Aqueous resin dispersion and aqueous coating composition containing the same
By using resin components with specific NH equivalents and multifunctional monomer amines in aqueous coatings, the problem of insufficient polishing properties of existing aqueous coating compositions at low temperatures is solved, and the field of automotive recoating is realized Excellent bonding and corrosion resistance.
Patent Information
- Application Number
- CN202080037680.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-23
- Filing Date
- 2020-04-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-04-23
AI Technical Summary
The existing water-based coating compositions are insufficient after curing at low temperatures, especially in the field of automotive recoating, and it is difficult to meet the requirements for bonding and corrosion resistance of the second primer layer.
Using a novel aqueous resin dispersion containing a resin component with 150-400 g/mol NH equivalent and 5-15% by weight of a multifunctional monomer amine, an amino functional resin mixture is formed by reacting an epoxy compound with an amine. Further reaction was carried out in the aqueous phase to prepare an aqueous two-component coating composition with excellent abrasive properties and bonding properties.
The coating composition that achieves rapid curing at low temperature has good grinding and bonding properties, and is suitable for two-coat primer and first two-coat mixed primer, especially suitable for the restoration of multi-layer paint systems and automotive recoatment. field.
Smart Images

Figure BDA0003366630410000201 
Figure BDA0003366630410000211 
Figure BDA0003366630410000212
Abstract
Description
[0001] The present invention relates to an aqueous resin dispersion, namely an aqueous resin dispersion (AD) comprising a resin component (R), wherein the resin component comprises a di- and / or multifunctional monomeric organic amine and a multifunctional polymeric organic amine. The present invention also relates to an aqueous coating composition comprising the resin dispersion (AD). The coating composition comprises a combination of a resin dispersion and an epoxy resin and has excellent applicability as an aqueous sandable surfacer or a top-surfacer. Thus, by applying the coating composition to a substrate and subsequently curing the coating composition, a surfacer layer having excellent sandability can be obtained, and therefore has excellent applicability, particularly in the field of repair. Prior art
[0002] In principle, waterborne surfacers and primer-surfacers are known which cure on the basis of epoxy-amine combinations and can in this way form corrosion-stable surfacer or primer-surfacer hybrid layers. Their spectrum of properties is rather complex and has the special features of the already mentioned corrosion stability and good adhesion to various substrates such as steel, galvanized steel, aluminum, electrocoatings and old paint systems.
[0003] However, care should be taken that the surfacer layers which are applied, in particular in the automotive recoating sector, have acceptable sandability even after curing at moderate temperatures and within the processing times customary in a paint shop. This sandability is very important in the painting process in order to produce a homogeneous surface for the subsequent layers, such as basecoat and clearcoat, and ultimately to give the painted surface an aesthetically high-quality appearance. However, the systems known from the prior art still have disadvantages, in particular with regard to sandability.
[0004] WO 97 / 49749 A1 discloses coating compositions based on aqueous epoxy systems containing specific epoxy-aminourethane adducts as curing agents. These are obtained by reacting very specific aminourethane compounds with epoxy compounds. The epoxy compounds are obtained by reacting polyalkylene polyethers with one or more amino groups. These adducts are used in aqueous two-component paints, especially automotive paints. The paints or paint coatings thus obtained have good sandability. It is documented that the paints described in EP 0 387 418 A2 have disadvantages in terms of their sandability.
[0005] EP 0387418 A2 discloses a curing agent for epoxy compounds and their use for the preparation of coatings and coverings. The curing agent is prepared by reacting a polyalkylene polyether amine with a stoichiometric excess of a di- and / or polyepoxide and then reacting the adduct with a stoichiometric excess of the amine. The coating compositions prepared with these curing agents have good storage stability and good curing properties. There is no mention of recoating, nor of the sandability of the coating or of the use of the curing agent in a surfacer.
[0006] EP 0610787 A2 describes curing agents for aqueous epoxy resin dispersions which are obtained by reacting an adduct (A) formed from polyepoxides and polyalkylene polyether polyols with a reaction product of an amine and an epoxide or with an amine and subsequently with an epoxide, the amine being used in each case in a stoichiometric excess. The problem to be solved is, for example, to achieve good adhesion and hardness in coating compositions comprising surfacers.
[0007] Problems and technical solutions
[0008] The problem addressed by the present invention is therefore to eliminate the disadvantages of the prior art and to provide an aqueous coating composition which, after application and curing, has good adhesion and corrosion protection properties, in particular in the case of automotive repainting, but which nevertheless has very good sandability even after a relatively short curing period at low temperatures. The composition is therefore particularly suitable as a surfacer and primer-surfacer or for producing a surfacer layer in a multicoat paint system.
[0009] It has been found that this object is achieved by a novel aqueous resin dispersion (AD) comprising a resin component (R) which comprises at least one di- and / or polyfunctional monomeric primary and / or secondary amine (M) and a polyfunctional polymeric organic amine having primary and / or secondary amino groups,
[0010] wherein the resin component (R) has an NH equivalent of 150-400 g / mol and a weight proportion of 5-15 wt % of di- and / or polyfunctional monomeric organic amine (M),
[0011] The polyfunctional polymeric organic amines having primary and secondary amino groups also include the following in mutually reactive form:
[0012] (i) at least one di- and / or polyfunctional organic epoxy compound, wherein the epoxy compound has an average epoxy equivalent weight of less than 400 g / mol,
[0013] (ii) at least one monomeric amine (M), and
[0014] (iii) at least one compound XR, in which X is a functional group reactive toward epoxy groups and R is an organic radical containing polyoxyalkylene units and not containing any other X groups,
[0015] And wherein the amine (M) comprises at least 65 mol % of an amine consisting of amino and hydrocarbon units.
[0016] The novel resin dispersion (AD) is also referred to as the dispersion of the invention. The invention also provides an aqueous two-component (2K) coating composition comprising the dispersion of the invention. In addition, the invention provides a method for preparing a coating using the coating composition. The invention provides at least one method for repairing a multilayer paint system having defects, which comprises applying the coating composition, curing the composition to produce a cured coating and subsequently sanding the coating. The invention also provides a coating prepared as described above and a coated substrate.
[0017] Detailed Description
[0018] Waterborne resin dispersion (AD)
[0019] The present invention firstly relates to an aqueous resin dispersion (AD) comprising a resin component (R).
[0020] The term "aqueous" in relation to dispersions such as resin dispersions, phases or aqueous coating compositions is known in principle. It means a dispersion or mixture containing a significant proportion of water as a solvent. It should be understood that aqueous systems may also contain at least a small amount of organic solvents, for example as a cosolvent with an emulsifier function to stabilize specific ingredients, such as resins, pigments or additives. In the context of the present invention, "aqueous" should preferably be understood to mean that the system, preferably dispersion, has at least 40% by weight, preferably at least 50% by weight, even more preferably at least 60% by weight of water, in each case based on the total amount of solvent present (i.e. water and organic solvent). The preferred proportion of water is again 50-99% by weight, especially 60-98% by weight, in each case based on the total amount of solvent present.
[0021] According to definitions known in principle, resins or resin components are also understood to mean products containing organic components, i.e. organic reaction products, oligomers and / or polymers and, if appropriate, monomers, as with the resin component (R). Resins have a more or less broad molar mass distribution and can generally be used as binders in coating compositions. Therefore, after curing, they form at least a certain proportion of the polymer network of the coating present.
[0022] According to the invention, the resin component (R) contains at least one di- and / or polyfunctional monomeric primary and / or secondary amine (M), ie at least one monomeric amine comprising at least two amino groups selected from primary and secondary amino groups. Of course, the additional presence of tertiary amino groups is not impossible.
