Battery, battery preparation method, battery testing method and electronic device
By setting a conductive film layer on the shell and the surface of the button battery, the direct welding of the pole ear and the shell is ensured, and the welding status is judged by the resistance value, the problem of low accuracy in welding detection of button battery in the prior art is solved. Improves the quality of the battery and welding success rate.
Patent Information
- Application Number
- CN202111166295.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-09-30
AI Technical Summary
The existing button batteries have low accuracy when detecting the success of welding of the electrode ears and steel shells, which may cause unwelded batteries to occur, affecting battery quality.
The conductive film layer is installed on the surface of the shell and the electrode, so that the electrode ear and the shell are directly in contact with each other successfully during external welding, and the welding status is judged by the resistance value to ensure that the internal resistance value of the battery is the standard value during welding and is not welded greater than the standard value.
The success rate and battery quality of the electrode welding to the shell are improved, and the welding status is determined by judging the resistance value of the conductive film layer to avoid misjudgment, which enhances the yield rate of the battery.
Smart Images

Figure CN113937428B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and more specifically, to a battery, a battery preparation method, a battery detection method and an electronic device. Background Art
[0002] Button batteries are increasingly used, especially in small mobile devices such as earphones. The positive and negative electrodes of the battery cell inside the button battery are connected to two steel shells respectively. The steel shells are sealed together to form a button battery, and the steel shells serve as positive and negative electrodes for conductivity.
[0003] After the two steel shells are encapsulated, at least one tab and the inner surface of one steel shell need to be welded by external welding. When using the external welding method, the tab and the steel shell need to have good contact to be welded successfully. The way to detect whether the tab and the steel shell are welded successfully is: generally, it is detected by powering on.
[0004] However, the accuracy of detecting whether the tabs and the steel shell are successfully welded is not high at present. Due to the small internal space of the button battery, the tabs may still come into contact with the shell, resulting in the tabs and the shell not being welded successfully. However, during the test, the battery is still shown to be in a conductive state, resulting in the tabs and the steel shell not being welded in the batteries shipped from the factory, affecting the battery quality. Summary of the invention
[0005] One object of the present application is to provide a new technical solution for a battery, a battery preparation method, a battery detection method and an electronic device.
[0006] According to a first aspect of the present application, a battery is provided. The battery comprises:
[0007] A housing having a receiving cavity formed therein;
[0008] A battery cell, wherein the battery cell is disposed in the accommodating cavity, and an end surface of the battery cell is opposite to an inner surface of the shell;
[0009] The battery core is provided with a pole ear, and the pole ear has a first surface arranged opposite to the inner surface of the shell;
[0010] A conductive film layer is provided on the inner surface of the housing and / or the first surface of the tab;
[0011] When the pole tab and the shell are in a welding state, the pole tab and the shell are in direct contact and welded;
[0012] When the pole tab and the shell are in an unwelded state, the pole tab and the shell are electrically connected through the conductive film layer, or the pole tab and the shell are not electrically connected.
[0013] Optionally, when the tab and the shell are in a welding state, the resistance value inside the battery is a standard resistance value;
[0014] When the tab and the shell are not welded, the resistance value inside the battery is greater than the standard resistance value.
[0015] Optionally, the material of the conductive film layer is solder.
[0016] Optionally, when the pole tab and the shell are in a welded state, a welding portion is formed between the pole tab and the shell, and the pole tab and the shell are in direct contact through the welding portion.
[0017] Optionally, the external welding method between the electrode tab and the shell is resistance welding.
[0018] According to the second aspect of the present application, a method for preparing the battery according to the first aspect is provided, the method comprising the following steps:
[0019] providing a housing;
[0020] Providing a battery cell, wherein the battery cell is arranged in the housing and has a tab;
[0021] Disposing a conductive film layer on the inner surface of the housing and / or the first surface of the tab;
[0022] The pole tab is welded to the shell by external welding, and the pole tab is directly in contact with and welded to the shell.
[0023] According to a third aspect of the present application, a method for detecting the battery described in the first aspect is provided. The detection method comprises the following steps:
[0024] Provide the battery to be tested;
[0025] Detect the resistance value inside the battery to be tested;
[0026] The resistance value is used to determine whether the electrode tab and the shell are successfully welded.
