Silver paste for electrode on the front side of crystalline silicon solar cells
Through the resin dissolution and silver powder wrapping method of sectional heating, the silver powder is ensured to be fully coated, the problem of incomplete resin coating is solved, the stability and photoelectric properties of silver paste are improved, and it is suitable for fine-line printing, achieving high efficiency photoelectric conversion efficiency and low cost silver paste preparation.
Patent Information
- Application Number
- CN202111318964.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-11-09
AI Technical Summary
In the prior art, the resin does not completely coat the silver powder, resulting in separation of the silver powder from the system, causing the EL yield to decrease and the problem of poor height and aspect ratio during the fine line printing process.
The resin dissolution and silver powder wrapping method is adopted to ensure that the silver powder is fully wrapped by the resin through the steps of high-temperature dissolution and segmental heating, and then the silver paste with high density and uniformity is formed by secondary dispersion and airflow. , combined with screen printing technology to prepare electrodes.
Improves the cladding integrity and adhesion of silver powder, extends the stability of silver paste, improves the photoelectric conversion efficiency, reduces the amount and cost of resin, is suitable for fine-wire printing, and solves the poor aspect ratio. question.
Smart Images

Figure BDA0003344799320000091 
Figure BDA0003344799320000101
Abstract
Description
Technical Field
[0001] The invention relates to a front fine grid and printed electrode silver paste for a crystalline silicon solar cell and a preparation method thereof, and belongs to the field of solar photovoltaic silver paste and solar crystalline silicon cells. Background Art
[0002] At present, the preparation process adopts a resin and a solvent that are dissolved at a certain temperature and then mixed with other raw materials such as silver powder and glass powder. There are common problems such as incomplete coating of the silver powder by the resin, or the surface of some silver powder is not coated with resin due to uneven mixing. During long-term use, some silver particles are separated from the system, resulting in a decrease in EL yield and other technical problems.
[0003] In view of the above technical defects, the present invention provides a silver paste for the front (fine grid and printing) electrode of a crystalline silicon solar cell and a preparation method thereof, which can effectively solve the problem of incomplete coating of silver powder particles by organic resin; solve the problem of decreased EL yield of the paste during long-term use in conventional organic production systems, and solve the problem of poor aspect ratio during fine line printing. Summary of the invention
[0004] The purpose of the present invention is to provide a silver paste for a front electrode of a crystalline silicon solar cell and a preparation method thereof in view of the existing technical defects.
[0005] A silver paste for the front electrode of a crystalline silicon solar cell comprises raw material components including organic resin, silver powder, glass powder, solvent and organic additives, and a preparation method comprising the following steps: resin dissolution, silver powder encapsulation, resin shaping, secondary dispersion and silver paste preparation.
[0006] The organic resin is selected from at least one of acrylic resin, modified acrylic resin, ethyl cellulose, methyl cellulose, polyvinyl butyral, polyvinyl acetal, polyvinyl alcohol, styrene, polystyrene, polyurethane resin, epoxy resin, phenolic resin, terpene resin, phenoxy resin and PMMA monomer.
[0007] The modified acrylic resin may be one or more of epoxy groups, polyester groups, polyurethane groups or silicone groups grafted into the acrylic resin in a modified manner.
[0008] The solvent includes, but is not limited to, alcohol solvents, ester solvents, highly polar solvents, non-polar solvents, alkane solvents, aromatic solvents, and the like.
[0009] Specifically, it is selected from at least one of alcohol ester dodecanol, terpineol, diethylene glycol butyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl ether acetate, propyl acetate, toluene, n-hexane, and cyclohexanone.
[0010] The average particle size of the silver powder can be several to several hundred nanometers or several to several tens of micrometers; or it can be a mixture of two or more silver powders with different particle sizes.
[0011] The silver powder may have a spherical, granular, flake or amorphous shape.
[0012] Preferably, the silver powder has a D50 of 0.5-3 μm and a tap density of 1-5 g / cm 3 , the preferred particle size is 1μm to 2μm.