[0023] In the context of the present invention, it is essential that the amine (M) used overall and therefore present in the aqueous dispersion (AD) comprises at least 65 mol % of amines consisting of amino and hydrocarbon units. It has been found that otherwise, the result is an adverse effect on the sandability. This means, therefore, that other functional groups, in particular for example hydroxyl, carboxyl or nitrile groups, are present only in small amounts. Preferably, the amine (M) comprises at least 75 mol %, more preferably at least 90 mol %, of amines consisting of amino and hydrocarbon units. Most preferably, the proportion of these amines is 100 mol %.
[0024] The proportion of the corresponding amines is essentially apparent from the amount of amine used. However, in the case of using products such as commercial products, the proportion of the corresponding amines can also be determined by analyzing the products (in which the amines may also be partially or completely covalently bonded to one another) to such an extent that the above conditions are directly clearly met (e.g. by gas chromatography (GC), mass spectrometry (MS) analysis).
[0025] Examples of suitable amines (M) are the monomeric aliphatic, aromatic and araliphatic (mixed aliphatic-aromatic) amines known in principle to the person skilled in the art.
[0026] Examples of di- and / or polyfunctional monomeric primary and / or secondary amines include the following: ethylenediamine, propylene-1,2-diamine, propylene-1,3-diamine, butane-1,4-diamine, octane-1,8-diamine, 1,3-diaminopentane, hexamethylenediamine, 2-methylpentamethylenediamine, neopentanediamine, cyclohexanediamine, 2,2,4-(2,4,4-)trimethylhexamethylenediamine, isophoronediamine, bis(aminomethyl)cyclohexane, bis(4-aminocyclohexyl)methane, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, dipropylenetriamine, bis(hexamethylenediamine), N,N-dimethylaminodipropylenetriamine, laurylpropylenediamine, 1,2- and 1,3-(m-)-phenylenediamine and 1,4-bis(aminomethyl)benzene. Other amines include aminoethylethanolamine or heterocyclic polyamines such as aminoethylpiperazine and bis(aminopropyl)piperazine.
[0027] Preference is given to difunctional primary and / or secondary amines (M), again preference is given to difunctional primary amines. Very particular preference is given to isophoronediamine and meta-xylylenediamine, and the resin component more preferably comprises a mixture of the two diamines. This means, therefore, that the amine (M) is a mixture of isophoronediamine and meta-xylylenediamine.
[0028] The proportion of the at least one di- and / or polyfunctional monomeric primary and / or secondary amine (M) is 5-15% by weight, preferably 6-14% by weight, more preferably 7-13% by weight, based on the resin component (R) (for test methods, see the Examples section).
[0029] The resin component (R) also contains polyfunctional polymeric organic amines having primary and / or secondary amino groups. Thus, in contrast to the monomeric amines already described, these are in particular not low molecular weight compounds having a discrete number of amino groups per molecule (constant for each molecule), but rather adducts or reaction products having polymeric properties and in which the number of amino groups per molecule can only be described by an average value.
[0030] The structure of the component described here, ie the structure of the polyfunctional polymeric organic amine having primary and / or secondary amino groups, can be deduced from the starting compounds further described below for the preparation of the resin component (R).
[0031] The resin component (R) has an NH equivalent weight of 150-400 g / mol, preferably 160-350 g / mol, more preferably 170-250 g / mol (for the determination method, see the Examples section).
[0032] The aqueous dispersion (AD) comprising the resin component (R) can be prepared, for example, by a two-step process (A+B), which will be described in detail below.
[0033] Step A
[0034] In the first step (A) of the reaction sequence, two starting components (Ia) and (Ib) are reacted with one another, namely the epoxy-functional resin mixture (Ia) and the component (Ib) containing at least one di- and / or polyfunctional monomeric primary and / or secondary amine (M). This produces an amino-functional resin mixture (I). It is therefore obvious that the amounts of components (Ia) and (Ib) are matched to one another so that the NH equivalents of component (Ib) are in molar excess relative to the epoxy groups of component (Ia).
[0035] The epoxy-functional resin mixture (Ia) contains the two components (Ia1) and (Ia2) described below in mutually reacted form. The resin mixture (Ia) preferably consists of these two components, ie is prepared exclusively by reaction of these two components.
[0036] Component (Ia1) is at least one di- and / or polyfunctional organic epoxy compound.
[0037] Therefore, the components (Ia1) that can be used are epoxy resins known in principle. Preferably, these epoxy compounds used have an average epoxy equivalent of less than 400 g / mol. It has been found that the correspondingly low average epoxy equivalent and therefore higher epoxy functionality of the component again lead to better sandability in the surface primer layer finally produced. More preferably, the average epoxy equivalent is less than 350 g / mol, preferably less than 300 g / mol, more preferably less than 250 g / mol. The average epoxy equivalent can be obtained by determining the epoxy equivalent of all epoxy compounds used (test methods see the Examples section) and weighing their mass proportion in the total weight of epoxy compounds. When using existing products such as commercial products (in which the epoxy compounds may have been covalently bonded), the average epoxy equivalent can also be determined by analyzing the product to an extent that it is immediately clear that it is below the above-mentioned upper limit (for example by gas chromatography (GC), mass spectrometry (MS) analysis).
[0038] Known epoxy resins are polycondensation resins which contain, on average, more than one epoxy group in the base molecule. For example, these are epoxy resins prepared by condensation of bisphenol A or bisphenol F with epichlorohydrin. These compounds contain hydroxyl groups along the chain and epoxy groups at the ends. Depending on the chain length of the epoxy resin, there are variations in the crosslinking capacity via the epoxy groups, precisely because the crosslinking capacity via the epoxy groups decreases with increasing chain length / molar mass. In the context of the present invention, any epoxy resin known per se to the person skilled in the art can ultimately be used, provided that they are within the above-mentioned epoxy equivalent range. For example, commercially available epoxy resins mentioned further below can be used, which can be obtained as solutions or dispersions in organic solvents or water.
[0039] Such epoxy resins are available, for example, as 100% systems or as solutions or dispersions in organic solvents or water.
[0040] Preferred components (Ia1) are averagely difunctional epoxides, since this is formed via epichlorohydrin in the above-mentioned standard synthesis.
[0041] Furthermore, it is preferred that the epoxy compound (Ia1) is a bisphenol A-based epoxy compound, i.e. an epoxy compound prepared by using bisphenol A. This also means more particularly that the epoxy compound does not contain any synthetically introduced bisphenol F. It has been found that this result in turn has a positive influence on the sandability of the surfacer layer finally produced.
[0042] Component (Ia2) is at least one compound XR in which X is a functional group reactive toward epoxy groups and R is an organic radical containing polyoxyalkylene units and not containing any further X groups. Preference is given to using exactly one compound XR as component (Ia2).
[0043] The X groups are groups known to the person skilled in the art, for example primary or secondary amino, hydroxyl, carboxyl or thiol groups.
[0044] It is essential that the compound XR has only one X group. Otherwise, the sandability of the surfacer layer finally produced is found to be adversely affected.
[0045] Preferred X groups are amino groups, with primary amino groups being preferred. In addition to the good reactivity of amino groups with epoxy groups, primary amines have 2N-H equivalents and therefore have 2 attachment sites to epoxides. In this way, compound XR can be attached to a side chain position of the molecule. The overall result of this is in turn beneficial to the sandability of the surface primer layer.
[0046] The R group is an organic group containing a polyoxyalkylene unit, particularly preferably polyethylene or polypropylene unit or mixed polyethylene / polypropylene unit. Preferably, except any molecular unit obtained by synthesis, the organic R group is composed of a polyoxyalkylene unit. For simplicity, the R group is also referred to as polyoxyalkylene. The molecular unit obtained by synthesis is, for example, an organic group of a molecule used when starting to form a polyoxyalkylene chain, such as an initiator alcohol, which initiates the polymerization of ethylene oxide and / or propylene oxide. Preferably, the R group is polyethylene, polypropylene or mixed polyethylene / polypropylene.
