Strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity and preparation method thereof
By controlling the amination and alkylation reactions in acrylic strong-base anion exchange resins and using acrylate cross-linking agents with high cross-linking degrees, the problems of poor mechanical strength and low exchange capacity of traditional resins are solved, and high resin performance is achieved. Mechanical strength and high exchange capacity avoid resin loss and contamination.
Patent Information
- Application Number
- CN202111013459.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-08-31
Smart Images

Figure CN113861316B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of resin materials, and in particular relates to an acrylic acid-based strongly basic anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity, and a preparation method thereof. Background Art
[0002] Ion exchange resin materials are widely used in the field of water treatment due to their adjustable structure, high adsorption capacity, strong selectivity and easy desorption and regeneration. Polyacrylic acid anion exchange resin has a high exchange capacity and capacity for electronegative weakly acidic organic matter due to its hydrophilic skeleton. At the same time, polyacrylic acid anion exchange resin has a strong ability to resolve organic matter and can tolerate pollution caused by soluble organic matter. The adsorption effect of acrylic acid-based strong base anion exchange resin on macromolecular organic matter humic acid and fulvic acid is far better than that of macroporous styrene-based ion exchange resin, and it is easier to elute and regenerate. Therefore, acrylic acid-based strong base anion exchange resin is widely used in biomedical engineering, chemical analysis, wastewater treatment and resource utilization.
[0003] The synthesis of traditional acrylic anion exchange resins requires the use of acrylic ester monomers, such as methyl acrylate, ethyl acrylate, glycidyl acrylate, etc. In the synthesis method of magnetic strong base anion exchange resin mentioned in US Patent No. 5900146, after the active monomer glycidyl methacrylate is polymerized, due to the epoxy group in the resin structure, it can directly react with trimethylamine hydrochloride to form a quaternary ammonium salt to form an acrylic strong base anion exchange resin. Compared with styrene ion exchange resins, acrylic anion exchange resins have poor mechanical strength. When the resin is applied to the water treatment process, it is better than mutual contact and friction, which will produce 5-10μm resin suspended particles, resulting in resin loss and secondary pollution of the water body. Generally, the pore structure of the resin can be adjusted by increasing the proportion of crosslinking agent, optimizing the composition and proportion of porogen, etc., so as to improve the mechanical strength of the resin. There are also reports that the mechanical strength of the resin can be significantly improved by doping inorganic nanoparticles during in-situ formation or synthesis inside the resin. However, inorganic nanoparticles also have the risk of secondary pollution caused by loss, and inorganic particles have poor tolerance to acidity and alkalinity. Therefore, the preparation of acrylic anion exchange resins with good structural stability and strong mechanical strength remains a technical problem to be solved. Summary of the invention
[0004] Purpose of the invention: In view of the problems existing in the prior art, the present invention provides an acrylic acid-based strong base anion exchange resin that can simultaneously adjust the mechanical strength and exchange capacity. The resin can control the crosslinking degree and exchange capacity according to the requirements of the use environment to ensure that the resin has a suitable exchange capacity and mechanical strength. In addition, the present invention effectively solves the problems of low crosslinking agent content in common acrylic acid-based strong base anion exchange resins and poor mechanical strength of the resin.
[0005] Another object of the present invention is to provide a method for preparing the acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity. The resin of the present invention can synchronously regulate the mechanical strength and exchange capacity of the resin by controlling the amination reaction process of amine ester exchange, and further synthesize the strong base anion exchange resin by an alkylation process.
[0006] Technical solution: In order to achieve the above-mentioned purpose, the present invention provides an acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity, wherein the structure of the resin skeleton includes The structural unit shown, wherein A is a group containing a quaternary ammonium salt, and group A is any one of the following 6 groups:
[0007]
[0008]
[0009] Wherein R1, R2, R3, R4, R5 are independently selected from C 1~4 Alkyl or hydroxy substituted C 1~4 Alkyl; n in group A is 0, 1, 2, 3, 4, 5 or 6, preferably, n in group A is 0, 1, 3; X represents Cl, Br, I or OH.
[0010] Preferably, R1, R2, R3, R4, and R5 are independently selected from methyl or ethyl.