[0013] The glass powder is lead-free glass, preferably Ca-B-Si-Bi glass.
[0014] Furthermore, the present invention provides a method for preparing silver paste for the front electrode of a crystalline silicon solar cell.
[0015] The specific steps include the following:
[0016] 1. Resin dissolution: Dissolve the organic resin in the solvent, heat to 80-120°C, stir and dissolve.
[0017] Specifically, the resin is dissolved in a solvent with a resin concentration of 0.1-0.5 wt %, heated to 80-120° C., stirred for 20-60 minutes, and stirred at a speed of 1000-3000 r / min.
[0018] Preferably, the present invention adopts a staged heating method to dissolve the resin: first heating to 80-100°C, stirring for 10-20 minutes, then heating a second time to a temperature greater than 100°C and less than 120°C, stirring for the remaining time (10-50 minutes).
[0019] The stirring can be mechanical stirring or ultrasonic-assisted mechanical stirring to reduce agglomeration.
[0020] The present invention utilizes the properties and characteristics of resin heating, and heats up the resin to dissolve first, which is beneficial to the subsequent layer-by-layer wrapping of silver powder and the expansion of different resin types; and the staged heating is beneficial to controlling the degree of resin dissolution and improving the uniformity and stability of the wrapped silver powder.
[0021] 2. Silver powder packaging:
[0022] Add silver powder to the resin solution, control the weight ratio of silver powder to resin to be 100-200:1, heat to 80-100℃, and stir. During this process, the resin will fully wrap the surface of the silver powder.
[0023] In order to adjust the dispersibility and coating degree of the silver powder in the resin, the present invention adopts appropriate temperature increase so that the resin forms layers of coating on the silver powder; in addition, a solvent can be added during the process of adding the silver powder to the resin to keep the silver powder particles fully wrapped in the resin system.
[0024] The solvent is the same as the solvent for dissolving the resin, and is selected from at least one of alcohol ester dodecanol, terpineol, diethylene glycol butyl ether, diethylene glycol dibutyl ether, diethylene glycol butyl ether acetate, propyl acetate, toluene, n-hexane, and cyclohexanone.
[0025] Preferably, the silver powder coating process also adopts staged heating: firstly, the temperature is raised to 50-60°C, stirred for 20-40 minutes, and then the temperature is further raised to 80-100°C, stirred for 20-40 minutes. The staged heating is conducive to controlling the density and uniformity of the silver powder coating.
[0026] 3. Resin shaping
[0027] After the coating process is completed, it is heated to 80-350°C and stirred for 10-60min to evaporate the solvent, then cooled to room temperature and dried to set the resin.
[0028] The drying is preferably vacuum drying, with a drying temperature of 80-120° C. and a drying time of 1-2 h.
[0029] 4. Secondary dispersion:
[0030] The mixed powder of the silver powder and the resin obtained in step 3 is subjected to air flow pulverization and air flow classification to redisperse the silver powder to obtain the resin-coated silver powder for preparing the slurry.
[0031] 5. Preparation of silver paste:
[0032] The resin-coated silver powder obtained in step 4 is mixed with an organic carrier, an additive, and a glass powder in a certain proportion to form a slurry, which is the electrode silver paste for the crystalline silicon solar cell.
[0033] The weight percentage of the slurry is 70-80% by weight of the silver powder, the weight percentage of the slurry is 5-10% by weight of the organic carrier, the weight percentage of the glass powder is 5-8%, and the rest is additives.
[0034] The organic carrier is selected from at least one of acrylic resin, modified acrylic resin, ethyl cellulose, methyl cellulose, polyvinyl butyral, polyvinyl acetal, polyvinyl alcohol, styrene, polystyrene, polyurethane resin, epoxy resin, phenolic resin, terpene resin, phenoxy resin and PMMA monomer.
[0035] The type of the resin in the organic vehicle may be the same as or different from the organic resin in step 1.
