 (for example, the diffraction angle scanning range is 20° to 70°, and the scanning step length is 0.02° / s), a protruding crystalline diffraction peak can be observed on the XRD spectrum after denoising. For example, when the material of the semiconductor layer 142 is indium gallium zinc oxide, there is a crystalline diffraction peak at a diffraction angle position of 25 to 35° on its XRD ray diffraction spectrum. For the same material of the same thickness, in the XRD spectrum obtained by the same XRD test, the higher the intensity of the crystalline diffraction peak at the same position, the smaller the half-height width, and the greater the ratio of the crystalline peak integral area to the total integral area, the higher the degree of crystallization. In addition, it is also possible to determine whether the material layer being tested is a crystalline phase layer by high-resolution transmission electron microscopy photographs and their selected area electron diffraction patterns.

[0084] If a comparative semiconductor layer with the same thickness as the semiconductor layer 142 is deposited with the same material as the semiconductor layer 142 using the same sputtering process as the semiconductor layer 142 (the only difference is that the temperature of the substrate is room temperature), the comparative semiconductor layer is an amorphous phase layer. The thickness of the crystalline phase semiconductor layer 142 and the comparative semiconductor layer are, for example, 50 to 100 angstroms. That is to say, although a material that can be crystallized at room temperature is used to form the semiconductor layer, an amorphous phase layer will still be formed at room temperature at a position very close to the deposition interface, such as the comparative semiconductor layer here. The amorphous phase comparative semiconductor layer is not easy to be found due to its small thickness, but it is easy to cause undercutting and drilling in the subsequent etching process. The inventors have found that using a higher temperature to deposit the oxide semiconductor material that can be crystallized at room temperature from the very beginning can form a crystalline phase layer within a thickness range very small (for example, 100 angstroms) from the deposition interface, such as the above-mentioned semiconductor layer 142. That is to say, a high temperature process is used to cause the room temperature crystallizable material to form a crystalline phase semiconductor layer 142 more quickly at a position closer to the deposition interface, replacing the amorphous comparison semiconductor layer formed at the same position at room temperature, thereby effectively avoiding possible undercutting and drilling in the subsequent etching process.

[0085] Here, the “crystalline phase layer” refers to an oxide semiconductor layer that mainly contains an oxide semiconductor in a crystalline phase state, and may also contain a tiny amorphous portion; the “amorphous phase layer” refers to a layer that mainly contains an oxide semiconductor in an amorphous phase state, and may also contain a tiny crystalline phase portion.

[0086] In this embodiment, the semiconductor layer 142 deposited at a higher temperature can directly form a crystalline phase layer on the surface (interface) 111, thereby replacing the defective layer existing at the corresponding position when the semiconductor layer 142 is deposited at room temperature, so as not to cause obvious undercutting and drilling formation in the subsequent composition process.

[0087] See also Figure 2D , a semiconductor layer 143 is deposited on the upper surface of the semiconductor layer 142 away from the substrate 110. The oxide semiconductor material of the semiconductor layer 143 can be deposited to form a crystalline phase layer at room temperature; for example, the oxide semiconductor material of the semiconductor layer 143 is the same as that of the semiconductor layer 142 to better avoid and reduce the defect area between the two. Of course, the present embodiment is not limited to this. In another example, the materials of the semiconductor layer 143 and the semiconductor layer 142 can be different. The material of the semiconductor layer 143 can be a metal oxide semiconductor material containing two or more metal elements of In, Ga, Zn, and Sn, for example, IGZO (136), IGZO (423), IGZO (132), IGZO (243), IGZO (153), IGO, ITZO, etc.

[0088] In this embodiment, the deposition temperature of the semiconductor layer 143 is not limited as long as the semiconductor layer 143 is formed into a crystalline phase layer. That is, the semiconductor layer 143 can be deposited into a crystalline phase layer at room temperature or at the first temperature.

[0089] Since the semiconductor layer 142 is deposited at a relatively high temperature, it has a higher crystallinity than when a material layer of the same thickness is deposited at room temperature. The higher crystallinity of the semiconductor layer 142 has a good inducing crystallization effect on the semiconductor layer 143 formed directly thereon, thereby enabling the semiconductor 143 to have better crystallinity. In other words, due to the inducing crystallization effect of the semiconductor layer 142 with a relatively high crystallinity, even when the semiconductor layer 143 is deposited at room temperature, the semiconductor layer 143 can have better crystallinity and density.

[0090] For example, the thickness of the semiconductor layer 143 is 4 to 8 times the thickness of the semiconductor layer 142. This thickness range has a better effect in avoiding drilling and undercutting and inducing crystallization. However, the present embodiment is not limited thereto.

[0091] The semiconductor layer 143 is directly formed on the crystallized semiconductor layer 142, and the crystallized semiconductor layer 142 has an inducing crystallization effect on it. Therefore, on the one hand, no matter the semiconductor layer 143 is deposited and formed at room temperature or at a higher temperature, there will be no defective layer that can cause obvious undercutting and drilling in the etching process at the interface between the semiconductor layer 142 and the semiconductor layer 143; on the other hand, the crystallized semiconductor layer 143 can be formed to be more uniform and dense, so it is not easy to be etched to form defects in the subsequent patterning process.

[0092] In one example, the semiconductor layer 143 and the semiconductor layer 142 are made of the same material and deposited at the same temperature, and thus no obvious interface may exist between the semiconductor layer 143 and the semiconductor layer 142 .

[0093] In another example, the semiconductor layer 143 and the semiconductor layer 142 are made of the same material, but the deposition temperature of the semiconductor layer 142 is higher (for example, the first temperature) and the semiconductor layer 143 is deposited at room temperature, then the crystallinity of the semiconductor layer 142 is greater than that of the semiconductor layer 143 with the same thickness.

[0094] Optionally, after forming the semiconductor stack 140, for example, an annealing treatment may be performed on the oxide semiconductor stack 140. Here, the heat treatment is performed in an air atmosphere at a temperature of 300° C. to 380° C. The heat treatment time is, for example, 30 minutes to 2 hours.