[0011] The acrylic acid-based strong base anion exchange resin has a particle size of 100 to 600 μm, a strong base exchange capacity of 2.0 to 4.5 mmol / g, a water content of 46 to 68%, a ball rate after grinding (national standard GB / T 12598-2001 method) of 80 to 99.9%, a wet true density of 1.1 to 1.3 g / mL, and a sedimentation rate of 50 to 90 m / h in 20° C. pure water.
[0012] The preparation method of the acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity of the present invention comprises: using acrylic acid-based monomer reactants, porogens, and initiators to form an oil phase, wherein the acrylic acid-based monomer reactants include monomers and crosslinking agents, or only include crosslinking agents, and are uniformly mixed with a water phase containing a dispersant under stirring, and the temperature is raised for suspension polymerization. Since the proportion of ester-based crosslinking agents in the monomer reactants is relatively high, highly crosslinked resin spheres are formed after suspension polymerization, and the mechanical strength and wet true density of the resin spheres are relatively high. The resin spheres after the polymerization reaction synchronously regulate the mechanical strength and exchange capacity of the resin by controlling the amination reaction process of amine ester exchange, that is, the resin ester groups participating in the amination reaction can exchange the resin to generate amine groups, and the ester groups not participating in the amination reaction still serve as crosslinking units to keep the resin at a relatively high mechanical strength. The resin after the amination reaction is further subjected to an alkylation reaction to form quaternary ammonium salt groups, and finally an acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity is prepared.
[0013] The method for preparing the acrylic acid-based strong base anion exchange resin capable of simultaneously regulating mechanical strength and exchange capacity specifically comprises the following steps:
[0014] (1) adding an oil phase containing an acrylic monomer reactant (monomer, crosslinking agent), a porogen, and an initiator to an aqueous phase containing a dispersant, stirring and heating, and extracting or washing the spheres after the reaction is completed and then drying them;
[0015] (2) aminating the resin spheres obtained in step (1) with one or more of ethylenediamine, N,N-dimethylpropylenediamine, N,N-dimethylbutylenediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine;
[0016] (3) washing and drying the resin after the amination in step (2);
[0017] (4) The resin spheres obtained in step (3) are reacted with an alkylating agent in an alkaline solution to obtain an acrylic acid-based strong base anion exchange resin capable of simultaneously regulating mechanical strength and exchange capacity.
[0018] Wherein, the monomer reactants in step (1) include monomers and crosslinking agents, and the weight ratio of their total mass to the porogen is 1:0.1 to 1:1.5, and the weight ratio of the monomers to the crosslinking agents in the monomer reactants is (0 to 0.2):1.
[0019] Wherein, the monomer in the monomer reactant in step (1) is one or more of methyl acrylate, ethyl acrylate, butyl acrylate, methyl methacrylate, butyl methacrylate, glycidyl methacrylate; the crosslinking agent includes at least one of ethylene glycol dimethacrylate, ethylene glycol diethyl diallyl ester and trimethylolpropyl trimethacrylate, and the total mass of one or more of the three accounts for more than 90% of the total mass of the crosslinking agent, and the crosslinking agent may also include divinylbenzene, and its mass accounts for 0-10% of the total mass of the crosslinking agent. The porogen is one or more of toluene, xylene, ethyl acetate, 200# solvent oil, isopropanol, n-butanol, liquid wax, n-heptane, n-octane, isooctane, and n-decane; the initiator is one or both of azobisisobutyronitrile and benzoyl peroxide.
[0020] Preferably, the crosslinking agent is one or both of trimethylolpropyl trimethacrylate and ethylene glycol dimethacrylate.
[0021] Preferably, the porogen is one or more of toluene or xylene. The weight ratio of the total weight of the monomer and the crosslinking agent to the porogen is preferably 1:0.1 to 1:1.0.
[0022] Preferably, in step (1) of the present invention, 0.5% to 2% by weight of an initiator based on the weight of the reactant system is added to the oil phase, and the initiator is stirred to fully dissolve.
[0023] The stirring speed of the stirring reaction in step (1) is 100 to 350 rpm, the temperature is controlled at 50 to 80° C., and after reacting for 2 to 8 hours, the temperature is kept at 85 to 95° C. for 4 to 15 hours.