[0036] The additive is selected from one or more of emulsifier, dispersant, defoamer, leveling agent, rheological additive, such as bisphenol A epoxy resin, methylimidazole, polyamide wax, tetraethyl titanate, etc.
[0037] The dispersant is selected from one or more of alcohol ethers, phenol ethers, ester ethers, silicones, polyether-modified types, PEG, and PPG.
[0038] The glass powder is a lead-free glass component, preferably a Ca-B-Si-Bi glass.
[0039] The glass powder includes calcium oxide, silicon dioxide, boron oxide, bismuth oxide, and one or more selected from the group consisting of lithium oxide, sodium oxide, potassium oxide, magnesium oxide, strontium oxide, barium oxide, phosphorus oxide, titanium oxide, and nickel oxide.
[0040] The organic carrier is composed of the following raw materials in weight percentage: 5% to 30% resin and 70% to 95% organic solvent, wherein the resin in the organic carrier can be some resins commonly used in existing front silver pastes or can be the precursor of such resin or other functional monomers.
[0041] Specifically, the resin is any one of acrylic resin, modified acrylic resin, ethyl cellulose, methyl cellulose, polyvinyl butyral, polyvinyl acetal, polyvinyl alcohol, styrene, polystyrene, polyurethane resin, epoxy resin, and maleic acid resin.
[0042] The present invention provides a solar cell electrode, which is prepared by the electrode silver paste obtained by the preparation method as described above. Preferably, the width of the solar cell electrode is 10 to 40 μm.
[0043] The present invention also provides a method for manufacturing a solar cell electrode, wherein the electrode silver paste obtained by the above-mentioned preparation method is prepared by screen printing:
[0044] The specifications of the screen during screen printing are: mesh number 400-520 mesh, wire diameter 10-15 μm, total thickness 25-30 μm, and opening 10-30 μm.
[0045] The present invention provides a solar cell, which adopts the electrode as mentioned above.
[0046] Beneficial effects of the present invention:
[0047] 1. In the process of preparing the front silver paste, the resin in the paste system is directly coated on the surface of the silver powder particles, so that the silver powder particles are more completely wrapped in the organic system, forming layer-by-layer coating, which is beneficial to improve the adhesion and reduce the separation of the silver particles from the system.
[0048] 2. The present invention adopts a preparation method for coating silver powder by first dissolving the resin at high temperature. The obtained positive silver paste system of silver powder and resin has a wider range of resin selection. Any resin that can be dissolved in a solvent can be used to coat the silver powder by the method of the present invention, which greatly improves the range of selection of coating resins, so that some resins that cannot be well dissolved in solvents can also be used in the organic system of the paste, expanding the application range of the resin and providing greater possibilities for better adaptation to fine line printing.
[0049] 3. The silver paste prepared by the present invention has high stability in long-term use. The positive silver paste prepared by the present invention has a stable EL yield in the early and late stages of product use. The EL does not produce cloudiness or blackening, which promotes the reaction between the silver electrode and silicon, thereby obtaining a higher photoelectric conversion efficiency.
[0050] 4. By adopting the preparation method of the present invention and optimizing the dosage of each component of the silver paste, the amount of resin used in the prepared front silver paste is less, only 5-10%, which is significantly lower than the 15-20% range in the prior art), which is conducive to fine line printing and reduces costs.
[0051] 5. The viscosity of the front silver paste prepared by the present invention is lower under the same system, and is more suitable for printing on large-area silicon wafers.
[0052] 6. The present invention is beneficial to improving the compatibility and uniformity of the resin and the stability and density of the resin coating by simply controlling the temperature rise process of the resin dissolution and the silver powder coating, effectively reducing the amount of organic resin used in the slurry preparation process and optimizing the stability and photoelectric performance of the front silver paste.
