A selective diffusion method for preparing N-type selective emitter crystalline silicon cell and its application

By using an amorphous silicon layer as a mask in an N-type crystalline silicon battery, the method of forming a selective diffusion is solved, and the problem of low conversion efficiency of N-type crystalline silicon battery is achieved efficient open circuit voltage, short circuit current and filling factor Improve and avoid the problem of uncontrollable boron doped layer concentration.

CN113948607BActive Publication Date: 2024-11-12CHINT NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110988456.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-26
Publication Date
2024-11-12
Estimated Expiration
2041-08-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively improve the conversion efficiency of N-type crystalline silicon batteries, especially because the selective emitter technology of boron diffusion is not suitable for N-type crystalline silicon batteries, resulting in low open circuit voltage, short-circuit current and filling factor of the battery.

Method used

Using an amorphous silicon layer as a mask, a light doped layer is formed by diffusion of low concentration boron, amorphous silicon layer is deposited, and laser grooves are performed to form a heavily doped layer with high concentration boron diffusion, and the non-metal area is removed after cleaning. The amorphous silicon achieves selective diffusion and forms emitters with low surface concentration, shallow PN junction and high concentration, deep PN junction.

Benefits of technology

The open circuit voltage, short circuit current and filling factor of the N-type crystalline silicon battery are improved, the metal paste contact resistance is reduced, the conversion efficiency of the battery is enhanced, and the problem of uncontrollable concentration in the boron doped layer is prevented.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113948607B_ABST
    Figure CN113948607B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of N-type crystalline silicon cells, and discloses a selective diffusion method for preparing N-type selective emitter crystalline silicon cells, comprising the following steps: (1) performing low-concentration boron diffusion on the front side of a silicon wafer after texturing to form a lightly doped layer; (2) depositing amorphous silicon on the lightly doped layer to form an amorphous silicon layer; (3) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area; (4) performing high-concentration boron diffusion on the metal contact area after removing the amorphous silicon to form a heavily doped layer; (5) cleaning to remove the amorphous silicon in the non-metal area. The selective diffusion method of the present invention uses an amorphous silicon layer as a mask, which can prevent the boron concentration in the formed doping layer from being uncontrollable, and is beneficial to improving the open circuit voltage, short circuit current and fill factor of the N-type crystalline silicon cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of N-type crystalline silicon cells, and in particular to a selective diffusion method for preparing an N-type selective emitter crystalline silicon cell. Background Art

[0002] Compared with P-type crystalline silicon cells, N-type crystalline silicon cells have the advantages of long minority carrier lifetime, no photo-induced degradation, good weak light effect, and small temperature coefficient. They are the hope for crystalline silicon solar cells to reach the highest theoretical efficiency. Boron diffusion is the core technology of N-type crystalline silicon cells. At present, the boron diffusion of mass-produced N-type crystalline silicon cells adopts the uniform junction process, and the square resistance control range is 80-120ohm. The uniform junction cell structure is mainly limited by the characteristics of the metal slurry. Low-concentration doping and shallow junction diffusion can effectively reduce the body and surface recombination probability of minority carriers, improve the carrier collection rate, reduce the reverse saturation current of the battery, and increase the open circuit voltage Voc and short-circuit current Isc of the battery, thereby effectively improving the conversion efficiency of the battery. However, the low-concentration shallow junction structure will pose new challenges to the metal electrode slurry. Low-concentration doping is prone to poor contact resistance, high battery series resistance, and low fill factor FF. At the same time, shallow junction diffusion is prone to increase the probability of electrode metal penetrating into the PN junction area, thereby reducing the conversion efficiency of the battery.

[0003] In order to obtain higher battery conversion efficiency, selective emitter technology was born. Low-concentration shallow junctions are used in non-metallic contact areas, and high-concentration deep junctions are used in metal contact areas. While increasing the open circuit voltage and short-circuit current of the battery, the series resistance of the battery is reduced, and the fill factor of the battery is increased, thereby effectively improving the conversion efficiency of the battery. At present, the laser SE technology for mass production of P-type crystalline silicon cells is relatively mature, but due to the differences in the diffusion speed of boron and phosphorus, the laser SE technology used to prepare the selective emitter of P-type crystalline silicon cells is not suitable for N-type crystalline silicon cells. The selective emitter technology of boron diffusion has become an urgent problem to be solved to improve the efficiency of N-type crystalline silicon cells.

