Rubber composition, vulcanized product and vulcanized molded product
By mixing chloroprene rubber with maleimide compounds and organic peroxides, a vulcanized compound with excellent heat resistance, low heat build-up and compression permanent deformation resistance is produced, which solves the vulcanization problems in the existing technology. It solves the problems of insufficient heat resistance and low heat build-up, and is suitable for a variety of industrial rubber parts.
Patent Information
- Application Number
- CN202080037182.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-08-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-12
AI Technical Summary
It has been difficult to provide a vulcanized product of chloroprene rubber having excellent heat resistance and low heat build-up properties with the prior art.
By mixing chloroprene-based rubber with a specific amount of a maleimide compound and an organic peroxide, a vulcanized product with excellent heat resistance, low heat build-up, and compression set resistance is produced.
It has improved the heat resistance, low heat generation and compression permanent deformation resistance of the sulfide, and is suitable for various industrial rubber parts.
Smart Images

Figure BDA0003362727610000211
Abstract
Description
Technical Field
[0001] The present invention relates to a rubber composition, a vulcanized product, a vulcanized molded product, and the like. Background Art
[0002] Chloroprene rubber has excellent mechanical properties, ozone resistance, chemical resistance, etc., and is used in a wide range of fields such as automobile parts, adhesives, and various industrial rubber parts by taking advantage of its characteristics. As a technology that can use chloroprene rubber, the rubber compositions described in the following Patent Documents 1 to 3 are known.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2016-23191
[0006] Patent Document 2: Japanese Patent Application Publication No. 2012-111899
[0007] Patent Document 3: Japanese Patent Application Laid-Open No. 9-268239 Summary of the invention
[0008] Problems to be solved by the invention
[0009] There is a demand for a rubber composition containing chloroprene rubber to provide a vulcanized product having excellent heat resistance and low heat generation (low heat generation property).
[0010] One aspect of the present invention is to provide a rubber composition that can produce a vulcanized product having excellent heat resistance and low heat build-up. Another aspect of the present invention is to provide a vulcanized product of the rubber composition. Another aspect of the present invention is to provide a vulcanized molded product of the rubber composition.
[0011] Means for solving problems
[0012] The inventors of the present application have conducted intensive studies to solve the above problems and have succeeded in obtaining a vulcanized product having excellent heat resistance and low heat build-up by mixing a specific amount of a maleimide compound and an organic peroxide with a chloroprene rubber, thereby completing the present invention.
[0013] One aspect of the present invention relates to a rubber composition comprising 100 parts by mass of a chloroprene rubber, 0.50 to 4.0 parts by mass of a maleimide compound, and 0.10 to 2.0 parts by mass of an organic peroxide.
[0014] Another aspect of the present invention relates to a vulcanized product of the rubber composition described above. Another aspect of the present invention relates to a vulcanized molded product of the rubber composition described above.
[0015] Effects of the Invention
[0016] One aspect of the present invention is to provide a rubber composition that can produce a vulcanized product having excellent heat resistance and low heat build-up. Another aspect of the present invention is to provide a vulcanized product of the rubber composition. Another aspect of the present invention is to provide a vulcanized molded product of the rubber composition. DETAILED DESCRIPTION
[0017] Hereinafter, a mode for carrying out the present invention will be described. It should be noted that the embodiment described below is an example showing a representative embodiment of the present invention, and the present invention is not limited to the embodiment described below.
[0018] "Above A" in the numerical range refers to A and the range exceeding A. "Below A" in the numerical range refers to A and the range less than A. In the numerical ranges recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range of other stages. In the numerical ranges recorded in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment. The so-called "A or B" can include either A and B, or both. Unless otherwise specified, the materials exemplified in this specification can be used alone or in combination of two or more. With respect to the content of each component in the composition, when there are multiple substances belonging to each component in the composition, unless otherwise specified, it refers to the total amount of the multiple substances present in the composition. Terms such as "process" not only refer to independent processes, but also include them in this term as long as the desired effect of the process can be achieved when it cannot be clearly distinguished from other processes. "(Meth)acrylate" refers to at least one of acrylate and its corresponding methacrylate. The same applies to "(meth)acrylic acid" and other similar expressions.
[0019] <Rubber Composition>
[0020] The rubber composition according to the present embodiment contains (1) 100 parts by mass of chloroprene (2-chloro-1,3-butadiene)-based rubber, (2) 0.50 to 4.0 parts by mass of a maleimide compound, and (3) 0.10 to 2.0 parts by mass of an organic peroxide. The rubber composition according to the present embodiment can provide a vulcanized product having excellent heat resistance and low heat build-up properties as a vulcanized product obtained by vulcanizing the rubber composition.
[0021] The inventors of the present application have succeeded in obtaining a vulcanized product having excellent heat resistance, low heat build-up and excellent compression set resistance by mixing the above-mentioned specific amounts of maleimide compounds and organic peroxides with chloroprene rubber. The rubber composition involved in this embodiment can also obtain a vulcanized product having excellent heat resistance, low heat build-up and excellent compression set resistance.
[0022] (1) Chloroprene rubber
[0023] Chloroprene rubber has a structural unit derived from chloroprene and has chloroprene as a monomer unit (chloroprene monomer unit). Chloroprene polymers include homopolymers of chloroprene, copolymers of chloroprene (copolymers of chloroprene and a monomer copolymerizable with chloroprene), etc., and mixtures of these polymers may also be used. The polymer structure of the polymer is not particularly limited.
[0024] Examples of monomers copolymerizable with chloroprene include (meth)acrylic acid esters (methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.), (meth)acrylic acid hydroxyalkyl esters (2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.), 2,3-dichloro-1,3-butadiene, 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, acrylonitrile, etc. The monomers copolymerizable with chloroprene are not limited to one kind. For example, the copolymer of chloroprene may be a copolymer obtained by copolymerizing three or more monomers including chloroprene.
[0025] From the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, low heat build-up and excellent compression set resistance, the chloroprene rubber preferably contains at least one selected from a homopolymer of chloroprene, a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a copolymer of chloroprene and acrylonitrile, and more preferably contains at least one selected from a homopolymer of chloroprene and a copolymer of chloroprene and acrylonitrile. The copolymer of chloroprene and 2,3-dichloro-1,3-butadiene is a copolymer having a structural unit derived from chloroprene and a structural unit derived from 2,3-dichloro-1,3-butadiene, and is a copolymer having chloroprene and 2,3-dichloro-1,3-butadiene as monomer units (chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units). The copolymer of chloroprene and acrylonitrile is a copolymer having a structural unit derived from chloroprene and a structural unit derived from acrylonitrile, and is a copolymer having chloroprene and acrylonitrile as monomer units (chloroprene monomer unit and acrylonitrile monomer unit).
