One-pot method for synthesizing ultra-high viscosity water-soluble block polyether
By using phosphazene catalysts and isocyanate crosslinkers in water-soluble block polyether synthesis, the problems of molecular weight control and self-polymerization of ethylene oxide in traditional technology are solved, and the effective synthesis of high viscosity water-soluble polyethers is achieved. , suitable for production environments of different scales.
Patent Information
- Application Number
- CN202011619432.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-12-31
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-12-31
AI Technical Summary
In the prior art, when synthesizing high viscosity water-soluble block polyethers, it is difficult to control the molecular weight, which easily leads to product turbidity and viscosity reduction. In particular, the self-polymerization of ethylene oxide and propylene oxide caused by traditional basic catalysts is difficult to solve.
Use phosphazene catalyst to replace alkaline catalysts, synthesize ultra-high viscosity water-soluble block polyethers through one pot method, use a mixture of ethylene oxide and propylene oxide to perform nucleophilic substitution reaction, and perform the terminal through isocyanate crosslinking agent. Cross-linking of primary hydroxyl groups produces macromolecular polyether polyols to prevent propylene oxide from self-polymerizing.
It effectively improves the molecular weight and water-soluble viscosity of polyethers, reduces the alkali metal content, avoids the explosive polymerization of polyethers, simplifies the production process, and is suitable for large and small- and medium-sized production environments.
Abstract
Description
Technical Field
[0001] The invention relates to a method for synthesizing ultra-high viscosity water-soluble block polyether by a one-pot method, and belongs to the technical field of negative electrode materials for sodium ion batteries. Background Art
[0002] Water-soluble high molecular weight polyether is an important raw material for synthetic and semi-synthetic metalworking fluids. The existing technology is to form a high-viscosity macromolecular compound by polymerizing a compound containing an active hydrogen initiator with compounds such as ethylene oxide and propylene oxide under the action of an alkaline catalyst. Its disadvantage is that it is extremely difficult to synthesize polyethers with a molecular weight of more than 100,000 due to the limitations of traditional alkaline catalysts. The introduced ethylene oxide and propylene oxide are prone to self-polymerization, which not only causes turbidity in the product, but also causes the molecular weight to fail to meet the expected requirements, thereby causing the product viscosity to decrease. Summary of the invention
[0003] The primary purpose of the present invention is to provide a one-pot method for synthesizing ultra-high viscosity water-soluble block polyethers in view of the problems existing in the prior art, and to synthesize ultra-high viscosity water-soluble block polyethers with a viscosity of >90,000 and water solubility.
[0004] The one-pot method for synthesizing ultra-high viscosity water-soluble block polyether of the present invention comprises the following steps in sequence:
[0005] Step 1: placing a compound containing active hydrogen in a reaction kettle containing an initial polyether, adding a phosphazene catalyst to catalyze a nucleophilic substitution reaction between the active hydrogen and the initial polyether, and heating the reaction kettle to 130-150° C. after evacuation to ensure that the water content is less than 0.1%wt, to obtain an initiator with a total hydroxyl mole number of α;
[0006] Step 2: introducing a mixture of ethylene oxide and propylene oxide into a reactor, causing the mixture of ethylene oxide and propylene oxide to undergo a nucleophilic substitution reaction with active hydrogen in the initiator to generate a new structure with active hydrogen, and the new structure with active hydrogen continues to undergo an epoxide ring reaction with the mixture of ethylene oxide and propylene oxide until the reaction is completed, and aging after the reaction until the pressure in the reactor remains unchanged to generate a polyether polyol terminated with a mixed alkane; the aging refers to a chemical change that allows the incompletely reacted ethylene oxide or propylene oxide to fully react;
[0007] Step 3: introducing ethylene oxide into the reactor, and reacting the ethylene oxide with the polyether polyol generated in step 2 under constant temperature to generate a polyether polyol terminated with ethylene oxide of primary hydroxyl groups; the polyether polyol terminated with mixed alkane is also converted into a polyether polyol terminated with ethylene oxide of primary hydroxyl groups, and aging the reactor until the pressure in the reactor remains unchanged after the reaction is completed; the aging refers to a chemical change that allows the incompletely reacted ethylene oxide to fully react;
[0008] Step 4: The temperature in the reactor is lowered to 30-65° C., and an isocyanate crosslinking agent is introduced; under non-vacuum conditions, the isocyanate in the isocyanate crosslinking agent reacts with the primary hydroxyl group in the ethylene oxide-terminated polyether polyol of the primary hydroxyl group to generate a macromolecular polyether polyol;
[0009] Step 5: After the reaction is completed, the temperature is raised to 120° C. and vacuum is applied to remove the remaining solvent in the isocyanate cross-linking agent after the reaction to obtain an ultra-high viscosity water-soluble block polyether.
