A full cellulose composite membrane for oil-water separation and its preparation method and application

By combining regenerated cellulose with reinforcing cellulose materials in an oil-water separation membrane using a molten salt-water system, a hydrophilic-underwater superoleophobic all-cellulose composite membrane was prepared, solving the problems of poor compatibility and low separation efficiency, and achieving efficient and biodegradable oil-water separation.

CN113908704BActive Publication Date: 2024-11-22INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202111310919.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-05
Publication Date
2024-11-22
Estimated Expiration
2041-11-05

AI Technical Summary

Technical Problem

Existing oil-water separation membranes suffer from poor compatibility, low separation efficiency, expensive raw materials, and are not environmentally friendly enough, making it difficult to meet the needs of green and sustainable development.

Method used

Regenerated cellulose dissolved and regenerated in a molten salt-water system was used as a matrix and combined with reinforcing cellulose materials to prepare a hydrophilic-underwater superoleophobic all-cellulose composite membrane. The separation efficiency was improved by adjusting the material structure and pore size.

Benefits of technology

It achieves efficient oil-water separation, the material is completely biodegradable, has good compatibility, excellent mechanical properties, is green and environmentally friendly, and the pore size has been changed from micrometers to nanometers to improve separation efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113908704B_ABST
    Figure CN113908704B_ABST
Patent Text Reader

Abstract

The present invention belongs to the field of bio-based degradable materials, and specifically relates to a full cellulose composite membrane for oil-water separation, a preparation method and an application thereof. In order to solve the problems of poor compatibility of the matrix and substrate of the composite material, low separation efficiency, expensive raw materials and solvent systems and not being environmentally friendly, the present invention uses a cheap porous reinforced cellulose material as a substrate, and by a simple composite method, regenerated cellulose is fused with the substrate to construct a full cellulose network, wherein the regenerated cellulose is obtained by dissolving cellulose in a green solvent system such as zinc chloride-water and then regenerating it. The micropores of the original reinforced cellulose material are filled, which greatly improves the mechanical properties of the composite membrane under dry and wet conditions, and at the same time, the special hydrophilic-underwater super-oleophobic wetting properties of the composite membrane make it applicable to an efficient oil-water separation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of bio-based degradable materials, and specifically relates to a full-cellulose composite membrane for oil-water separation and a preparation method and application thereof. Background Art

[0002] In recent years, the rapid development of industry has inevitably led to serious water pollution problems. Among them, industrial emissions and oil leaks have caused oily wastewater to increase year by year, seriously affecting the marine ecological environment and human drinking water health. Traditional oil-water separation processes, such as gravity separation, high-speed centrifugation, chemical oil dispersants, etc., have a series of problems such as high energy consumption, complex process, and expensive equipment, which limits its application in the separation process. Membrane separation technology has become a very effective means in the oil-water separation process due to its simple operation. Common polymer membranes, such as polysulfone (PSF), polyimide (PI), polyvinylidene fluoride (PVDF) and polydimethylsiloxane (PDMS), have good separation efficiency, but they are difficult to be degraded by environmental microorganisms, and are prone to oil blockage during the separation process, which does not meet the contemporary green and sustainable requirements. Therefore, there is a need to find an efficient, low-cost, and green oil-water separation membrane to solve the above problems.

[0003] As a pure green substrate, porous cellulose reinforced materials are often used in composite materials for oil-water separation. The porous cellulose reinforced material has multiple hydroxyl groups on the surface, high surface energy, and is easy to undergo physical or chemical crosslinking with the external matrix. Its own macropores also help the matrix to adhere. Patent CN108854567A: A method for preparing an oil-water separation membrane, wherein the filter paper is directly immersed in a super-hydrophobic polymer solution, and a super-hydrophobic-super-oleophilic composite separation membrane is obtained after the solvent evaporates. However, this separation membrane only allows oil to pass through, and the oil phase present in the separation membrane is difficult to handle during the subsequent circulation process. Patent CN112982020A: A method for preparing a high-strength, high-efficiency oil-water separation filter paper, wherein nickel-doped hydroxy copper sulfate nanosheets are deposited on the surface of cellulose filter paper modified by crosslinking polyethyleneimine and glutaraldehyde to obtain a high-efficiency composite filter paper with super-hydrophilic-underwater super-oleophobic properties, but since the nanosheets are incompatible with the substrate material to form a heterogeneous structure, there is a risk of surface matrix shedding, which is easy to cause secondary pollution of copper and nickel heavy metals. Patent CN113005815A: A full-cellulose composite paper for oil-water separation, and its preparation method and application. Well-dispersed nanocellulose is attached to the surface of the filter paper to form a super-hydrophilic-underwater super-oleophobic composite filter paper. The nanocellulose on the surface of the material is homogeneous with the base filter paper, has strong hydrogen bonding, and is not easy to peel off from the base material. However, the nanocellulose is expensive and not suitable for large-scale production. Summary of the invention