[0047] The weight average molecular weight of compounds (Ia2) can vary within wide ranges, for example from 800 to 2200 g / mol (determined by size exclusion chromatography coupled to light scattering).
[0048] The compounds XR can be prepared in-house or obtained commercially. For example, the clearly preferred polyoxyalkylene monoamines are commercially available under the name "Jeffamine" from Huntsman.
[0049] The epoxy-functional resin mixture (Ia) contains two components (Ia1) and (Ia2) in a mutually reactive form. Thus, the epoxy groups of component (Ia1) and the X groups of component (Ia2) react with each other. The corresponding reaction schemes and conditions are known to those skilled in the art and do not require any further mention.
[0050] Component (Ia) is an epoxy-functional resin mixture. Therefore, it is obvious from the raw materials that components (Ia1) and (Ia2) are used in such a way that the epoxy groups of component (Ia1) are in excess relative to the reactive unit mole stoichiometry of the X group. The number of reactive units means the number of potential attachment sites for each epoxy group. For hydroxyl or secondary amino groups, for example, there is one reactive unit for each X group. For primary amino groups, there are two reactive units (two NH functional groups). Preferably, the molar ratio of the epoxy reactive units of the epoxy groups of compound (Ia1) and the X groups of component (Ia2) is 10-1.1, more preferably 5-1.5, and particularly preferably 3.5-1.8.
[0051] The amount of epoxy groups in component (Ia1) can be obtained or appropriately adjusted in a known manner according to the purpose by determining the epoxy equivalent. The amount of reactive units in the X group is obtained by test methods known per se for determining the amount of functional groups X, for example by determining the amine value, OH value or acid value (DIN 53176: 2002-11, DIN 53240-3: 2016-03, DIN EN ISO 2114 correction 1: 2006-11).
[0052] Component (Ia) preferably has an epoxy equivalent weight of 500 to 1500 g / mol, more preferably 600 to 1200 g / mol.
[0053] The component (Ib) which reacts with the component (Ia) comprises at least one di- and / or polyfunctional monomeric primary and / or secondary amine (M). Preferably, the component (Ib) consists of at least one such amine (M).
[0054] Examples of suitable amines (M) have already been described above as constituents of the resin component (R). All statements and preferred variants made here apply correspondingly to the amines in component (Ib).
[0055] Resin mixture (I) is an amino-functional resin mixture, so its preparation requires an excess of NH equivalents relative to the functional groups of components (Ia) and (Ib) to be reacted with each other. In particular, the NH equivalent of resin mixture (I) is 50-140g / mol, preferably 70-130g / mol (determination method see the embodiment part). In addition, resin mixture (I) contains 17.5-40% by weight, preferably 25-35% by weight of di- and / or polyfunctional monomer primary and / or secondary amine (M), i.e. component (Ib). Both of these standards can be adjusted by those skilled in the art by appropriately selecting the molar amount of the two components and the knowledge of the quantitative conversion of epoxy and NH functional groups under conditions and reaction schemes known per se. In addition, the examples below give a more specific overview again. Possible reaction schemes and corresponding conditions are known to those skilled in the art and do not require any further mention. Preferably, resin mixture (I) is dispersed in water after its preparation, and in this case is an aqueous dispersion.
[0056] The resin mixture (I) can be prepared as described above and is thus obtained in the form of an aqueous dispersion. Aqueous dispersions of the resin mixture (I) are likewise commercially available (for example as Beckopox VEH 2849w / 80WA (from Allenex)).
[0057] Step B
[0058] In the second step (B) of the reaction sequence, two starting components (IIa) and (IIb) are reacted with one another in the aqueous phase, namely component (IIa) of the amino-functional resin mixture (I) and component (IIb) containing at least one di- and / or polyfunctional organic epoxy compound and having an average epoxy equivalent weight of less than 400 g / mol, preferably less than 350 g / mol, more preferably less than 250 g / mol. Optionally, after removal of the organic solvent used, this produces an aqueous dispersion (AD) comprising the resin component (R). It is evident from the properties of the resin component (R) already mentioned in the form detailed above that the amounts of components (IIa) and (IIb) are matched to one another so that the NH equivalents of component (IIa) are in molar excess relative to the epoxy groups of component (IIb).
[0059] Preference is given to using the direct reaction product of step (A) as component (IIa), which is optionally supplemented only with solvents or auxiliaries such as emulsifiers. This is because the resin mixture (I) is obtained as an aqueous dispersion after step (A) and can therefore be used directly in step (B) carried out in the aqueous phase. Component (IIa) preferably does not contain any other ingredients that can react with component (IIb) other than the reaction product.
[0060] Component (IIb) preferably consists of at least one, preferably exactly one, di- and / or polyfunctional organic epoxy compound, the epoxy equivalent of which satisfies the above-mentioned prerequisites. Examples of suitable epoxy compounds are those already described above as component (Ia1). All the statements made here and the preferred variants apply accordingly to the epoxy compounds in component (IIb).
[0061] The solids content of the aqueous dispersion (AD) is, for example, 25 to 45% by weight (for test methods, see the Examples section).
[0062] The above-described method is a preferred method variant, which also allows, for example, the use of existing commercial products (e.g., the above-described Beckopox VEH 2849w / 80W). For example, in the case of using the above-described commercial products, the dispersion (AD) of the present invention can be obtained by simple modification with a suitable epoxide (because, except for this last reaction, all other reaction methods have been implemented in the production of commercial products). However, it should be understood that other forms of provision of the dispersion (AD) and thus the resin component (R) present therein can also be selected. Thus, for example, by adjusting the appropriate stoichiometric ratio of amine and epoxide, the provision can be achieved in a one-step process, in which all starting components react together. It is also possible to first react the components referred to above as components (Ia1) and (Ia2) with each other, and then to obtain the dispersion (AD) or the resin component (R) by reacting the intermediate simultaneously with other epoxides and the monomeric amine (M).
[0063] Preferably, the resin component (R) consists of the at least one di- and / or polyfunctional monomeric primary and / or secondary amine (M) and a polyfunctional polymeric organic amine having primary and / or secondary amino groups.
[0064] It is also preferred that the polyfunctional polymeric organic amine having primary and secondary amino groups consists of the above-mentioned starting materials in a reacted form. Therefore, the polymeric amine preferably consists of the following materials:
[0065] (i) at least one di- and / or polyfunctional organic epoxy compound, wherein the epoxy compound has an average epoxy equivalent weight of less than 400 g / mol,
[0066] (ii) at least one monomeric amine (M), wherein the amine (M) comprises at least 65 mol % of amines consisting of amino and hydrocarbon units, and
[0067] (iii) at least one compound XR, wherein X is a functional group reactive toward epoxy groups and R is an organic radical containing polyoxyalkylene units and not containing any other X groups.
[0068] Of course, the person skilled in the art can adjust the amounts and ratios of the various starting components without difficulty. In any case, they are selected within a certain degree of freedom in construction in order to obtain the NH equivalents to be achieved according to the invention and the ratios of the monomeric amines (M) to be achieved according to the invention.
[0069] As can be seen from the above, in the preferred method, component (i) is equivalent to the above-mentioned component (IIb), preferably equivalent to component (Ia1) and component (IIb), component (ii) is equivalent to component (Ib), and component (iii) is equivalent to component (Ia2). The preferred embodiments described within the scope of the method are of course also applicable to the scope of components (i), (ii) and (iii).
[0070] Waterborne two-component (2K) coating compositions
[0071] The present invention also relates in particular to aqueous 2K coating compositions comprising an aqueous dispersion (AD).