[0010] Furthermore, the compound containing active hydrogen in step 1 is a mixture of a liquid polyhydroxy compound and a liquid monohydroxy compound, the liquid polyhydroxy compound is ethylene glycol, propylene glycol and glycerol, and the liquid monohydroxy compound is propylene glycol monomethyl ether or propylene glycol monobutyl ether.
[0011] Furthermore, the amount of the phosphazene catalyst added is 1-5‰ of the total feed mass.
[0012] Furthermore, the molar ratio of ethylene oxide to propylene oxide in step 2 is 50:(92-25), and the amount of the mixture of ethylene oxide and propylene oxide added is (60-180) mol of the mixture of ethylene oxide and propylene oxide for every 1 mol of hydroxyl groups contained in the initiator.
[0013] Furthermore, the amount of ethylene oxide added in step 3 is 2α-4α in mole.
[0014] Furthermore, in step 4, the amount of the isocyanate cross-linking agent added is such that the molar ratio of the isocyanate in the reaction kettle to the total hydroxyl group of the polyether is 1:(0.9-1.15).
[0015] Furthermore, the isocyanate crosslinking agent contains 1-10%wt of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate or a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate.
[0016] Furthermore, the solvent used in the isocyanate cross-linking agent is ether, acetone, tetrahydrofuran or ethyl acetate, or any combination thereof.
[0017] Furthermore, the vacuum in step 1 is 5 mmHg.
[0018] The present invention has achieved the following beneficial effects: 1. In the present invention, the phosphazene catalyst is used instead of the alkaline catalyst to increase the viscosity of the initial polyether, and the alkali metal content in the polyether can be reduced, and the catalysis of the alkali metal on the amination reaction can be effectively avoided without refining, thereby avoiding the explosion of the polyether to carry out the block polymerization of the isocyanate, thereby effectively increasing the molecular weight of the polyether and further increasing the viscosity of the water-soluble block polyether.
[0019] 2. By using isocyanate crosslinking agents, it is possible to use the polyether with terminal primary hydroxyl groups for crosslinking without synthesizing a polyether with a very large molecular weight, thereby obtaining a high-viscosity water-soluble polyether, which has low requirements on production equipment and reaction conditions, and can avoid the self-polymerization of propylene oxide; the present invention uses diisocyanate, each diisocyanate molecule contains 2 -NCO structures, which can chemically react with the primary hydroxyl groups in the ethylene oxide end-capping of the primary hydroxyl groups. Since each polyether has multiple hydroxyl groups, it can be crosslinked into a large molecular weight polyether polyol, which greatly increases the molecular weight of the polyether and increases the viscosity of the polyether.
[0020] 3. The polyhydroxy compound and the monohydroxy compound in step 1 can be mixed in any proportion to adjust the viscosity and state of the ultra-high viscosity water-soluble block polyether finally obtained.
[0021] 4. By using isocyanate cross-linking agents and auxiliary acidic reverse catalysts, the reaction rate of the initial reaction between isocyanate and polyether is reduced, and a more stable and controllable product is obtained.