[0026] When a copolymer of chloroprene is used as the chloroprene rubber, from the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, low heat generation and excellent compression set resistance, the content (copolymerization amount) of the structural unit derived from chloroprene is preferably in the following range based on the total mass of the chloroprene rubber. The content of the structural unit derived from chloroprene is preferably 50% by mass or more, more preferably more than 50% by mass, further preferably 60% by mass or more, particularly preferably 70% by mass or more, extremely preferably 80% by mass or more, very preferably 85% by mass or more, and further preferably 90% by mass or more. The content of the structural unit derived from chloroprene is less than 100% by mass, preferably 99% by mass or less, more preferably 95% by mass or less, further preferably 93% by mass or less, and further preferably 91% by mass or less. From the above viewpoints, the content of the structural unit derived from chloroprene is preferably 50% by mass or more and less than 100% by mass.
[0027] When using a copolymer of chloroprene as a chloroprene rubber, from the viewpoint of easily obtaining a sulfide with excellent heat resistance, low heat generation and excellent compression set resistance, and from the viewpoint of easily presenting the effect brought by copolymerizing these monomers, the content (copolymerization amount) of the structural unit from the monomer copolymerizable with chloroprene is preferably in the following range based on the total mass of the chloroprene rubber. The content of the structural unit is preferably 50% by mass or less, more preferably less than 50% by mass, further preferably 40% by mass or less, particularly preferably 30% by mass or less, extremely preferably 20% by mass or less, very preferably 15% by mass or less, and further preferably 10% by mass or less. The content of the structural unit exceeds 0% by mass, preferably 1% by mass or more, more preferably 5% by mass or more, further preferably 7% by mass or more, and particularly preferably 9% by mass or more. From the above viewpoint, the content of the structural unit is preferably more than 0% by mass and is 50% by mass or less. From the same viewpoint, the content of the structural unit from acrylonitrile preferably satisfies the above-mentioned ranges.
[0028] The chloroprene rubber (chloroprene homopolymer, chloroprene copolymer, etc.) may be sulfur-modified chloroprene rubber, thiol-modified chloroprene rubber, xanthate-modified chloroprene rubber, dithiocarbonate-based chloroprene rubber, trithiocarbonate-based chloroprene rubber, urethane-based chloroprene rubber, etc. When a chloroprene homopolymer is used as the chloroprene rubber, the chloroprene homopolymer preferably includes a thiol-modified chloroprene rubber from the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, low heat build-up and excellent compression set resistance.
[0029] From the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, low heat build-up and excellent compression set resistance, the weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (molecular weight polydispersity, Mw / Mn) of the chloroprene rubber are preferably in the following ranges.
[0030] The weight average molecular weight of the chloroprene rubber is preferably 10×10 3 g / mol or more, more preferably 50×10 3 g / mol or more, more preferably 100×10 3 g / mol or more, particularly preferably 300×10 3 g / mol or more, and most preferably 400×10 3 g / mol or more, particularly preferably 450×10 3 The weight average molecular weight of the chloroprene rubber is preferably 5000×10 3 g / mol or less, more preferably 3000×10 3 g / mol or less, more preferably 2000×10 3 g / mol or less, particularly preferably 1000×10 3 g / mol or less, and most preferably 800×10 3 g / mol or less, and most preferably 500×10 3 From the above viewpoints, the weight average molecular weight of the chloroprene rubber is preferably 10×10 3 ~5000×10 3 g / mol, more preferably 100×10 3 ~2000×10 3 g / mol, more preferably 300×10 3 ~1000×10 3 g / mol.
[0031] The number average molecular weight of the chloroprene rubber is preferably 1×10 3 g / mol or more, more preferably 5×10 3 g / mol or more, more preferably 10×10 3 g / mol or more, particularly preferably 50×10 3 g / mol or more, and most preferably 100×10 3 g / mol or more, and particularly preferably 130×10 3 The number average molecular weight of the chloroprene rubber is preferably 1000×10 3 g / mol or less, more preferably 800×10 3g / mol or less, more preferably 500×10 3 g / mol or less, particularly preferably 300×10 3 g / mol or less, and most preferably 200×10 3 g / mol or less, and most preferably 150×10 3 From the above viewpoints, the number average molecular weight of the chloroprene rubber is preferably 1×10 3 ~1000×10 3 g / mol, more preferably 10×10 3 ~500×10 3 g / mol, more preferably 50×10 3 ~300×10 3 g / mol.
[0032] The molecular weight distribution of the chloroprene rubber is preferably 1.0 or more, more preferably 1.5 or more, further preferably 2.0 or more, particularly preferably 2.5 or more, extremely preferably 3.0 or more, very preferably 3.2 or more, and further preferably 3.4 or more. The molecular weight distribution of the chloroprene rubber is preferably 10 or less, more preferably 8.0 or less, further preferably 5.0 or less, particularly preferably 4.0 or less, extremely preferably 3.8 or less, very preferably 3.5 or less, and further preferably 3.4 or less. From the above viewpoints, the molecular weight distribution of the chloroprene rubber is preferably 1.0 to 10, more preferably 2.0 to 5.0, and further preferably 2.5 to 4.0.
[0033] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the chloroprene rubber can be measured by gel permeation chromatography (GPC) and can be obtained in terms of polystyrene. Specifically, they can be measured by the method described in Examples.
[0034] The content of the chloroprene rubber is preferably 50% by mass or more, more preferably more than 50% by mass, further preferably 70% by mass or more, particularly preferably 90% by mass or more, extremely preferably 95% by mass or more, very preferably more than 95% by mass, further preferably 96% by mass or more, further preferably 98% by mass or more, and particularly preferably 99% by mass or more, based on the total mass of the rubber component contained in the rubber composition, from the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, low heat build-up properties, and excellent compression set resistance. The rubber component contained in the rubber composition may be composed of the chloroprene rubber (substantially 100% by mass of the rubber component contained in the rubber composition is the chloroprene rubber).
[0035] Based on the total mass of the rubber composition, the content of chloroprene rubber is preferably in the following range. From the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, low heat generation and excellent compression set resistance, the content of chloroprene rubber is preferably 30% by mass or more, more preferably 40% by mass or more, further preferably 45% by mass or more, particularly preferably 50% by mass or more, extremely preferably more than 50% by mass, very preferably 55% by mass or more, and further preferably 60% by mass or more. From the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, low heat generation and excellent compression set resistance, the content of chloroprene rubber is preferably 90% by mass or less, more preferably 85% by mass or less, further preferably 80% by mass or less, particularly preferably 75% by mass or less, extremely preferably 70% by mass or less, and very preferably 65% by mass or less. From the above viewpoint, the content of chloroprene rubber is preferably 30 to 90% by mass, more preferably 40 to 80% by mass, and further preferably 50 to 70% by mass.