[0027] Optionally, when the electrode tab and the shell are in a welding state, the internal resistance value of the battery is a standard resistance value;
[0028] When the electrode tab and the shell are not welded, the resistance value inside the battery is greater than the standard resistance value.
[0029] According to a third aspect of the present application, an electronic device is provided, comprising the battery according to the first aspect.
[0030] One technical effect of the present application is that the present application provides a battery, which includes a shell, a battery cell and a conductive film layer. A conductive film layer is provided on the inner surface of the shell and / or the first surface of the pole ear. During the external welding process, the pole ear of the present application is in direct contact with the shell and electrically connected, and the shell and the pole ear will be welded successfully. If after welding the shell and the pole ear, the shell and the pole ear are still isolated by the conductive film layer, the shell and the pole ear are not welded successfully. The present application provides a conductive film layer on the inner surface of the shell and / or the first surface of the pole ear, which is convenient for the inspection personnel to judge whether the shell and the pole ear are in a welding state.
[0031] Other features and advantages of the present application will become apparent from the following detailed description of exemplary embodiments of the present application with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The accompanying drawings, which constitute a part of the specification, illustrate embodiments of the present application and, together with the description, serve to explain the principles of the present application.
[0033] Figure 1 The structure of the battery of this application is shown as follows Figure 1 .
[0034] Figure 2 The structure of the battery of this application is shown as follows Figure 2 .
[0035] Figure 3 Shown is a schematic diagram of the structure of the battery cell of this application.
[0036] Figure 4 Shown is a flow chart of the battery preparation method of the present application.
[0037] Figure 5 Shown is a flow chart of the battery detection method of the present application.
[0038] Description of reference numerals:
[0039] 1. Shell; 11. First shell; 12. Second shell; 13. Insulating component; 2. Battery cell; 21. Tab; 21a. First tab; 21b. Second tab; 3. Conductive film layer; 31. Welding part. DETAILED DESCRIPTION
[0040] Various exemplary embodiments of the present application will now be described in detail with reference to the accompanying drawings. It should be noted that unless otherwise specifically stated, the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present application.
[0041] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the present application, its application, or uses.
[0042] Techniques and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the techniques and equipment should be considered part of the specification.
[0043] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0044] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0045] According to one embodiment of the present disclosure, a battery is provided. Figure 1-Figure 3 As shown, the battery comprises: a shell 1, wherein a receiving cavity is formed in the shell 1; a battery cell 2, wherein the battery cell 2 is arranged in the receiving cavity, and the end surface of the battery cell 2 is opposite to the inner surface of the shell 1; and a tab 21 is arranged on the battery cell 2, wherein the tab 21 has a first surface arranged opposite to the inner surface of the shell 1.
[0046] A conductive film layer 3 is provided on the inner surface of the housing 1 and / or the first surface of the pole ear 21; when the pole ear 21 and the housing 1 are in a state of successful welding, the pole ear 21 is in direct contact with and welded to the housing 1;
[0047] When the pole tab 21 and the shell 1 are not welded, the pole tab 21 and the shell 1 are electrically connected through the conductive film layer 3 , or the pole tab 21 and the shell 1 are not electrically connected.
[0048] In other words, the battery mainly includes a shell 1 , a battery cell 2 , and a conductive film layer 3 .
[0049] The housing 1 comprises a first housing 11 and a second housing 12. The first housing 11 comprises a first annular side wall and a first bottom connected to the first annular side wall. The second housing 12 comprises a second annular side wall and a second bottom connected to the second annular side wall.
[0050] The first shell 11 and the second shell 12 are sleeved and arranged to enclose and form a receiving cavity. For example, the first shell 11 is buckled inside the second shell, the first annular side wall partially overlaps with the second annular side wall, and the first bottom and the second bottom are opposite.
[0051] An insulating member 13 is provided between the first housing 11 and the second housing 12 , and the insulating member 13 isolates the first housing 11 from the second housing 12 .
[0052] The battery cell 2 is disposed in the accommodating cavity enclosed by the shell 1. The battery cell 2 is formed by winding the positive electrode sheet, the separator and the negative electrode sheet. The wound battery cell 2 has two end faces, one of which is opposite to the first bottom of the first shell 11, and the other end face is opposite to the second bottom of the second shell 12.
