A method for preparing a conveyor belt for a turning machine

Through mixed textiles of fibers with different shrinkage rates and far-infrared heating technology, a high-strength curved conveyor belt is formed, which solves the problems of structural damage and edge fluffing of existing conveyor belts during the turning process, ensuring food safety.

CN113942280BActive Publication Date: 2024-10-18SHANGHAI YONGLI TRANSPORTATION SYST CO LTD
View PDF 27 Cites 0 Cited by

Patent Information

Application Number
CN202111324069.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-10
Publication Date
2024-10-18
Estimated Expiration
2041-11-10

AI Technical Summary

Technical Problem

The warp and weft structure of the existing conveyor belt is damaged during the turning process, resulting in a decrease in strength and easy fluffing of the edges, which affects food safety.

Method used

By mixing fibers with different shrinkage rates to form a special fabric layer, and using far-infrared heating to naturally bend the fabric into a curvature, combined with the process of PU glue and calendering the PU layer, a high-strength and arc-shaped conveyor belt is formed.

Benefits of technology

It achieves the natural bending of the fabric without destroying the warp and weft structure, improves the strength of the conveyor belt, prevents edge fluffing, ensures food safety and prevents the growth of microorganisms.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113942280B_ABST
    Figure CN113942280B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing a conveyor belt for a turning machine, comprising: step S1: arranging a plurality of yarns with different shrinkage rates in sequence to weave a plain fabric; step S2: drying and shaping the fabric obtained in step S1 until the fabric is bent to a required curvature to obtain a curved fabric; step S3: applying PU glue to the curved fabric obtained in step S2; step S4: calendering a PU layer on the fabric coated with PU glue obtained in step S3 to obtain the conveyor belt. The present invention utilizes fibers with different shrinkage rates to form a special fabric layer through mixed weaving, so that the fabric is naturally bent into a certain curvature, the warp and weft structure of the fabric is not damaged, so that the conveyor belt has a higher strength, and the curvature meets the need for the conveyor belt to perform turning and conveying. At the same time, the edge of the fabric will not fluff during use, preventing the growth of microorganisms, and helping to ensure the safety of the conveyed food.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of conveyor belts, and in particular relates to a method for preparing a conveyor belt for a turning machine. Background Art

[0002] Conveyor belts are widely used in modern industry. For example, PU light conveyor belts are generally made of polyester fabric as the skeleton material. They are mainly used to transport light and medium-weight items. They have the advantages of light weight, long life, easy installation, and low friction. They are widely used in industries such as food baking. During the use of conveyor belts, there will be occasions where they need to turn and convey. For this situation, the current common method is to use conventional conveyor belts and cut them into the required dimensions. However, the warp and weft structure of the conveyor belt fabric layer will be destroyed during the cutting process. Figure 1 and 2 As shown, the strength of the conveyor belt is reduced, and the edge of the conveyor belt is prone to fuzzing during use. Summary of the invention

[0003] In view of the above-mentioned problems existing in the prior art, the purpose of the present invention is to provide a method for preparing a conveyor belt for a turning machine, by utilizing fibers with different shrinkage rates and forming a special fabric layer through mixed weaving, so that the fabric can be naturally bent into a certain curvature, and the warp and weft structures of the fabric are not damaged, so that the conveyor belt has higher strength, and the arc shape meets the needs of the conveyor belt for turning transportation. At the same time, the edges of the fabric will not fluff during use, preventing the growth of microorganisms and helping to ensure the safety of the transported food.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] A method for preparing a conveyor belt for a turning machine comprises the following steps:

[0006] Step S1: arranging a plurality of yarns with different shrinkage rates in sequence to weave a plain fabric;

[0007] Step S2: drying and shaping the fabric obtained in step S1 until the fabric is bent to a desired curvature to obtain a curved fabric;

[0008] Step S3: coating the curved fabric obtained in step S2 with PU glue;

[0009] Step S4: Calendering a PU layer on the fabric coated with PU glue obtained in step S3 to obtain the conveyor belt.

[0010] As a further improvement of the above technical solution:

[0011] The plain fabric obtained in step S1 has the same weft yarn material and different warp yarn shrinkage rates, and the warp yarns are arranged in order from high to low or from low to high according to the shrinkage rate.

[0012] The fabric density obtained in step S1 is 40*30 to 43*23 strands per square inch.

[0013] In step S2, the fabric is dried and characterized by far-infrared heating.

[0014] During far-infrared heating, the temperature is 180-200°C.

[0015] In step S3, the drying temperature is 150°C.

[0016] In step S4, when the PU layer is calendered, the extrusion temperature is 200-210°C.

[0017] In step S4, the thickness of the calendered PU layer is 0.3 mm.

[0018] In step S4, when the PU layer is calendered, the surface temperature of the fabric is maintained at 130-150°C.

[0019] In step S4, when the PU layer is calendered, the composite pressure is 15-20Pa.

[0020] The beneficial effects of the present invention are as follows: fibers with different shrinkage rates are used to form a special fabric layer through mixed weaving, so that the fabric is naturally bent into a certain arc, and the warp and weft structures of the fabric are not damaged, so that the conveyor belt has higher strength, and the arc shape meets the need for the conveyor belt to perform turning transportation. At the same time, the fabric edge will not fuzz during use, preventing the growth of microorganisms and helping to ensure the safety of the transported food. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the warp and weft structure of common fabrics in the prior art.

[0022] Figure 2 It is a schematic diagram of the structure of cutting ordinary fabric into arcs in the prior art.

[0023] Figure 3 It is a schematic diagram of the structure of the fabric before being treated according to the present invention.