[0053] 7. The preparation process of the present invention is simple and easier to industrialize, solving the problem of poor aspect ratio during fine line printing. DETAILED DESCRIPTION
[0054] The present invention is further described below in conjunction with specific examples, but the present invention is not limited to the following examples. The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0055] Example 1
[0056] 1. Resin dissolution:
[0057] The acrylic resin was dissolved in ethanol solvent (100 L), the concentration of the resin was controlled to be 0.1%, the heating temperature was 100° C., the stirring time was 60 minutes, and the stirring speed was 2000 r / min to obtain a dissolved resin;
[0058] 2. Silver powder packaging:
[0059] After the resin is fully dissolved, add silver powder into the solution. The ratio of silver powder to resin is 200:1. Set the temperature to 80℃ and stir at 2000r / min for 60 minutes. During this process, the resin will fully wrap the surface of the silver powder.
[0060] 3. Resin shaping:
[0061] After coating, set the temperature to 300°C and continue stirring to evaporate the solvent in the mixture. Stir for 40 minutes (when the volatilization is about 80%), then stop stirring. Place the slurry of silver powder, resin and solvent in a tray, dry it in a vacuum drying oven at 80°C for 1 hour, and then cool it to room temperature to allow the resin to set.
[0062] 4. Secondary dispersion:
[0063] The mixed powder of the silver powder and the resin obtained in step 3 is subjected to air flow pulverization and air flow classification to obtain the resin-coated silver powder for preparing the slurry.
[0064] The powder with a particle size of 0.5-5 μm is obtained through air flow crushing and air flow classification.
[0065] 5. Mix to obtain silver paste:
[0066] The resin-coated silver powder obtained in step 4 is mixed with an organic carrier, an organic additive, and a glass powder in a mass ratio of 70%, 10%, 12%, and 8% to form a slurry. The slurry is uniformly stirred and three-rolled before testing.
[0067] The organic carrier is 5 wt % acrylic resin / ethanol solvent; the organic additive is an organosilicon dispersant (purchased from Shanghai Gongyao International).
[0068] Example 2 (ratio of silver powder to resin)
[0069] 1. Resin dissolution:
[0070] The acrylic resin was dissolved in ethanol solvent (100 L), the concentration of the resin was controlled to be 0.1%, the heating temperature was 100° C., the stirring time was 60 minutes, and the stirring speed was 2000 r / min to obtain a dissolved resin;
[0071] 2. Silver powder packaging:
[0072] After the resin is fully dissolved, add silver powder into the solution. The ratio of silver powder to resin is 100:1. Set the temperature to 80℃ and stir at 2000r / min for 60 minutes. During this process, the resin will fully wrap the surface of the silver powder.
[0073] 3. Resin shaping:
[0074] After coating, set the temperature to 300°C and continue stirring to evaporate the solvent in the mixture. Stir for 40 minutes (when the volatilization is about 80%), then stop stirring. Place the slurry of silver powder, resin and solvent in a tray, dry it in a vacuum drying oven at 80°C for 1 hour, and then cool it to room temperature to allow the resin to set.
[0075] 4. Secondary dispersion:
[0076] The mixed powder of the silver powder and the resin obtained in step 3 is subjected to air flow pulverization and air flow classification to obtain the resin-coated silver powder for preparing the slurry.
[0077] 5. Mix to obtain silver paste:
[0078] The resin-coated silver powder obtained in step 4 was mixed with an organic carrier, an organic additive, and a glass powder in a mass ratio of 70%, 10%, 12%, and 8% to form a slurry. The slurry was uniformly stirred and three-rolled for testing. The organic carrier was 5wt% acrylic resin / ethanol solvent; the organic additive was a phenol ether dispersant (purchased from Shanghai Gongyao International, ED series).
[0079] Example 3
[0080] The method of Example 1 is followed, except that step 1: dissolving methyl cellulose in alcohol ester twelve solvent (100 L), controlling the resin concentration to 0.1%, heating temperature to 100° C., stirring time to 60 minutes, stirring speed to 2000 r / min, to obtain dissolved resin; the other steps are the same as Example 1.