[0036] The method for producing chloroprene rubber comprises a polymerization step of polymerizing a raw material monomer containing chloroprene. The chloroprene rubber can be obtained, for example, by emulsion polymerizing a raw material monomer containing chloroprene (for example, a raw material monomer containing chloroprene as a main component) using an emulsifying dispersant in the presence of a polymerization reaction catalyst, a catalyst activator, a polymerization initiator, a chain transfer agent, and the like.
[0037] Examples of the emulsifying dispersant include alkali metal salts of saturated or unsaturated fatty acids having 6 to 22 carbon atoms, alkali metal salts of rosin acid or disproportionated rosin acid (e.g. potassium rosinate), and alkali metal salts of formaldehyde condensates of β-naphthalenesulfonic acid (e.g. sodium salt).
[0038] Examples of the polymerization catalyst include inorganic peroxides such as potassium sulfate; and organic peroxides such as ketone peroxides, peroxyketals, hydroperoxides, dialkyl peroxides, and diacyl peroxides.
[0039] Examples of the catalyst activator include sodium sulfite, potassium sulfite, iron (II) oxide, anthraquinone, sodium β-sulfonate, formamidinesulfinic acid, and L-ascorbic acid.
[0040] The polymerization initiator is not particularly limited, and a known polymerization initiator generally used in the emulsion polymerization of chloroprene can be used. Examples of the polymerization initiator include potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, tert-butyl hydroperoxide, and the like.
[0041] The chain transfer agent is not particularly limited, and a known chain transfer agent commonly used in the emulsion polymerization of chloroprene can be used. Examples of the chain transfer agent include long-chain alkyl mercaptans such as n-dodecyl mercaptan, tert-dodecyl mercaptan, and n-octyl mercaptan; xanthate compounds such as diisopropyl xanthate disulfide and diethyl xanthate disulfide; triiodomethane; benzyl 1-pyrrole dithiocarbamate (also known as benzyl 1-pyrrole dithiocarbamate), benzyl phenyl dithiocarbamate, 1-benzyl-N,N-dimethyl-4-aminodithiobenzoate, 1-benzyl-4-methoxydithiobenzoate, 1-phenylethyl imidazole dithiocarbamate (also known as 1-phenylethyl imidazole dithiocarbamate), and benzyl 1-(2-pyrrolidone) dithiocarbamate (also known as benzyl 1-(2-pyrrolidone) dithiocarbamate). , benzyl phthalimidodithiocarbamate (also known as benzyl phthalimidodithiocarbamate), 2-cyanopropyl-2-yl 1-pyrroledithiocarbamate (also known as 2-cyanopropyl-2-yl 1-pyrroledithiocarbamate), 2-cyanobutyl-2-yl 1-pyrroledithiocarbamate (also known as 2-cyanobutyl-2-yl 1-pyrroledithiocarbamate), benzyl 1-imidazoledithiocarbamate (also known as benzyl 1-imidazoledithiocarbamate), 2-cyanopropyl-2-yl N,N-dimethyldithiocarbamate, benzyl N,N-diethyldithiocarbamate, cyanomethyl 1-(2-pyrrolidone)dithiocarbamate, N,N-diethyldithiocarbamate 2-(Ethoxycarbonylbenzyl)propan-2-yl formate, 1-phenylethyl dithiobenzoate, 2-phenylpropan-2-yl dithiobenzoate, 1-acet-1-yl-ethyl dithiobenzoate, 1-(4-methoxyphenyl)ethyl dithiobenzoate, benzyl dithioacetate, ethoxycarbonylmethyl dithioacetate, 2-(ethoxycarbonyl)propan-2-yl dithiobenzoate, 2-cyanopropan-2-yl dithiobenzoate, tert-butyl dithiobenzoate, 2,4,4-trimethylpentan-2-yl dithiobenzoate, 2-(4-chlorophenyl)-propan-2-yl dithiobenzoate, 3-vinylbenzyl dithiobenzoate, 4-vinylbenzyl dithiobenzoate, benzyl ethoxyphosphinyl dithiocarboxylate, tert-butyl trithioperoxybenzoate, 2-phenylpropan-2-yl 4-chlorodithiobenzoate, 1-methyl-1-phenylethyl naphthalene-1-carboxylate, 4-cyano-4-methyl-4-thiobenzylsulfanylbutyric acid, dibenzyl tetrathioterephthalate, carboxymethyl dithiobenzoate, poly(ethylene oxide) having dithiobenzoate end groups, poly(ethylene oxide) having 4-cyano-4-methyl-4-thiobenzylsulfanylbutyric acid end groups, 2-[(2-phenylethylthio)sulfanyl]propionic acid, 2-[(2-phenylethylthio)sulfanyl]succinic acid, potassium 3,5-dimethyl-1H-pyrazole-1-dithiocarboxylate, 3,5-dimethyl-1H-pyrazole-1-dithiocarboxylate,5-Dimethyl-1H-pyrazole-1-dithiocarbamate cyanomethyl ester, methyl (phenyl) dithiocarbamate cyanomethyl ester, 4-chlorodithiobenzoic acid benzyl ester, 4-chlorodithiobenzoic acid phenyl methyl ester, 4-chlorodithiobenzoic acid 4-nitrobenzyl ester, 4-chlorodithiobenzoic acid phenyl propan-2-yl ester, 4-chlorodithiobenzoic acid 1-cyano-1-methylethyl ester, 4-chlorodithiobenzoic acid 3-chloro-2-butylene ester, 2-chloro-2-butenyl dithiobenzoate, benzyl dithioacetate, 3-chloro-2-butenyl-1H-pyrrole-1-dithiocarboxylic acid, 2-cyanobutane-2-yl 4-chloro-3,5-dimethyl-1H-pyrazole-1-dithiocarboxylate, methyl (phenyl) dithiocarbamate cyanomethyl ester, 2-cyano-2-propyl dodecyl trithiocarbonate, dibenzyl trithiocarbonate, trithiocarbonic acid butyl benzyl ester, 2-[[(butylthio)thiomethyl]thio]propanoic acid, 2-[[(dodecylthio)thiomethyl]thio]propanoic acid, 2-[[(butylthio)thiomethyl]thio]succinic acid, 2-[[(dodecylthio)thiomethyl]thio]succinic acid, 2-[[(dodecylthio)thiomethyl]thio]-2-methylpropanoic acid, 2,2'-[thiocarbonylbis(thio)]bis[ 2-methylpropionic acid], 2-amino-1-methyl-2-oxoethyl butyl trithiocarbonate, 2-[(2-hydroxyethyl)amino]-1-methyl-2-oxoethyl benzyl trithiocarbonate, 3-[[[(tert-butyl)thio]thiomethyl]thio]propionic acid, cyanomethyl dodecyl trithiocarbonate, diethylaminobenzyl trithiocarbonate, dibutylaminobenzyl trithiocarbonate and other thiocarbonyl compounds, etc.