[0004] For example, patent CN200910029673.9 discloses a selective diffusion process for crystalline silicon solar cells, including high-concentration phosphorus diffusion in the front electrode grid line area and low-concentration phosphorus diffusion outside the front electrode area, including the following steps: first, after cleaning and texturing the silicon wafer, a dense silicon dioxide film is prepared on the silicon wafer as a diffusion barrier layer, and then laser grooving technology is used to selectively remove the oxide film in the electrode grid line area and form a groove of a certain depth, and then high-concentration phosphorus diffusion is performed to form heavy doping in the electrode area and light doping outside the electrode area. When this method is applied to the preparation of N-type selective emitter crystalline silicon cells, since the diffusion rate of boron in silicon oxide is faster than that in crystalline silicon, it is easy to cause uncontrollable surface concentration, affecting the performance of the selective emitter. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a selective diffusion method for preparing N-type selective emitter crystalline silicon cells. The method uses an amorphous silicon layer as a mask, which can prevent the boron concentration in the formed doping layer from being uncontrollable, and is beneficial to improving the open circuit voltage, short circuit current and fill factor of the N-type crystalline silicon cell.

[0006] The specific technical scheme of the present invention is:

[0007] A selective diffusion method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0008] (1) Diffusion of low-concentration boron is performed on the front side of the silicon wafer after texturing to form a lightly doped layer;

[0009] (2) depositing amorphous silicon on the lightly doped layer to form an amorphous silicon layer;

[0010] (3) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0011] (4) high concentration boron diffusion is performed in the metal contact area after the amorphous silicon is removed to form a heavily doped layer;

[0012] (5) Cleaning to remove amorphous silicon from non-metallic areas.

[0013] The above method can be used to achieve selective diffusion, forming an emitter with a low surface concentration and a shallow PN junction in the non-metallic contact area, which can reduce the probability of minority carrier recombination, improve the carrier collection rate, reduce the reverse saturation current of the battery, increase the open circuit voltage Voc and short circuit current Isc of the battery, and reduce the contact resistance with the metal slurry, thereby improving the fill factor FF of the battery; forming an emitter with a high concentration and a deep PN junction in the metal contact area can reduce the contact resistance of the metal slurry contact area, while reducing the risk of the slurry burning through the PN, thereby improving the fill factor FF of the battery.

[0014] Furthermore, the present invention uses an amorphous silicon layer as a mask. Since boron diffuses very slowly in amorphous silicon, it can prevent boron from penetrating the amorphous silicon layer and causing uncontrollable boron concentration in the formed doping layer, which is beneficial to improving the open circuit voltage, short circuit current and fill factor of the N-type crystalline silicon battery. In addition, the polysilicon mask can be removed by cleaning and will not remain in the selective emitter to affect the battery performance.

[0015] Preferably, in step (1), the diffusion resistance of the low-concentration boron diffusion is 140-200 ohm, and the surface concentration (boron atoms) is 1.0e 19 ~1.5e 19 atoms / cm 3 , the junction depth is 0.3~0.6μm.

[0016] Preferably, in step (4), the diffusion resistance of the high concentration boron diffusion is 60-100 ohm, and the surface concentration (boron atoms) is 2.0e 19 ~3.0e 19 atoms / cm 3 , the junction depth is 0.6~1.0μm.

[0017] Preferably, in step (2), the thickness of the amorphous silicon layer is 80 to 200 nm.

[0018] Preferably, in step (2), amorphous silicon is deposited on the lightly doped layer by low pressure chemical vapor deposition (LPCVD).

[0019] A selective diffusion method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0020] (I) depositing amorphous silicon on the front side of the silicon wafer after texturing to form an amorphous silicon layer;

[0021] (II) performing laser grooving on the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0022] (III) high concentration boron diffusion is performed in the metal contact area after the amorphous silicon is removed to form a heavily doped layer;

[0023] (IV) cleaning to remove amorphous silicon from non-metallic areas;

[0024] (V) Low-concentration boron diffusion is performed on the front side of the cleaned silicon wafer to form a lightly doped layer.