[0004] In view of the problems in the prior art, such as poor compatibility of composite materials, low separation efficiency, expensive and environmentally friendly raw materials and solvent systems, the present invention provides a kind of all-cellulose composite membrane for oil-water separation and its preparation method and application. The preparation method selects the regenerated cellulose dissolved and regenerated by the molten salt-water system as a matrix, and the reinforced cellulose material is used as a substrate to prepare a hydrophilic-underwater super-oleophobic green and degradable all-cellulose composite membrane that can be used for efficient oil-water separation through a simple composite process. This composite membrane composed of all-cellulose can adjust the structure and pore size of the material by changing the preparation process conditions, and can also increase the underwater super-oleophobicity of the material; good compatibility facilitates the stability of the structure and gives the material good mechanical properties; green and pollution-free raw materials, and the solvent system make the entire production process more green and environmentally friendly.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A full cellulose composite membrane for oil-water separation is composed of a base material and a cellulose matrix. The base material is a reinforced cellulose material, and the cellulose matrix is ​​regenerated cellulose added from the outside and obtained by cellulose phase transformation.

[0007] Furthermore, the cellulose is one of α-microcrystalline cellulose powder, cotton pulp, cotton linters, or a mixture of several of them in any ratio; the reinforced cellulose material is one of commercial filter paper, cotton cloth, and gauze. Such cellulose is mainly α-cellulose, has fewer impurities, and is easy to dissolve. Such reinforced cellulose materials are low in price, porous, and have excellent mechanical strength, and are a good choice as base materials.

[0008] A method for preparing a full cellulose composite membrane for oil-water separation comprises the following steps:

[0009] Step 1, adding cellulose to a zinc chloride-water system, heating to dissolve the cellulose, and obtaining a cellulose solution;

[0010] Step 2, compounding the enhanced cellulose material with the cellulose solution obtained in step 1, regenerating in an anti-solvent immediately after compounding, and obtaining a full cellulose composite membrane after drying. The full cellulose composite membrane for oil-water separation prepared by the above method has good compatibility between the matrix and the substrate, stable structure, excellent mechanical strength, obvious effect when used for oil-water separation, and the material is completely green and degradable.

[0011] Furthermore, in the step 1, the mass ratio of zinc chloride to water in the zinc chloride-water system is 2.0 to 2.5:1, and the mass ratio of cellulose to the zinc chloride-water system is 1:25 to 100. Within this range, the mass ratio of the zinc chloride-water system is 2+ The complex is not completely formed with water, so the hydroxyl groups of cellulose can further react with Zn 2+The mass ratio of cellulose to zinc chloride-water system is within this range, the dissolution effect is good, and the solution viscosity is moderate and suitable as a flow matrix.

[0012] Furthermore, the heating temperature in step 1 is 60-90° C. When the heating temperature and stirring reaction are within this range, the cellulose is completely dissolved and the required time is short.

[0013] Furthermore, the compounding temperature in step 2 is 20-60° C. Compounding at the above temperature can ensure the fluidity of the matrix solution and ensure that the zinc chloride-water system does not significantly degrade the substrate. The compounding method is solution impregnation and surface coating. By using the impregnation or coating method, the cellulose material can be enhanced to combine with the cellulose solution in a short time.

[0014] Furthermore, the anti-solvent in step 2 is a mixture of deionized water, methanol, ethanol, a 5-10% mass fraction of hydrochloric acid aqueous solution, a sulfuric acid aqueous solution, a phosphoric acid aqueous solution, and an acetic acid aqueous solution, or a mixture of several of them in any proportion. The above solvents have a certain solubility in zinc chloride. During the regeneration process, the zinc chloride in the composite membrane can be replaced to prevent the influence of zinc chloride on the subsequent process.