[0042] The polymerization temperature of the chloroprene rubber is not particularly limited. Generally, the temperature for emulsion polymerization is preferably 0 to 50° C., more preferably 20 to 50° C. The final polymerization rate of the chloroprene rubber obtained in the above-mentioned polymerization step is not particularly limited. It is preferably arbitrarily adjusted within the range of 30 to 100%. In order to adjust the final conversion rate, a polymerization terminator for stopping the polymerization reaction may be added to stop the polymerization when the desired conversion rate is reached.
[0043] The polymerization terminator is not particularly limited, and a commonly used polymerization terminator can be used. Examples of the polymerization terminator include thiodiphenylamine (also known as phenothiazine), 4-tert-butylcatechol, and 2,2-methylenebis-4-methyl-6-tert-butylphenol.
[0044] Next, unreacted monomers can be removed from the polymer solution obtained in the polymerization step. The method is not particularly limited, and an example thereof is a stripping method. Then, the pH can be adjusted, and the chloroprene rubber can be obtained through the steps of freeze coagulation, water washing, hot air drying, etc. as a common method.
[0045] (2) Maleimide compounds
[0046] The maleimide compound is a compound having a skeleton derived from maleimide. The maleimide compound can be used as a vulcanizing agent in the rubber composition. Examples of the maleimide compound include N,N'-phenylene bismaleimide (N,N'-o-phenylene bismaleimide, N,N'-m-phenylene bismaleimide, N,N'-p-phenylene bismaleimide, etc.), N,N'-diphenylmethane bismaleimide (N,N'-(4,4'-diphenylmethane) bismaleimide, etc.), 2,2-bis[4-(4-maleimidephenylene)] Bismaleimide compounds such as bismaleimide (2,2,4-trimethyl) hexane, bismaleimide compounds such as bismaleimide (2,2,4-trimethyl) hexane, and the like. From the viewpoint of easily improving the heat resistance, low heat generation and compression set resistance of the sulfide (for example, a vulcanized molded article), it is preferred to contain a bismaleimide compound, and the maleimide compound more preferably contains at least one selected from N,N'-phenylene bismaleimide and N,N'-diphenylmethane bismaleimide, further preferably contains N,N'-phenylene bismaleimide, and particularly preferably contains N,N'-m-phenylene bismaleimide.
[0047] The content of the maleimide compound is 0.50 to 4.0 parts by mass relative to 100 parts by mass of the chloroprene rubber. When the content of the maleimide compound is 0.50 parts by mass or more, the vulcanization of the rubber composition is fully carried out, so the low heat generation of the vulcanized product is improved, and the compression set resistance of the vulcanized product is easily improved. When the content of the maleimide compound is 4.0 parts by mass or less, the rubber elasticity of the vulcanized product (e.g., a vulcanized molded product) can be fully ensured, so the heat resistance of the vulcanized product (e.g., elongation at break after heat aging) is improved.
[0048] From the viewpoint of easily obtaining a sulfide having excellent heat resistance, low heat generation and excellent compression set resistance, the content of the maleimide compound is preferably 0.70 parts by mass or more, more preferably 1.0 parts by mass or more, further preferably 1.2 parts by mass or more, particularly preferably 1.5 parts by mass or more, extremely preferably 1.8 parts by mass or more, and very preferably 2.0 parts by mass or more. From the viewpoint of easily obtaining a sulfide having excellent heat resistance, low heat generation and excellent compression set resistance, the content of the maleimide compound is preferably 3.8 parts by mass or less, more preferably 3.5 parts by mass or less, further preferably 3.2 parts by mass or less, particularly preferably 3.0 parts by mass or less, extremely preferably 2.8 parts by mass or less, very preferably 2.5 parts by mass or less, further preferably 2.2 parts by mass or less, and further preferably 2.0 parts by mass or less. From the above viewpoints, the content of the maleimide compound is preferably 0.70 to 3.0 parts by mass, more preferably 1.0 to 3.0 parts by mass, and further preferably 1.0 to 2.0 parts by mass. The content of the maleimide compound may be 2.2 parts by mass or more, 2.5 parts by mass or more, 2.8 parts by mass or more, or 3.0 parts by mass or more. The content of the maleimide compound may be 1.8 parts by mass or less, 1.5 parts by mass or less, 1.2 parts by mass or less, 1.0 parts by mass or less, or 0.70 parts by mass or less.
[0049] Based on the total mass of the rubber composition, the content of the maleimide compound is preferably in the following range. From the perspective of easily obtaining a vulcanized product having excellent heat resistance, low heat generation and excellent compression set resistance, the content of the maleimide compound is preferably 0.10% by mass or more, more preferably 0.20% by mass or more, further preferably 0.30% by mass or more, particularly preferably 0.40% by mass or more, extremely preferably 0.50% by mass or more, very preferably 0.70% by mass or more, further preferably 1.0% by mass or more, and further preferably 1.2% by mass or more. From the perspective of easily obtaining a vulcanized product having excellent heat resistance, low heat generation and excellent compression set resistance, the content of the maleimide compound is preferably 3.0% by mass or less, more preferably 2.8% by mass or less, further preferably 2.5% by mass or less, particularly preferably 2.0% by mass or less, extremely preferably 1.8% by mass or less, very preferably 1.5% by mass or less, and further preferably 1.3% by mass or less. From the above viewpoints, the content of the maleimide compound is preferably 0.10 to 3.0 mass %, more preferably 0.20 to 2.8 mass %, and further preferably 0.50 to 2.0 mass %. The content of the maleimide compound may be 1.3 mass % or more, 1.5 mass % or more, or 1.8 mass % or more. The content of the maleimide compound may be 1.2 mass % or less, 1.0 mass % or less, 0.70 mass % or less, 0.50 mass % or less, or 0.40 mass % or less.