[0025] Compared with forming a lightly doped layer → depositing a mask → laser grooving → forming a heavily doped layer → removing the mask, the method of depositing a mask → laser grooving → forming a heavily doped layer → removing the mask → forming a lightly doped layer is adopted. In this scheme, light doping is formed in the last step, which has the advantages of more controllable doping concentration and junction depth in the lightly doped area, can further improve the open circuit voltage and short circuit current, and has better process stability.

[0026] Preferably, in step (I), the thickness of the amorphous silicon layer is 80-200 nm.

[0027] Preferably, in step (I), amorphous silicon is deposited on the lightly doped layer by low pressure chemical vapor deposition (LPCVD).

[0028] Preferably, in step (III), the diffusion resistance of the high concentration boron diffusion is 60-100 ohm, and the surface concentration (boron atoms) is 2.0e 19 ~3.0e 19 atoms / cm 3, the junction depth is 0.6~1.0μm.

[0029] Preferably, in step (V), the diffusion resistance of the low concentration boron diffusion is 140-200 ohm, and the surface concentration (boron atoms) is 1.0e 19 ~1.5e 19 atoms / cm 3 , the junction depth is 0.3~0.6μm.

[0030] A method for preparing an N-type selective emitter crystalline silicon cell using the selective diffusion method comprises the following steps: after the selective diffusion is completed by the selective diffusion method, the borosilicate glass (BSG) on the back and the edge is removed by etching, then a silicon oxide layer and a phosphorus-doped polysilicon layer are deposited on the back, annealing and de-coating are performed, and then an aluminum oxide passivation layer and a front silicon nitride layer are deposited on the front of the silicon wafer in sequence, and a back silicon nitride layer is deposited on the back of the silicon wafer, and after screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0031] Preferably, the thickness of the aluminum oxide passivation layer is 3-10 nm, the thickness of the front silicon nitride layer is 70-90 nm, and the thickness of the back silicon nitride layer is 70-90 nm.

[0032] Compared with the prior art, the present invention has the following advantages:

[0033] (1) The present invention forms an emitter with low surface concentration and shallow PN junction in the non-metal contact area and forms an emitter with high concentration and deep PN junction in the metal contact area, which can improve the open circuit voltage, short circuit current and fill factor of N-type crystalline silicon cells;

[0034] (2) The present invention uses an amorphous silicon layer as a mask to achieve selective diffusion, which can prevent the boron concentration in the formed doping layer from being uncontrollable, and is beneficial to improving the open circuit voltage, short circuit current and fill factor of the N-type crystalline silicon battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a schematic diagram of the front structure of an N-type selective emitter crystalline silicon cell obtained by the present invention. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with the embodiments.

[0037] Overall embodiment

[0038] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0039] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0040] (2) Selective diffusion:

[0041] Option 1:

[0042] (2.1) Low concentration boron diffusion is performed on the front side of the silicon wafer after texturing, with a diffusion resistance of 140-200 ohm and a surface concentration of 1.0e 19 ~1.5e 19 atoms / cm 3 , the junction depth is 0.3 to 0.6 μm, forming a lightly doped layer (i.e. P + layer);

[0043] (2.2) depositing amorphous silicon on the lightly doped layer using an LPCVD method to form an amorphous silicon layer with a thickness of 80 to 200 nm;

[0044] (2.3) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0045] (2.4) After removing the amorphous silicon, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 60-100 ohm and a surface concentration of 2.0e 19 ~3.0e 19 atoms / cm 3 , the junction depth is 0.6~1.0μm, forming a heavily doped layer (i.e. P ++ layer);

[0046] (2.5) cleaning to remove amorphous silicon from non-metallic areas;

[0047] Option 2:

[0048] (2.1) using LPCVD to deposit amorphous silicon on the front side of the textured silicon wafer to form an amorphous silicon layer with a thickness of 80 to 200 nm; (2.2) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0049] (2.3) After removing the amorphous silicon, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 60-100 ohm and a surface concentration of 2.0e 19 ~3.0e 19 atoms / cm 3 , the junction depth is 0.6~1.0μm, forming a heavily doped layer (i.e. P ++ layer);

[0050] (2.4) cleaning to remove amorphous silicon from non-metallic areas;