[0053] The battery cell 2 is provided with a tab 21. The tab 21 includes a first tab 21a and a second tab 21b. The first tab 21a is electrically connected to the positive electrode sheet, and the second tab 21b is electrically connected to the negative electrode sheet; or the first tab 21a is electrically connected to the negative electrode sheet, and the second tab 21b is connected to the positive electrode sheet.
[0054] The tab 21 is disposed on the battery cell 2, and the tab 21 is bent so that the first surface of the tab 21 is disposed opposite to the inner surface of the housing 1. For example, the first surface of the tab 21 is disposed opposite to one of the bottom surfaces of the housing 1. At the same time, the second surface of the tab 21 is disposed opposite to the end surface of the battery cell 2, wherein an insulating pad is disposed between the second surface of the tab 21 and the battery cell 2 to prevent the second surface of the tab 21 from contacting the end surface of the battery cell 2 and causing a short circuit in the battery.
[0055] In the embodiment of the present application, a conductive film layer 3 is provided between the shell 1 and the tab 21. When the shell 1 and the tab 21 are welded by external welding, it is convenient for the inspector to judge whether the shell 1 and the tab 21 are successfully welded, and avoid the situation where the tab 21 is only attached to the shell 1 (the tab 21 and the shell 1 are not welded. But due to the narrow internal space, the tab 21 is attached to the inner surface of the shell 1). In the case where the tab 21 is attached to the shell 1, when testing this type of battery, the resistance value inside the battery is the same as the resistance when the tab 21 and the shell 1 are in the welding state, which will mislead the inspector to judge whether the battery is qualified.
[0056] In the embodiments of this application, refer to Figure 3 As shown, the electrode tab 21 includes a first electrode tab 21 a and a second electrode tab 21 b . A first conductive film layer is disposed on the first electrode tab 21 a , and a second conductive film layer is disposed on the second electrode tab 21 b .
[0057] In the embodiment of the present application, a conductive film layer 3 is provided on the inner surface of the housing 1 and / or on the first surface of the tab 21. In one embodiment, a conductive film layer 3 is provided on the inner surface of the housing 1. In another embodiment, a conductive film layer 3 is provided on the first surface of the tab 21. In yet another embodiment, a conductive film layer 3 is provided on both the inner surface of the housing 1 and the first surface of the tab 21.
[0058] Figure 2 Schematic diagram of the tab 21 and the housing 1 in an unwelded state. Figure 2As shown, when the shell 1 and the tab 21 are welded by external welding, if the shell 1 and the tab 21 are welded, but in fact the two are not welded, the welding condition is not clear to the inspector, and it is only clear after the inspection. At this time, when the inspector inspects the battery, since the conductive film layer 3 is set between the shell 1 and the tab 21, the conductive film layer 3 separates the shell 1 and the tab 21, and the shell 1 and the tab 21 are electrically connected through the conductive film layer 3. When the battery to be inspected is inspected by the inspection equipment, the resistance value inside the battery includes the resistance of the conductive film layer, and the resistance value inside the battery is relatively large.
[0059] Or the tab 21 and the housing 1 are not welded, and the tab 21 and the housing 1 are not connected. For example, the tab 21 is not in contact with the conductive film layer 3, and the tab 21 is not in contact with the inner surface of the housing 1. At this time, the battery is in an open circuit state, and the resistance inside the battery is infinite.
[0060] Figure 1 FIG. 2 is a schematic diagram showing that the electrode tab 21 and the housing 1 are successfully welded. Figure 1 As shown, although the conductive film layer 3 is located between the shell 1 and the tab 21, the tab 21 is in direct contact with the inner surface of the shell 1 and is welded. When the shell 1 and the tab 21 are welded by external welding, if the shell 1 and the tab 21 are welded by external welding, the shell 1 and the tab 21 are actually welded successfully. However, the welding condition tester is not clear, and it is only clear after the test. In the case of external welding, the energy generated by the external welding method acts on the shell 1 and the tab 21 on the one hand, and the energy generated by the external welding method also acts on the conductive film layer 3 on the other hand. The energy generated by the external welding method makes part of the tab 21 and part of the shell 1 in a molten state, so that the tab 21 and the shell 1 can be directly in contact and welded. When the battery to be tested is tested by the testing equipment, since the tab 21 is in direct contact with the shell 1 and welded, the current inside the battery will not pass through the conductive film layer 3. Therefore, when the tab 21 is successfully welded to the shell 1, the resistance value inside the battery does not include the resistance value of the conductive film layer 3, and the resistance value inside the battery is small.