[0050] (3) Organic peroxides
[0051] The organic peroxide can be used as a vulcanization aid in the rubber composition. Examples of the organic peroxide include dicumyl peroxide, benzoyl peroxide, 1,1-bis(tert-butylperoxy)-3,5,5-trimethylcyclohexane, diisobutyryl peroxide, cumyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di(4-tert-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, tert-hexyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, tert-butyl peroxyneoheptanoate, tert-hexyl peroxypivalate, and tert-butyl peroxypivalate. tert-Butyl ester, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutyl peroxy-2-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-di(2-ethylhexanoyl peroxy)hexane, tert-hexyl peroxy-2-ethylhexanoate, di(4-methylbenzoyl) peroxide, tert-butyl peroxy-2-ethylhexanoate, di(3-methylbenzoyl) peroxide, benzoyl (3-methylbenzoyl) peroxide, diperoxybenzoyl, 1,1-di(tert-butylperoxy)-2-methylcyclohexane 1,1-di(tert-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(tert-hexylperoxy)cyclohexane, 1,1-di(tert-butylperoxy)cyclohexane, 2,2-di(4,4-di(tert-butylperoxy)cyclohexyl)propane, tert-hexyl peroxyisopropyl monocarbonate, tert-butyl peroxymaleate, tert-butyl peroxy-3,5,5-trimethylhexanoate, tert-butyl peroxylaurate, tert-butyl peroxyisopropyl monocarbonate, tert-butyl peroxy-2-ethylhexyl monocarbonate, tert-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, ethyl peroxide tert-Butyl peroxide, 2,2-di(tert-butylperoxy)butane, tert-butyl peroxybenzoate, 4,4-di(tert-butylperoxy)valerate, 1,4-bis[(tert-butylperoxy)isopropyl]benzene, di-tert-hexyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, tert-butylcumyl peroxide, di-tert-butyl peroxide, terpene hydroperoxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, tert-butyl hydroperoxide, etc. From the viewpoint of easily improving the low heat generation property and compression set resistance of the vulcanized product (e.g., vulcanized molded article), the organic peroxide preferably contains at least one selected from peroxyketals and dialkyl peroxides, more preferably contains at least one selected from 4,4-di(tert-butylperoxy)valerate and 1,4-bis[(tert-butylperoxy)isopropyl]benzene, and further preferably contains 1,4-bis[(tert-butylperoxy)isopropyl]benzene.
[0052] The content of the organic peroxide is 0.10 to 2.0 parts by mass relative to 100 parts by mass of the chloroprene rubber. When the content of the organic peroxide is 0.10 parts by mass or more, the effect of promoting the vulcanization of the rubber composition can be fully obtained, and thus the vulcanization is fully carried out, so that the heat resistance (e.g., elongation at break after heat aging) and low heat generation of the vulcanized material are improved, and the compression set resistance of the vulcanized material is easily improved. When the content of the organic peroxide is 2.0 parts by mass or less, the rapid increase of the vulcanization density is suppressed, so that the heat resistance (e.g., elongation at break after heat aging) of the vulcanized material is improved.
[0053] From the viewpoint of easily obtaining a sulfide having excellent heat resistance, low heat build-up and excellent compression set resistance, the content of the organic peroxide is preferably 0.15 parts by mass or more, more preferably 0.20 parts by mass or more, further preferably 0.30 parts by mass or more, and particularly preferably 0.40 parts by mass or more. From the viewpoint of easily obtaining a sulfide having excellent heat resistance, the content of the organic peroxide is preferably 1.8 parts by mass or less, more preferably 1.7 parts by mass or less, further preferably 1.5 parts by mass or less, particularly preferably 1.2 parts by mass or less, extremely preferably 1.0 parts by mass or less, very preferably 0.80 parts by mass or less, further preferably 0.50 parts by mass or less, and further preferably 0.40 parts by mass or less. From the above viewpoints, the content of the organic peroxide is preferably 0.15 to 1.8 parts by mass, more preferably 0.20 to 1.0 parts by mass, and further preferably 0.30 to 0.80 parts by mass. From the viewpoint of easily obtaining a sulfide having excellent low heat generation and excellent compression set resistance, the content of the organic peroxide is preferably 0.50 parts by mass or more, more preferably 0.80 parts by mass or more, further preferably 1.0 parts by mass or more, particularly preferably 1.2 parts by mass or more, extremely preferably 1.5 parts by mass or more, and very preferably 1.7 parts by mass or more. The content of the organic peroxide may be 0.30 parts by mass or less, 0.20 parts by mass or less, or 0.15 parts by mass or less.
[0054] The content of the organic peroxide is preferably in the following range based on the total mass of the rubber composition. From the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, low heat build-up and excellent compression set resistance, the content of the organic peroxide is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, further preferably 0.06% by mass or more, particularly preferably 0.07% by mass or more, extremely preferably 0.10% by mass or more, very preferably 0.15% by mass or more, further preferably 0.20% by mass or more, further preferably 0.24% by mass or more. From the viewpoint of easily obtaining a vulcanized product having excellent heat resistance, the content of the organic peroxide is preferably 2.0% by mass or less, more preferably 1.8% by mass or less, further preferably 1.5% by mass or less, particularly preferably 1.2% by mass or less, extremely preferably 1.0% by mass or less, very preferably 0.80% by mass or less, further preferably 0.50% by mass or less, further preferably 0.30% by mass or less, and particularly preferably 0.25% by mass or less. From the above viewpoints, the content of the organic peroxide is preferably 0.01 to 2.0% by mass, more preferably 0.05 to 1.5% by mass, and further preferably 0.20 to 0.80% by mass. From the viewpoint of easily obtaining a sulfide having excellent low heat generation and excellent compression set resistance, the content of the organic peroxide is preferably 0.25% by mass or more, more preferably 0.30% by mass or more, further preferably 0.50% by mass or more, particularly preferably 0.80% by mass or more, and extremely preferably 1.0% by mass or more. The content of the organic peroxide may be 0.24% by mass or less, 0.20% by mass or less, 0.15% by mass or less, 0.10% by mass or less, 0.07% by mass or less, or 0.06% by mass or less.
[0055] The mass ratio A / B of the content A of the maleimide compound relative to the content B of the organic peroxide is preferably in the following range. From the viewpoint of easily obtaining a sulfide having excellent balance among heat resistance, low heat generation and compression set resistance, the mass ratio A / B is preferably 1.0 or more, more preferably 1.2 or more, further preferably 1.3 or more, particularly preferably 1.5 or more, extremely preferably 2.0 or more, very preferably 3.0 or more, further preferably 4.0 or more, further preferably 5.0 or more. From the viewpoint of easily obtaining a sulfide having excellent balance among heat resistance, low heat generation and compression set resistance because a sharp rise in vulcanization density is not likely to occur, thereby easily suppressing the decrease in heat resistance (e.g., elongation at break after heat aging) and compression set resistance, the mass ratio A / B is preferably 20 or less, more preferably 15 or less, further preferably 10 or less, particularly preferably 9.0 or less, extremely preferably 8.0 or less, very preferably 7.0 or less, further preferably 6.0 or less, further preferably 5.0 or less. From the above viewpoints, the mass ratio A / B is preferably 1.0 to 20, more preferably 1.0 to 10, further preferably 1.0 to 7.0, and particularly preferably 2.0 to 7.0. The mass ratio A / B may be 6.0 or more, 7.0 or more, 8.0 or more, 9.0 or more, 10 or more, or 15 or more. The mass ratio A / B may be 4.0 or less, 3.0 or less, 2.0 or less, 1.5 or less, 1.3 or less, or 1.2 or less.