[0024] Preferably, in step (1) of the present invention, the aqueous phase comprises water, a dispersant and an inorganic salt. The dispersant is selected from one or more of gelatin, polyvinyl alcohol 1788, hydroxyethyl cellulose, sodium dodecylbenzene sulfonate, and sodium lignin sulfonate; preferably one or two of hydroxyethyl cellulose and polyvinyl alcohol 1788; the inorganic salt is one or two of salt and sodium sulfate, preferably sodium sulfate; in the aqueous phase, the dispersant accounts for 0.2% to 3% by mass, the salt accounts for 0 to 20%, the sodium sulfate accounts for 0 to 10%, and the balance is water;
[0025] Wherein, in step (2), the resin spheres obtained in step (1) are aminated with one or more of ethylenediamine, N,N-dimethylpropylenediamine, N,N-dimethylbutylenediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine in an amount of 1 to 8 times the mass of the resin at 120 to 260° C. for 6 to 30 hours.
[0026] Preferably, in step (2) of the present invention, the progress of the amination reaction is regulated by controlling the time and temperature of the amination reaction, that is, the ester groups in the resin spheres participating in the reaction can generate amine groups in the resin, and the ester groups not participating in the reaction still serve as cross-linking units to keep the resin at a high mechanical strength. By controlling the amination reaction process of amine ester exchange, the mechanical strength and exchange capacity of the resin are synchronously regulated.
[0027] Preferably, the resin obtained in step (3) is repeatedly washed with one or more of methanol, ethanol and acetone, then washed with water for several times, and dried at 30-50°C.
[0028] Wherein, in step (4), the alkylating agent is selected from one or more of methyl chloride, ethyl chloride, methyl bromide, ethyl bromide, methyl iodide and ethyl iodide, the weight ratio of the alkylating agent to the resin is 1:1 to 8:1, and the reaction is carried out at 40 to 120° C. for 2 to 48 hours.
[0029] Preferably, the weight ratio of the alkylating agent to the resin is 3:1 to 6:1. Specifically, the weight ratio of the alkylating agent to the resin is 1:1, or 2:1, or 3:1, or 3.5:1, or 4:1, or 4.5:1, or 5:1, or 6:1, or 7:1, or 8:1.
[0030] The application of the acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity described in the present invention in separating and removing electronegative substances in various water bodies. Principle: The present invention utilizes acrylic acid-based monomer reactants (monomers and crosslinking agents), porogens, and initiators to form an oil phase, which is evenly mixed with a water phase containing a dispersant under stirring, and the temperature is raised to perform suspension polymerization. Since the proportion of ester-based crosslinking agents in the monomer reactants is relatively high, resin spheres with a high degree of crosslinking are formed after suspension polymerization, and the mechanical strength and wet true density of the resin spheres are relatively high. The resin spheres after the polymerization reaction synchronously regulate the mechanical strength and exchange capacity of the resin by controlling the amination reaction process of amine ester exchange, and further undergo an alkylation reaction to form quaternary ammonium salt groups, and finally prepare acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity.
[0031] Usually, the cross-linking agent only has the cross-linking function. The cross-linking agent mainly selected in the present invention has similar properties to the monomer, and can be used as a cross-linking unit and amination reaction as a functional unit. The part participating in the amination reaction can make the resin have exchange capacity just like the monomer function, and the part not participating in the reaction can still be used as a cross-linking unit to increase the mechanical strength of the resin.
[0032] The crosslinking agent of the present invention can be used as a crosslinking unit and a functional unit for amination reaction, thereby increasing the utilization efficiency of the monomer and the crosslinking agent, having a high exchange capacity and high mechanical strength. The present invention can prove that the roundness rate of the resin after grinding can reach more than 80% (80-99.9%), which is higher than the traditional acrylic acid anion exchange resin (roundness rate after grinding is 55.0-75.0%). Since the degree of amination reaction can be controlled, the exchange capacity and mechanical strength of the resin can be regulated by controlling the amination reaction process.
[0033] In addition, in the prior art, divinylbenzene is usually used as a crosslinking agent, which is not easy to polymerize with acrylic acid monomers, so the amount used cannot be too much. In addition, the purity of commercial divinylbenzene is generally only 50%, which will introduce a large number of other impurities, and if the amount of divinylbenzene crosslinking agent is too much, the exchange capacity of the resin will be greatly reduced, and there will be no application effect.