[0061] The present application provides a battery, which includes a shell 1, a battery cell 2 and a conductive film layer 3. A conductive film layer 3 is provided on the inner surface of the shell 1 and / or the first surface of the pole tab 21. During the external welding process, the shell 1 and the pole tab 21 will be successfully welded only when the pole tab 21 is in direct contact with the shell 1 and electrically connected. If after welding the shell 1 and the pole tab 21, the shell 1 and the pole tab 21 are still isolated by the conductive film layer 3, the shell 1 and the pole tab 21 are not successfully welded. The present application provides a conductive film layer 3 on the inner surface of the shell 1 and / or the first surface of the pole tab 21, which is convenient for the inspector to judge whether the shell 1 and the pole tab 21 are successfully welded, and further facilitates the inspector to judge whether the battery is qualified.
[0062] In one embodiment, when the electrode tab 21 and the housing 1 are successfully welded, the resistance value inside the battery is a standard resistance value;
[0063] When the tab 21 and the housing 1 are not welded, the resistance value inside the battery is greater than the standard resistance value.
[0064] When the pole tab 21 and the shell 1 are in a state of successful welding, when the battery to be tested is tested by the testing equipment, since the pole tab 21 is in direct contact and welding with the shell 1, the current inside the battery will not pass through the conductive film layer 3. Therefore, when the pole tab 21 and the shell 1 are successfully welded, the resistance value inside the battery does not include the resistance value of the conductive film layer 3, and the resistance value inside the battery is small. The resistance value inside the battery is ohmic resistance. For example, the resistance value inside the battery includes the sum of the electrode material, electrolyte, and diaphragm resistance.
[0065] When the tab 21 and the shell 1 are successfully welded, the resistance value inside the battery is a standard resistance value. The standard resistance value is a range value. When the resistance value inside the battery detected is within the range value, it can be determined that the tab 21 and the shell 1 in the detected battery are welded.
[0066] Specifically, when the tab 21 is in direct contact with the shell 1 (the resistance value of the battery internal resistance (excluding the conductive film layer) is very small, generally in the order of micro-ohms or milliohms), the conductive film layer 3 is equivalent to a load set inside the battery, the conductive film layer 3 is connected to the inside of the battery, the conductive film layer 3 is equivalent to being short-circuited, and the resistance value in the conductive film layer 3 is much greater than the resistance value inside the battery in the successful welding state. According to the principle of current path selection, the current will not choose to flow into the conductive film layer 3 (large resistance value). Therefore, when the tab 21 is successfully welded to the shell 1, the resistance value inside the battery is less than the resistance value inside the battery when the tab 21 and the shell 1 are not welded.
[0067] When the tab 21 and the housing 1 are not welded successfully, the tab 21 and the housing 1 are separated by the conductive film layer 3. For example, in one embodiment, the tab 21 and the housing 1 are electrically connected through the conductive film layer 3. The resistance value inside the battery is an ohmic resistance. For example, the resistance value inside the battery includes the sum of the electrode material, the electrolyte, the diaphragm resistance and the conductive film layer 3.
[0068] Therefore, when the pole tab 21 and the shell 1 are not welded successfully, the conductive film layer 3 is connected between the pole tab 21 and the shell 1. Therefore, when the pole tab 21 and the shell 1 are not welded successfully, the resistance value inside the battery is greater than the standard resistance value.
[0069] Or when the tab 21 and the shell 1 are not welded, the tab 21 and the shell 1 are not connected. For example, the tab 21 is not in contact with the conductive film layer 3, and the tab 21 is not in contact with the inner surface of the shell 1. At this time, the battery is in a short circuit state, and the resistance inside the battery is infinite. Therefore, when the tab 21 and the shell 1 are not welded successfully, the resistance value inside the battery is greater than the standard resistance value.