[0081] Example 4
[0082] The method of Example 1 is followed, except that step 1: dissolving acrylic resin in ethanol solvent (100 L), controlling the resin concentration to 0.1%, heating to 85° C., stirring for 20 minutes, then continuing to heat to 105° C., stirring for 40 minutes, stirring at a speed of 2000 r / min, to obtain dissolved resin; the other steps are the same as those of Example 1.
[0083] Example 5
[0084] 1. Resin dissolution:
[0085] The acrylic resin was dissolved in diethylene glycol butyl ether solvent (100 L), the concentration of the resin was controlled to be 0.6%, the heating temperature was 95° C., the stirring time was 60 minutes, and the stirring speed was 2000 r / min to obtain a dissolved resin;
[0086] 2. Silver powder packaging:
[0087] After the resin is fully dissolved, add silver powder to the solution. The ratio of silver powder to resin is 150:1. Set the temperature to 80°C and stir at 2000r / min for 60 minutes. During this process, the resin will fully wrap the surface of the silver powder.
[0088] 3. Resin shaping:
[0089] After coating, set the temperature to 280℃ and continue stirring to evaporate the solvent in the mixture. Stir for 30 minutes (when the volatilization is about 80%), then stop stirring. Place the slurry of silver powder, resin and solvent in a tray, dry it in a vacuum drying oven at 80℃ for 1 hour, and then cool it to room temperature to set the resin.
[0090] 4. Secondary dispersion:
[0091] The mixed powder of the silver powder and the resin obtained in step 3 is subjected to air flow pulverization and air flow classification to obtain the resin-coated silver powder for preparing the slurry.
[0092] 5. Mix to obtain silver paste:
[0093] The resin-coated silver powder obtained in step 4 is mixed with an organic carrier, an organic additive, and a glass powder in a mass ratio of 75%, 8%, 10%, and 7% to form a slurry. The organic carrier is a 10wt% phenolic resin / diethylene glycol butyl ether solvent; the organic additive is an organic silicon dispersant. The slurry is uniformly stirred and three-rolled before testing.
[0094] Example 6
[0095] The method of Example 1 is the same, except that step 2 also adopts the stepwise heating method:
[0096] Silver powder coating: After the resin is fully dissolved, add silver powder into the solution. The ratio of silver powder to resin is 200:1. Set the temperature to 60℃ and stir at 2000r / min for 30 minutes. Then continue to heat to 80℃ and continue stirring at 2000r / min for 30 minutes. During this process, the resin will fully coat the surface of the silver powder.
[0097] Comparative Example 1
[0098] Steps 1-4 were omitted, and silver powder was directly mixed with organic carrier, organic additive and glass powder in a mass ratio of 70%, 10%, 12% and 8% to form a slurry. The organic carrier was 5wt% acrylic resin / ethanol solvent; the organic additive was a dispersant. The slurry was uniformly stirred and three-roll milled before testing.
[0099] Comparative Example 2
[0100] 1. Resin dissolution:
[0101] Dissolve the acrylic resin in ethanol solvent (100 L), control the resin concentration to 0.1%, stir for 60 minutes, and stir at a speed of 2000 r / min;
[0102] 2. Silver powder packaging:
[0103] Add silver powder to the resin in step 1, the ratio of silver powder to resin is 200:1, and continue stirring for 60 minutes at a stirring speed of 2000 r / min. During this process, the resin will fully wrap the surface of the silver powder. The other steps are the same as in Example 1.
[0104] The silver paste prepared in the embodiment and the comparative example was made into solar cells by screen printing. The screen specification was a knotless screen of 520 mesh, a wire diameter of 11 μm, and a line width of 13 μm. The sintering peak temperature was 750°C. The tester was used to test the electrical properties of the sintered solar cells, including short-circuit current density (Isc), open-circuit voltage (Voc), fill factor (FF) Rs (series resistance of the solar cell), Rsh (parallel resistance of the solar cell), viscosity (Brookfield DV2T viscometer, 5 rpm, 25°C) and photoelectric conversion efficiency (Eta). The results are shown in Table 1.