[0056] (4) Other compounds
[0057] The rubber composition involved in this embodiment may contain a rubber component (excluding chloroprene rubber); a vulcanizing agent (excluding maleimide compounds); a vulcanization accelerator; a vulcanization aid (excluding organic peroxides); a plasticizer; carbon black; a filler (reinforcement material); a processing aid; an anti-aging agent, etc. as components different from the above-mentioned components.
[0058] The rubber component may or may not contain chlorinated polyethylene. The content of chlorinated polyethylene may be 5% by mass or less, less than 5% by mass, 3% by mass or less, 1% by mass or less, or less than 1% by mass based on the total mass of the rubber component contained in the rubber composition.
[0059] The vulcanizing agent is not particularly limited, but preferably a metal oxide. Examples of the metal oxide include zinc oxide, magnesium oxide, lead oxide, lead tetraoxide, iron trioxide, titanium dioxide, calcium oxide, and hydrotalcite. The content of the vulcanizing agent (excluding the maleimide compound) may be 3 to 15 parts by mass relative to 100 parts by mass of the chloroprene rubber.
[0060] As the vulcanization accelerator, a compound commonly used in the vulcanization of chloroprene rubber can be used. Examples of the vulcanization accelerator include thiourea-based, guanidine-based, thiuram-based, thiazole-based vulcanization accelerators; dimethylammonium hydrogen isophthalate; 1,2-dimercapto-1,3,4-thiadiazole derivatives, etc. Examples of the thiourea-based vulcanization accelerator include ethylene thiourea, diethyl thiourea, trimethyl thiourea, triethyl thiourea, N,N'-diphenyl thiourea, etc., preferably at least one selected from trimethyl thiourea and ethylene thiourea.
[0061] From the viewpoint of increasing the vulcanization speed or vulcanization density of the rubber composition, the rubber composition involved in the present embodiment may contain at least one compound selected from difunctional ester compounds and trifunctional ester compounds as a vulcanization aid. Specific examples of difunctional ester compounds and trifunctional ester compounds include trimethylolpropane, ethylene glycol dimethacrylate, triallyl isocyanate, triallyl cyanate, etc.
[0062] As the plasticizer, there is no particular limitation as long as it is compatible with the chloroprene rubber, and examples thereof include vegetable oil (rapeseed oil, etc.), phthalate plasticizer, DOS, DOA, ester plasticizer, polyether ester plasticizer, thioether plasticizer, aromatic oil, naphthenic oil, etc., and one or more thereof can be used according to the characteristics required by the rubber composition. The content of the plasticizer can be 5 to 50 parts by mass relative to 100 parts by mass of the chloroprene rubber.
[0063] Examples of the filler (reinforcement material) include carbon black, silica, clay, talc, calcium carbonate, etc. The content of the filler may be 5 to 100 parts by mass based on 100 parts by mass of the chloroprene rubber.
[0064] Examples of the processing aid include fatty acids such as stearic acid, paraffin-based processing aids such as polyethylene, and fatty acid amides. The content of the processing aid (excluding organic peroxides) may be 0.5 to 5 parts by mass based on 100 parts by mass of the chloroprene rubber.
[0065] Examples of the antioxidant include amine antioxidants, imidazole antioxidants, metal carbamates, phenol antioxidants, waxes, etc. Examples of amine antioxidants that have a good effect of improving heat resistance include 4,4'-bis(α,α-dimethylbenzyl)diphenylamine and octylated diphenylamine, and 4,4'-bis(α,α-dimethylbenzyl)diphenylamine has a particularly good effect of improving heat resistance.
[0066] The rubber composition according to the present embodiment can be obtained by kneading the above-mentioned components at a temperature lower than the vulcanization temperature thereof. As a kneading device, a mixer, a Banbury mixer, a kneader, a two-roll mixer, etc. can be used.
[0067] <Unvulcanized molded article, vulcanized article, and vulcanized molded article>
[0068] The unvulcanized molded body according to the present embodiment uses the rubber composition according to the present embodiment, and is a molded body (molded product) of the rubber composition (unvulcanized state) according to the present embodiment. The method for manufacturing the unvulcanized molded body according to the present embodiment comprises a step of molding the rubber composition (unvulcanized state) according to the present embodiment. The unvulcanized molded body according to the present embodiment is formed by the rubber composition (unvulcanized state) according to the present embodiment.
[0069] The vulcanized product according to the present embodiment is a vulcanized product of the rubber composition according to the present embodiment. The method for producing the vulcanized product according to the present embodiment includes a step of vulcanizing the rubber composition according to the present embodiment.
[0070] The vulcanized molded body involved in the present embodiment is a vulcanized molded body of the rubber composition involved in the present embodiment. The vulcanized molded body involved in the present embodiment uses the sulfide involved in the present embodiment and is a molded body (molded product) of the sulfide involved in the present embodiment. The vulcanized molded body involved in the present embodiment is formed by the sulfide involved in the present embodiment. Regarding the vulcanized molded body involved in the present embodiment, the change rate of the compression permanent deformation of the vulcanized molded body measured under the test conditions of 130° C. (test temperature) and 72 hours (test time) in accordance with JIS K 6262:2013 is preferably 40% or less. With respect to the vulcanized molded body involved in the present embodiment, it is preferred that 0.01 to 2% by mass of a maleimide compound is contained based on the total mass of the vulcanized molded body.
[0071] The vulcanized molded body according to the present embodiment can be obtained by molding a vulcanized product obtained by vulcanizing the rubber composition (unvulcanized state) according to the present embodiment, or can be obtained by vulcanizing a molded body obtained by molding the rubber composition (unvulcanized state) according to the present embodiment. The method for manufacturing the vulcanized molded body according to the present embodiment comprises a step of molding the vulcanized product according to the present embodiment, or a step of vulcanizing the unvulcanized molded body according to the present embodiment.
[0072] The unvulcanized molded body, sulfide and vulcanized molded body involved in this embodiment can be used as rubber parts in various industrial fields such as buildings, structures, ships, railways, coal mines, and automobiles, and can be used as rubber parts for automobiles (for example, automobile sealing materials), hose materials, rubber molds, gaskets, rubber rollers, industrial cables, industrial conveyor belts, etc.