[0095] In the above method, the composition and film formation conditions are controlled to form the semiconductor stack 140. In order to confirm the crystal state of the oxide semiconductor layer just after film formation (before annealing treatment) in the above method, the inventors of the present application conducted the following analysis.

[0096] First, sample substrates 1 to 4 having a single-layer semiconductor film are prepared. Sample substrate 1 is prepared by forming a film layer of a first oxide semiconductor material on a glass substrate by sputtering. Sample substrates 2 and 3 are prepared by forming a film layer of a second oxide semiconductor material on a glass substrate at different temperatures. Sample substrate 4 is prepared by forming a film layer of a third oxide semiconductor material on a glass substrate. Here, the first to third oxide semiconductor materials are, for example, In-Ga-Zn-O system materials. In sample substrates 1 to 4, the thickness of the film layer of the semiconductor material on the glass substrate is, for example, 100 angstroms. Table 1 shows the composition of the target used when forming the In-Ga-Zn-O system semiconductor film layer and the film formation conditions of the In-Ga-Zn-O system semiconductor film.

[0097] [Table 1]

[0098]

[0099] Next, X-ray diffraction (XRD) analysis was performed on each sample substrate obtained. FIG. 3A to FIG. 3D X-ray diffraction patterns of sample substrates 1 to 4 are shown in FIG.

[0100] from FIG. 3A to FIG. 3D It can be seen that the X-ray diffraction patterns of all sample substrates have a broad peak P1 at 2θ=20-25°. This is considered to be a peak caused by the glass substrate. Figure 3A and 3B As shown, the X-ray diffraction patterns of sample substrates 1 and 2 have no crystalline peaks except for the peak P1 of the glass substrate, so it can be confirmed that the semiconductor film layer on sample substrate 1 (which may correspond to the semiconductor layer 141) and the semiconductor film layer on sample substrate 2 (which may correspond to the comparative semiconductor layer) are amorphous films; sample 2 may also contain a small amount of microcrystalline regions, but the overall structure is mainly amorphous, so the XRD pattern shows no crystalline diffraction peaks; as shown Figure 3C As shown in the figure, the X-ray diffraction pattern of sample substrate 3 has a peak P2 of crystallinity near 2θ=32° in addition to the peak P1 of the glass substrate. Sample 3 also contains a small amount of amorphous regions, but the overall structure is mainly crystalline, so the XRD pattern shows a crystalline diffraction peak. In addition, as Figure 3D As shown, the X-ray diffraction pattern of sample substrate 4 has a crystalline peak P3 near 2θ=32° in addition to the peak P1 of the glass substrate. Therefore, it can be confirmed that the semiconductor film layer on sample substrate 3 (which may correspond to semiconductor layer 142) and the semiconductor film layer on sample substrate 4 (which may correspond to semiconductor layer 143) are both crystalline film layers. Peak P3 of sample substrate 4 is sharper (with a smaller peak width) than peak P2 of sample substrate 3, so it can be seen that the semiconductor film of sample substrate 4 has higher crystallinity. When semiconductor layer 143 is formed at room temperature, its XRD peak position is slightly shifted to the right compared to the seed layer (i.e., the peak position of the crystallization peak of semiconductor layer 143 prepared at room temperature is about 32.2°, and the peak position of the crystallization peak of semiconductor layer 142 prepared at a higher first temperature is about 31.8°)

[0101] In addition, even if the above-mentioned annealing treatment is performed on the sample substrates 1 and 2, the semiconductor film layer thereon still maintains the amorphous phase state. If the sample substrates 3 and 4 are subjected to the annealing treatment, the crystallinity of the semiconductor film layer thereon may be further increased.

[0102] As described above, a single-layer semiconductor film is formed on a substrate, and its crystal state is investigated. However, in the case where a plurality of semiconductor films are stacked to form a stacked semiconductor layer, it is difficult to investigate the crystal state of each semiconductor film separately by XRD analysis. For example, the crystal state of each layer of the stacked semiconductor layer can be investigated by TEM observation of a cross section of the stacked semiconductor layer. In addition, for example, the composition of each layer in the stacked semiconductor layer can also be analyzed by XPS, AES, etc.

[0103] See below Figures 4A to 4D The crystal state of each layer in the semiconductor stack formed in an example of the present embodiment and the above-mentioned comparative semiconductor layer are described. For example, in this example, the semiconductor layer 141 is formed by sputtering using a target material having an atomic ratio of In:Ga:Zn of 4:2:3. A mixed gas of rare gas atoms such as argon and an oxidizing gas can be used as a sputtering gas (atmosphere). The oxidizing gas may be O2, CO2, O3, H2O, N2O, etc. Here, a mixed gas containing Ar gas and oxygen (O2) gas is used. The proportion of oxygen gas during film formation by sputtering is set to, for example, a partial pressure ratio of 5% or more and 20% or less. In addition, the substrate temperature during film formation is set to, for example, any temperature between room temperature and 100°C. The pressure of the gas atmosphere (sputtering pressure) is not particularly limited as long as it is within the range in which the plasma can be discharged stably, but is set to, for example, 0.1 to 3.0 Pa.

[0104] Figure 4A TEM images and FFT-converted diffraction patterns of the semiconductor layer 141 are shown. Figure 4A In the left figure, no obvious crystallization is observed in the TEM electron microscope image of the semiconductor layer 141; see Figure 4A In the right figure, the diffraction pattern of the FFT conversion of the semiconductor layer 141 has only one diffuse central spot, that is, an amorphous halo, which confirms that the semiconductor layer 141 is an amorphous phase layer.

[0105] The semiconductor layer 142 is formed by sputtering using a target material having an atomic ratio of In:Ga:Zn of 1:3:6. A mixed gas containing Ar gas and oxygen (O2) gas is used as the sputtering gas. For example, the partial pressure ratio is set to be greater than 0% and less than 50%, preferably, greater than 0% and less than 20%. In addition, the base substrate temperature during film formation is set to the above-mentioned first temperature (greater than 100°C), for example. The pressure of the gas atmosphere (sputtering pressure) is set to 0.1 to 3.0 Pa, for example.