[0072] As is known, the 2K composition means that component (1) (coat base component) to be defined in more detail further below and component (2) (curing component) as defined below are prepared and stored separately from one another and are not combined until shortly before application. As is known, the processing time or pot life (i.e. the time during which the coating composition can be processed at room temperature (15-25° C., in particular 20° C.) without causing an increase in viscosity (which is due, for example, to a corresponding crosslinking reaction at room temperature) so severe that application is no longer possible) depends on the ingredients used in components (1) and (2). In the context of the present invention, the processing time of the coating composition is preferably at least 2 minutes to 60 minutes, more preferably at least 5 minutes to 60 minutes. A particular advantage of the two-component coating composition is that, in particular, no high temperatures are required for curing. Preferably, after application to the substrate, the coating composition of the invention is cured at not more than 80° C., particularly preferably not more than 65° C.
[0073] Curing is understood to mean a process known to the person skilled in the art, in other words, the conversion of a coating composition applied as a film to a substrate into a ready-to-use state, in other words, into a state in which the substrate provided with the coating can be put into its intended use. With regard to the central problem to be solved in the context of the present invention, namely to obtain good sandability, sandability and subsequent recoatability are of course criteria for the intended use. Curing is achieved in particular by chemical reaction of reactive functional groups of the binder components present in the different components (1) and (2) of the coating composition. In the context of the present invention, therefore, particular mention should be made of the reaction of the amino or NH functional groups of the resin component (R) with the epoxy groups of at least one other resin component present in the respective other main component (binder component or curing component) of the 2K coating composition in this case. As a result of these crosslinking reactions and the parallel evaporation of any organic solvent and / or water present, a coating film is formed, i.e. a cured coating (cured coating) is produced. Activation of the reaction can be achieved by thermal energy, although in the case of the present invention there is the advantage, as mentioned above, that high temperatures are not required.
[0074] The term "binder" or "binder component" in this context refers to the non-volatile matter of the coating material, excluding pigments and fillers, according to the relevant DIN EN ISO 4618. Specific binder components in this context and also resin components (R) are therefore also the other resin components or coating additives already mentioned above which contain functional groups for crosslinking with NH functional groups.
[0075] However, merely for the sake of clarity, the term "binder" is used primarily in connection with the resin component of the binder component (1) which is primarily responsible for film formation, whereas the resin component present in the curing component (2) is primarily referred to as a curing agent or crosslinking agent. Typically, in addition to the binder and the solvent, the binder component (1) also contains all or most of the other functional ingredients of the composition, such as pigments, fillers and additives, whereas the curing component (2) contains, in addition to the solvent and any additives present, only the resin component intended for crosslinking. The terms "binder component" and "curing component" in connection with 2K coating compositions are known to those skilled in the art and also have essential characteristics and therefore have distinguishing features within a certain construction range.
[0076] Of course, in order to complete the 2K coating composition, at least one further main component may also be present. This means that, in addition to the base component (1) and the curing component (2), other ingredients such as solvents or additives may be added to the at least one other main component, for example after the two main components (1) and (2) have been added. However, the composition still complies with the definition of a 2K coating composition, since the number of components containing the components that are cross-linked with each other and are responsible for film formation is two.
[0077] 2K coating compositions have excellent suitability as surfacer and top-surfacer and can be used as is. Therefore, the 2K coating composition is preferably a surfacer or a top-surfacer. The functions, constructions and areas of use of surfacer and top-surfacer are known in principle to those skilled in the art and have distinguishing properties in this respect. In the case of automotive OEM finishing, the surfacer is usually applied as an intermediate layer (applied to a previously cured electrocoat), cured separately and then overcoated with a basecoat and a clearcoat. Top-surfacer primers are used in particular in the field of automotive repainting, where they are responsible for filling in locally damaged areas in the initial paint system and for obtaining suitable adhesion on the substrate and ensuring corrosion protection.
[0078] The 2K coating composition contains as an essential component an aqueous dispersion (AD) containing a resin component (R). The amount of dispersion (AD) is preferably selected here so that the proportion of the resin component (R) is 10-30% by weight, more preferably 15-25% by weight, based on the solid content of the coating composition.
[0079] The 2K coating composition further contains at least one other resin component containing epoxy groups. The epoxy groups can react with NH functional groups to form a network structure and in this way contribute to the curing of the coating prepared from the coating composition. The corresponding epoxy resins are known and are also described further with respect to components (Ia1) and (IIb). Preferred epoxy resins have an epoxy equivalent weight of less than 400 g / mol, preferably 100 to less than 400 g / mol, more preferably 150-300 g / mol.
[0080] The proportion of other resin components is, for example, 15 to 40% by weight, more preferably 20 to 30% by weight, based on the solid content of the coating composition.
[0081] Preferably, the molar ratio of the NH functional groups of the resin component (I) to the epoxy groups of the other resin components is 0.7:1 to 0.95:1, for example 0.9:1.
[0082] It follows directly from the above statements that the aqueous dispersion (AD) comprising the resin component (R) and the at least one further resin component having epoxy groups is present in different essential components of the components present in any case in the composition (binder component (1) and curing component (2)).
[0083] 2K coating compositions are aqueous, ie contain at least water as solvent. The exact definition of "aqueous" has been described further above.
[0084] 2K coating compositions preferably comprise further ingredients, in particular those which are suitable as surfacers or primer-surfacers. Pigments and fillers should especially be mentioned in this context.
[0085] Preferred pigment is black and / or white pigment.Therefore, priming paint preferably contains at least one black pigment or at least one white pigment or at least one white pigment and a black pigment.This means that priming paint of the present invention preferably has black, white or (various grayscales) gray.Certainly, it is not impossible to have other pigments.
[0086] Preferred black pigments are typical organic and inorganic black pigments, especially inorganic black pigments, which are commercially available in powder form. Particular mention should be made of pigment black (carbon black), iron oxide (Fe3O4) pigments such as typical synthetic iron oxides (available, for example, under the trade name Bayferrox from Lanxess), mixed oxide pigments such as manganese black or spinel black. Very particular preference is given to pigment black (carbon black) and iron oxide pigments.
[0087] Preferred white pigments are typical inorganic white pigments, such as titanium dioxide (for example the rutile pigment known under the Kronos trade name from Kronos), zinc oxide, zinc sulfide or antimony trioxide. Very particular preference is given to titanium dioxide, especially in its rutile modification.
[0088] Further preferred pigments are those known under the umbrella term "anticorrosive pigments". Zinc phosphate is particularly preferred here. Although zinc phosphate has a white color, it is not classified as a white pigment but as an anticorrosive pigment due to its anticorrosive effect.
[0089] The proportion of the pigments is preferably 15 to 25% by weight, in particular 20% by weight, based in each case on the solids content of the coating composition.
[0090] The fillers preferably present are all inorganic and organic fillers known per se and well known to the person skilled in the art, preferably inorganic fillers. Thus, fillers include in particular substances known to the person skilled in the art, which are used, for example, in particulate form or in powder form to obtain specific physical properties of the coating composition and which are insoluble in the corresponding medium of use. These include in particular carbonates such as calcium carbonate or barium carbonate, sulfates such as calcium sulfate and barium sulfate, silicates and phyllosilicates such as talc, pyrophyllite, mica, kaolin, precipitated calcium silicate, aluminum silicate, calcium / aluminum silicate, sodium / aluminum silicate and mullite, silicon dioxide such as quartz, cristobalite, precipitated silicon dioxide or in particular pyrogenic silicon dioxide obtainable, for example, under the trade name Aerosil (from Evonik), metal oxides and hydroxides, for example aluminum hydroxide and magnesium hydroxide.
[0091] The proportion of fillers is preferably from 30 to 50% by weight, in particular from 30 to 40% by weight, in each case based on the solids content of the coating composition.
[0092] In addition, the coating composition may also contain at least one additive. Examples of such additives are light stabilizers, antioxidants, degassing agents, emulsifiers, slip additives, polymerization inhibitors, adhesion promoters, leveling agents, film-forming aids, thickeners, sag control agents (SCA) or corrosion inhibitors. They are used in conventional and known amounts. The same applies to the possible use of organic solvents, but their amounts are selected so that they do not change the aqueous characteristics of the coating composition.