[0034] The present invention focuses on preparing a strong base anion exchange resin that can simultaneously regulate mechanical strength and exchange capacity, effectively solving the problems of single functions of monomers and crosslinking agents when preparing traditional acrylic anion exchange resins. The prior art monomers commonly use methyl acrylate, ethyl acrylate, glycidyl acrylate (GMA), etc. Among them, the resin formed by GMA has low exchange capacity and poor mechanical strength. Methyl acrylate and ethyl acrylate are more commonly used, and they all need to undergo amine ester exchange reaction. The crosslinking agent of the present invention selects a specific acrylate crosslinking agent, which can be used as both a crosslinking agent and a monomer. Therefore, when performing amine ester exchange reaction, it is similar to the monomer. The crosslinking unit can participate in the reaction to generate a functional group, or it can only be used as a crosslinking unit (the higher the crosslinking degree, the higher the mechanical strength, and the crosslinking degree will be reduced after participating in the amination reaction). It can be specifically determined by controlling the amine ester exchange conditions, so the exchange capacity and mechanical strength of the resin can be synchronously regulated according to the use requirements.
[0035] The specific crosslinking agent used in the present invention is very important. That is, an acrylate series crosslinking agent, such as one or more of ethylene glycol dimethacrylate, ethylene glycol diethyl diallyl ester, trimethacrylate (trimethylolpropyl) ester, and divinylbenzene. The present invention can make the resin have exchange groups through a specific amine ester exchange reaction, and by controlling the process, the exchange capacity and mechanical strength of the resin can be synchronously regulated.
[0036] Beneficial effects: Compared with the prior art, the present invention has the following advantages:
[0037] The present invention provides an acrylic acid series strong base anion exchange resin with adjustable mechanical strength and exchange capacity and a preparation method thereof. The acrylic acid series strong base anion exchange resin with adjustable mechanical strength and exchange capacity prepared by the method can adjust the exchange capacity and mechanical strength of the resin by controlling the amination reaction process of amine ester exchange. According to the national test standard for the ball rate of the resin after grinding, the strong base anion exchange resin prepared by the method of the present invention has high mechanical strength, and the ball rate of the resin after grinding can reach more than 80% (80-99.9%), which is higher than the traditional acrylic acid series anion exchange resin (the ball rate after grinding is 55.0-75.0%). The resin also has a high wet true density and sedimentation rate, so that it is easy to separate in the process of practical application. In addition, the resin of the present invention is less broken in the water treatment process, can be recycled for a long time, thereby reducing the cost of water treatment, and can replace the traditional strong base anion exchange resin for separating and removing electronegative substances in various water bodies, such as soluble organic matter, and nitrates, phosphates and other anions.
[0038] The strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity prepared by the present invention does not contain any inorganic nanoparticles, which is different from the prior art that can enhance the mechanical strength and stability of the resin by inorganic nanoparticles, and thus does not cause secondary pollution caused by the loss of inorganic nanoparticles; by controlling the amine ester exchange reaction, the exchange capacity and mechanical strength of the resin can be adjusted according to the use requirements; since the crosslinking agent content of the resin is very high (monomer: crosslinking agent=0.02-0.2:1), the resin can be guaranteed to have a high crosslinking degree, thereby ensuring that the resin has a high mechanical strength and structural stability, and will not cause pollution caused by 5-10μm resin suspended particles.
[0039] The invention has simple preparation, abundant raw material sources and can be used in large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 This is a scanning electron microscope image of an acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity as described in the present invention. DETAILED DESCRIPTION
[0041] The present invention can be better understood according to the following examples. It is easy for those skilled in the art to understand that the contents described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims. The materials, reagents, etc. used in the following examples, unless otherwise specified, can be obtained from commercial sources. The experimental methods for which specific conditions are not specified in the examples are usually carried out under conventional conditions or under conditions recommended by the manufacturer.
[0042] Wherein: The wet true density is determined by reference to GB 8330-87 determination method of wet true density of ion exchange resin.
[0043] The determination of the sphericity after grinding refers to GB / T 12598-2001 Determination of the sphericity of ion exchange resin penetration and the sphericity after grinding.
[0044] The moisture content determination refers to GB / T 5757-2008 ion exchange resin moisture content determination method.
[0045] Reference for sedimentation velocity determination, Chen Xiuzhi et al. Experiment on the hydrodynamic properties of weak acid exchange resin [J]. Journal of University of Science and Technology Beijing, 2001, 23(5): 398-400.
[0046] The exchange capacity was determined by referring to the method for determination of exchange capacity of chloride-type strong basic anion exchange resin GB / T11992-1989.
