Polymers, adhesive compositions and articles derived from (meth)acrylate macromonomers

By using the adhesive composition prepared by the (meth)acrylate copolymer, the problem of insufficient adhesion of the adhesive in the prior art under high impact and dynamic deformation conditions is solved, providing suitable flexible and foldable electrons Efficient impact resistance and compliant adhesive for the equipment.

CN113966352BActive Publication Date: 2024-11-083M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080041054.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-13
Filing Date
2020-05-27
Publication Date
2024-11-08
Estimated Expiration
2040-05-27

AI Technical Summary

Technical Problem

Pressure-sensitive adhesives in existing electronic devices are difficult to maintain adhesion in the face of high impact and dynamic deformation, especially in the tendency of equipment simplification and thickness reduction, which lacks good impact resistance, compliance and recovery. It is difficult to meet the needs of flexible and foldable products.

Method used

Adhesive compositions formed from (meth)acrylate copolymers, including poly(ethyleneoxy) groups, poly(propyleneoxy) groups or poly(ethyleneoxy-co-propylene (meth)acrylate macromonomer of the base oxygen group, alkyl (meth)acrylate and carboxylic acid containing (meth)acrylate, have low glass transition temperature and crosslinking characteristics, and are used for Pressure-sensitive adhesives with excellent adhesion strength and impact resistance are prepared.

Benefits of technology

It achieves good adhesion under high strain and impact conditions, and is suitable for flexible and foldable electronic devices, improving the durability and foldable performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003388924570000031
    Figure BDA0003388924570000031
  • Figure BDA0003388924570000032
    Figure BDA0003388924570000032
  • Figure BDA0003388924570000341
    Figure BDA0003388924570000341
Patent Text Reader

Abstract

The present invention provides a (meth)acrylate copolymer derived from a polymerizable composition comprising a (meth)acrylate macromonomer, an adhesive composition that is a pressure-sensitive adhesive and comprises the (meth)acrylate copolymer, and an article comprising the adhesive composition. The article may be, for example, an adhesive tape, an electronic device, or a flexible and / or foldable article. The article may be advantageously used in foldable and / or flexible electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] In electronic devices, particularly mobile electronic devices (e.g., handheld or wearable electronic devices), pressure sensitive adhesives (PSAs) are generally used to bond cover glass (or lenses) to the bottom display module of the electronic device, to bond touch sensors to cover glass and display, or to bond the lower components of the display to the housing. Pressure sensitive adhesives used in mobile electronic devices are generally optically transparent adhesives (OCAs). For these applications (often referred to as electronic bonding or e-bonding), PSA and OCA should have sufficiently high-strength adhesion, so that not only when mobile electronic devices are operated under normal conditions, but also when they are deformed by external forces (e.g., bending, folding, flexing) or suffer traumatic forces (e.g., mobile electronic devices fall onto hard surfaces), properly maintain good adhesion to these components. About deformation, when users sit on a chair while electronic devices are in their pockets or when they press down on electronic devices with their buttocks, the components of the electronic device may be deformed. Under such conditions, the pressure sensitive adhesive should have enough adhesion strength to maintain, for example, adhesion to cover glass (sometimes referred to as wrinkle resistance). With respect to traumatic forces, the pressure sensitive adhesive should have sufficient drop resistance or impact resistance so that the pressure sensitive adhesive maintains adhesion of the assembly even when a large instantaneous impact is applied to the portable electronic device when the portable electronic device is dropped.

[0002] Adhesives that can dissipate energy and resist the peel forces associated with high strain events (e.g., flexing and folding) and high strain rate events (such as those experienced during a device drop) have gained increasing importance to the electronic device industry. The ability to produce pressure sensitive adhesives that resist debonding (via interfacial or cohesive failure modes) during these high impact and dynamic deformations has become a highly desirable property, including traditional performance metrics such as good peel, shear, tensile adhesion, and creep resistance, and has therefore become a commercially attractive performance criterion for achieving continued product differentiation in this competitive, fast-paced market space.

[0003] Given the electronics industry trends toward device simplification (i.e., combining layers and / or layer functions) and reducing bond area and overall device thickness (and in addition requiring increased flexibility), there is an increasing need for adhesive tapes with good impact resistance, conformability, and recovery. Adhesives with this balance of dichotomous properties are needed, especially in flexible and / or foldable articles. Summary of the invention

[0004] The present invention provides a (meth)acrylate copolymer formed from a polymerizable composition, the polymerizable composition comprising a (meth)acrylate macromer, an adhesive composition that is a pressure-sensitive adhesive and comprises the (meth)acrylate copolymer, and an article comprising the adhesive composition. The article comprises a layer of the adhesive composition positioned adjacent to a substrate. The article may be, for example, an adhesive tape, or may be another article that is flexible and foldable, such as a part of a flexible and / or foldable electronic device.