[0093] The solids content of the 2K coating composition can vary depending on the requirements of the individual case, but is preferably 70-85% by weight. The solids content is primarily determined by the viscosity required for application, more particularly spray application, and can therefore be adjusted by the person skilled in the art based on his or her general technical knowledge, optionally with the aid of a few exploratory tests.
[0094] The 2K coating composition can be prepared using conventional and known mixing methods and mixing units for preparing coating compositions, such as stirred tanks, stirred mills, extruders, kneaders, Ultraturrax, inline dissolvers, static mixers, toothed ring dispersers, expansion nozzles and / or microfluidizers. Of course, it should be pointed out that component (1) (binder component) and component (2) (curing component) are prepared and stored separately from one another and, as described above, are combined and mixed only immediately before the coating composition is applied to the substrate.
[0095] The present invention further provides a method for preparing a coating on a substrate, wherein the coating composition of the present invention is applied to the substrate and then a coating film is formed. It should be understood that in the context of the method of the present invention using the coating composition, the above-mentioned specific and preferred embodiments of the coating composition are equally applicable.
[0096] The coating composition of the invention can be applied to the substrate in particular in the layer thicknesses customary in the automotive industry, for example 5 to 200 μm, preferably 10 to 150 μm, more preferably 30 to 70 μm. The layer thickness is to be understood as the dry film layer thickness after curing as described below. For example, known methods are used here, such as spraying, scraping, painting, pouring, dipping, immersion, dripping or rolling. Preferably, a spraying method is used.
[0097] After applying the composition of the present invention, a polymer film or a cured coating film is formed therefrom. Thus, the applied composition is cured by known methods. Curing is carried out at a temperature of, for example, 15-120° C., in particular 20-80° C., most preferably 20-65° C. These preferred relatively low curing temperatures are in particular due to the fact that the coating composition is a (2K) coating composition, in which case, in particular, only a low curing temperature is required for thermal crosslinking. The curing time can vary very significantly in each case, for example between 5 minutes and 16 hours, preferably between 20 minutes and 80 minutes. These preferred shorter curing times are in particular caused by the fact that the composition of the present invention only requires a shorter curing time at still lower temperatures in order to have sufficient hardness to enable the cured coating to be polished. In this respect, a very particularly preferred curing operation is carried out at 40-65° C. for 20-80 minutes.
[0098] In each case, prior to curing, a flash evaporation may optionally be carried out, for example at room temperature (about 15 and 25° C.), for example for 1 to 60 minutes. In the context of the present invention, flash evaporation means the evaporation of organic solvents and / or water, as a result of which the paint dries but has not yet cured, more particularly has not yet formed a completely crosslinked coating film.
[0099] Curing then provides the coated substrate of the invention, which likewise forms part of the subject matter of the present invention. The invention also provides a coating produced from the composition.
[0100] Substrates used are, for example, metal substrates, preferably those used in the automotive industry (vehicle construction). Advantageously, unalloyed and alloyed steels and / or iron, zinc and aluminum substrates and the corresponding alloys are used.
[0101] If it is stated above that the composition is applied to a substrate, this does not, however, necessarily mean that the composition must be applied directly to a metal substrate. Instead, there may be at least one further layer between the metal substrate and the layer formed by the composition. This is the case, for example, when the coating composition is used as a surfacer in OEM finishing. This is because in this case there is at least one electrocoat layer between the surfacer layer and the metal substrate. In other words, the substrate to which the composition of the invention is applied is therefore a metal substrate coated with an electrocoat layer.
[0102] However, as mentioned above, the coating compositions of the invention can be used particularly advantageously as primer-surfacers in the recoating sector, in particular in the automotive recoating sector, and in this case, after only a short curing period at moderate temperatures, have properties such as good adhesion, corrosion protection and sandability.
[0103] Therefore, in a particular embodiment of the present invention, the substrate is a metal substrate that has been completely painted, especially those painted with a multi-layer automotive paint system, wherein each multi-layer coating has local damage (defects). More particularly, these are automobile bodies or parts thereof with damage such as stone chip damage, etc. Therefore, in the damaged area, the initial multi-layer coating has been at least partially separated by external action. Then, the coating composition of the present invention is used as a first-stage mixed primer for the repair of these damaged areas, i.e., recoating. Usually, in the recoating operation, before applying the primer, the damaged initial coated substrate is cleaned and polished. This removes any only insufficiently bonded and partially separated areas of the initial coating present and / or the corrosion products that have been formed, and especially also locally exposes the metal substrate. Therefore, this is a complex substrate surface with a wide range of different interfaces. One interface here is the interface with the fully exposed metal substrate. Other interfaces and edges can be found in the areas between the damaged, cleaned and polished parts and in the areas around these parts with a complete initial paint system. At all these interfaces, the same coating composition must be used to ensure sufficient adhesion. The composition of the invention therefore offers great advantages since even in such demanding areas excellent adhesion, corrosion resistance and grindability are achieved.
[0104] In a preferred embodiment of the present invention, after the cured coating, especially the surfacer or the first surfacer mixed primer layer, is prepared from the composition of the present invention, other coating compositions are applied and a multi-coat paint system is formed. These other coating compositions are especially standard basecoats and clearcoats.
[0105] The present invention will be explained below by way of examples. Example
[0106] Determination method
[0107] The proportion of monomer amine in aqueous dispersion
[0108] The determination is carried out by gas chromatography in accordance with DIN 51 405:
[0109] The sample was directly injected into a split injector of a gas chromatograph with a flame ionization detector and separated on a column with a polar phase (polyethylene glycol; 50 m fused silica capillary column with polyethylene glycol phase) and a non-polar phase (polydimethylsiloxane; 50 m fused silica capillary column with polydimethylsiloxane phase). Evaluation was performed by the ISTD% method.
[0110] On an analytical balance, weigh approximately 100-500 mg of sample (depending on the amine content) accurately to 0.1 mg into a 5 mL snap-top vial. Weigh approximately 5% ISTD diglyme accurately to 0.1 mg and add to the sample. Dilute the sample with 5 mL of THF. (If the sample is not soluble in THF, a suitable solvent must be found experimentally.)
[0111] The samples thus prepared were analyzed on an Agilent 7890 gas chromatograph. Injections were performed by autosampler.
[0112] Gas chromatography conditions:
[0113] Oven program: 40°C (holding time 5 minutes) (3°C / minute) → 100°C (10°C / minute) → 230°C (holding time 5 minutes)
[0114] Carrier gas: Hydrogen
[0115] Separation columns: Agilent Innowax: length 50 m, membrane thickness 0.2 μm, diameter 0.2 mm, pressure 1.0 bar, HP-1, length 50 m, membrane thickness 0.33 μm, diameter 0.2 mm, pressure 1.3 bar
[0116] Injector temperature: 250°C (lower if necessary)
[0117] Injection volume: 0.3μL (manual injection 0.3-0.6μL)
[0118] Detector: Flame ionization detector
[0119] Detector temperature: 275°C
[0120] Split flow: 15mL / min
[0121] The amines are identified by their retention times on polar and nonpolar columns (see comparative chromatograms). For unknown components, GC / MS analysis is necessary.
[0122] The amines to be tested and the internal standard are weighed accurately to 0.1 mg, according to the approximate proportion in the sample on an analytical balance. The amine concentration in the total calibration solution corresponds to the amine concentration in the prepared sample (the concentration of the amine is calculated by the GC analyzer program). Subsequently, the calibration solution is analyzed under the same conditions as the samples and the substance-specific correction factor is determined.
[0123] The amine content of the samples was calculated by the ISTD% method with the aid of the GC analyzer program.