[0073] As a method for molding the rubber composition (unvulcanized state) and the vulcanized product according to the present embodiment, press molding, extrusion molding, calendaring molding, etc. can be cited. The temperature for vulcanizing the rubber composition can be appropriately set according to the composition of the rubber composition, preferably 140 to 220° C., and more preferably 160 to 190° C. The vulcanization time for vulcanizing the rubber composition can be appropriately set according to the composition of the rubber composition, the shape of the unvulcanized molded body, etc., and can be 10 to 60 minutes.
[0074] Example
[0075] <Manufacture of Chloroprene-Acrylonitrile Copolymer Rubber>
[0076] In a polymerization tank having an internal volume of 3 liters and equipped with a heating and cooling jacket and a stirrer, 24 parts by mass of chloroprene monomer, 24 parts by mass of acrylonitrile monomer, 0.5 parts by mass of diethyl xanthate disulfide, 200 parts by mass of pure water, 5.00 parts by mass of potassium rosinate (manufactured by HARIMA CHEMICALS, INC.), 0.40 parts by mass of sodium hydroxide, and 2.0 parts by mass of sodium salt of β-naphthalenesulfonic acid formaldehyde condensate (manufactured by Kao Corporation) were added. 0.1 parts by mass of potassium persulfate as a polymerization initiator was added, and emulsion polymerization was carried out at a polymerization temperature of 40° C. under a nitrogen flow. The above-mentioned chloroprene monomer was added in batches 20 seconds after the start of polymerization, and the batch addition flow rate was adjusted by a solenoid valve based on the heat change of the refrigerant in 10 seconds from the start of polymerization, and the flow rate was adjusted again every 10 seconds thereafter, thereby continuously carrying out the addition. When the polymerization rate relative to the total amount of the chloroprene monomer and the acrylonitrile monomer reached 50%, 0.02 parts by mass of phenothiazine was added as a polymerization terminator to terminate the polymerization. Then, unreacted monomers in the reaction solution were removed under reduced pressure to obtain a chloroprene-acrylonitrile copolymer latex.
[0077] The above-mentioned polymerization rate of the chloroprene-acrylonitrile copolymer latex is calculated based on the dry mass of the chloroprene-acrylonitrile copolymer latex when it is air-dried. Specifically, it is calculated using the following formula (I). In the formula, the so-called "solid content concentration" refers to the concentration of the solid content [mass %] after heating 2g of the sampled chloroprene-acrylonitrile copolymer latex at 130°C to remove the volatile components such as solvent (water), volatile chemicals, and raw materials. The so-called "total charge amount" refers to the total amount of raw materials, reagents and solvents (water) charged to the polymerization tank from the start of polymerization to a certain time. The so-called "evaporation residue amount" refers to the mass of chemicals that have not volatilized under the condition of 130°C and remain in the form of solid components together with the polymer among the chemicals and raw materials charged from the start of polymerization to a certain time. The monomer charge amount is the sum of the monomers initially charged to the polymerization tank and the monomers added in batches from the start of polymerization to a certain time. It should be noted that the so-called "monomer" here refers to the total amount of chloroprene monomer and acrylonitrile monomer.
[0078] Polymerization rate [%] = {(total charge amount [g] × solid content concentration [mass %] / 100) - (evaporation residue amount [g])} / monomer charge amount [g] × 100 (I)
[0079] The pH of the chloroprene-acrylonitrile copolymer latex was adjusted to 7.0 using acetic acid or sodium hydroxide, and then the chloroprene-acrylonitrile copolymer latex was frozen and coagulated on a metal plate cooled to -20°C to perform emulsion destruction, thereby obtaining a sheet. The sheet was washed with water and then dried at 130°C for 15 minutes, thereby obtaining a solid chloroprene-acrylonitrile copolymer rubber.
[0080] The above-mentioned chloroprene-acrylonitrile copolymer rubber was made into a solution with a sample concentration of 0.1 mass % using THF, and then the weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) of the chloroprene-acrylonitrile copolymer rubber were measured (based on standard polystyrene conversion) using a high-efficiency GPC device (TOSOH HLC-8320GPC: manufactured by Tosoh Corporation). At this time, a TSK guard column HHR-H was used as a pre-column, and three HSKgel GMHHR-Hs were used as analytical columns. The sample was made to flow out under the conditions of a sample pump pressure of 8.0 to 9.5 MPa, a flow rate of 1 mL / min, and 40° C., and detected using a differential refractometer.
[0081] The elution time and the molecular weight were obtained using a calibration curve prepared by measuring the standard polystyrene samples (9 in total) with known molecular weights listed below.
[0082] Mw=8.42×10 6 , 1.09×10 6,7.06×10 5 4.27×10 5 , 1.90×10 5 , 9.64×10 4 ,
[0083] 3.79×10 4 , 1.74×10 4 , 2.63×10 3
[0084] The weight average molecular weight (Mw) of chloroprene-acrylonitrile copolymer rubber is 473×10 3 g / mol, and the number average molecular weight (Mn) is 138×10 3 g / mol, and the molecular weight distribution (Mw / Mn) is 3.4.
[0085] The content of the structural unit derived from acrylonitrile in the chloroprene-acrylonitrile copolymer rubber was calculated from the content of nitrogen atoms in the chloroprene-acrylonitrile copolymer rubber. Specifically, the content of nitrogen atoms in 100 mg of the chloroprene-acrylonitrile copolymer rubber was measured using an elemental analyzer (SUMIGRAPH 220F: manufactured by Sumika Analysis Center Co., Ltd.), and the content of the structural unit derived from acrylonitrile was calculated. The amount of the structural unit derived from acrylonitrile was 9.9% by mass.
[0086] The above-mentioned elemental analysis was performed as follows. The furnace temperature was set to 900°C for the reaction furnace, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector. Oxygen as the combustion gas was flowed at 0.2 ml / min, and helium as the carrier gas was flowed at 80 ml / min. The standard curve was prepared using aspartic acid (10.52%) with a known nitrogen content as the standard substance.
[0087] <Manufacturing of Rubber Composition>
[0088] The chloroprene rubber, maleimide compound and organic peroxide described in Table 1 were kneaded with 5 parts by mass of zinc oxide, 4 parts by mass of magnesium oxide, 10 parts by mass of a plasticizer, 40 parts by mass of a filler, 1 part by mass of a processing aid and 3 parts by mass of an antioxidant using an 8-inch open roll to obtain rubber compositions of Examples 1 to 9 and Comparative Examples 1 to 6.