[0005] In a first aspect, a (meth)acrylate copolymer is provided, the (meth)acrylate copolymer comprising monomer units derived from a polymerizable component, the polymerizable component comprising (1) a (meth)acrylate macromonomer comprising a poly(ethylene oxide) group, a poly(propylene oxide) group, or a poly(ethylene oxide-co-propylene oxide) group, (2) an alkyl (meth)acrylate, and (3) a (meth)acrylate-containing carboxylic acid. The (meth)acrylate macromonomer has a number average molecular weight of no greater than 900 g / mol and is present in an amount of at least 5 wt % based on the total weight of the polymerizable component. The (meth)acrylate-containing carboxylic acid is present in an amount of no greater than 15 wt % based on the total weight of the polymerizable component. The (meth)acrylate copolymer has a glass transition temperature of no greater than -15°C.

[0006] In a second aspect, an adhesive composition comprising the (meth)acrylate copolymer of the first aspect is provided. In many embodiments, the (meth)acrylate copolymer is crosslinked. The adhesive composition is generally a pressure-sensitive adhesive.

[0007] In a third aspect, an article is provided, the article comprising a substrate and an adhesive composition positioned adjacent to the substrate. The adhesive composition is the same as described above in the second aspect.

[0008] The term "and / or" such as in the expression A and / or B means A alone, B alone, or both A and B.

[0009] The term "polymer" refers to homopolymers, copolymers, terpolymers, etc. The term "copolymer" is used herein to refer to a polymeric material prepared from at least two different polymerizable components.

[0010] The term "polymerizable component" refers to a compound that can undergo polymerization (i.e., the compound has a polymerizable group). The polymerizable component typically has an ethylenically unsaturated group, such as a (meth)acryloyl-containing group or a vinyl group that is a polymerizable group. A compound having a polymerizable group may be referred to as a "monomer."

[0011] As used herein, the term "macromer" refers to a monomer having a polymerizing group. Macromer is a subset of the term "monomer."

[0012] The term "monomer unit" refers to the reaction product of the polymerizable components (i.e., monomers (including macromonomers)) in the (meth)acrylate copolymer. For example, the monomer unit of acrylic acid

[0013]

[0014] for

[0015]

[0016] Wherein an asterisk (*) indicates a site of attachment to another group, such as another monomer unit or a terminal group in a (meth)acrylate copolymer.

[0017] The term "(meth)acryloyl" refers to a group having the formula CH2=CR-(CO)-, wherein R is hydrogen (for an acryloyl group) or methyl (for a methacryloyl group).

[0018] The term "(meth)acrylate" refers to methacrylate and / or acrylate. Likewise, the term "(meth)acrylic acid" refers to methacrylic acid and / or acrylic acid, and the term "(meth)acrylamide" refers to methacrylamide and / or acrylamide.

[0019] The term "(meth)acrylate macromer" refers to a monomer having a single (meth)acryloyloxy group (i.e., a group having the formula CH2=CR-(CO)-O-, where R is hydrogen or methyl) plus a poly(ethylene oxide) group, a poly(propylene oxide) group, or a poly(ethylene oxide-co-propylene oxide) group.

[0020] The term "poly(ethylene oxide) group" refers to a group containing at least 3 ethylene oxide (-(C2H4O)-) groups, and the term "poly(propylene oxide) group" refers to a group containing at least 3 propylene oxide (-(C3H6O)-) groups.

[0021] The term "poly(ethylene oxide-co-propylene oxide) group" comprises at least 3 groups having at least one ethylene oxide group and at least one propylene oxide group. The poly(ethylene oxide-co-propylene oxide) group is a copolymer group.

[0022] The term "vinyl" refers to a polymerizable component having the group CH2=CH- but not being part of a (meth)acryloyl group.

[0023] The term "polymerizable composition" refers to a reaction mixture that undergoes polymerization. It contains polymerizable components and any other materials that may be included in a reaction mixture, such as free radical initiators, chain transfer agents, antioxidants, solvents, and the like.