[0047] Example 1
[0048] Add 500g of 2% by weight hydroxyethyl cellulose and 10% sodium sulfate aqueous solution into a 2L three-necked flask, and control the stirring speed at 150rpm. Add a mixture of 10g methyl acrylate, 10g divinylbenzene, 100g trimethylol acrylate (trimethylolpropyl), 1.0g azobisisobutyronitrile, and 100g toluene into the above three-necked flask and heat to 50°C, keep for 8 hours, heat to 85°C, keep for 15 hours and then discharge; wash the discharged material with ethanol and dry it to obtain resin spheres, add ethylenediamine 4 times the weight of the resin and keep at 130°C for 8 hours and then discharge; after discharging, wash with ethanol and then with water until neutral, and dry at 30-50°C; after drying, add 300mL of 10% liquid alkali, add 450g methyl chloride, react at 40°C for 10 hours and then discharge, and wash after conversion with NaCl. The scanning electron microscope image of the obtained resin is shown in the example Figure 1 shown.
[0049] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 300 to 500 μm, a wet true density of 1.14 g / mL, a spherical rate of 94% after grinding, a water content of 63%, a sedimentation velocity of 83.2 m / h, and a strong base exchange capacity of 3.23 mmol / g.
[0050] According to the type of amination reagent added, its basic structural formula is determined as follows:
[0051]
[0052] Wherein, in group A, n=0.
[0053] Example 2
[0054] 500g of a 0.2% by weight polyvinyl alcohol 1788 and a 15% sodium chloride aqueous solution were added to a 2L three-necked flask, and the stirring speed was controlled at 200rpm. 120g of trimethylolpropyl trimethacrylate (all crosslinking agent, no monomer, and the amount of divinylbenzene was 0), 1.0g of benzoyl peroxide, 100g of toluene, 2g of 200 # Add the solvent oil mixture to the above three-necked flask and heat it to 55°C, keep it for 8 hours, heat it to 85°C, keep it for 10 hours and then discharge it. Wash the discharged material with ethanol and dry it to get the resin spheres, add 2.5 times the weight of the resin ethylenediamine and keep it at 180°C for 20 hours and then discharge it. After washing, add 300mL of 10% liquid caustic soda and 480g of methyl chloride, react at 40°C for 3 hours and then discharge it, and wash it after conversion with NaCl.
[0055] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 200 to 500 μm, a wet true density of 1.28 g / mL, a spherical rate of 98% after grinding, a water content of 58%, a sedimentation velocity of 87.9 m / h, and a strong base exchange capacity of 3.43 mmol / g.
[0056] According to the type of amination reagent added, its basic structural formula is determined as follows:
[0057]
[0058] Wherein, in group A, n=0.
[0059] In Example 2, only a cross-linking agent is used, and there is no monomer in the traditional sense. The cross-linking agent can be used as a monomer, which not only has excellent strong base exchange capacity, but also has higher mechanical strength.
[0060] Example 3
[0061] Add 500g of a 1.5% by weight polyvinyl alcohol 1788, 6% sodium chloride, and 2% sodium sulfate aqueous solution into a 2L three-necked flask, and control the stirring speed at 300rpm. Add a mixed solution of 5g ethyl acrylate, 70g trimethylolpropyl trimethacrylate, 30g ethylene glycol dimethacrylate, 1.5g azobisisobutyronitrile, 1.0g benzoyl peroxide, 50g xylene, and 65g isopropanol into a three-necked flask and heat to 60°C, keep for 6 hours, heat to 85°C and keep for 6 hours before discharging. Wash the discharged material with ethanol and dry it, add 6 times the weight of diethylenetriamine of the resin and keep it at 180°C for 20 hours before discharging. After washing, add 350mL of 10% liquid caustic soda, add 500g ethyl chloride, react at 60°C for 20 hours and then discharge. Transform with NaCl and wash.
[0062] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 180 to 500 μm, a wet true density of 1.08 g / mL, a sphericity of 88% after grinding, a water content of 54%, a sedimentation velocity of 77.9 m / h, and a strong base exchange capacity of 3.03 mmol / g.
[0063] According to the type of amination reagent added, its basic structural formula is determined as follows:
[0064]
[0065] Wherein, in group A, n=1.