[0024] Figure 4 It is a schematic diagram of the fabric of the present invention being formed into an arc shape after being processed. DETAILED DESCRIPTION

[0025] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0026] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0027] A method for preparing a conveyor belt for a turning machine comprises the following steps:

[0028] Step S1: Arrange a plurality of yarns with different shrinkage rates in sequence to weave into a plain fabric.

[0029] In this step, the plain fabric obtained has the same weft yarn material and different warp yarn shrinkage rates, and the warp yarns are arranged in order from high to low or from low to high according to the shrinkage rate.

[0030] In this embodiment, Figure 3 As shown, the warp yarn is polyester fiber, and three polyester fibers with different shrinkage rates are selected as the warp yarn, namely high shrinkage fiber 1, medium shrinkage fiber 2 and low shrinkage fiber 3, and the shrinkage rates of high shrinkage fiber 1, medium shrinkage fiber 2 and low shrinkage fiber 3 decrease in sequence. High shrinkage fiber 1, medium shrinkage fiber 2 and low shrinkage fiber 3 are arranged in sequence and interwoven with weft yarn to form a plain fabric.

[0031] The fabric density obtained in this step is 40*30 to 43*23 strands per square inch.

[0032] Step S2: Drying and shaping the fabric obtained in step S1 until the fabric is bent to a required curvature to obtain a curved fabric.

[0033] In this step, the fabric is dried and characterized by far infrared heating. During far infrared heating, the temperature is 180-200°C. After heating, the high shrinkage fiber 1, the medium shrinkage fiber 2 and the low shrinkage fiber 3 all shrink to varying degrees. The shrinkage degrees of the high shrinkage fiber 1, the medium shrinkage fiber 2 and the low shrinkage fiber 3 decrease in sequence. Figure 4 As shown. Different warp yarns have different shrinkage rates. When the initial length is the same, the warp yarn with a high shrinkage rate shrinks more and is shorter after shrinkage; the warp yarn with a low shrinkage rate shrinks less and is longer. Arranging them in order from short to long can form an arc.

[0034] Step S3: Apply PU glue to the bottom of the curved fabric obtained in step S2.

[0035] In this step, the primer glue is used to bond the fabric and the PU layer. After the glue is applied, it is dried at a drying temperature of 150°C.

[0036] Step S4: Calendering a PU layer on the fabric coated with PU glue obtained in step S3 to obtain the conveyor belt.

[0037] In this step, the PU layer is calendered by an extrusion device at an extrusion temperature of 200-210°C. The thickness of the calendered PU layer is 0.3 mm. The composite pressure is 15-20 Pa, which is the pressure when the PU layer is composited with the fabric. When calendering the PU layer, the fabric surface temperature is maintained at 130-150°C.

[0038] In summary, the technical solution adopts fibers with different shrinkage rates, forms a special fabric layer through mixed weaving, and then utilizes the shrinkage rates of different fibers to heat the fabric so that the fabric naturally bends into a certain arc.

[0039] The conveyor belt obtained based on the above method includes a fabric layer, an adhesive layer and a PU layer. The fabric layer is the skeleton layer of the conveyor belt, and the adhesive layer bonds the fabric layer and the PU layer. The warp and weft structure of the fabric layer of the conveyor belt is not damaged, so that the conveyor belt has a higher strength. The fabric layer can form an arc to meet the needs of the conveyor belt for turning and conveying. At the same time, the fabric edge will not fluff during use, preventing the growth of microorganisms, which helps to ensure the safety of the conveyed food.

[0040] Finally, it is necessary to explain here that the above embodiments are only used to further illustrate the technical solution of the present invention in detail and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above content of the present invention all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a conveyor belt for a turning machine, It is characterized in that The steps include: Step S1: arranging a plurality of yarns with different shrinkage rates in sequence to weave a plain fabric; Step S2: drying and shaping the fabric obtained in step S1 until the fabric is bent to a desired curvature to obtain a curved fabric; Step S3: coating the curved fabric obtained in step S2 with PU glue; Step S4: Calendering a PU layer on the fabric coated with PU glue obtained in step S3 to obtain the conveyor belt; The plain fabric obtained in step S1 has the same weft yarn material and different warp yarn shrinkage rates, and the warp yarns are arranged in order from high to low or from low to high according to the shrinkage rate.

2. The preparation method according to claim 1, Features: The fabric density obtained in step S1 is 40*30 to 43*23 strands per square inch.

3. The preparation method according to claim 1, Features: In step S2, the fabric is dried and characterized by far-infrared heating.

4. The preparation method according to claim 3, Features: During far-infrared heating, the temperature is 180-200°C.

5. The preparation method according to claim 1, Features: In step S3, the drying temperature is 150°C.

6. The preparation method according to claim 1, Features: In step S4, when the PU layer is calendered, the extrusion temperature is 200-210°C.

7. The preparation method according to claim 1, Features: In step S4, the thickness of the calendered PU layer is 0.3 mm.

8. The preparation method according to claim 1, Features: In step S4, when the PU layer is calendered, the surface temperature of the fabric is maintained at 130-150°C.

9. The preparation method according to claim 1, Features: In step S4, when the PU layer is calendered, the composite pressure is 15-20Pa.

Citation Information

Patent Citations

  • Composite conveying belt

    CN101535152A

  • Light conveying belt and preparation method thereof

    CN101979283A

  • Burr-proof thermoplastic polyurethane elastic body conveying belt for food industry and manufacture method thereof

    CN102424233A

  • Woven fabric with double layers of plain grids and one glazed and beaded side and production process of woven fabric

    CN102677363A

  • Highly shrinkable acrylic filament yarn

    CN1031730A