[0015] Furthermore, the drying temperature in step 2 is 10-100° C. When the membrane material is dried within this temperature range, water can be completely removed while maintaining its good performance.

[0016] The invention discloses an application of a full cellulose composite membrane for oil-water separation, which is applied to oil-water separation.

[0017] Furthermore, the oil-water separation is separation of oil-water mixture and separation of oil-in-water emulsion containing emulsifier.

[0018] Preferably, the oil phase in the oil-water mixture and the oil-in-water emulsion is an organic solvent such as petroleum ether, anisole, toluene, xylene, n-hexane, cyclohexane, n-heptane, dichloromethane, chloroform, carbon tetrachloride, etc., edible oils such as soybean oil, rapeseed oil, peanut oil, olive oil, etc., and industrial oils such as crude oil, kerosene, diesel, gasoline, etc., or a mixture of at least two of them in any proportion.

[0019] Compared with the prior art, the present invention has the following advantages:

[0020] 1. Zinc chloride-water is used as the solvent of cellulose, avoiding the use of organic solvents, making the system more green and economical; the base and matrix of the material are both cellulose, avoiding the problem of weak matrix bonding and falling off due to different qualities, and the prepared material is completely biodegradable.

[0021] 2. The pore size of the prepared all-cellulose composite membrane has changed from the original micropore to nanopore, which is more conducive to blocking oil penetration and greatly increases the efficiency of oil-water separation.

[0022] 3. The all-cellulose composite membrane has good mechanical properties in both dry and wet states, which is a significant improvement over the original commercial filter paper. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is the XRD result of the all-cellulose composite film prepared in Example 6 of the present invention;

[0024] Figure 2 The contact angle of water in air and the contact angle of oil underwater of the all-cellulose composite membrane prepared in Example 6 of the present invention;

[0025] Figure 3 This is a scanning electron microscope image of the all-cellulose composite membrane prepared in Example 6 of the present invention;

[0026] Figure 4 This is a graph showing the color change before and after the all-cellulose composite membrane prepared in Example 6 of the present invention filtered the anisole-in-water emulsion. DETAILED DESCRIPTION

[0027] The present invention is described clearly and completely below in conjunction with the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited thereby.

[0028] In order to test the application effect of the prepared all-cellulose composite membrane, the prepared all-cellulose composite membrane was pre-soaked in deionized water and then fixed on an oil-water separation experimental device. 20 mL of deionized water was mixed with 20 mL of petroleum ether and separated. The separation efficiency of the oil-water mixture was calculated by the mass method. After 20 mL of deionized water was mixed with 1 mL of anisole, 10 mg of sodium dodecyl sulfate was added and the mixture was mixed under strong mechanical stirring to obtain an oil-in-water emulsion, which was separated. The separation efficiency of the oil-in-water emulsion was calculated using a UV-visible spectrophotometer.

[0029] Example 1

[0030] A full-cellulose composite membrane for oil-water separation is composed of a base material and a cellulose matrix. The base material is commercial filter paper, and the cellulose matrix is ​​regenerated cellulose obtained by phase transformation of α-microcrystalline cellulose powder added from the outside.

[0031] A method for preparing a full cellulose composite membrane for oil-water separation comprises the following steps:

[0032] Weigh 20g zinc chloride and 0.3g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 60℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 20℃, soak the commercial filter paper in the cellulose solution for 1min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in a 5% hydrochloric acid aqueous solution to regenerate it, and wash it to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane was measured by a drop shape analyzer to be 9°, and the contact angle of oil under water was 142°. The tensile strength of the dry film was 38MPa and the tensile strength of the wet film was 8MPa obtained by a universal testing machine. The separation efficiency of oil-water mixture is 95.4%; the separation efficiency of oil-in-water is 97.8%.

[0033] Example 2

[0034] Weigh 25g zinc chloride and 0.40g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 70℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 20℃, soak the commercial filter paper in the cellulose solution for 5min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in a 5% hydrochloric acid aqueous solution to regenerate it, and wash it to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane was measured by a drop shape analyzer to be 15°, and the contact angle of oil under water was 143°. The tensile strength of the dry film was 40MPa and the tensile strength of the wet film was 9MPa obtained by a universal testing machine. The separation efficiency of oil-water mixture is 96.1%; the separation efficiency of oil-in-water is 98.0%.