[0024] As used herein, the term "pressure sensitive adhesive" or "PSA" is used in accordance with the conventional manner of the Pressure Sensitive Tape Council, according to which pressure sensitive adhesives are known to have properties including: (1) strong and persistent tack, (2) adhesion with light finger pressure, (3) sufficient ability to remain on an adherend, and (4) sufficient cohesive strength to allow clean removal from an adherend. Materials that have been found to function well as PSAs include polymers designed and formulated to exhibit the desired viscoelastic properties that achieve a desired balance of initial tack, peel adhesion, and shear holding power. PSAs are characterized by being tacky, typically at room temperature (e.g., 20°C). Of great importance to all PSAs is the desired balance of adhesion and cohesion, which is often achieved by optimizing the physical properties of the elastomer, such as the glass transition temperature and modulus. For example, if the glass transition temperature (T g ) or the modulus is too high and exceeds the Dahlquist standard for viscosity (3×10 6 Dyne / cm 2 ), the material will not be tacky and cannot be used as a PSA material per se.

[0025] As used herein, the term "glass transition temperature" (which may be written interchangeably as "T g ”) refers to the glass transition temperature of a homopolymer formed from a monomer (which may be a macromonomer). The glass transition temperature of a polymer material is usually measured by dynamic mechanical analysis (DMA) as the maximum value of the loss tangent value (δ).

[0026] As used herein, "flexible" refers to substrates and / or articles that can undergo a rolling action with a bending radius of 200 mm or less, 100 mm or less, 50 mm or less, 20 mm or less, 10 mm or less, 5 mm or less, 4 mm or less, 3 mm or less, 2 mm or less, or 1 mm or less without failure or visible defects such as delamination, cracking, crazing, or haziness.

[0027] As used herein, "foldable" refers to a substrate and / or article that can undergo repeated flexing or folding, such as up to 1,000 folds, up to 10,000 folds, up to 25,000 folds, up to 50,000 folds, up to 25,000 folds, up to 100,000 folds, or even up to 200,000 folds, without failure or visible defects, such as delamination, cracking, crazing, or clouding. In this context, a fold is formed in a substrate or article that is relatively flat when it is bent (i.e., folded) upon itself so that one portion thereof covers another portion. The bend radius for folding is typically 200 mm or less, 100 mm or less, 50 mm or less, 20 mm or less, 10 mm or less, 5 mm or less, 4 mm or less, 3 mm or less, 2 mm or less, or 1 mm or less.

[0028] In this article, the term "comprising" and its variant forms do not have a limiting meaning where these terms appear in the specification and claims. Such terms will be understood to imply the inclusion of the stated steps or elements or groups of steps or elements, but do not exclude any other steps or elements or groups of steps or elements. The so-called "consisting of..." means including and limited to the content following the phrase "consisting of...". Therefore, the phrase "consisting of..." indicates that the listed elements are required or mandatory, and no other elements may be present. "Substantially consisting of..." means including any elements listed after the phrase, and is limited to other elements that do not hinder or contribute to the activity or effect specified for the listed elements in the present disclosure. Therefore, the phrase "substantially consisting of..." indicates that the listed elements are required or mandatory, but other elements are optional and may or may not exist, depending on whether they substantially affect the activity or effect of the listed elements. Any element or combination of elements referred to in this specification with open language (e.g., comprises and its derivatives) is considered to be additionally referred to with closed language (e.g., consisting of… and its derivatives) and with partially closed language (e.g., consisting essentially of… and its derivatives).

[0029] The words "preferred" and "preferably" refer to embodiments of the present disclosure that may provide certain benefits in certain circumstances. However, other claims may also be preferred under the same or other circumstances. In addition, the statement of one or more preferred claims does not mean that other claims are unavailable, and is not intended to exclude other claims from the scope of the present disclosure.

[0030] In this application, terms such as "a", "an", and "the" are not intended to refer to only a single entity, but include general categories, specific examples of which may be used for illustration. The terms "a", "an", "the", and "the" are used interchangeably with the term "at least one". The phrases "at least one of" and "comprising at least one of" followed by a list refer to any one of the items in the list and any combination of two or more items in the list.

[0031] As used herein, the term "or" is generally used in its ordinary sense including "and / or" unless the context clearly dictates otherwise.

[0032] The term "and / or" means one or all of the listed elements, or a combination of any two or more of the listed elements.

[0033] In addition, all numerical values ​​are assumed to be modified by the term "about", and in certain embodiments preferably by the term "exactly". As used herein, with respect to a measured amount, the term "about" refers to a deviation in the measured amount that would be expected by a skilled person who takes the measurements with a certain degree of care, commensurate with the goal of the measurement and the precision of the measuring equipment used. In this article, "at most" a number (e.g., at most 50) includes the number (e.g., 50).