[0106] Figure 4B TEM images and FFT-converted diffraction patterns of the semiconductor layer 142 are shown. Figure 4B In the left figure, the semiconductor layer 142 can be clearly observed in the TEM electron microscope image; see Figure 4BIn the right figure of FIG. 1 , a dot pattern appears in the diffraction pattern of the semiconductor layer 142 converted by FFT, confirming that the semiconductor layer 142 is a crystalline phase layer.

[0107] The semiconductor layer 143 is formed by sputtering using a target having an atomic ratio of In:Ga:Zn of 1:3:6. A mixed gas containing Ar gas and oxygen (O2) gas is used as the sputtering gas. For example, the partial pressure ratio is set to be greater than 0% and less than 50%, and greater than 0% and less than 50%. The substrate temperature and sputtering pressure during film formation may also be the same as those during formation of the semiconductor layer 142.

[0108] Figure 4C TEM images and FFT-converted diffraction patterns of the semiconductor layer 143 are shown. Figure 4C In the left figure, the TEM electron microscope image of the semiconductor layer 143 can be observed to have obvious crystallization; see Figure 4C In the right figure, a dot pattern appears in the diffraction pattern of the FFT conversion of the semiconductor layer 143, confirming that the semiconductor layer 143 is a crystalline phase layer. In this example, the deposition process and materials of the semiconductor layers 142 and 143 are the same, there is no significant difference between the semiconductor layers 142 and 143, and there is no obvious boundary area. The crystallinity of the semiconductor layer 142 is lower than or equal to the crystallinity of the semiconductor layer 143. That is, in terms of the overall crystal volume and the ratio of crystalline / amorphous, the semiconductor layer 142 is smaller than the semiconductor layer 143. See Figure 4B and 4C , the lattice arrangement of semiconductor layer 143 is more long-range ordered than that of semiconductor layer 142; see Figure 4B and 4C In the right figure, the diffraction spots corresponding to the semiconductor layer 143 are clearer than the diffraction spots corresponding to the semiconductor layer 142.

[0109] The comparative semiconductor layer is formed by sputtering using a target having an atomic ratio of In:Ga:Zn of 1:3:6. A mixed gas containing Ar gas and oxygen (O2) gas is used as the sputtering gas. For example, the partial pressure ratio is set to be greater than 0% and less than 20%. In addition, the base substrate temperature during film formation is set to room temperature, for example. The pressure of the gas atmosphere (sputtering pressure) is set to 0.1 to 3.0 Pa, for example.

[0110] Figure 4D TEM images and FFT-converted diffraction patterns of the comparative semiconductor layer 141 are shown. Figure 4D In the left figure, no obvious crystallization is observed in the TEM electron microscope image of the semiconductor layer; see Figure 4D In the right figure, the diffraction pattern of the FFT conversion of the comparison semiconductor layer has only one diffuse central spot, that is, the amorphous halo, which confirms that the comparison semiconductor layer is an amorphous phase layer.

[0111] Next, see Figure 2E , a patterning process is performed on the semiconductor stack 140 to form a channel stack 1400. The channel stack 1400 includes a channel layer 1410, a seed layer 1420, and a channel layer 1430. The channel layer 1410, the seed layer 1420, and the channel layer 1430 are parts of the semiconductor layer 141, the semiconductor layer 142, and the semiconductor layer 143, respectively.

[0112] Here, the patterning process performed on the semiconductor stack 140 includes, for example:

[0113] Coating a photoresist layer on the semiconductor stack 140;

[0114] Performing exposure and development on the photoresist layer to form a photoresist pattern P;

[0115] The semiconductor stack 140 is wet-etched with the photoresist pattern as a shield to obtain the channel stack 1400. For example, the wet etching uses H2SO4+HNO3+H2O as an etching solution or HNO3+CH3COOH+H3PO4+H2O as an etching solution. Here, since there is no defective layer or the thickness of the defective layer is small enough at the interface 111 between the seed layer 1420 and the channel layer 1410, no obvious undercut and drilling will be caused at the interface 111 during the wet etching process; and

[0116] The photoresist pattern is removed.

[0117] For example, for the same etching solution, the ratio of the etching rate of the third semiconductor layer to the etching rate of the second semiconductor layer is in the range of 0.2 to 5. The same etching solution is, for example, HNO3+CH3COOH+H3PO4+H2O etching solution or H2SO4+HNO3+H2O etching solution.

[0118] See also Figure 2F , forming a source 181 and a drain 182 on the substrate 110 having the channel stack 1400; and forming a passivation layer 150 on the substrate 110 having the source 181 and the drain 182. The source 181 and the drain 182 are, for example, directly lapped on the channel stack 1400. The source 181 and the drain 182 may include one or more of Au, Ag, Cu, Ni, Pt, Pd, Al, Mo, etc. The source 181 and the drain 182 may be a single-layer metal or a multi-layer metal.

[0119] See also Figure 2H , a light emitting element and an encapsulation layer 240 are formed on the passivation layer 150 .

[0120] In the present embodiment, the light-emitting element is an organic light-emitting diode (OLED) 225. In addition, the light-emitting element may also be a quantum dot light-emitting diode (QLED), etc., but the embodiments of the present disclosure are not limited thereto. For example, in other embodiments, the semiconductor substrate may be an array substrate for a liquid crystal display device or an electronic paper display device, and in this case, there is no need to form a light-emitting element on the planarization layer of the semiconductor substrate; for example, in the case of a liquid crystal display device, a pixel electrode for controlling the deflection of a liquid crystal material is formed on the planarization layer of the semiconductor substrate, and a common electrode may be further formed on the same layer or a different layer of the pixel electrode; in the case of an electronic paper display device, the pixel electrode and the electronic ink layer on the planarization layer of the semiconductor substrate, the pixel electrode is used as a voltage for applying to drive the charged microparticles in the electronic ink to move for display operation.