[0070] In the embodiment of the present application, a conductive film layer 3 is provided between the pole ear 21 and the shell 1. When the pole ear 21 and the shell 1 are not successfully welded, when the battery is tested, the detected resistance value will increase significantly, and then the battery in which the pole ear 21 and the shell 1 are not successfully welded can be detected, thereby improving the yield rate of the battery.
[0071] In one embodiment, the material of the conductive film layer 3 is solder.
[0072] For example, the conductive film layer 3 is a paste copper-based solder composed of silver-phosphorus-copper-tin alloy powder, flux and adhesive. The copper-based solder has a relatively large resistance value.
[0073] It should be noted that the present embodiment does not limit the material of the conductive film layer 3 , as long as it can conduct electricity and have a relatively large resistance value.
[0074] In order to allow the inspector to more clearly detect the connection status between the tab 21 and the housing 1, the resistance value of the conductive film layer 3 is as large as possible. For example, the resistance value range of the conductive film layer 3 can be greater than 100Ω or 1000Ω, which is set according to actual needs.
[0075] In one embodiment, when the pole tab 21 and the shell 1 are successfully welded, a welding portion 31 is formed between the pole tab 21 and the shell 1 , and the pole tab 21 is in direct contact with the shell 1 through the welding portion 31 .
[0076] Specifically, the welding portion 31 is formed when the pole tab 21 and the shell 1 are electrically connected by external welding. The welding portion 31 includes the melted pole tab 21, the melted shell 1 and the melted conductive film layer 3. When the pole tab 21 and the shell 1 are in a state of successful welding, the melted pole tab 21 and the melted shell 1 are directly connected together, so that the pole tab 21 and the shell 1 are directly in contact and welded.
[0077] For example, in the case of external welding, the energy generated by the external welding method acts on the lower shell 1 and the tab 21 on the one hand, and on the other hand, the energy generated by the external welding method also acts on the conductive film layer 3. The energy generated by the external welding method makes part of the tab 21, part of the conductive film layer 3, and part of the shell 1 in a molten state, so that the tab 21 can directly contact with the shell 1 and form a weld.
[0078] Specifically, two current paths are formed inside the battery. Since the tab 21 is directly in contact and welded with the shell 1 through the welding portion 31, the tab 21 to the shell 1 is a current path; since part of the conductive film layer 3 is also melted, the tab 21 to the conductive film layer 3 to the shell 1 is a current path.
[0079] When the tab 21 is in direct contact with the shell 1 (the resistance value inside the battery (excluding the conductive film layer, that is, the current path from the tab 21 to the shell 1) is very small, generally in the order of micro-ohms or milliohms); for another current path, the conductive film layer 3 is equivalent to a load set inside the battery, the conductive film layer 3 is connected inside the battery, the conductive film layer 3 is equivalent to being short-circuited, and the resistance value in the conductive film layer 3 is much greater than the resistance value inside the battery when the welding is successful. According to the current path selection principle, the current will not choose to flow into the conductive film layer 3 (large resistance value). Therefore, when the tab 21 is successfully welded to the shell 1, the resistance value inside the battery is less than the resistance value inside the battery when the tab 21 and the shell 1 are not welded.
[0080] Figure 2 This is a case where no welded portion 31 is formed inside the battery. Figure 2As shown, when the shell 1 and the tab 21 are welded by external welding, if the shell 1 and the tab 21 are welded, but in fact the two are not welded, the welding condition tester is not clear, and it is necessary to test it before it becomes clear. At this time, when the tester is testing the battery (testing whether the battery is qualified), since the conductive film layer 3 is set between the shell 1 and the tab 21, the conductive film layer 3 separates the shell 1 and the tab 21, and the shell 1 and the tab 21 are not in direct contact, but are electrically connected through the conductive film layer 3. When the battery is tested, the resistance value inside the battery is greater than the standard resistance value (the resistance value inside the battery when the tab 21 and the shell 1 are successfully welded), and then it can be detected that the tab 21 inside the battery is not welded to the shell 1, and the battery is unqualified.