[0124] Epoxy equivalent
[0125] The determination was carried out in accordance with DIN EN ISO 3001.
[0126] Solid content (non-volatile components)
[0127] Unless otherwise stated, the solids content (also called solids fraction, solids content, non-volatile fraction) is determined in accordance with DIN EN ISO 3251 at 130° C.; 60 minutes, starting weight 1.0 g.
[0128] Ratio of polymerized organic amine (polymerized amine) in aqueous dispersion
[0129] The determination is carried out similarly to the determination of the solids content, except that the sample is kept at 130° C. for 8 hours (instead of 60 minutes). In this way, it is ensured that the residual proportion of any non-volatile monomeric amine (M) is negligibly small and that the measurement result corresponds to the parameters assigned to this result.
[0130] Ratio of the resin mixture (I) or the resin components in the aqueous dispersion
[0131] This ratio results from the sum of the monomeric amine ratio and the polymeric amine ratio in the aqueous dispersion.
[0132] The proportion of monomeric amine or polymeric amine in the resin mixture (I) or the resin component (R)
[0133] The proportion of monomeric amines in the resin mixture (I) or the resin component (R) is obtained by dividing the proportion of monomeric amines in the aqueous dispersion by the sum of the proportion of monomeric amines and the proportion of polymeric amines in the aqueous dispersion. The proportion of polymeric amines is determined in a corresponding manner.
[0134] NH equivalent
[0135] The NH equivalent of the resin component (R) and the resin mixture (I) is determined in the following continuous manner.
[0136] a)
[0137] First, the NH equivalent weight of the resin mixture (I) present in the aqueous dispersion is determined. For this purpose, firstly, the different mass ratios of primary and secondary amino groups in the aqueous dispersion (each in % nitrogen) are determined by the aliphatic amine method according to DIN EN ISO 9702 (October 1998). The mass ratios obtained are then used to obtain the molar amount of NH functional groups in 100 g of the aqueous dispersion by the following calculation:
[0138] n(NH)=(m(N from primary amino groups) / (14 g / mol))*2+m(N from secondary amino groups) / (14 g / mol) (wherein "m" represents the mass ratio measured in each case).
[0139] The molar amount of NH functional groups and the mass of the sample (100 g) ultimately lead to the NH equivalent weight of the sample (aqueous dispersion), ie the mass of the sample in which 1 mol of NH functional groups is present.
[0140] By determining the ratio of the resin mixture of the sample, the NH equivalent weight of the resin mixture (I) can then be calculated:
[0141] (NH equivalent (resin mixture (I)) = NH equivalent (sample) * ratio (resin mixture in sample)
[0142] The proportion of the resin mixture in the sample is expressed as the sum of the polymeric amine proportion and the monomeric amine proportion (see above).
[0143] b)
[0144] The NH equivalent of the resin component (R) is then calculated from the previously determined NH equivalent of the resin mixture (I), the mass of the resin mixture (I) used in step (B), the mass of the component (IIb) used in step (II) and the molar amount of epoxy groups used in the component (IIb) (determined by the mass of the component (IIb) used and the epoxy equivalent). This assumes that the epoxy groups react quantitatively with the NH functional groups. The total mass of the resin component (R) is obtained by adding the mass of the resin mixture (I) used and the mass of the component (IIb) used. Aqueous dispersions according to the invention (AD) and comparative dispersions c (AD)
[0145] Aqueous dispersion (AD1)
[0146] 683.00 g of Beckopox VEH 2849W (aqueous dispersion of resin mixture (I), the resin mixture containing 27.5% by weight of monomeric amines (isophoronediamine and xylylenediamine) and 72.5% by weight of polymeric amines, and additionally having an NH equivalent of 108 g / mol) and 1663.77 g of demineralized water were combined in a reaction vessel, stirred continuously and kept at 95° C. for 1 hour. Subsequently, the mixture was cooled to 70° C., 163.44 g of a mixture of bisphenol A diglycidyl ether epoxy resin having an average epoxy equivalent of 186.5 g / mol, 39.46 g of a polyalkylene polyether epoxide based on polypropylene oxide having an average epoxy equivalent of 395 g / mol, and 81.96 g of ethoxypropanol were added; 81.47 g of methyl ethyl ketone and 81.72 g of isobutanol were metered in continuously over a period of 4 hours while stirring, and the mixture was kept at 70° C. for a further hour. The reaction product thus obtained was cooled to 45° C. The viscosity of the product was 150-250 mPas at 25° C.
[0147] In a subsequent process step, the process solvents isobutanol and methyl ethyl ketone were removed from the product by distillation under reduced pressure. The resulting aqueous dispersion (AD1) had a residual content of isobutanol and methyl ethyl ketone of <0.5% (gas chromatography).
[0148] The resin component (R) content in the aqueous dispersion was 33.4 wt% (2.4 wt% monomeric amine, 31% polymeric amine). Therefore, the resin component had a monomeric amine (M) content of 7.2 wt%. In addition, the resin component had an amine equivalent (NH equivalent) of 171 g / mol.
[0149] Aqueous dispersion (AD2)
[0150] 683.00 g of Beckopox VEH 2849W (an aqueous dispersion of a resin mixture (I) containing 27.5% by weight of monomeric amines (isophoronediamine and xylylenediamine) and 72.5% by weight of polymeric amines, and additionally having an NH equivalent of 108 g / mol), 266.11 g of methyl ethyl ketone and 1395.96 g of (softened) water were combined in a reaction vessel, stirred continuously and kept at 70° C. for 1 hour. Subsequently, a mixture of 163.44 g of a bisphenol A diglycidyl ether epoxy resin having an average epoxy equivalent of 186.5 g / mol, 39.46 g of a polyalkylene polyether epoxide based on polypropylene oxide having an average epoxy equivalent of 395 g / mol, and 81.96 g of ethoxypropanol was added; 81.47 g of methyl ethyl ketone and 81.72 g of isobutanol were metered in continuously over a period of 4 hours while stirring, and the mixture was kept at 70° C. for a further hour. The reaction product thus obtained was cooled to 45° C. The viscosity of the product was 150-250 mPas at 25° C.
[0151] In a subsequent process step, the process solvents isobutanol and methyl ethyl ketone were removed from the product by distillation under reduced pressure. The resulting aqueous dispersion (AD2) had a residual content of isobutanol and methyl ethyl ketone of <0.5% (gas chromatography).
[0152] The content of the resin component (R) in the aqueous dispersion was 33 wt% (2.4 wt% of monomeric amine, 31% of polymeric amine). Therefore, the resin component had a monomeric amine (M) content of 7.2 wt%. In addition, the resin component had an amine equivalent (NH equivalent) of 171 g / mol.
[0153] Aqueous dispersion (AD3)
[0154] Step (A)
[0155] 1000 g of a polyalkylene polyether monoamine based on propylene oxide / ethylene oxide (Jeffamine M2070, primary amine functional groups (=2 NH functional groups)) with an average molecular weight of 2000 g / mol and 448.8 g of a bisphenol A diglycidyl ether-based epoxy resin with an average epoxy equivalent of 186.5 g / mol were mixed in a reaction vessel, and then the internal temperature was maintained at 130° C. for 1 hour and at 80-90° C. for a further 2 hours. The epoxy equivalent of the product thus obtained was 1035 g / mol. The viscosity of the product was 6734 mPas at 23° C.
[0156] 96.43 g of the reaction product thus obtained were mixed with 33.9 g of isophorone diamine and 27.12 g of meta-xylylenediamine in a reaction vessel and then kept at an internal temperature of 60° C. for 1 hour and at 80-90° C. for a further 2 hours. After cooling to 50° C., dilution with water (solids content 80%) was carried out. The resin mixture (I) present in the dispersion had an amine equivalent (NH equivalent) of 105 g / mol. The viscosity of the product was 1540 mPas at 23° C.