[0035] Example 3

[0036] Weigh 25g zinc chloride and 0.46g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 30℃, soak the commercial filter paper in the cellulose solution for 7min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in a 5% sulfuric acid aqueous solution for regeneration, and wash to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 8°, and the contact angle of oil under water is 150°, as measured by a drop shape analyzer. The tensile strength of the dry film is 33MPa, and the tensile strength of the wet film is 7MPa, as measured by a universal testing machine. The separation efficiency of oil-water mixture is 95.1%; the separation efficiency of oil-in-water is 96.3%.

[0037] Example 4

[0038] Weigh 25g zinc chloride and 0.35g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 40℃, soak the commercial filter paper in the cellulose solution for 9min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in a 5% phosphoric acid aqueous solution for regeneration, and wash to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 21°, and the contact angle of oil under water is 152°, measured by a drop shape analyzer. The tensile strength of the dry film is 46MPa, and the tensile strength of the wet film is 11MPa, obtained by a universal testing machine. The separation efficiency of oil-water mixture is 96.9%; the separation efficiency of water-in-oil is 99.1%.

[0039] Example 5

[0040] Weigh 25g zinc chloride and 0.35g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 90℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 50℃, soak the commercial filter paper in the cellulose solution for 12min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in a 10% hydrochloric acid aqueous solution to regenerate, and wash to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane was measured by a drop shape analyzer to be 18°, and the contact angle of oil under water was 148°. The tensile strength of the dry film was 42MPa and the tensile strength of the wet film was 10MPa obtained by a universal testing machine. The separation efficiency of oil-water mixture is 97.1%; the separation efficiency of oil-in-water is 99.2%.

[0041] Example 6

[0042] Weigh 25g zinc chloride and 0.70g α-microcrystalline cellulose powder into a flask, add 10mL deionized water, and stir at 80°C for 30min to dissolve the cellulose into a transparent viscous liquid. In a high and low temperature box at 30°C, soak the commercial filter paper in the cellulose solution for 9min, then take it out and scrape off the excess cellulose solution on the surface. Immediately soak it in a 10% by mass sulfuric acid aqueous solution to regenerate it, and wash it to obtain a wet all-cellulose composite membrane. After fixing the wet membrane, place it in a vacuum drying oven at 40°C to completely dry it to obtain a all-cellulose composite membrane. Figure 1, XRD results show that the characteristic diffraction peaks of cellulose appear at 2θ = 14.9°, 16.4°, 22.8° and 34.2°. After fitting, it is shown that the composite film is a mixture of type I and type II cellulose; Figure 2 The instantaneous contact angle of water in air and oil in water of the all-cellulose composite membrane measured by drop shape analyzer was 32° and 152° respectively; Figure 3 Scanning electron microscopy shows that the commercial filter paper has been filled with regenerated cellulose and has nanopores; the tensile strength of the dry film obtained by the universal testing machine is 54MPa, and the tensile strength of the wet film is 16MPa. The separation efficiency of oil-water mixture is 98.2%; the separation efficiency of water-in-oil is 99.9%. Figure 4 It can be seen that the color of the emulsion changes from milky white to colorless before and after separation.

[0043] Example 7

[0044] Weigh 25g zinc chloride and 0.70g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. When the cellulose solution is preheated to 50℃, the surface of the commercial filter paper is coated, and then immediately immersed in a 10% mass fraction hydrochloric acid aqueous solution for regeneration and washing to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 6°, and the contact angle of oil under water is 146°, as measured by a drop shape analyzer. The tensile strength of the dry film is 25MPa, and the tensile strength of the wet film is 4MPa, as measured by a universal testing machine. The separation efficiency of oil-water mixture is 90.2%; the separation efficiency of oil-in-water is 93.0%.