[0022] 5. The present invention can simply and quickly synthesize high-viscosity water-soluble polyethers, which can be produced not only by large-scale equipment, but also is particularly suitable for the production environment of small and medium-sized companies. DETAILED DESCRIPTION Specific embodiment 1
[0024] Step 1: placing a compound containing active hydrogen in a reaction kettle containing 9.21 g (containing 0.3 mol of hydroxyl group) of propylene glycol and 9 g (containing 0.1 mol of hydroxyl group) of propylene glycol monomethyl ether as an initial polyether, adding 2‰wt% of phosphazene catalyst to catalyze the nucleophilic substitution reaction between active hydrogen and the initial polyether, and heating the reactor to 130°C after evacuation to ensure that the water content is within 0.1%wt, and obtaining an initiator with a total hydroxyl mole of 0.4 mol;
[0025] Step 2: introducing a mixture of 792 g (18 mol) of ethylene oxide and 5220 g (50 mol) of propylene oxide into a reactor, causing the mixture of ethylene oxide and propylene oxide to undergo a nucleophilic substitution reaction with the active hydrogen in the initiator to generate a new structure with active hydrogen, and the new structure with active hydrogen continues to undergo an epoxy ring reaction with the mixture of ethylene oxide and propylene oxide until the reaction is completed, and aging after the reaction until the pressure in the reactor remains unchanged to generate a polyether polyol terminated with a mixed alkane; the aging refers to a chemical change that allows the incompletely reacted ethylene oxide or propylene oxide to fully react;
[0026] Step 3: 70.4 g (1.6 mol) of ethylene oxide is introduced into the reactor. Under constant temperature conditions, ethylene oxide reacts with the new structure with active hydrogen generated in step 2 to generate a primary hydroxyl group-capped ethylene oxide polyether polyol. The mixed alkane-capped polyether polyol is also converted into a primary hydroxyl group-capped ethylene oxide polyether polyol. After the reaction is completed, the reactor is aged until the pressure in the reactor remains unchanged. The aging refers to a chemical change that allows the incompletely reacted ethylene oxide to fully react.
[0027] Step 4: The temperature in the reactor is lowered to 30° C., and 38.28 g of a diisocyanate crosslinking agent with a concentration of 5% wt is introduced; under non-vacuum conditions, the diisocyanate in the diisocyanate crosslinking agent reacts with the primary hydroxyl group in the ethylene oxide-terminated polyether polyol of the primary hydroxyl group to generate a macromolecular polyether polyol;
[0028] Step 5: After the reaction is completed, the temperature is raised to 120° C. and vacuum is applied to remove the remaining solvent in the isocyanate cross-linking agent after the reaction to obtain an ultra-high viscosity water-soluble block polyether. Specific embodiment 2
[0030] Step 1: placing a compound containing active hydrogen in a reaction kettle containing 7.6 g of 1,2-propylene glycol (containing 0.2 mol of hydroxyl group) and 26.4 g of propylene glycol monobutyl ether (containing 0.2 mol of hydroxyl group) of an initial polyether, adding 2‰wt% of a phosphazene catalyst to catalyze a nucleophilic substitution reaction between active hydrogen and the initial polyether, and heating the reactor to 150°C after evacuation to ensure that the water content is within 0.1%wt, thereby obtaining an initiator having a total hydroxyl mole of 0.4 mol;
[0031] Step 2: introducing a mixture of 1584 g (36 mol) of ethylene oxide and 2088 g (36 mol) of propylene oxide into a reactor, causing the mixture of ethylene oxide and propylene oxide to undergo a nucleophilic substitution reaction with the active hydrogen in the initiator to generate a new structure with active hydrogen, and the new structure with active hydrogen continues to undergo an epoxy ring reaction with the mixture of ethylene oxide and propylene oxide until the reaction is completed, and aging after the reaction until the pressure in the reactor remains unchanged to generate a polyether polyol terminated with a mixed alkane; the aging refers to a chemical change that allows the incompletely reacted ethylene oxide or propylene oxide to fully react;
[0032] Step 3: 35.2 (0.8 mol) of ethylene oxide is introduced into the reactor. Under constant temperature conditions, ethylene oxide reacts with the new structure with active hydrogen generated in step 2 to generate a polyether polyol terminated with ethylene oxide of primary hydroxyl groups. The polyether polyol terminated with mixed alkane is also converted into a polyether polyol terminated with ethylene oxide of primary hydroxyl groups. After the reaction is completed, the reaction is aged until the pressure in the reactor remains unchanged. The aging refers to a chemical change that allows the incompletely reacted ethylene oxide to fully react.