[0051] (2.5) Low concentration boron diffusion is performed on the front side of the cleaned silicon wafer, with a diffusion resistance of 140 to 200 ohms and a surface concentration of 1.0e 19 ~1.5e 19atoms / cm 3 , the junction depth is 0.3 to 0.6 μm, forming a lightly doped layer (i.e. P + layer);

[0052] (3) Etching to remove the borosilicate glass on the back and edges;

[0053] (4) using LPCVD to deposit a silicon oxide layer and a phosphorus-doped polysilicon layer on the back of the silicon wafer;

[0054] (5) Annealing;

[0055] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0056] (7) Aluminum oxide is deposited on the front of the silicon wafer to form an aluminum oxide passivation layer (i.e., AlO) with a thickness of 3 to 10 nm. x layer);

[0057] (8) Depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer (i.e., SiN x layer);

[0058] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 70 to 90 nm;

[0059] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained, and its front structure is as follows Figure 1 shown.

[0060] Example 1

[0061] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0062] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0063] (2) Selective diffusion:

[0064] (2.1) Low concentration boron diffusion is performed on the front side of the silicon wafer after texturing, with a diffusion resistance of 140 ohm and a surface concentration of 1.2e 19 atoms / cm 3 , the junction depth is 0.6μm, forming a lightly doped layer;

[0065] (2.2) depositing amorphous silicon on the lightly doped layer using an LPCVD method to form an amorphous silicon layer with a thickness of 80 nm;

[0066] (2.3) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0067] (2.4) After removing the amorphous silicon, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 60 ohm and a surface concentration of 3.0 e 19 atoms / cm 3 , the junction depth is 1.0 μm, forming a heavily doped layer;

[0068] (2.5) cleaning to remove amorphous silicon from non-metallic areas;

[0069] (3) Etching to remove the borosilicate glass on the back and edges;

[0070] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0071] (5) Annealing;

[0072] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0073] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 6 nm;

[0074] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 70 nm;

[0075] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 70 nm;

[0076] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0077] Example 2

[0078] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0079] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0080] (2) Selective diffusion:

[0081] (2.1) Low concentration boron diffusion is performed on the front side of the silicon wafer after texturing, with a diffusion resistance of 170 ohm and a surface concentration of 1.2e 19 atoms / cm 3 , the junction depth is 0.5μm, forming a lightly doped layer;

[0082] (2.2) depositing amorphous silicon on the lightly doped layer using an LPCVD method to form an amorphous silicon layer with a thickness of 140 nm;

[0083] (2.3) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0084] (2.4) After removing the amorphous silicon, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 70 ohm and a surface concentration of 2.5e 19 atoms / cm 3 , the junction depth is 0.9μm, forming a heavily doped layer;

[0085] (2.5) cleaning to remove amorphous silicon from non-metallic areas;

[0086] (3) Etching to remove the borosilicate glass on the back and edges;

[0087] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0088] (5) Annealing;

[0089] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0090] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 6 nm;

[0091] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 80 nm;

[0092] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 80 nm;

[0093] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0094] Example 3

[0095] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0096] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0097] (2) Selective diffusion:

[0098] (2.1) Low concentration boron diffusion is performed on the front side of the silicon wafer after texturing, with a diffusion resistance of 200 ohm and a surface concentration of 1.0e 19 atoms / cm 3 , the junction depth is 0.4μm, forming a lightly doped layer;

[0099] (2.2) depositing amorphous silicon on the lightly doped layer using an LPCVD method to form an amorphous silicon layer with a thickness of 200 nm;

[0100] (2.3) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0101] (2.4) After removing the amorphous silicon, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 60 ohm and a surface concentration of 3.0 e 19 atoms / cm 3 , the junction depth is 1.0 μm, forming a heavily doped layer;

[0102] (2.5) cleaning to remove amorphous silicon from non-metallic areas;

[0103] (3) Etching to remove the borosilicate glass on the back and edges;

[0104] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0105] (5) Annealing;

[0106] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0107] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 7 nm;

[0108] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 80 nm;

[0109] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 80 nm;

[0110] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0111] Example 4

[0112] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0113] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0114] (2) Selective diffusion:

[0115] (2.1) using LPCVD to deposit amorphous silicon on the front side of the silicon wafer after texturing to form an amorphous silicon layer with a thickness of 80 nm;