[0045] Example 8

[0046] Weigh 20g zinc chloride and 1.20g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. When the cellulose solution is preheated to 30℃, the surface of the commercial filter paper is coated, and then immediately immersed in a 10% mass fraction phosphoric acid aqueous solution for regeneration and washing to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 5°, and the contact angle of oil under water is 148°, as measured by a drop shape analyzer. The tensile strength of the dry film is 21MPa, and the tensile strength of the wet film is 6MPa, as measured by a universal testing machine. The separation efficiency of oil-water mixture is 91.3%; the separation efficiency of oil-in-water is 93.5%.

[0047] Example 9

[0048] Weigh 25g zinc chloride and 0.70g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. When the cellulose solution is preheated to 30℃, the surface of the cotton cloth is coated, and then immediately immersed in deionized water for regeneration and washing to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 10℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 8°, and the contact angle of oil under water is 138°, as measured by a drop shape analyzer. The tensile strength of the dry film is 29MPa, and the tensile strength of the wet film is 25MPa, as measured by a universal testing machine. The separation efficiency of oil-water mixture is 93.5%; the separation efficiency of oil-in-water is 94.1%.

[0049] Example 10

[0050] Weigh 25g zinc chloride and 0.70g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. When the cellulose solution is preheated to 60℃, the surface of the gauze is coated, and then immediately immersed in deionized water for regeneration and washing to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 60℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane was measured by a drop shape analyzer to be 12°, and the contact angle of oil under water was 140°. The tensile strength of the dry film was 28MPa and the tensile strength of the wet film was 28MPa obtained by a universal testing machine. The separation efficiency of oil-water mixture is 93.3%; the separation efficiency of oil-in-water is 94.9%.

[0051] Embodiment 11

[0052] Weigh 25g zinc chloride and 0.35g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 70℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 40℃, soak the cotton cloth in the cellulose solution for 9min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in deionized water for regeneration, wash and obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 80℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 9°, and the contact angle of oil under water is 150°, as measured by a drop shape analyzer. The tensile strength of the dry film is 38MPa, and the tensile strength of the wet film is 30MPa, as measured by a universal testing machine. The separation efficiency of oil-water mixture is 95.1%; the separation efficiency of oil-in-water is 97.6%.

[0053] Example 12

[0054] Weigh 25g zinc chloride and 0.70g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 90℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 50℃, soak the gauze in the cellulose solution for 12min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in a 10% hydrochloric acid aqueous solution to regenerate it, and wash it to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 80℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane was measured by a drop shape analyzer to be 11°, and the contact angle of oil under water was 149°. The tensile strength of the dry film was 31MPa and the tensile strength of the wet film was 20MPa obtained by a universal testing machine. The separation efficiency of oil-water mixture is 95.6%; the separation efficiency of oil-in-water is 96.6%.

[0055] Example 13

[0056] Weigh 25g zinc chloride and 0.70g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 50℃, soak the gauze in the cellulose solution for 7min, take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in anhydrous ethanol for regeneration, wash to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 20℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 8°, and the contact angle of oil under water is 148°, which is measured by a drop shape analyzer. The tensile strength of the dry film is 30MPa, and the tensile strength of the wet film is 23MPa, which is obtained by a universal testing machine. The separation efficiency of oil-water mixture is 91.9%; the separation efficiency of water-in-oil is 95.4%.

[0057] Embodiment 14

[0058] Weigh 25g zinc chloride and 0.70g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 30℃, soak the commercial filter paper in the cellulose solution for 12min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in methanol to regenerate it, and wash it to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 100℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane was measured by a drop shape analyzer to be 30°, and the contact angle of oil under water was 151°. The tensile strength of the dry film was 48MPa and the tensile strength of the wet film was 15MPa obtained by a universal testing machine. The separation efficiency of oil-water mixture is 96.9%; the separation efficiency of oil-in-water is 99.2%.

[0059] Embodiment 15

[0060] Weigh 25g zinc chloride and 0.30g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 60℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 30℃, soak the commercial filter paper in the cellulose solution for 12min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in a 5% acetic acid aqueous solution for regeneration, and wash to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 23°, and the contact angle of oil under water is 148°, as measured by a drop shape analyzer. The tensile strength of the dry film is 44MPa, and the tensile strength of the wet film is 12MPa, as measured by a universal testing machine. The separation efficiency of oil-water mixture is 96.4%; the separation efficiency of oil-in-water is 98.3%.