[0081] Or when the welding portion 31 is not formed inside the battery, the tab 21 and the shell 1 are not connected. For example, the tab 21 is not in contact with the conductive film layer 3, and the tab 21 is not in contact with the inner surface of the shell 1. At this time, the battery is in an open circuit state, and the resistance inside the battery is infinite. When the battery is tested, the resistance value inside the battery is greater than the standard resistance value (the resistance value inside the battery when the tab 21 is successfully welded to the shell 1), and it can be detected that the tab 21 inside the battery is not welded to the shell 1, and the battery is unqualified.
[0082] Figure 1 This is a case where a welding portion 31 is formed inside the battery. Figure 1 As shown, the shell 1 and the pole lug 21 are directly in contact and welded together at the welding portion 31. When the shell 1 and the pole lug 21 are welded by external welding, the shell 1 and the pole lug 21 are actually welded successfully. However, the welding condition is not clear to the inspector, and it is only clear after the inspection. In the case of external welding, the energy generated by the external welding method acts on the shell 1 and the pole lug 21 on the one hand, and on the other hand, the energy generated by the external welding method also acts on the conductive film layer 3. The energy generated by the external welding method forms a welding portion 31 between the pole lug 21 and the shell 1, and the pole lug 21 and the shell 1 are directly in contact and welded through the welding portion 31.
[0083] When testing the battery, if the resistance value inside the battery is within the standard resistance value (the resistance value in the closed circuit when the tab 21 and the shell 1 are successfully welded), it can be detected that the tab 21 inside the battery is welded to the shell 1, and the battery is qualified.
[0084] In one embodiment, the external welding method of the tab 21 and the shell 1 is resistance welding.
[0085] In a specific embodiment, the pole tab 21 and the shell 1 are welded by resistance welding. For example, the shell 1 and the pole tab 21 are welded by a double-needle welding head. A conductive path is formed between the positive electrode welding head, the first shell 11, and the negative electrode welding head or the positive electrode welding head, the second shell 12, and the negative electrode welding head. At the moment when the double-needle welding head is energized, a welding portion 31 is formed between the pole tab 21 and the shell 1, and the pole tab 21 and the shell 1 are directly in contact and welded through the welding portion 31. The pole tab 21 and the shell 1 are directly in contact and welded together at the welding portion 31.
[0086] In an optional embodiment, a conductive film layer 3 is coated on the first surface of the tab 21 and / or the inner surface of the shell 1. For example, when the tab 21 and the shell 1 are welded by resistance welding, the conductive film layer 3 can increase the resistance value between the shell 1 and the tab 21. In this way, when resistance welding is performed, the current flows through the shell 1, the conductive film layer 3 and the tab 21, and the conductive film layer 3 can effectively increase the resistance value between the shell 1 and the tab 21. Since the current generated by the resistance welding acts on the conductive film layer 3, the heat generated during resistance welding is relatively large, which improves the welding effect of the shell 1 and the tab 21 at the welding portion 31.
[0087] In one embodiment, the thickness of the conductive film layer 3 is in the range of 0.01 mm to 0.03 mm. The thickness of the conductive film layer 3 is in this range, which facilitates the formation of the welding portion 31 inside the battery.
[0088] According to the second aspect of the present application, a method for preparing a battery is provided. Figure 4 As shown, the method for preparing the battery comprises the following steps:
[0089] S101: Provide a housing 1;
[0090] The housing 1 comprises a first housing 11 and a second housing 12. The first housing 11 comprises a first annular side wall and a first bottom connected to the first annular side wall. The second housing 12 comprises a second annular side wall and a second bottom connected to the second annular side wall.
[0091] The first shell 11 and the second shell 12 are sleeved and arranged to enclose and form a receiving cavity. For example, the first shell 11 is buckled inside the second shell, the first annular side wall partially overlaps with the second annular side wall, and the first bottom and the second bottom are opposite.
[0092] An insulating member is provided between the first housing 11 and the second housing 12 to isolate the first housing 11 from the second housing 12 .
[0093] S102: providing a battery cell 2, wherein the battery cell 2 is disposed in the housing 1, and a tab 21 is disposed on the battery cell 2;
[0094] The battery cell 2 is placed in the accommodating cavity formed by the shell 1. A first pole tab 21a and a second pole tab 21b are welded on the battery cell 2. The first pole tab 21a is a positive pole tab 21, and the second pole tab 21b is a negative pole tab 21; or the first pole tab 21a is a negative pole tab 21, and the second pole tab 21b is a positive pole tab 21.