[0116] (2.2) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0117] (2.3) After removing the amorphous silicon, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 60 ohm and a surface concentration of 3.0e 19 atoms / cm 3, the junction depth is 1.0 μm, forming a heavily doped layer;

[0118] (2.4) cleaning to remove amorphous silicon from non-metallic areas;

[0119] (2.5) Low concentration boron diffusion is performed on the front side of the cleaned silicon wafer, with a diffusion resistance of 140 ohm and a surface concentration of 1.2e 19 atoms / cm 3 , the junction depth is 0.6μm, forming a lightly doped layer;

[0120] (3) Etching to remove the borosilicate glass on the back and edges;

[0121] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0122] (5) Annealing;

[0123] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0124] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 6 nm;

[0125] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 80 nm;

[0126] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 80 nm;

[0127] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0128] Example 5

[0129] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0130] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0131] (2) Selective diffusion:

[0132] (2.1) using LPCVD to deposit amorphous silicon on the front side of the silicon wafer after texturing to form an amorphous silicon layer with a thickness of 140 nm;

[0133] (2.2) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0134] (2.3) After removing the amorphous silicon, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 70 ohm and a surface concentration of 2.5e 19 atoms / cm3 , the junction depth is 0.9μm, forming a heavily doped layer;

[0135] (2.4) cleaning to remove amorphous silicon from non-metallic areas;

[0136] (2.5) Low concentration boron diffusion is performed on the front side of the cleaned silicon wafer, with a diffusion resistance of 170 ohm and a surface concentration of 1.2e 19 atoms / cm 3 , the junction depth is 0.5μm, forming a lightly doped layer;

[0137] (3) Etching to remove the borosilicate glass on the back and edges;

[0138] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0139] (5) Annealing;

[0140] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0141] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 6 nm;

[0142] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 80 nm;

[0143] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 80 nm;

[0144] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0145] Example 6

[0146] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0147] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0148] (2) Selective diffusion:

[0149] (2.1) Using LPCVD method to deposit amorphous silicon on the front side of the silicon wafer after texturing, forming an amorphous silicon layer with a thickness of 200 nm;

[0150] (2.2) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area;

[0151] (2.3) After removing the amorphous silicon, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 90 ohm and a surface concentration of 2.0e 19atoms / cm 3 , the junction depth is 0.7μm, forming a heavily doped layer;

[0152] (2.4) cleaning to remove amorphous silicon from non-metallic areas;

[0153] (2.5) Low concentration boron diffusion is performed on the front side of the cleaned silicon wafer, with a diffusion resistance of 200 ohm and a surface concentration of 1.0e 19 atoms / cm 3 , the junction depth is 0.4μm, forming a lightly doped layer;

[0154] (3) Etching to remove the borosilicate glass on the back and edges;

[0155] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0156] (5) Annealing;

[0157] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0158] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 10 nm;

[0159] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 75 nm;

[0160] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 75 nm;

[0161] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0162] Comparative Example 1

[0163] A method for preparing an N-type crystalline silicon cell emitter comprises the following steps:

[0164] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0165] (2) Boron diffusion is performed on the front side of the silicon wafer after texturing, with a diffusion resistance of 100 ohm and a surface concentration of 1.2e 19 atoms / cm 3 , the junction depth is 0.8μm, forming a doped layer;

[0166] (3) Etching to remove the borosilicate glass on the back and edges;

[0167] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0168] (5) Annealing;

[0169] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0170] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 6 nm;

[0171] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 70 nm;

[0172] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 70 nm;

[0173] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0174] Comparative Example 2

[0175] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0176] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0177] (2) Selective diffusion:

[0178] (2.1) Low concentration boron diffusion is performed on the front side of the silicon wafer after texturing, with a diffusion resistance of 140 ohm and a surface concentration of 1.2e 19 atoms / cm 3 , the junction depth is 0.6μm, forming a lightly doped layer;

[0179] (2.2) depositing silicon oxide on the lightly doped layer by a thermal oxidation method to form a silicon oxide layer with a thickness of 80 nm;

[0180] (2.3) laser grooving the silicon oxide layer to remove the silicon oxide in the metal contact area;