[0066] Example 4
[0067] Add 500g of 2.0% gelatin and 15% sodium chloride aqueous solution to a 2L three-necked flask, and control the stirring speed at 150rpm. Add a mixture of 40g butyl methacrylate, 100g trimethylolpropyl trimethacrylate, 1g azobisisobutyronitrile, 1.5g benzoyl peroxide, 80g xylene, and 60g n-heptane to a three-necked flask and heat to 70°C, keep for 6 hours, heat to 92°C, keep for 5 hours and then discharge. Wash the discharged material with ethanol and dry it, add 8 times the weight of tetraethylenepentamine of the resin and keep at 170°C for 20 hours before discharging. After washing, add 400mL of 10% liquid alkali, add 900g methyl chloride, react at 80°C for 25 hours and then discharge. Transform with NaCl and wash.
[0068] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 200 to 500 μm, a wet true density of 1.15 g / mL, a spherical rate of 88% after grinding, a water content of 52%, a sedimentation velocity of 82.5 m / h, and a strong base exchange capacity of 3.37 mmol / g.
[0069] According to the type of amination reagent added, its basic structural formula is determined as follows:
[0070]
[0071] Wherein, in group A, n=3.
[0072] Example 5
[0073] Add 500g of 1.0% hydroxyethyl cellulose, 0.2% sodium lignin sulfonate, and 3% sodium sulfate aqueous solution in a weight ratio to a 2L three-necked flask, and control the stirring speed at 250rpm. Add a mixed solution of 120g trimethylol propyl acrylate, 10g divinylbenzene, 2.0g azobisisobutyronitrile, 80g toluene, and 50g cyclohexanol to a three-necked flask and heat to 70°C, keep for 5 hours, heat to 95°C, keep for 6 hours, and then discharge. Wash the discharged material with ethanol and dry it, add 5 times the weight of tetraethylene pentamine of the resin and keep it at 180°C for 10 hours before discharging. After washing, add 400mL of 10% liquid caustic soda, add 800g ethyl chloride, react at 120°C for 20 hours, then discharge, and wash after transformation with NaCl.
[0074] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 200 to 500 μm, a wet true density of 1.18 g / mL, a sphericity of 98% after grinding, a water content of 57%, a sedimentation velocity of 80.9 m / h, and a strong base exchange capacity of 3.23 mmol / g.
[0075] According to the type of amination reagent added, its basic structural formula is determined as follows:
[0076]
[0077] Wherein, in group A, n=3.
[0078] Example 6
[0079] Add 500g of 1.0% gelatin, 0.5% sodium lignin sulfonate, and 15% sodium chloride aqueous solution in a weight ratio into a 2L three-necked flask, and control the stirring speed at 150rpm. Add a mixture of 120g ethylene glycol dimethacrylate, 10g methyl acrylate, 2g divinylbenzene, 1.75g benzoyl peroxide, 100g xylene, and 50g isooctane into a three-necked flask and heat to 70°C, keep for 4 hours, heat to 95°C, keep for 5 hours and then discharge. Wash the discharged material with ethanol and dry it, add 7 times the weight of diethylenetriamine of the resin and keep at 160°C for 16 hours before discharging. After washing, add 500mL of 10% liquid alkali, add 650g methyl chloride, react at 60°C for 18 hours and then discharge, and wash after transformation with NaCl.
[0080] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 200 to 500 μm, a wet true density of 1.18 g / mL, a sphericity of 91% after grinding, a water content of 55%, a sedimentation velocity of 77.9 m / h, and a strong base exchange capacity of 3.43 mmol / g.
[0081] According to the type of amination reagent added, its basic structural formula is determined as follows:
[0082]
[0083] Wherein, in group A, n=1.
[0084] Example 7
[0085] Add 500g of 0.8% hydroxyethyl cellulose, 0.5% sodium lignin sulfonate, and 2% sodium sulfate aqueous solution in a weight ratio into a 2L three-necked flask, and control the stirring speed at 100rpm. Add a mixed solution of 100g trimethylol propyl acrylate, 10g divinylbenzene, 1.5g azobisisobutyronitrile, and 160g toluene into a three-necked flask and heat to 70°C, keep for 4 hours, heat to 95°C, keep for 8 hours, and then discharge. Wash the discharged material with ethanol and dry it, add 4 times the weight of tetraethylene pentamine of the resin at 180°C and keep for 10 hours before discharging. After washing, add 350mL of 10% liquid alkali, add 750g of ethyl chloride, react at 100°C for 24 hours, then discharge, and wash after transformation with NaCl.