[0121] Taking an organic light emitting diode as an example, the organic light emitting diode includes a first driving electrode 210, a second driving electrode 230, and a light emitting layer 220 between the first driving electrode 210 and the second driving electrode 230. The first driving electrode 210 is formed on a flat surface of the planarization layer 190, the light emitting layer 220 is formed on the first driving electrode 210, and the second driving electrode 230 is formed on the light emitting layer 220.

[0122] In addition, the semiconductor substrate 100 further includes a pixel defining layer 250 having an opening to define a light emitting area, and the light emitting layer 220 is formed in the opening. For example, the second driving electrode 230 may be a common electrode, which may be disposed on the entire or a portion of the display area, covering a plurality of pixels, i.e., shared by a plurality of pixels. When an appropriate voltage is applied between the first driving electrode 210 and the second driving electrode 230, one of the first driving electrode 210 and the second driving electrode 230 injects holes into the light emitting layer 220, and the other injects electrons into the light emitting layer 220. Electrons and holes recombine with each other in the light emitting layer 220 to generate excitons, and light is emitted by the energy generated when the excitons fall back from an excited state to a ground state.

[0123] The encapsulation layer (or encapsulation layer) 240 covers the second driving electrode 230. The encapsulation layer 240 can seal the organic light emitting diode, thereby reducing or preventing the degradation of the organic light emitting diode caused by moisture and / or oxygen included in the environment. For example, the encapsulation layer 240 may include a structure in which an inorganic layer and an organic layer are stacked.

[0124] It can be understood that in this embodiment, the thin film transistor TFT1 on the substrate includes a gate 170 , a channel stack 1400 , a source 181 and a drain 182 .

[0125] In one example, the band gap Eg1 of the channel layer 1410, the band gap Eg2 of the seed layer 1420, and the band gap Eg3 of the channel layer 1430 satisfy: Eg1<Eg2≤Eg3; the conduction band bottom energy level Ec1 of the channel layer 1410, the conduction band bottom energy level Ec2 of the seed layer 1420, and the conduction band bottom energy level Ec3 of the channel layer 1430 satisfy: │Ec1│>│Ec2│≥│Ec3│; the valence band top energy level Ec1 of the channel layer 1410, the valence band top energy level Ec2 of the seed layer 1420, and the valence band top energy level Ec3 of the channel layer 1430 satisfy: │Ev1│<│Ev2│≤│Ev3│. See Figure 2H , the thin film transistor TFT1 has a bottom gate structure, and the channel layer 1410 is located between the gate 170 and the channel layer 1430. In this case, the band gap of the channel layer 1410 is the smallest, and its energy band structure is located below the seed layer 1420 and the channel layer 1430. When the thin film transistor is working, due to the band gap difference, the channel layer 1410 is a high carrier concentration material, and the carriers generated by it need to cross the band gap difference barrier of the seed layer 1420 and the channel layer 1430 before they can jump to other film layers. Therefore, most of the carriers are confined in the channel layer 1410. The role of using the seed layer 1420 is, on the one hand, to remove the defective layer and thus the bottom cutting and drilling problem, and on the other hand, to reduce internal interface defects and improve device stability; at the same time, as a crystalline material, the seed layer 1420 is more matched with the channel layer 1430, and the interface defects are lower; the role of the channel layer 1430 is: on the one hand, it has high crystallinity, which can block the etching damage of the source and drain etchant, reduce the bombardment of the passivation layer deposition, prevent the diffusion of source and drain elements, prevent the diffusion of elements such as oxygen, etc. On the other hand, the large band gap can ensure that the minimum carriers diffuse from the channel layer 1410 to the channel layer 1430, thereby reducing carrier loss; therefore, in the semiconductor substrate manufactured according to the embodiment of the present disclosure, the carrier mobility and stability of the thin film transistor are effectively improved.

[0126] Figure 5A A scanning electron microscope photograph showing a thin film transistor in a semiconductor substrate according to an embodiment of the present disclosure; Figure 5B A scanning electron microscope photograph showing a channel stack of a thin film transistor in a semiconductor substrate according to an embodiment of the present disclosure when the photoresist thereon is not removed when the channel stack is formed by using a first etching solution; Figure 5C A scanning electron microscope photograph is shown in which the photoresist on a channel stack of a thin film transistor in a semiconductor substrate according to an embodiment of the present disclosure is not removed when the channel stack is formed by using a second etching solution.

[0127] Figure 5A The scanning electron microscope image corresponds to Figure 2HThe thin film transistor in the semiconductor substrate shown in FIG. The gate electrode 170 is located on the upper surface of the deposition substrate 110 . The gate insulating layer 160 is located on the gate electrode 170 . The channel stack 1400 is located on the gate insulating layer 160 , and the source electrode 181 and the drain electrode 182 are overlapped at both ends of the channel stack 1400 .

[0128] from Figure 5B The structure of the channel stack 1400 and the source 181 at the overlap position can be clearly seen. Figure 5B The channel stack 1400 has a bottom surface 1401 and a side surface 1402 facing the substrate 110, and the plane where the side surface 1402 is located intersects with the plane where the bottom surface 1401 is located. The bottom surface 1401 and the side surface 1402 are both planes. The first angle between the bottom surface 1402 and the side surface 1401 is 20° to 70°. For example, the first angle is preferably 45°. Figure 5B The channel stack 1400 shown is formed by etching with a first etching solution, for example, the composition of the first etching solution is HNO3+CH3COOH+H3PO4+H2O.

[0129] In another example, if the channel stack 1400 is formed by etching with a second etching solution, the composition of the second etching solution is, for example, H2SO4+HNO3+H2O, then the channel stack 1400 will be formed as Figure 5C Shape shown.