[0181] (2.4) After removing silicon oxide, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 60 ohm and a surface concentration of 3.0 e 19 atoms / cm 3 , the junction depth is 1.0 μm, forming a heavily doped layer;

[0182] (2.5) cleaning to remove silicon oxide from non-metallic areas;

[0183] (3) Etching to remove the borosilicate glass on the back and edges;

[0184] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0185] (5) Annealing;

[0186] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0187] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 6 nm;

[0188] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 70 nm;

[0189] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 70 nm;

[0190] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0191] Comparative Example 3

[0192] A method for preparing an N-type selective emitter crystalline silicon cell comprises the following steps:

[0193] (1) Texturing the surface of silicon wafer to form a pyramid velvet surface;

[0194] (2) Selective diffusion:

[0195] (2.1) using thermal oxidation to deposit silicon oxide on the front side of the silicon wafer after texturing to form a silicon oxide layer with a thickness of 80 nm;

[0196] (2.2) laser grooving the silicon oxide layer to remove the silicon oxide in the metal contact area;

[0197] (2.3) After removing silicon oxide, high concentration boron is diffused in the metal contact area, with a diffusion resistance of 60 ohm and a surface concentration of 3.0 e 19 atoms / cm 3 , the junction depth is 1.0 μm, forming a heavily doped layer;

[0198] (2.4) cleaning to remove silicon oxide from non-metallic areas;

[0199] (2.5) Low concentration boron diffusion is performed on the front side of the cleaned silicon wafer, with a diffusion resistance of 140 ohm and a surface concentration of 1.2e 19 atoms / cm 3 , the junction depth is 0.6μm, forming a lightly doped layer;

[0200] (3) Etching to remove the borosilicate glass on the back and edges;

[0201] (4) depositing a 1.0 nm thick silicon oxide layer and a 110 nm thick phosphorus-doped polysilicon layer on the back of the silicon wafer using the LPCVD method;

[0202] (5) Annealing;

[0203] (6) Remove PSG and RCA cleaning and remove the front side plating;

[0204] (7) depositing aluminum oxide on the front side of the silicon wafer to form an aluminum oxide passivation layer with a thickness of 3 nm;

[0205] (8) depositing silicon nitride on the aluminum oxide passivation layer to form a front silicon nitride layer with a thickness of 70 nm;

[0206] (9) depositing silicon nitride on the back side of the silicon wafer, with a back side silicon nitride layer having a thickness of 70 nm;

[0207] (10) After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

[0208] Test Case

[0209] The emitters prepared in Examples 1 to 6 and Comparative Examples 1 to 3 were made into N-type crystalline silicon cells by conventional methods. The open circuit voltage Voc, short circuit current Isc and fill factor FF of the cells were tested. The results are shown in Table 1.

[0210] Table 1

[0211]

[0212]

[0213] By analyzing the data in Table 1, we can draw the following conclusions:

[0214] (1) Comparative Example 1 uses one-time doping to obtain a common emitter, and Examples 1 and 4 use the method of the present invention to obtain a selective emitter. Compared with Comparative Example 1, the open circuit voltage, short circuit current, and fill factor of the batteries in Examples 1 and 4 are increased, and the battery efficiency is increased by 0.17% and 0.21%, respectively. The reason is that: in the selective emitter, the non-metallic contact area forms an emitter with low surface concentration and shallow PN junction, which reduces the probability of minority carrier recombination, improves the carrier collection rate, reduces the reverse saturation current of the battery, increases the open circuit voltage and short circuit current of the battery, and reduces the contact resistance with the metal slurry, thereby improving the fill factor of the battery; the metal contact area forms an emitter with high concentration and deep PN junction, which reduces the contact resistance of the metal slurry contact area, and at the same time reduces the risk of the slurry burning through the PN, thereby improving the fill factor of the battery.

[0215] (2) Examples 1 and 4 use amorphous silicon as a mask, while Comparative Examples 2 and 3 use silicon oxide as a mask. Compared with Comparative Example 2, the open circuit voltage, short circuit current, and fill factor of the battery in Example 1 are increased, thereby increasing the battery efficiency by 0.09%; compared with Comparative Example 3, the open circuit voltage, short circuit current, and fill factor of the battery in Example 4 are increased, and the efficiency is increased by 0.05%. The reason is that when silicon oxide is used as a mask, since the diffusion rate of boron in silicon oxide is faster than that in crystalline silicon, it is easy to cause uncontrollable surface concentration, affecting the performance of the selective emitter; and when an amorphous silicon layer is used as a mask, since the diffusion of boron in amorphous silicon is very slow, it can prevent boron from penetrating the amorphous silicon layer, resulting in uncontrollable boron concentration in the formed doping layer, which is beneficial to improving battery performance.