[0105] Table 1 Silver paste performance test
[0106]
[0107]
[0108] It can be seen that the setting of the temperature increase, temperature control and other conditions in the process of resin coating silver powder in the present invention can optimize the uniformity and stability of the resin coating, and by heating the resin to dissolve the resin, the selection range of the resin can be broadened. Any resin that can be dissolved in a solvent can be used to coat the silver powder by the method mentioned in the present invention, which greatly improves the selection range of the coating resin. In addition, the positive silver paste prepared by the present invention has good electrical properties, and has excellent Eta and EL gate breaking effects compared with the comparative example 2 without heating (which is simply mixed and cannot form a coating structure) or the uncoated comparative example 1.
[0109] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments / methods or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.
[0110] Those skilled in the art should understand that the above embodiments are only for the purpose of clearly illustrating the present application, and are not intended to limit the scope of the present application. For those skilled in the art, other changes or modifications may be made based on the above disclosure, and these changes or modifications are still within the scope of the present application.
Claims
1. A method for preparing silver paste for front electrode of crystalline silicon solar cells, It is characterized in that It includes the following steps: 1) Resin dissolution: dissolve the organic resin in the solvent, heat to 80-120℃, stir and dissolve; 2) Silver powder coating: Add silver powder to the resin solution, control the weight ratio of silver powder to resin to be 100-200:1, heat to 80-100℃, stir, and the resin fully coats the surface of the silver powder; 3) Resin shaping: After the coating process is completed, heat to 80-350℃, stir for 10-60min to evaporate the solvent, then cool to room temperature and dry to shape the resin; 4) Secondary dispersion: The mixed powder obtained in step 3) is subjected to air flow pulverization and air flow classification to redisperse the silver powder to obtain resin-coated silver powder for preparing slurry; 5) preparing silver paste: the resin-coated silver powder obtained in step 4) is mixed with an organic carrier, an organic additive and a glass powder in a certain proportion to form a slurry to obtain the electrode silver paste for the crystalline silicon solar cell; the organic resin is selected from at least one of acrylic resin, modified acrylic resin, ethyl cellulose, methyl cellulose, polyvinyl butyral, polyvinyl acetal, polyvinyl alcohol, polystyrene, polyurethane resin, epoxy resin, phenolic resin, terpene resin and phenoxy resin.
2. The preparation method according to claim 1, It is characterized in that Silver powder has a D50 of 0.5-3μm and a tap density of 1-5g / cm 3 .
3. The preparation method according to claim 2, It is characterized in that The silver powder has a D50 of 1 μm to 2 μm and has a spherical, granular, flake or amorphous shape.
4. The preparation method according to claim 1, It is characterized in that The glass powder is lead-free glass powder.
5. The preparation method according to claim 4, It is characterized in that The glass powder is Ca-B-Si-Bi glass.
6. The preparation method according to claim 1, It is characterized in that The organic carrier is composed of the following raw materials in weight percentage: 5% to 30% resin and 70% to 95% organic solvent; The resin is selected from at least one of acrylic resin, modified acrylic resin, ethyl cellulose, methyl cellulose, polyvinyl butyral, polyvinyl acetal, polyvinyl alcohol, polystyrene, polyurethane resin, epoxy resin, phenolic resin, terpene resin and phenoxy resin.
7. The preparation method according to claim 1, It is characterized in that Step 1) Use a staged heating method to dissolve the resin: first heat to 80-100°C, keep stirring for 10-20 minutes, then heat for a second time to a temperature greater than 100°C and less than 120°C, and keep stirring for the rest of the time.
8. The preparation method according to claim 1, It is characterized in that Step 2) The silver powder encapsulation process adopts staged heating: first heat to 50-60°C, stir for 20-40 minutes, then continue to heat to 80-100°C, stir for 20-40 minutes.
9. A solar cell electrode, prepared from the electrode silver paste obtained by the preparation method according to any one of claims 1 to 8.
10. A solar cell prepared by using the electrode according to claim 9.