[0130] See also Figure 5C , the channel stack 1400 has a bottom surface 1401 facing the substrate 110 and a side surface 1403 intersecting with the bottom surface 1401. The side surface 1403 includes a first sub-side surface 1403-1 and a second sub-side surface 1403-2. The plane where the first sub-side surface 1403-1 is located intersects with the plane where the bottom surface 1401 is located. The plane where the second sub-side surface 1403-2 is located intersects with the plane where the first sub-side surface 1403-1 is located and the plane where the bottom surface 1401 is located. The bottom surface 1401, the first sub-side surface 1403-1 and the second sub-side surface 1403-2 are, for example, all planes. The second angle between the bottom surface 1401 and the first sub-side surface 1403-1 is 50° to 80°. The third angle between the second sub-side surface 1403-2 and the bottom surface 1401 is 20° to 70°. The second angle is different from the third angle. Here, the first angle, the second angle and the third angle can all be understood as the slope angles of the channel stack.

[0131] Figure 5D FIG. 2 shows the IV characteristic test result of the thin film transistor in the embodiment of the present disclosure. Figure 5D It can be seen that the IV characteristics of the thin film transistor in this embodiment have almost no fluctuation in the off state, compared with the situation in the related art (see Figure 7C ), the electrical performance of the thin film transistor TFT1 in this embodiment is significantly improved.

[0132] from Figures 5A to 5D It can be seen that in the thin-film transistor according to the embodiment of the present disclosure, due to the presence of the seed layer deposited at a relatively high temperature at a position extremely close to the deposition interface, the side of the channel stack is substantially flat, and the slope angle is also within the above-mentioned favorable angle range, thereby making the stacked channel have a more uniform structure and the thin-film transistor have more stable electrical properties.

[0133] It can be understood that the embodiment of the present disclosure does not limit the number of sub-layers included in the semiconductor layer 141 (channel layer 1410 ).

[0134] Fig. 6A and 6B Schematic diagrams of the structures of a semiconductor substrate having a semiconductor stack and a channel stack formed thereon according to an example of an embodiment of the present disclosure are respectively shown; Fig. 6A and Figure 6B In the manufacturing stage, they can correspond to Figure 2D and 2E . See Fig. 6A and 6B In this example, the semiconductor layer 141 includes a first semiconductor sublayer 141-1 and a second semiconductor sublayer 141-2. Correspondingly, the channel layer 1410 includes a first channel sublayer 1410-1 and a second channel sublayer 1410-2. The first semiconductor sublayer 141-1 is located between the second semiconductor sublayer 141-2 and the gate 170. The first channel sublayer 1410-1 is located between the second channel sublayer 1410-2 and the gate 170. The first semiconductor sublayer 141-1 and the first channel sublayer 1410-1 are amorphous phase layers, and the second semiconductor sublayer 141-2 and the second channel 1410-2 are crystalline phase layers. In this case, for example, the surface of the second semiconductor sublayer 141-2 away from the base substrate 110 is the deposition interface 111 of the semiconductor layer 142; that is, the surface of the second channel sublayer 1410-2 away from the base substrate 110 is the deposition interface 111 of the seed layer 1420.

[0135] Figure 6C and 6D Schematic diagrams of structures of a semiconductor substrate having a semiconductor stack and a channel stack formed thereon according to another example of an embodiment of the present disclosure are respectively shown. Figure 6C and Fig.6D In the manufacturing stage, they can correspond to Figure 2D and 2E . See Figure 6C and 6DIn this example, the semiconductor layer 141 includes a first semiconductor sublayer 141-1, a second semiconductor sublayer 141-2, and a third semiconductor sublayer 141-3. Correspondingly, the channel layer 1410 includes a first channel sublayer 1410-1, a second channel sublayer 1410-2, and a third channel sublayer 1410-3. The first semiconductor sublayer 141-1 is located between the second semiconductor sublayer 141-2 and the gate 170, and the third semiconductor sublayer 141-3 is located between the first semiconductor sublayer 141-1 and the gate 170. Correspondingly, the first channel sublayer 1410-1 is located between the second channel sublayer 1410-2 and the gate 170, and the third channel sublayer 1410-3 is located between the first channel sublayer 1410-1 and the gate 170. The first semiconductor sublayer 141-1 and the first channel sublayer 1410-1 are amorphous phase layers, the second semiconductor sublayer 141-2 and the second channel 1410-2 are crystalline phase layers, and the third semiconductor sublayer 141-3 and the third channel 1410-3 are crystalline phase layers. In this case, for example, the surface of the second semiconductor sublayer 141-2 away from the base substrate 110 is the interface 111 of the subsequent deposition of the semiconductor layer 142; that is, the surface of the second channel sublayer 1410-2 away from the base substrate 110 is the deposition interface 111 of the seed layer 1420.

[0136] Figures 7A to 7H A schematic diagram of a substrate structure corresponding to each step in a method for manufacturing a semiconductor substrate 200 according to another embodiment of the present disclosure is shown.

[0137] See also Fig. 7A , a base substrate 110 is provided, and a light shielding portion 121 and a buffer layer 130 are formed on the base substrate 110. The base substrate 110 may be a rigid substrate or a flexible substrate. For example, the material of the base 110 may be glass, polyimide, polycarbonate, polyethylene, polyacrylate or polyethylene terephthalate, etc. The light shielding portion 121 may include one or more of Au, Ag, Cu, Ni, Pt, Pd, Al, Mo, etc. The light shielding portion 121 may be a single metal layer or a plurality of metal layers (metal stack). The buffer layer 130 may be formed as a single layer of silicon nitride (SiNx) or silicon oxide (SiO2) or a stacked layer of silicon nitride (SiNx) and silicon oxide (SiO2).

[0138] See also Figures 7B to 7D A physical vapor deposition process, such as a sputtering process, is used to form a semiconductor stack 140' on the buffer layer 130. The semiconductor stack 140 includes a semiconductor layer 141', a semiconductor layer 142', and a semiconductor layer 143'.