[0061] Example 16

[0062] Weigh 25g zinc chloride and 0.70g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. In a high and low temperature box at 30℃, soak the commercial filter paper in the cellulose solution for 9min, then take it out, scrape off the excess cellulose solution on the surface, and immediately soak it in a 10% acetic acid aqueous solution for regeneration, and wash to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 32°, and the contact angle of oil under water is 152°, as measured by a drop shape analyzer. The tensile strength of the dry film is 51MPa, and the tensile strength of the wet film is 15MPa, as measured by a universal testing machine. The separation efficiency of oil-water mixture is 98.4%; the separation efficiency of oil-in-water is 99.7%.

[0063] Embodiment 17

[0064] Weigh 25g zinc chloride and 1.40g α-microcrystalline cellulose powder in a flask, add 10mL deionized water, stir at 80℃ for 30min to dissolve cellulose into a transparent viscous liquid. When the cellulose solution is preheated to 50℃, the surface of the commercial filter paper is coated, and then immediately immersed in a 10% mass fraction hydrochloric acid aqueous solution for regeneration and washing to obtain a wet all-cellulose composite membrane. After the wet membrane is fixed, it is placed in a vacuum drying oven at 40℃ to completely dry to obtain a all-cellulose composite membrane. The instantaneous contact angle of water in the air of the all-cellulose composite membrane is 5°, and the contact angle of oil under water is 139°, which is measured by a drop shape analyzer. The tensile strength of the dry film is 28MPa, and the tensile strength of the wet film is 5MPa, which is obtained by a universal testing machine. The separation efficiency of oil-water mixture is 92.8%; the separation efficiency of oil-in-water is 95.7%.

Claims

1. Application of a full cellulose composite membrane in oil-water separation, characterized in that: The all-cellulose composite membrane is composed of a base material and a cellulose matrix, wherein the base material is a reinforced cellulose material, and the cellulose matrix is ​​regenerated cellulose obtained by phase transformation of cellulose added from the outside; The preparation method is as follows: Step 1, adding cellulose to a zinc chloride-water system, heating and stirring to dissolve the cellulose, and obtaining a cellulose solution; Step 2, compounding the enhanced cellulose material with the cellulose solution obtained in step 1, regenerating in an anti-solvent immediately after compounding, and obtaining a full cellulose composite membrane after drying; The anti-solvent in step 2 is one or a mixture of deionized water, methanol, ethanol, a 5-10% by mass hydrochloric acid aqueous solution, a 5-10% by mass sulfuric acid aqueous solution, a 5-10% by mass phosphoric acid aqueous solution, and a 5-10% by mass acetic acid aqueous solution in any proportion; The reinforced cellulose material is one of commercial filter paper, cotton cloth and gauze; the cellulose is one of α-microcrystalline cellulose powder, cotton pulp and cotton linters or a mixture of several of them in any ratio.

2. The use of a full cellulose composite membrane in oil-water separation according to claim 1, characterized in that: In the step 1, the mass ratio of zinc chloride to water in the zinc chloride-water system is 2.0-2.5:1, and the mass ratio of cellulose to the zinc chloride-water system is 1:25-100.

3. The use of a full cellulose composite membrane in oil-water separation according to claim 1, characterized in that: The heating temperature in step 1 is 60-90°C.

4. The use of a full cellulose composite membrane in oil-water separation according to claim 1, characterized in that: The compounding temperature in step 2 is 20-60° C., and the compounding method is solution dipping and surface coating.

5. The use of a full cellulose composite membrane in oil-water separation according to claim 1, characterized in that: The drying temperature in step 2 is 10-100°C.

6. The use of a full cellulose composite membrane in oil-water separation according to claim 1, characterized in that: The oil-water separation is separation of oil-water mixture and separation of oil-in-water emulsion containing emulsifier.

Citation Information

Patent Citations

  • Oil-water separation membrane preparation method

    CN108854567A

  • Preparation method of high-strength and efficient oil-water separation filter paper

    CN112982020A

  • Holocellulose composite paper for oil-water separation as well as preparation method and application of holocellulose composite paper

    CN113005815A

  • Method for treating oil-containing sewage by utilizing oil-water separator

    CN105858930A

  • Preparation method of lignosulfonate cellulose composite film

    CN110283349A