[0157] Step (B)
[0158] 683.00 g of the reaction product of step (A) and 1663.768 g of (demineralized) water were combined in a reaction vessel, stirred continuously and kept at 95° C. for 1 hour. Subsequently, the mixture was cooled to 70° C., 163.44 g of a mixture of bisphenol A diglycidyl ether epoxy resin having an average epoxy equivalent of 186.5 g / mol, 39.46 g of a polyoxypropylene-based polyalkylene polyether epoxide having an average epoxy equivalent of 395 g / mol, and 81.96 g of ethoxypropanol were added; 81.47 g of methyl ethyl ketone and 81.72 g of isobutyl alcohol were metered in continuously over a period of 4 hours while stirring, and the mixture was kept at about 70° C. for a further hour. The reaction product thus obtained was cooled to 45° C. The viscosity of the product was 150-250 mPas at 25° C.
[0159] In the subsequent process step, the process solvents isobutanol and methyl ethyl ketone were removed from the product by distillation under reduced pressure. The residual content of isobutanol and methyl ethyl ketone in the resulting aqueous dispersion (AD3) was <0.5% (gas chromatography). The resin component had an amine equivalent weight (NH equivalent) of 177 g / mol.
[0160] c(AD2)
[0161] 1200 g (1.2 mol or 2.4 OH equivalents) of an ethylene oxide-based polyalkylene polyether having an average molecular weight of 1200 g / mol and 1984.62 g (10.67 epoxy equivalents) of a bisphenol A diglycidyl ether-based epoxy resin having an average epoxy equivalent weight of 186.5 g / mol were mixed in a reaction vessel and the internal temperature was then raised to 120-130° C. with continuous stirring. Subsequently, 6.5 g of Anchor 1040 (BF3-monoethylamine catalyst) was added and the temperature was further raised to 160° C. and maintained at 160° C. for a further 4 hours until an epoxy equivalent weight of 417 g / mol was reached. The mixture was then cooled to 55° C. and 82.549 g of di-n-propylamine was added. Stirring was continued at 55° C. until an EEW of 482 g / mol was reached. The mixture was then heated to 60° C. and another 174.11 g of (demineralized) water was added.
[0162] 1605.22 g of isophorone diamine (corresponding to 9.4 mol or 37.77 NH equivalents) and 575.96 g of meta-xylylenediamine (corresponding to 4.2 mol or 16.91 NH equivalents) were mixed in a reactor and heated to an internal temperature of 60° C. Subsequently, 3447.78 g of the above reaction product were added over 30 minutes with continuous mixing. This raised the internal temperature to about 75° C., and stirring was continued at this temperature for 90 minutes. Then, n-butyl glycidyl ether was added over 20 minutes with stirring. This raised the internal temperature to about 80° C., and stirring was continued at this temperature for 60 minutes. Then, a further 1374 g of (demineralized) water were added, which cooled the product to 40° C.
[0163] The resin mixture present in the reaction mixture had an amine equivalent weight (NH equivalent weight) of 125 g / mol.
[0164] c(AD3)
[0165] 897.41 g of c (AD2) and 1868.00 g of demineralized water were heated to 95° C. in a reactor while stirring. The mixture was subsequently cooled to 70° C., 163.44 g (0.437 mol) of a mixture of bisphenol A diglycidyl ether epoxy resin having an average epoxy equivalent of 186.5 g / mol, 39.46 g 44 g of a polyalkylene polyether epoxide based on polyoxypropylene having an average epoxy equivalent of 395 g / mol, and 81.96 g of ethoxypropanol were added; 81.47 g of methyl ethyl ketone and 81.72 g of isobutanol were metered in over 2 hours, and the mixture was kept at about 70° C. for a further hour.
[0166] The reaction product thus obtained was cooled to 45° C. The viscosity of the product was 150-500 mPas at 25° C.
[0167] In a subsequent process step, the process solvents isobutanol and methyl ethyl ketone are removed from the product by distillation under reduced pressure. The residual content of isobutanol and methyl ethyl ketone in the resulting aqueous dispersion is <0.5%.
[0168] The resin mixture present in the dispersion had an amine equivalent weight (NH equivalent) of 203 g / mol.
[0169] c(AD6)
[0170] Dispersion c (AD6) was prepared analogously to step (A) of dispersion (AD3), except that only meta-xylylenediamine was used instead of a mixture of isophoronediamine and meta-xylylenediamine. The proportion of meta-xylylenediamine was increased accordingly to ensure that the same molar amount of monomeric amine was used.
[0171] The resin mixture present in the dispersion had an amine equivalent weight (NH equivalent weight) of 100 g / mol.
[0172] Table A gives a further overview of the prepared aqueous dispersions. In addition, further commercially available dispersions used as further comparative dispersions c(AD) in aqueous coating compositions are listed (see below).
[0173] Table A:
[0174]
[0175]
[0176] Coating compositions of the present invention and comparative coating compositions
[0177] Various inventive and comparative coating compositions were prepared by the following general preparation method.
[0178] The base component (1) and curing component (2) of the coating composition are prepared by combining the ingredients and mixing thoroughly in a dissolver and optionally a bead mill. The ingredients and their amounts can be found in Tables B and C below.
[0179] To prepare the coating composition itself, the binder components are each mixed with the curing components and optionally additional water. Within 1 hour of completion, the composition is used as described below, ie, it is applied to a substrate and subsequently cured.
[0180] Table B: Coating compositions having a binder component comprising an aqueous dispersion (AD) and c(AD)
[0181]
[0182]
[0183] Added water I1 I2 C1 I3 C2 C3 C4 Weight Weight Weight Weight Weight Weight Weight water 15.5 12.0 16.0 17.0 6.5 13.0 0.0
[0184] index I1 I2 C1 I3 C2 C3 C4 Pigment to Binder Ratio (P / B) 1.6 1.4 1.0 1.4 1.4 1.1 0.8 DIN4 flow time, seconds 19 20 20 20 20 20 23
[0185] Table C: Coating compositions having a binder component containing an epoxy resin
[0186]
[0187]
[0188] Curing components I4 I5 C5 C6 I6 C7 C8 Element Weight Weight Weight Weight Weight Weight Weight (AD1) 54.81 (AD2) 56.81 (AD3) 65.38 c(AD6) 31.35 c(AD1) 33.09 c(AD2) 19.31 c(AD3) 62.81 Butyl glycol 1.22 1.21 0.69 0.72 1.21 0.95 1.58 Halox 570 0.60 0.61 0.34 0.36 0.61 0.47 0.79 water 4.26 1.97 1.92 2.03 26.67 13.83 Total curing agent 60.9 60.6 34.3 36.2 67.2 47.4 79.0
[0189] Added water I4 I5 C5 C6 I6 C7 C8 Weight Weight Weight Weight Weight Weight Weight water 0 0 11 5 0 2 0
[0190] index I4 I5 C5 C6 I6 C7 C8 Pigment to Binder Ratio (P / B) 1.1 1.1 1.4 1.4 1.1 1.2 1.0 DIN4 flow time, seconds 24 24 24 24 26 24 16
[0191] Preparation of coating using the coating composition
[0192] Polishability
[0193] To test the suitability of a coating composition as a primer-surfacer or to determine the sanding characteristics, coatings were prepared by the following preparation method and then examined for sanding properties.
[0194] The substrates used were steel plates (60 cm x 50 cm). These were pre-treated / cleaned as follows: cleaned with 360-4 Glaurit metal cleaner, polished with a P80 die from Mirka, cleaned again to remove polishing dust with 360-4 Glaurit. Exhaust for 15 minutes.
[0195] The coating composition was stirred and applied to the substrate with a standard spray gun (e.g. SATA 100B F 1.6 mm RP, 2.0 bar) in a thin continuous spraying operation, flashed for 5 minutes, applied in a further full spraying operation, flashed for 10 minutes and then cured in an oven at a temperature of 60° C. or at room temperature for different time periods (35-60 minutes) of 14-16 hours. In each case, the layer thickness was 60-80 μm (Dualscope MP40, ED10 probe, from Fischer).