[0139] See also Figure 7B, at a relatively high first temperature, a semiconductor layer 142' of a crystalline phase is deposited on an upper surface (interface) 111' of the buffer layer 130 away from the base substrate 110. The upper surface 111' is the interface between the buffer layer 130 and the atmosphere in the deposition chamber before the semiconductor layer 142' is formed, and is the interface between the buffer layer 130 and the semiconductor layer 142' after the semiconductor layer 142' is formed. The first temperature is greater than or equal to 100°C. Preferably, the first temperature is greater than or equal to 120°C.

[0140] The semiconductor layer 142' in this embodiment is the same as the semiconductor layer 142 in the previous embodiment in terms of material, thickness, crystallinity, and formation process, so repeated description is omitted. Here, the semiconductor layer 142' in this embodiment and the semiconductor layer 142 in the above embodiment may correspond to the first semiconductor layer.

[0141] See also Figure 7C , a semiconductor layer 143' is deposited on the upper surface of the semiconductor layer 142' away from the base substrate 110. The semiconductor layer 143' in this embodiment corresponds to the semiconductor layer 143 in the previous embodiment in terms of material, crystallinity, thickness, and formation process, so repeated description is omitted here. Here, the semiconductor layer 143' in this embodiment and the semiconductor layer 143 in the above embodiment may correspond to the second semiconductor layer.

[0142] In this embodiment, the semiconductor layer 142' deposited at a higher temperature can directly form a crystalline phase layer on the surface (interface) 111' to replace the defective layer existing on the interface when the semiconductor layer 142' is deposited at room temperature, so as not to cause obvious undercutting and drilling formation in the subsequent composition process.

[0143] See also Fig.7D , a semiconductor layer 141' is deposited on the upper surface of the semiconductor layer 143' away from the base substrate 110. The semiconductor layer 141' in this embodiment corresponds to the semiconductor layer 141 in the previous embodiment in terms of material, thickness, crystallinity, sublayers, and formation process, so repeated descriptions are omitted here. Here, the semiconductor layer 141' in this embodiment and the semiconductor layer 141 in the above embodiment may correspond to the third semiconductor layer.

[0144] In the embodiment of the present disclosure, since the semiconductor layer 143' has good crystallinity and the semiconductor layer 141' deposited thereon is in an amorphous phase, although the semiconductor layer 143' and the semiconductor layer 141' are made of different materials, there is no need to form a structural layer similar to the seed layer described above between the two. Of course, the embodiment of the present disclosure is not limited thereto.

[0145] See also Fig. 7E, a patterning process is performed on the semiconductor stack 140' to form a channel stack 1400'. The channel stack 1400' includes a channel layer 1410', a seed layer 1420', and a channel layer 1430'. The channel layer 1410', the seed layer 1420', and the channel layer 1430' are respectively a part of the semiconductor layer 141', the semiconductor layer 142', and the semiconductor layer 143'. Here, the channel layer 1430' in the present embodiment and the channel layer 1430 in the previous embodiment may correspond to the first channel layer, and the channel layer 1410' in the present embodiment and the channel layer 1410 in the previous embodiment may correspond to the second channel layer.

[0146] Here, the patterning process performed on the semiconductor stack 140 ′ is similar to the patterning process performed on the semiconductor stack 140 in the previous embodiment, and will not be described in detail herein.

[0147] See also Figure 7F , a gate 170 ′ and a gate insulating layer 160 ′ are formed on the base substrate 110 having the channel stack 1400 ′ formed thereon.

[0148] See also Figure 7G An intermediate dielectric layer 151 is formed on the substrate 110 having the gate 170 ′ and the gate insulating layer 160 ′ formed thereon; a source 181 ′ and a drain 182 ′ are formed on the intermediate dielectric layer 151 ; the source 181 ′ and the drain 182 ′ are electrically connected to the channel stack 1400 ′ through vias in the intermediate dielectric layer 150 .

[0149] See also Figure 7H A planarization layer 190 is formed on the base substrate 110 on which the source electrode 181 ′ and the drain electrode 182 ′ are formed. A light emitting element 225 and an encapsulation layer 240 are formed on the planarization layer 190 .

[0150] In one example, the band gap Eg1 of the channel layer 1410', the band gap Eg2 of the seed layer 1420' and the band gap Eg3 of the channel layer 1430' satisfy: Eg1<Eg2≤Eg3; the conduction band bottom energy level Ec1 of the channel layer 1410', the conduction band bottom energy level Ec2' of the seed layer 1420' and the conduction band bottom energy level Ec3 of the channel layer 1430 satisfy: │Ec1│>│Ec2│≥│Ec3│; the valence band top energy level Ec1 of the channel layer 1410', the valence band top energy level Ec2 of the seed layer 1420' and the valence band top energy level Ec3 of the channel layer 1430' satisfy: │Ev1│<│Ev2│≤│Ev3│. See Figure 7H, the thin film transistor TFT2 has a top gate structure, and the channel layer 1410' (the second channel layer) is located between the gate 170' and the channel layer 1430' (the first channel layer). In this case, the band gap of the channel layer 1410' is the smallest, and its band structure is located below the seed layer 1420' and the channel layer 1430'. When the thin film transistor is working, due to the difference in band gaps, the channel layer 1410', as a material with a high carrier concentration, the carriers generated by it need to cross the barrier of the difference in band gaps between the seed layer 1420' and the channel layer 1430' before they can jump to other film layers. Therefore, most of the carriers are confined in the channel layer 1410'. The role of using the seed layer 1420' is, on the one hand, to remove the defective layer and thus the bottom cutting drilling problem, and on the other hand, to reduce internal interface defects and improve device stability; at the same time, as a crystalline material, the seed layer 1420' is more matched with the channel layer 1430', and the interface defects are lower; the role of the channel layer 1430' is: on the one hand, it has high crystallinity, which can block the etching damage of the source and drain etchant, reduce the bombardment of the passivation layer deposition, prevent the diffusion of source and drain elements, prevent the diffusion of elements such as oxygen, etc. On the other hand, the large band gap can ensure that the minimum carriers diffuse from the channel layer 1410' to the channel layer 1430', thereby reducing carrier loss; therefore, in the semiconductor substrate manufactured according to the embodiment of the present disclosure, the carrier mobility and stability of the thin film transistor are effectively improved.