[0086] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 200 to 500 μm, a wet true density of 1.12 g / mL, a sphericity of 96% after grinding, a water content of 58%, a sedimentation velocity of 82.3 m / h, and a strong base exchange capacity of 3.13 mmol / g.
[0087] According to the type of amination reagent added, its basic structural formula is determined as follows:
[0088]
[0089] Wherein, in group A, n=3.
[0090] Example 8
[0091] Add 500g of polyvinyl alcohol 1788 containing 1.5% by weight, 0.2% hydroxyethyl cellulose, and 8% sodium chloride aqueous solution into a 2L three-necked flask, and control the stirring speed at 100rpm. Add a mixed solution of 10g ethyl acrylate, 50g trimethylol propyl acrylate, 50g ethylene glycol dimethacrylate, 1.5g azobisisobutyronitrile, 1.5g benzoyl peroxide, 70g xylene, and 55g isopropanol into a three-necked flask and heat to 60°C, keep for 6 hours, heat to 85°C and keep for 8 hours before discharging. Wash the discharged material with ethanol and dry it, add 7 times the weight of diethylenetriamine of the resin and keep it at 190°C for 22 hours before discharging. After washing, add 400mL of 10% liquid caustic soda, add 500g ethyl chloride, react at 60°C for 20 hours and then discharge. Transform with NaCl and wash.
[0092] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 180 to 500 μm, a wet true density of 1.13 g / mL, a sphericity of 91% after grinding, a water content of 55%, a sedimentation velocity of 73.9 m / h, and a strong base exchange capacity of 3.09 mmol / g.
[0093] According to the type of amination reagent added, its basic structural formula is determined as follows:
[0094]
[0095] Wherein, in group A, n=1.
[0096] Comparative Example 1
[0097] Comparative Example 1 adopts the preparation method of Example 1, except that: any one or more of the cross-linking agents described in the present invention: ethylene glycol dimethacrylate, ethylene glycol diethyl diallyl ester, and trimethacrylate (trimethylolpropyl) ester are not used, and the resulting resin is similar to the commercial strong base anion exchange resin D213.
[0098] The specific preparation process is:
[0099] Add 500g of 2% hydroxyethyl cellulose and 10% sodium sulfate aqueous solution by weight into a 2L three-necked flask, and control the stirring speed at 150rpm. Add a mixed solution of 110g methyl acrylate, 10g divinylbenzene, 1.0g azobisisobutyronitrile, and 100g toluene into the above three-necked flask and heat to 50°C, keep for 8 hours, heat to 85°C, keep for 15 hours, and then discharge; wash the discharged material with ethanol and dry it to obtain resin spheres, add ethylenediamine 4 times the weight of the resin, keep at 130°C for 8 hours, and then discharge; wash the discharged material with ethanol and then wash it with water until neutral, and dry it at 30-50°C; after drying, add 300mL of 10% liquid alkali, add 450g methyl chloride, react at 40°C for 10 hours, discharge it, and convert it with NaCl and wash it.
[0100] The obtained acrylic acid-based strong base anion exchange resin, which can simultaneously regulate mechanical strength and exchange capacity, has a particle size mainly distributed in the range of 250 to 500 μm, a wet true density of 1.11 g / mL, a sphericity of 56% after grinding, a water content of 60%, a sedimentation velocity of 78.9 m / h, and a strong base exchange capacity of 3.33 mmol / g.
[0101] Comparative Example 1 shows that if the specific cross-linking agent of the present invention is not used, only the exchange capacity can be controlled, the mechanical strength of the resin is poor, and the exchange capacity and mechanical strength cannot be regulated at the same time.
Claims
1. An acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity, characterized in that: The structure of the resin skeleton includes The structural unit shown, wherein A is a group containing a quaternary ammonium salt, and group A is any one of the following 6 groups: wherein R1, R2, R3, R4, R5 are independently selected from methyl or ethyl; wherein n in the group A is 0, 1, 2, 3, 4, 5 or 6; X represents Cl, Br, I or OH; The preparation method of the acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity comprises: using acrylic acid-based monomer reactants, porogens, and initiators to form an oil phase, wherein the acrylic acid-based monomer reactants only include a crosslinking agent, and are uniformly mixed with a water phase containing a dispersant under stirring, and the temperature is raised to perform suspension polymerization to form highly crosslinked resin spheres, and the resin spheres after the polymerization reaction are synchronously regulated in terms of mechanical strength and exchange capacity of the resin by controlling the amination reaction process of amine ester exchange, and the resin after the amination reaction is further subjected to an alkylation reaction to form a quaternary ammonium salt group, and finally the acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity is prepared; The crosslinking agent is selected from one or more of ethylene glycol dimethacrylate, ethylene glycol diethyl diallyl ester, and trimethylolpropyl trimethacrylate.