[0089] The chloroprene rubber described in Table 1, 5 parts by mass of zinc oxide, 4 parts by mass of magnesium oxide, 10 parts by mass of a plasticizer, 40 parts by mass of a filler, 1 part by mass of a processing aid, 3 parts by mass of an antioxidant, and 1 part by mass of a vulcanization accelerator were kneaded using an 8-inch open roll to obtain a rubber composition of Comparative Example 7.
[0090] The components for obtaining the rubber composition are shown below.
[0091] Chloroprene rubber 1: Chloroprene-acrylonitrile copolymer rubber prepared by the above method
[0092] Chloroprene rubber 2: mercaptan-modified chloroprene rubber (homopolymer of mercaptan-modified chloroprene), raw rubber, Mooney viscosity ML 1+4 (100℃)=60, made by Denka Co., Ltd.
[0093] Maleimide compound 1: N,N'-m-phenylene bismaleimide, "Vulnoc (registered trademark) PM" manufactured by Ouchi Shinko Chemical Industry
[0094] Maleimide compound 2: N,N'-(4,4'-diphenylmethane)bismaleimide, "BMI-1000" manufactured by Yamato Chemical Industry Co., Ltd.
[0095] Organic peroxide 1: 1,4-bis[(tert-butylperoxy)isopropyl]benzene, "Perbutyl (registered trademark) P-40" manufactured by NOF Corporation
[0096] Organic peroxide 2: 4,4-di(tert-butylperoxy)valerate n-butyl ester, "Perhexa (registered trademark) V-40" manufactured by NOF Corporation
[0097] Zinc oxide: Vulcanizing agent, "Zinc oxide type 2" manufactured by Sakai Chemical Industry Co., Ltd.
[0098] Magnesium oxide: sulfidizing agent, Kyowa Chemical Industry Co., Ltd. "Kyowamag (registered trademark) 30"
[0099] Plasticizer: Polyether ester plasticizer, "Adekacizer (registered trademark) RS-700" manufactured by ADEKA Corporation
[0100] Filler: Carbon black, Asahi Carbon Co., Ltd. "Asahi #60UG"
[0101] Processing aid: Lubricant, stearic acid, "Stearic Acid 50S" manufactured by Shin Nippon Rika Co., Ltd.
[0102] Antiaging agent: 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, "NOCRACK (registered trademark) CD" manufactured by Ouchi Shinko Chemical Industry Co., Ltd.
[0103] Vulcanization accelerator: "NOCCELER TMU" manufactured by Ouchi Shinko Chemical Industry
[0104] <Manufacturing of Vulcanized Molded Body>
[0105] The rubber composition was press-vulcanized at 180° C. for 30 minutes to produce a sheet-shaped vulcanized molded body having a thickness of 2 mm.
[0106] <Evaluation of Vulcanized Molded Article>
[0107] The above-mentioned vulcanized molded body was evaluated as follows. The evaluation results are shown in Table 1.
[0108] (Heat resistance)
[0109] The vulcanized molded body was subjected to a tensile test according to JIS K 6251:2010 to measure the elongation at break X1 (Eb). After the vulcanized molded body was placed under the conditions of 130°C and 72 hours, a tensile test was performed according to JIS K 6257:2017 to measure the elongation at break X2 (Eb). The rate of change of elongation at break (ΔEb, unit: %) was calculated according to the following formula. The case where the rate of change of elongation at break was -30% or more was judged to be good.
[0110] Change rate (%) = [(X2-X1) / X1] × 100
[0111] (Compression set resistance (CS))
[0112] The change rate of compression set before and after the vulcanized molded body was left to stand under the test conditions of 130° C. for 72 hours was measured in accordance with JIS K 6262: 2013. A change rate of compression set of 40% or less was judged to be good.
[0113] (Low heat generation)
[0114] The low heat generation property was evaluated using the Goodrich Flexometer (Goodrich Flexometer: JIS K 6265). The Goodrich Flexometer is a test method for evaluating fatigue properties based on the heat generation inside the test piece by applying dynamic repetitive loads to a test piece such as vulcanized rubber. Specifically, a static initial load is applied to the test piece under certain temperature conditions, and then a sinusoidal vibration of a certain amplitude is applied to measure the heat generation temperature and creep amount of the test piece that change over time. Using the above-mentioned vulcanized molded body, the heat generation (ΔT, unit: ℃) was measured under the conditions of a temperature of 50°C, a strain of 0.175 inches, a load of 55 pounds, and a vibration number of 1800 times per minute in accordance with JIS K 6265:2018. The heat generation of 40°C or less was judged to be good.
[0115] [Table 1]
[0116]
[0117] The results shown in Table 1 show that the rubber compositions of the examples can provide vulcanized products (vulcanized molded products) having excellent heat resistance, low heat build-up, and excellent compression set resistance. Such vulcanized products can be suitably used as various rubber parts.
Claims
1. A rubber composition comprising 100 parts by mass of a chloroprene rubber, 0.70 to 3.0 parts by mass of a maleimide compound, and 0.10 to 2.0 parts by mass of an organic peroxide, The mass ratio A / B of the content A of the maleimide compound to the content B of the organic peroxide is 2.0 to 20, The content of the chloroprene rubber is 90% by mass or more based on the total mass of the rubber component contained in the rubber composition.
2. The rubber composition according to claim 1, wherein The mass ratio A / B of the content A of the maleimide compound to the content B of the organic peroxide is 2.0-10.
3. The rubber composition according to claim 1 or 2, wherein: The chloroprene rubber includes at least one selected from a homopolymer of chloroprene, a copolymer of chloroprene and 2,3-dichloro-1,3-butadiene, and a copolymer of chloroprene and acrylonitrile.
4. The rubber composition according to claim 1 or 2, wherein The content of the chloroprene rubber is 98% by mass or more based on the total mass of the rubber component contained in the rubber composition.
5. The rubber composition according to claim 3, wherein The content of the chloroprene rubber is 98% by mass or more based on the total mass of the rubber component contained in the rubber composition. 6 . A vulcanizate, which is a vulcanizate of the rubber composition according to claim 1 .
7. A vulcanized molded product, which is a vulcanized molded product of the rubber composition according to any one of claims 1 to 5.
8. The vulcanized molded article according to claim 7, wherein the rate of change in compression set measured under test conditions of 130°C for 72 hours in accordance with JIS K 6262:2013 is 40% or less.
Citation Information
Patent Citations
Low-exothermic rubber composition and roll thereof
JP1997268239A
Chloroprene rubber composition, and vulcanizate and molding thereof
JP2012111899A
Rubber composition
JP2016023191A
Motorcycle engine rubber gasket with excellent heat stability
CN105419034A
Low-temperature vulcanized chloroprene rubber cable sheath material as well as preparation method and cable sheath thereof