[0151] In the above embodiment, an oxide semiconductor thin film transistor and a corresponding pixel structure on a semiconductor substrate are used as an example to illustrate that the semiconductor substrate is used as an active matrix substrate of a display device. In the active matrix substrate of another embodiment of the present disclosure, the oxide semiconductor thin film transistor can be used not only as a switching element provided in each pixel, but also as a circuit element (monolithicized) for peripheral circuits such as a driver.

[0152] The embodiments of the present disclosure can be widely applied to various semiconductor devices having oxide semiconductor thin film transistors, such as circuit substrates such as active matrix substrates, liquid crystal display devices, organic electroluminescent (EL) display devices and inorganic electroluminescent display devices, MEMS display devices and other display devices, image sensor devices and other camera devices, image input devices, fingerprint reading devices, semiconductor memories and other electronic devices.

[0153] There are a few points to note:

[0154] (1) In the drawings of the embodiments of the present disclosure, only the structures related to the embodiments of the present disclosure are involved, and other structures can refer to the general design.

[0155] (2) In the absence of conflict, features in the same embodiment or in different embodiments of the present disclosure may be combined with each other.

[0156] Although the disclosure has been described in detail above with general descriptions and specific implementation methods, it is obvious to those skilled in the art that some modifications or improvements may be made to the embodiments of the disclosure. Therefore, these modifications or improvements made without departing from the spirit of the disclosure are within the scope of protection claimed by the disclosure.

Claims

1. A method for manufacturing a semiconductor substrate, comprising: providing a substrate base plate; A semiconductor stack including a first semiconductor layer, a second semiconductor layer and a third semiconductor layer is formed on the substrate by a physical vapor deposition process, comprising: When the substrate is at a first temperature, forming the first semiconductor layer at an interface on the substrate, wherein the material of the first semiconductor layer is a first oxide semiconductor material; directly forming the second semiconductor layer on the first semiconductor layer, wherein the material of the second semiconductor layer is a second oxide semiconductor material; and forming the third semiconductor layer, wherein the material of the third semiconductor layer is a third oxide semiconductor material; Performing a composition process on the semiconductor stack so that the first semiconductor layer, the second semiconductor layer and the third semiconductor layer are patterned into a seed layer, a first channel layer and a second channel layer, respectively, wherein the seed layer, the first channel layer and the second channel layer constitute a channel stack; forming a gate and a gate insulating layer on the substrate; and forming a source electrode and a drain electrode on the substrate having the channel stack formed thereon, wherein the source electrode and the drain electrode are electrically connected to the channel stack. The second channel layer is located between the gate and the first channel layer, the first oxide semiconductor material is different from the third oxide semiconductor material, and the first channel layer and the seed layer are both crystalline phase layers. Wherein, both the first oxide semiconductor material and the second oxide semiconductor material can be formed into a crystalline phase at a second temperature, the second temperature is less than or equal to 40° C., and the first temperature is greater than or equal to 100° C.; The band gap Eg1 of the second channel layer, the band gap Eg2 of the seed layer and the band gap Eg3 of the first channel layer satisfy: Eg1<Eg2≤Eg3; The conduction band bottom energy level Ec1 of the second channel layer, the conduction band bottom energy level Ec2 of the seed layer and the conduction band bottom energy level Ec3 of the first channel layer satisfy: |Ec1|>|Ec2|≥|Ec3|; A valence band top energy level Ec1 of the second channel layer, a valence band top energy level Ec2 of the seed layer, and a valence band top energy level Ec3 of the first channel layer satisfy: |Ev1|<|Ev2|≤|Ev3|.

2. The manufacturing method according to claim 1, wherein: The gate is located between the channel stack and the substrate, and the interface is a surface of the third semiconductor layer away from the substrate.

3. The manufacturing method according to claim 1, further comprising: An insulating layer is formed on the base substrate, wherein the insulating layer is located between the first semiconductor layer and the base substrate, the channel stack is located between the gate and the base substrate, and the interface is a surface of the insulating layer away from the base substrate.

4. The manufacturing method according to claim 1, wherein: The channel stack has a bottom surface and a side surface facing the base substrate, the bottom surface and the side surface are both planes, and a first angle between the bottom surface and the side surface is 20° to 70°.

5. The manufacturing method according to claim 1, wherein: The channel stack has a bottom surface and a side surface facing the substrate, the side surface includes a first sub-side surface and a second sub-side surface, the bottom surface, the first sub-side surface and the second sub-side surface are all planes, a second angle between the bottom surface and the first sub-side surface is 50° to 80°, a third angle between the second sub-side surface and the bottom surface is 20° to 70°, and the second angle is different from the third angle.

6. The manufacturing method according to claim 1, wherein: The third semiconductor layer is an amorphous phase layer.

7. The manufacturing method according to claim 1, wherein: The electron mobility of the third semiconductor layer is greater than the electron mobility of the first semiconductor layer and the second semiconductor layer.

8. The manufacturing method according to claim 1, wherein: The thickness of the second semiconductor layer is 4 to 8 times the thickness of the first semiconductor layer.

9. The manufacturing method according to claim 1, wherein: The seed layer has a thickness of 50 angstroms to 100 angstroms.

10. The manufacturing method according to claim 1, wherein: The first temperature is greater than 120°C.

11. The manufacturing method according to claim 1, wherein: The first oxide semiconductor material of the first semiconductor layer and the second oxide semiconductor material of the second semiconductor layer are the same, and the second semiconductor layer is formed at the second temperature.

12. The manufacturing method according to any one of claims 1 to 11, wherein: Each of the first oxide semiconductor material and the second oxide semiconductor material contains two or more metal elements among In, Ga, Zn, and Sn.

13. The manufacturing method according to claim 12, wherein: Each of the first oxide semiconductor material and the second oxide semiconductor material is an IGZO material, wherein the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 7%-14%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 20%-40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 50%-70%.