2. The acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity according to claim 1, characterized in that: The acrylic acid-based strong base anion exchange resin has a particle size of 100-600 μm, a strong base exchange capacity of 2.0-4.5 mmol / g, a water content of 46-68%, a ball rate of 80-99.9% after grinding, a wet true density of 1.1-1.3 g / mL, and a sedimentation rate of 50-90 m / h in 20° C. pure water.
3. A method for preparing the acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity as claimed in claim 1, comprising: The oil phase is composed of acrylic acid monomer reactants, porogens and initiators. The acrylic acid monomer reactants only include a crosslinking agent, which is uniformly mixed with a water phase containing a dispersant under stirring, and suspended polymerization is performed by heating to form highly crosslinked resin spheres. The resin spheres after the polymerization reaction are synchronously regulated in terms of mechanical strength and exchange capacity by controlling the amination reaction process of amine ester exchange. The resin after the amination reaction is further subjected to an alkylation reaction to form a quaternary ammonium salt group, and finally an acrylic acid strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity is prepared.
4. The preparation method according to claim 3, characterized in that: The method for preparing the acrylic acid-based strong base anion exchange resin capable of synchronously regulating mechanical strength and exchange capacity specifically comprises the following steps: (1) adding an oil phase containing an acrylic acid monomer reactant, a porogen and an initiator to an aqueous phase containing a dispersant, stirring the mixture for reaction, and extracting or washing the spheres after the reaction is completed and then drying them; (2) aminating the resin spheres obtained in step (1) with one or more of ethylenediamine, N,N-dimethylpropylenediamine, N,N-dimethylbutylenediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine; (3) washing and drying the resin after the amination in step (2); (4) The resin spheres obtained in step (3) are reacted with an alkylating agent in an alkaline solution to obtain an acrylic acid-based strong base anion exchange resin capable of simultaneously regulating mechanical strength and exchange capacity.
5. The preparation method according to claim 4, characterized in that: In step (1), the weight ratio of the total mass of the monomer reactants to the porogen is 1:0.1 to 1:1.
5.
6. The preparation method according to claim 4, characterized in that: In step (1), the acrylic monomer reactants only include a crosslinking agent, and the crosslinking agent is selected from one or more of ethylene glycol dimethacrylate, ethylene glycol diethyl diallyl ester, and trimethylolpropyl trimethacrylate; the porogen is one or more of toluene, xylene, ethyl acetate, 200# solvent oil, isopropanol, n-butanol, liquid wax, n-heptane, n-octane, isooctane, and n-decane; and the initiator is one or two of azobisisobutyronitrile and benzoyl peroxide.
7. The preparation method according to claim 4, characterized in that: The stirring speed of the stirring reaction in step (1) is 100-350 rpm, the temperature is controlled at 50-80° C., and after reacting for 2-8 hours, the mixture is kept at 85-95° C. for 4-15 hours.
8. The preparation method according to claim 4, characterized in that: In step (2), the resin spheres obtained in step (1) are aminated with one or more of ethylenediamine, N,N-dimethylpropylenediamine, N,N-dimethylbutylenediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine in an amount of 1 to 8 times the mass of the resin at 120 to 260° C. for 6 to 30 hours.
9. The preparation method according to claim 4, characterized in that: In step (4), the alkylating agent is selected from one or more of methyl chloride, ethyl chloride, methyl bromide, ethyl bromide, methyl iodide and ethyl iodide, the weight ratio of the alkylating agent to the resin is 1:1 to 8:1, and the reaction is carried out at 40 to 120° C. for 2 to 48 hours.
Citation Information
Patent Citations
Polymer beads and method for preparation thereof
US5900146A
Magnetic microsphere resin for removing nitrate nitrogen selectively, and preparation method thereof
CN102430433A
Supermacroporous strong base anion exchange resin with quaternary amine group and preparation process thereof
CN102671718A