[0216] (3) Example 1 adopts the sequence of "forming a lightly doped layer → depositing a mask → laser grooving → forming a heavily doped layer → removing the mask" for selective diffusion, while Example 4 adopts the sequence of "depositing a mask → laser grooving → forming a heavily doped layer → removing the mask → forming a lightly doped layer". Compared with Example 1, the open circuit voltage and short circuit current of the battery in Example 4 increased, and the battery efficiency increased by 0.17%. The reason is that the sequence in Example 4 has the advantages of more controllable doping concentration and junction depth in the lightly doped region, which can further increase the open circuit voltage and short circuit current, and has better process stability.

[0217] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0218] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A selective diffusion method for preparing an N-type selective emitter crystalline silicon cell, characterized in that: The following steps are involved: (1) Low-concentration boron diffusion is performed on the front side of the silicon wafer after texturing to form a lightly doped layer; the diffusion sheet resistance of the low-concentration boron diffusion is 140~200 ohm / sq, and the surface concentration is 1.0e 19 ~1.5e 19 atoms / cm 3 , the junction depth is 0.3~0.6 μm; (2) depositing amorphous silicon on the lightly doped layer to form an amorphous silicon layer; (3) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area; (4) High-concentration boron diffusion is performed in the metal contact area after the amorphous silicon is removed to form a heavily doped layer; the diffusion resistance of the high-concentration boron diffusion is 60~100 ohm / sq, and the surface concentration is 2.0e 19 ~3.0e 19 atoms / cm 3 , junction depth is 0.6~1.0 μm; (5) Cleaning to remove amorphous silicon from non-metallic areas.

2. The selective diffusion method according to claim 1, characterized in that: In step (2), the thickness of the amorphous silicon layer is 80-200 nm.

3. A selective diffusion method for preparing an N-type selective emitter crystalline silicon cell, characterized in that: The following steps are involved: (I) depositing amorphous silicon on the front side of the silicon wafer after texturing to form an amorphous silicon layer; (II) laser grooving the amorphous silicon layer to remove the amorphous silicon in the metal contact area; (III) high concentration boron diffusion is performed in the metal contact area after the amorphous silicon is removed to form a heavily doped layer; the diffusion resistance of the high concentration boron diffusion is 60-100 ohm / sq, and the surface concentration is 2.0e 19 ~3.0e 19 atoms / cm 3 , the junction depth is 0.6~1.0μm; (IV) cleaning to remove amorphous silicon from non-metallic areas; (V) performing low-concentration boron diffusion on the front side of the cleaned silicon wafer to form a lightly doped layer; the diffusion sheet resistance of the low-concentration boron diffusion is 140-200 ohm / sq, and the surface concentration is 1.0e 19 ~1.5e 19 atoms / cm 3 , the junction depth is 0.3~0.6 μm.

4. The selective diffusion method according to claim 3, characterized in that: In step (I), the thickness of the amorphous silicon layer is 80-200 nm.

5. A method for preparing an N-type selective emitter crystalline silicon cell using the selective diffusion method as claimed in any one of claims 1 to 4, characterized in that: The following steps are involved: After the selective diffusion is completed by the selective diffusion method, the borosilicate glass on the back and the edge is removed by etching, and then a silicon oxide layer and a phosphorus-doped polysilicon layer are deposited on the back, annealing and de-plating are performed, and then an aluminum oxide passivation layer and a front silicon nitride layer are deposited in sequence on the front of the silicon wafer, and a back silicon nitride layer is deposited on the back of the silicon wafer. After screen printing and sintering, an N-type selective emitter crystalline silicon cell is obtained.

6. The method according to claim 5, characterized in that The thickness of the aluminum oxide passivation layer is 3-10 nm, the thickness of the front silicon nitride layer is 70-90 nm, and the thickness of the back silicon nitride layer is 70-90 nm.