[0095] S103: disposing a conductive film layer 3 on the inner surface of the housing 1 and / or the first surface of the electrode tab 21;
[0096] For example, the material of the conductive film layer 3 is solder.
[0097] The conductive film layer 3 is formed on the inner surface of the housing 1 and / or the first surface of the tab 21 by coating or spraying. The thickness of the conductive film layer 3 is in the range of 0.01-0.03 mm.
[0098] The conductive film layer 3 is formed on the first surface of the pole tab 21 by coating or spraying. The conductive film layer 3 may be coated on the first surface of the pole tab 21, and then the pole tab 21 coated with the conductive film layer 3 is welded to the battery cell 2; or after the pole tab 21 is welded to the battery cell 2, before the battery cell 2 is assembled in the second shell 12, the conductive film layer 3 is coated on the first surface of the pole tab 21; or after the pole tab 21 is welded to the battery cell 2, and the battery cell 2 welded with the pole tab 21 is assembled in the second shell 12, the conductive film layer 3 is coated on the first surface of the pole tab 21.
[0099] S104: welding the tab 21 to the inner surface of the shell 1 by external welding, so that the tab 21 is in direct contact with the shell 1 and welded.
[0100] The first shell 11 is buckled onto the second shell 12 to encapsulate the battery. The tab 21 is welded to the shell 1 by external welding. Specifically, the energy generated by the external welding is used to form a welding portion 31 between the tab 21 and the shell 1, and the tab 21 and the shell 1 are directly in contact and welded together at the welding portion 31.
[0101] In the embodiment of the present application, the battery includes a shell 1, a battery cell 2 and a conductive film layer 3. A conductive film layer 3 is provided on the inner surface of the shell 1 and / or the first surface of the tab 21. During the external welding process, the tab 21 of the present application is in direct contact with the shell 1 and electrically connected, and the shell 1 and the tab 21 will be welded successfully. If after welding the shell 1 and the tab 21, the shell 1 and the tab 21 are still isolated by the conductive film layer 3 or no electrical connection is formed at all, the shell and the tab are not welded successfully. The present application provides a conductive film layer 3 on the inner surface of the shell 1 and / or the first surface of the tab 21, which is convenient for the inspection personnel to judge whether the shell 1 and the tab 21 are welded inside the battery.
[0102] According to the third aspect of the present application, a battery detection method is provided. Figure 5 As shown, the battery detection method includes the following steps:
[0103] S201: providing a battery to be tested;
[0104] S202: Detecting the resistance value inside the battery to be tested;
[0105] S203: judging whether the tab 21 and the housing 1 are in a welding state according to the resistance value inside the battery.
[0106] Further, when the tab 21 and the shell 1 are not welded, the tab 21 and the shell 1 are separated by the conductive film layer 3. For example, the tab 21 and the shell 1 are electrically connected through the conductive film layer 3; or the tab 21 and the shell 1 are separated but not electrically connected.
[0107] Specifically, when the tab 21 is in direct contact with the shell 1 (the resistance value of the battery internal resistance (excluding the conductive film layer, that is, the current path from the tab 21 to the shell 1) is very small, generally in the order of micro-ohms or milliohms); for another current path, the conductive film layer 3 is equivalent to a load set inside the battery, the conductive film layer 3 is connected to the inside of the battery, the conductive film layer 3 is equivalent to being short-circuited, and the resistance value in the conductive film layer 3 is much greater than the resistance value inside the battery in the successful welding state. According to the current path selection principle, the current will not choose to flow into the conductive film layer 3 (large resistance value). Therefore, when the tab 21 and the shell 1 are successfully welded, the resistance value inside the battery is less than the resistance value inside the battery when the tab 21 and the shell 1 are not welded.
[0108] Specifically, when the tab 21 and the shell 1 are not welded, the conductive film layer 3 is disposed between the shell 1 and the tab 21, and the conductive film layer 3 separates the shell 1 from the tab 21. The shell 1 and the tab 21 are not in direct contact, but are electrically connected through the conductive film layer 3. When the battery is tested, the resistance value inside the battery is greater than the standard resistance value.