[0033] Step 4: The temperature in the reactor is lowered to 65° C., and 34.8 g of a diisocyanate crosslinking agent with a concentration of 3% wt is introduced; under non-vacuum conditions, the diisocyanate in the diisocyanate crosslinking agent reacts with the primary hydroxyl group in the ethylene oxide-terminated polyether polyol of the primary hydroxyl group to generate a macromolecular polyether polyol;
[0034] Step 5: After the reaction is completed, the temperature is raised to 120° C. and vacuum is applied to remove the remaining solvent in the isocyanate cross-linking agent after the reaction to obtain an ultra-high viscosity water-soluble block polyether. Specific embodiment three
[0036] Step 1: placing a compound containing active hydrogen in a reaction kettle containing 7.6 g of 1,2-propylene glycol (containing 0.2 mol of hydroxyl group) and 26.4 g of propylene glycol monobutyl ether (containing 0.2 mol of hydroxyl group) of an initial polyether, adding 2‰wt% of a phosphazene catalyst to catalyze a nucleophilic substitution reaction between active hydrogen and the initial polyether, and evacuating the reactor and heating it to 140°C to ensure that the water content is within 0.1%wt, thereby obtaining an initiator having a total hydroxyl mole of 0.4 mol;
[0037] Step 2: introducing a mixture of 1320 g (30 mol) of ethylene oxide and 2320 g (30 mol) of propylene oxide into a reactor, causing the mixture of ethylene oxide and propylene oxide to undergo a nucleophilic substitution reaction with the active hydrogen in the initiator to generate a new structure with active hydrogen, and the new structure with active hydrogen continues to undergo an epoxy ring reaction with the mixture of ethylene oxide and propylene oxide until the reaction is completed, and aging after the reaction until the pressure in the reactor remains unchanged to generate a polyether polyol terminated with a mixed alkane; the aging refers to a chemical change that allows the incompletely reacted ethylene oxide or propylene oxide to fully react;
[0038] Step 3: 35.2 (0.8 mol) of ethylene oxide is introduced into the reactor. Under constant temperature conditions, ethylene oxide reacts with the new structure with active hydrogen generated in step 2 to generate a polyether polyol terminated with ethylene oxide of primary hydroxyl groups. The polyether polyol terminated with mixed alkane is also converted into a polyether polyol terminated with ethylene oxide of primary hydroxyl groups. After the reaction is completed, the reaction is aged until the pressure in the reactor remains unchanged. The aging refers to a chemical change that allows the incompletely reacted ethylene oxide to fully react.
[0039] Step 4: The temperature in the reactor is lowered to 40° C., and 69.2 g of a diisocyanate crosslinking agent having a concentration of 1% is introduced; under non-vacuum conditions, the diisocyanate in the diisocyanate crosslinking agent reacts with the primary hydroxyl group in the ethylene oxide-terminated polyether polyol of the primary hydroxyl group to generate a macromolecular polyether polyol;
[0040] Step 5: After the reaction is completed, the temperature is raised to 120° C. and vacuum is applied to remove the remaining solvent in the isocyanate cross-linking agent after the reaction to obtain an ultra-high viscosity water-soluble block polyether.