[0196] After curing, the coating or coated substrate was stored at 20°C for 20 minutes and then its properties were checked.
[0197] For this purpose, 09560 black control powder (from 3M) was applied to the coated surface and dry-ground by means of an Excenter (FESTOOL LEX3), 5 mm stroke and sandpaper from RODIM (standard P400 type) until the black control powder was completely removed.
[0198] The grindability was evaluated as follows:
[0199] Polishability evaluation:
[0200] Sandpaper reviews:
[0201] 0 → No clogging (very good sandability)
[0202] 1 → Minimal clogging (sandability is still acceptable)
[0203] 2 → Blockage, forming small "nodules" (poor polishability)
[0204] 3 → Severe clogging, formation of "nodules" (spacers) (very poor polishability)
[0205] By using a black control powder, clogging of the paint on the sandpaper is very easy to identify. No clogging means that the sanded material is obtained in the form of a fine dust and therefore does not clog the sandpaper and does not lead to difficult-to-remove residues on the coating surface.
[0206] The results are shown in Tables D and E. The letter "B" preceding each coating composition indicates that the coating was a cured coating.
[0207] Table D: Grinding results
[0208] CI1 CI2 CC1 CI3 CC2 CC3 CC4 Drying time, minutes 35 35 35 40 40 40 40 Drying temperature, °C 60 60 60 60 60 60 60 Polishing results 0 1 3 0 3 2 3
[0209] The results show that the coatings according to the invention (produced from the coating compositions according to the invention) have significantly improved sandability. In particular, a comparison of the systems according to the invention with the CC1 system shows that the epoxy post-modification of the commercial product Beckopox VEH 2849 and the associated increase in the NH equivalent weight (and therefore also the molecular weight) lead to a significant improvement in sandability. The use of the commercial product Beckopox EH 613 (c(AD4)) with an NH equivalent weight that is too low also does not lead to satisfactory results in terms of sandability (CC3). The same applies to the use of Beckopox EH 623w (c(AD5)), which contains acrylonitrile in the amine component. In particular, the CC4 system also shows that the use of epoxy resins with an epoxy equivalent weight that is too high (450 g / mol) leads to poor sandability.
[0210] Table E: Grinding results:
[0211] I4 I5 C5 C6 I6 C7 C8 Drying time, minutes 40 40 40 40 40 40 40 Drying temperature, °C 60 60 60 60 60 60 60 Polishing results 0 0 3 3 3 3 3 Drying time, minutes 50 50 50 50 50 50 50 Drying temperature, °C 60 60 60 60 60 60 60 Polishing results 3 2 1 3 3 Drying time, minutes 60 60 60 60 60 60 60 Drying temperature, °C 60 60 60 60 60 60 60 Polishing results 3 0 0
[0212] Once again, the results clearly show that the systems according to the invention lead to improved sandability. While systems I4 and I5 already have the best sandability at a drying time of only 40 minutes, system I6 has acceptable sandability at least at a drying time of 50 minutes. In absolute terms, all comparative systems have insufficient or poor sandability at a drying time of 50 minutes.
[0213] Other research
[0214] In addition, using the coating composition, multi-layer paint systems (using standard basecoat and clearcoat) were also prepared, and in addition, the coating composition was used as a first surface mixed primer to repair a previously prepared multi-layer paint system with defects. In the latter case, the coating composition was applied to the multi-layer paint system with defects in the defect area on the metal substrate, cured and polished. Then the basecoat and clearcoat were applied. The system of the present invention leads to excellent adhesion of the overall structure and therefore has the best applicability.
Claims
1. An aqueous resin dispersion (AD) comprising a resin component (R), the resin component (R) comprising at least one di- and / or polyfunctional monomeric primary and / or secondary amine (M) and a polyfunctional polymeric organic amine having primary and / or secondary amino groups, wherein the resin component (R) has an NH equivalent of 150-400 g / mol and a weight proportion of 5-15 wt % of di- and / or polyfunctional monomeric organic amine (M), The polyfunctional polymeric organic amines having primary and secondary amino groups also include the following in mutually reactive form: (i) at least one di- and / or polyfunctional organic epoxy compound, wherein the epoxy compound has an average epoxy equivalent weight of less than 400 g / mol, (ii) at least one monomeric amine (M), and (iii) at least one compound XR, in which X is a functional group reactive toward epoxy groups and R is an organic radical containing polyoxyalkylene units and not containing any other X groups, And wherein the amine (M) comprises at least 65 mol % of an amine consisting of amino and hydrocarbon units.
2. The aqueous resin dispersion (AD) according to claim 1, wherein the amine (M) is a difunctional primary and / or secondary amine.
3. The aqueous resin dispersion (AD) according to claim 2, wherein the amine (M) is a difunctional primary amine.
4. The aqueous resin dispersion (AD) according to claim 1, wherein the resin component (R) has an NH equivalent weight of 170-250 g / mol.
5. The aqueous resin dispersion (AD) according to claim 2, wherein the resin component (R) has an NH equivalent weight of 170-250 g / mol.
6. The aqueous resin dispersion (AD) according to any one of claims 1 to 5, wherein the X group in compound (iii) is a primary amino group.
7. The aqueous resin dispersion (AD) according to claim 6, wherein compound (iii) is a primary polyoxyalkylene monoamine.
8. The aqueous resin dispersion (AD) according to any one of claims 1 to 5, wherein the at least one di- and / or polyfunctional organic epoxy compound of component (i) has an average epoxy equivalent weight of less than 250 g / mol.
9. The aqueous resin dispersion (AD) according to claim 7, wherein the at least one di- and / or polyfunctional organic epoxy compound of component (i) has an average epoxy equivalent weight of less than 250 g / mol.
10. An aqueous resin dispersion (AD) as claimed in any one of claims 1 to 5, wherein the polymeric organic amine consists of components (i), (ii) and (iii).
11. The aqueous resin dispersion (AD) as claimed in any one of claims 1 to 5, wherein the resin component (R) consists of at least one di- and / or polyfunctional monomeric primary and / or secondary amine (M) and a polyfunctional polymeric organic amine having primary and / or secondary amino groups.
12. The aqueous resin dispersion (AD) as claimed in any one of claims 1 to 5, wherein the amine (M) comprises at least 75 mol % of amine consisting of amino and hydrocarbon units.
13. The aqueous resin dispersion (AD) according to claim 12, wherein the amine (M) comprises at least 90 mol % of amine consisting of amino and hydrocarbon units.
14. The aqueous resin dispersion (AD) according to claim 13, wherein the amine (M) comprises 100 mol % of an amine consisting of amino and hydrocarbon units.
15. A water-based two-component coating composition comprising a base component (1) and a curing component (2), in: I) the base component (1) comprises at least one aqueous dispersion as claimed in any one of claims 1 to 14, and the curing component (2) comprises at least one epoxy resin, wherein the epoxy resin has an average epoxy equivalent weight of less than 400 g / mol, or II) The base component (1) comprises at least one epoxy resin, wherein the epoxy resin has an average epoxy equivalent weight of less than 400 g / mol, and the curing component (2) comprises at least one aqueous dispersion according to any one of claims 1 to 14.
16. The coating composition according to claim 15, Features The coating composition is a surfacer or a top-surfacer.
17. A method of preparing a cured coating on a substrate, wherein a coating composition as claimed in claim 15 or 16 is applied to a substrate and then cured.
18. A method of repairing a multi-layer paint system having defects, comprising applying the coating composition of claim 15 or 16 in the defective area, curing the composition to produce a cured coating, and then sanding the cured coating.
19. A coating prepared by the method of claim 17 or 18.