[0109] Or the tab 21 and the housing 1 are not welded. For example, the tab 21 is not in contact with the conductive film layer 3, and the tab 21 is not in contact with the inner surface of the housing 1. At this time, the battery is in an open circuit state, and the resistance inside the battery is infinite. When the battery is tested, the resistance value inside the battery is greater than the standard resistance value.
[0110] In this embodiment, a conductive film layer 3 is provided on the inner surface of the housing 1 and / or the first surface of the tab 21 , so that the inspector can judge whether the housing 1 and the tab 21 are welded together.
[0111] According to a fourth aspect of the present application, an electronic device is provided. The electronic device includes the battery described above. For example, the electronic device may be a mobile phone, a tablet computer, a headset, or other device that requires a battery to provide energy.
[0112] The above embodiments focus on the differences between the various embodiments. As long as the different optimization features between the various embodiments are not contradictory, they can be combined to form a better embodiment. Considering the simplicity of the text, they will not be repeated here.
[0113] Although some specific embodiments of the present application have been described in detail by way of example, it should be understood by those skilled in the art that the above examples are only for illustration, not for limiting the scope of the present application. It should be understood by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present application. The scope of the present application is defined by the appended claims.
Claims
1. A battery, characterized in that: include: A housing (1), wherein a receiving cavity is formed in the housing (1); A battery core (2), the battery core (2) being arranged in the accommodating cavity, and an end surface of the battery core (2) being opposite to an inner surface of the shell (1); The battery core (2) is provided with a pole lug (21), and the pole lug (21) has a first surface arranged opposite to the inner surface of the shell (1); A conductive film layer (3), wherein the conductive film layer (3) is arranged on the inner surface of the housing (1) and / or the first surface of the electrode tab (21), and the material of the conductive film layer (3) is solder; The shell (1) comprises a first shell (11) and a second shell (12); the battery cell (2) is placed in the second shell (12); the first shell (11) is snapped onto the second shell (12) to encapsulate the battery; and the tab (21) and the shell (1) are welded by external welding; When the pole tab (21) and the shell (1) are in a welded state, the pole tab (21) and the shell (1) are in direct contact and welded, the conductive film layer (3) is connected to the inside of the battery, and the conductive film layer (3) is short-circuited; When the pole tab (21) and the shell (1) are in an unwelded state, the pole tab (21) and the shell (1) are electrically connected via the conductive film layer (3), and the resistance value inside the battery includes the resistance value of the conductive film layer itself; When the electrode tab (21) and the shell (1) are in a welded state, the resistance value inside the battery is a standard resistance value; When the pole tab (21) and the shell (1) are in an unwelded state, the resistance value inside the battery is greater than the standard resistance value.
2. The battery according to claim 1, characterized in that When the pole lug (21) and the shell (1) are in a welded state, a welding portion (31) is formed between the pole lug (21) and the shell (1), and the pole lug (21) and the shell (1) are in direct contact via the welding portion (31).
3. The battery according to claim 1, characterized in that The pole tab (21) and the shell (1) are externally welded in a resistance welding manner.
4. A method for preparing a battery according to any one of claims 1 to 3, characterized in that: The following steps are involved: Providing a housing (1); Providing a battery core (2), wherein the battery core (2) is arranged in the housing (1), and a pole lug (21) is arranged on the battery core (2); Providing a conductive film layer (3) on the inner surface of the housing (1) and / or the first surface of the electrode tab (21); The pole tab (21) and the shell (1) are welded by external welding, and the pole tab (21) and the shell (1) are in direct contact and welded.
5. A method for detecting a battery according to any one of claims 1 to 3, characterized in that: The following steps are involved: Provide the battery to be tested; Detect the resistance value inside the battery to be tested; Whether the electrode tab (21) and the housing (1) are in a welding state is determined based on the resistance value.
6. The battery detection method according to claim 5, characterized in that: When the electrode tab (21) and the shell (1) are in a welded state, the internal resistance value of the battery is a standard resistance value; When the electrode tab (21) and the shell (1) are in an unwelded state, the resistance value inside the battery is greater than the standard resistance value.
7. An electronic device, characterized in that: A battery comprising the battery according to any one of claims 1 to 3.