[0041] The effects of the above embodiments are compared in Table 1:
[0042] Case Foam (recipe) Viscosity (40℃) Viscosity Index Color (platinum-cobalt colorimetry) Specific embodiment 1 60 100000 500 30 Specific embodiment 2 43 85000 425 30 Specific embodiment 3 55 120000 440 30 Pluracol® V-10 (BASF) 89 66000 504 >30
[0043] It can be seen that the viscosity of the product manufactured by the method of the present invention is much greater than that of similar polymer polyether products.
[0044] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A one-pot method for synthesizing ultra-high viscosity water-soluble block polyethers, characterized in that: The steps are as follows: Step 1: placing a compound containing active hydrogen in a reaction kettle containing an initial polyether, adding a phosphazene catalyst to catalyze a nucleophilic substitution reaction between the active hydrogen and the initial polyether, and heating the reaction kettle to 130-150° C. after evacuation to ensure that the water content is less than 0.1%wt, to obtain an initiator with a total hydroxyl mole number of α; Step 2: introducing a mixture of ethylene oxide and propylene oxide into a reactor, causing the mixture of ethylene oxide and propylene oxide to undergo a nucleophilic substitution reaction with active hydrogen in the initiator to generate a new structure with active hydrogen, which continues to react with ethylene oxide and propylene oxide until the reaction is completed, and aging after the reaction until the pressure in the reactor remains unchanged to generate a polyether polyol terminated with a mixed alkane; the aging refers to a chemical change that allows the incompletely reacted ethylene oxide or propylene oxide to fully react; Step 3: introducing ethylene oxide into the reactor, and reacting the ethylene oxide with the polyether polyol generated in step 2 under constant temperature to generate a polyether polyol terminated with ethylene oxide of primary hydroxyl groups; the polyether polyol terminated with mixed alkane is also converted into a polyether polyol terminated with ethylene oxide of primary hydroxyl groups, and aging the reactor until the pressure in the reactor remains unchanged after the reaction is completed; the aging refers to a chemical change that allows the incompletely reacted ethylene oxide to fully react; Step 4: The temperature in the reactor is lowered to 30-65° C., and an isocyanate crosslinking agent is introduced; under non-vacuum conditions, the isocyanate in the isocyanate crosslinking agent reacts with the primary hydroxyl group in the ethylene oxide-terminated polyether polyol of the primary hydroxyl group to generate a macromolecular polyether polyol; Step 5: After the reaction is completed, the temperature is raised to 120° C. and vacuum is applied to remove the remaining solvent in the isocyanate cross-linking agent after the reaction to obtain an ultra-high viscosity water-soluble block polyether; The active hydrogen-containing compound in step 1 is a mixture of a liquid polyhydroxy compound and a liquid monohydroxy compound, wherein the liquid polyhydroxy compound is any one or any combination of ethylene glycol, propylene glycol, and glycerol, and the liquid monohydroxy compound is propylene glycol monomethyl ether and / or propylene glycol monobutyl ether; The added mass of the phosphazene catalyst is 1-5‰ of the total feed mass; The molar ratio of ethylene oxide to propylene oxide in step 2 is 50:(92-25), and the amount of the mixture of ethylene oxide and propylene oxide added is: for every 1 mol of hydroxyl groups contained in the initiator, there is (60-180) mol of the mixture of ethylene oxide and propylene oxide; The amount of ethylene oxide added in step 3 is 2α-4α in mole; In step 4, the amount of the isocyanate cross-linking agent added is such that the molar ratio of the isocyanate in the reaction kettle to the total hydroxyl group of the polyether is 1:(0.9-1.15).
2. The method for synthesizing ultra-high viscosity water-soluble block polyether by one-pot method according to claim 1, characterized in that: The isocyanate crosslinking agent contains 1-10%wt of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate or a mixture of 2,4-toluene diisocyanate and 2,6-toluene diisocyanate.
3. The method for synthesizing ultra-high viscosity water-soluble block polyether by one-pot method according to claim 2, characterized in that: The solvent used in the isocyanate cross-linking agent is any one of ether, acetone, tetrahydrofuran, and ethyl acetate, or any combination thereof.