14. The manufacturing method according to claim 12, wherein: Each of the first oxide semiconductor material and the second oxide semiconductor material is an IGZO material, wherein the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 35%-50%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 10%~40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 20%~40%.

15. The manufacturing method according to claim 1, wherein: The third semiconductor layer includes a first semiconductor sublayer and a second semiconductor sublayer, the first semiconductor sublayer is between the gate and the second semiconductor sublayer, the first semiconductor sublayer is a crystalline phase layer, and the second semiconductor sublayer is an amorphous phase layer, The gate is located between the channel stack and the substrate, and the interface is a surface of the second semiconductor sublayer away from the substrate.

16. The manufacturing method according to claim 15, wherein: The third semiconductor layer further includes a third semiconductor sublayer, the third semiconductor sublayer is located between the gate and the first semiconductor sublayer, and the third semiconductor layer is a crystalline phase layer.

17. The manufacturing method according to any one of claims 1 to 11, wherein: For the same etching solution, the ratio of the etching rate of the third semiconductor layer to the etching rate of the second semiconductor layer is in the range of 0.2 to 5.

18. A semiconductor substrate, comprising: substrate substrate; as well as A thin film transistor on a substrate, wherein the thin film transistor comprises a gate, a gate insulating layer, a channel stack and a source and drain electrically connected to the channel stack, the channel stack comprising: a seed layer of a first oxide semiconductor material, a first channel layer of a second oxide semiconductor material and a second channel layer of a third oxide semiconductor material, wherein the second channel layer is located between the gate and the first channel layer, the second oxide semiconductor material is different from the third oxide semiconductor material, the first channel layer and the seed layer are both crystalline phase layers, the first oxide semiconductor material and the second oxide semiconductor material are both materials that can be formed into a crystalline phase at a second temperature, the second temperature is less than or equal to 40° C., and the first oxide semiconductor material is formed at a temperature greater than or equal to 100° C.; Wherein, the semiconductor substrate further comprises an interface on the substrate, the distance between the surface of the first channel layer facing the substrate and the interface is less than or equal to 100 angstroms, and the seed layer is located between the interface and the surface of the first channel layer facing the substrate; The band gap Eg1 of the second channel layer, the band gap Eg2 of the seed layer and the band gap Eg3 of the first channel layer satisfy: Eg1<Eg2≤Eg3; The conduction band bottom energy level Ec1 of the second channel layer, the conduction band bottom energy level Ec2 of the seed layer and the conduction band bottom energy level Ec3 of the first channel layer satisfy: |Ec1|>|Ec2|≥|Ec3|; A valence band top energy level Ec1 of the second channel layer, a valence band top energy level Ec2 of the seed layer, and a valence band top energy level Ec3 of the first channel layer satisfy: |Ev1|<|Ev2|≤|Ev3|.

19. The semiconductor substrate according to claim 18, wherein: The gate is located between the channel stack and the substrate, and the interface is a surface of the second channel layer away from the substrate.

20. The semiconductor substrate according to claim 18, further comprising: An insulating layer on the substrate, wherein the insulating layer is located between the seed layer and the substrate, the channel stack is located between the gate and the substrate, and the interface is a surface of the insulating layer away from the substrate.

21. The semiconductor substrate according to claim 18, wherein The channel stack has a bottom surface and a side surface facing the base substrate, the bottom surface and the side surface are both planes, and a first angle between the bottom surface and the side surface is 20° to 70°.

22. The semiconductor substrate according to claim 18, wherein The channel stack has a bottom surface and a side surface facing the substrate, the side surface includes a first sub-side surface and a second sub-side surface, the bottom surface, the first sub-side surface and the second sub-side surface are all planes, a second angle between the bottom surface and the first sub-side surface is 50° to 80°, a third angle between the second sub-side surface and the bottom surface is 20° to 70°, and the second angle is different from the third angle.

23. The semiconductor substrate according to claim 18, wherein The second channel layer is an amorphous phase layer.

24. The semiconductor substrate according to claim 18, wherein The electron mobility of the second channel layer is greater than the electron mobility of the seed layer and the first channel layer.

25. The semiconductor substrate according to claim 18, wherein The thickness of the first channel layer is 4 to 8 times the thickness of the seed layer.

26. The semiconductor substrate according to claim 18, wherein The seed layer has a thickness of 50 angstroms to 100 angstroms.

27. The semiconductor substrate according to claim 18, wherein The first oxide semiconductor material is the same as the second oxide semiconductor material.

28. The semiconductor substrate according to any one of claims 18 to 27, wherein Each of the first oxide semiconductor material and the second oxide semiconductor material contains two or more metal elements among In, Ga, Zn, and Sn.

29. The semiconductor substrate according to claim 28, wherein The first oxide semiconductor material is IGZO material, wherein the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 7%-14%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 20%-40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 50%-70%.

30. The semiconductor substrate according to claim 28, wherein The first oxide semiconductor material is IGZO material, wherein the ratio of the number of In atoms to the total number of In, Ga and Zn atoms is 35%-50%; the ratio of the number of Ga atoms to the total number of In, Ga and Zn atoms is 10%-40%; the ratio of the number of Zn atoms to the total number of In, Ga and Zn atoms is 20%-40%.

31. The semiconductor substrate according to claim 18, wherein The second channel layer includes a first channel sublayer and a second channel sublayer, the first channel sublayer is between the gate and the second channel sublayer, the first channel sublayer is a crystalline phase layer, and the second channel sublayer is an amorphous phase layer, The gate is located between the channel stack and the substrate, and the interface is a surface of the second channel sublayer away from the substrate.

32. The semiconductor substrate according to claim 31, wherein The second channel layer further includes a third channel sublayer, wherein the third channel sublayer is located between the gate and the first channel sublayer, and the third channel layer is a crystalline phase layer.

33. The semiconductor substrate according to any one of claims 18 to 27, wherein: For the same etching solution, the ratio of the etching rate of the second channel layer to the etching rate of the first channel layer is in the range of 0.2 to 5.