[0034] Also herein, the recitations of numerical ranges by endpoints include all numbers subsumed within that range as well as the endpoints (eg, 1 to 5 includes 1, 1.5, 2, 2.75, 3, 3.80, 4, 5, etc.).

[0035] As used herein, the term "room temperature" refers to a temperature of 20°C to 25°C or 22°C to 25°C.

[0036] The terms "in the range" or "within a range" (and similar expressions) include the endpoints of the range.

[0037] The grouping of alternative elements or embodiments disclosed herein should not be construed as restrictive. Each group member may be cited and protected by claims alone or with other members in the group or other elements found therein in any combination and protected by claims. It is contemplated that one or more members of the group may be included in the group or deleted from the group for reasons of convenience and / or patentability. When any such inclusion or deletion occurs, the specification is deemed to contain the modified group in this article, thereby satisfying the written description of all Markush groups used in the appended claims.

[0038] When a group occurs more than once in a formula described herein, each group is "independently" selected, whether or not explicitly stated. For example, when more than one R group is present in a formula, each R group is independently selected.

[0039] References throughout this specification to "one embodiment," "an embodiment," "certain embodiments," or "some embodiments," etc., mean that a particular feature, configuration, composition, or characteristic described in connection with the embodiment is included in at least one embodiment of the present invention. Thus, the appearance of such phrases in various places throughout this specification are not necessarily referring to the same embodiment of the present invention. Furthermore, the particular features, configurations, compositions, or characteristics may be combined in any suitable manner in one or more embodiments.

[0040] The above summary of the invention disclosed herein is not intended to describe each disclosed embodiment or each implementation mode of the present invention. The following description illustrates exemplary embodiments in more detail. In many places of the application, guidance is provided by lists of examples. These embodiments can be used in various combinations. In each case, the cited list is only used as a representative group and should not be understood as an exclusive list. Therefore, the scope of the present disclosure should not be limited to the specific illustrative structures described herein, but should at least extend to the structures described by the language of the claims and the equivalents of these structures. Any elements positively cited as alternatives in this specification may be explicitly included in the claims or excluded from the claims in any combination as needed. Although various theories and possible mechanisms may have been discussed herein, such discussions should not be used to limit the subject matter that can be protected by the claims under any circumstances. DETAILED DESCRIPTION

[0041] The present disclosure provides a (meth)acrylate copolymer, an adhesive composition containing the (meth)acrylate copolymer, and an article containing the adhesive composition positioned adjacent to a substrate. The article may be, for example, an adhesive tape, or may be another flexible and foldable article, such as a part of a flexible and / or foldable electronic device.

[0042] The (meth)acrylate copolymer comprises monomer units derived from a polymerizable component, the polymerizable component comprising (1) a (meth)acrylate macromonomer comprising a poly(ethylene oxide) group, a poly(propylene oxide) group, or a poly(ethylene oxide-co-propylene oxide) group, (2) an alkyl (meth)acrylate, and (3) a (meth)acrylate-containing carboxylic acid. The (meth)acrylate macromonomer has a number average molecular weight of no greater than 900 g / mole and is present in an amount of at least 5 wt % based on the total weight of the polymerizable component. The (meth)acrylate-containing carboxylic acid is present in an amount of no greater than 15 wt % based on the total weight of the polymerizable component. The (meth)acrylate copolymer has a glass transition temperature of no greater than -15°C.

[0043] The (meth)acrylate copolymer is used to form an adhesive composition. In addition to the (meth)acrylate copolymer, the adhesive composition may optionally include other components. In many embodiments, the (meth)acrylate copolymer is crosslinked. The adhesive composition is typically a pressure-sensitive adhesive.

[0044] The adhesive composition is used to prepare various articles. The adhesive composition advantageously has good peel adhesion strength and remains adhered to the substrate even when the article is flexed, folded or impacted. In some embodiments, the adhesive composition is used in electronic devices, including those that are flexible and / or foldable.

[0045] (Meth)acrylate copolymer

[0046] The (meth)acrylate copolymer is formed from a polymerizable component comprising (1) a (meth)acrylate macromonomer comprising a poly(ethylene oxide) group, a poly(propylene oxide) group, or a poly(ethylene oxide-co-propylene oxide) group, (2) an alkyl (meth)acrylate, and (3) a (meth)acrylate-containing carboxylic acid. Other additional optional monomers may be included in the polymerizable component. In many embodiments, the (meth)acrylate copolymer is crosslinked. Crosslinking can be performed, for example, by adding a crosslinking agent to the polymerizable component.

[0047] In many embodiments, the polymerizable components used to form the (meth)acrylate copolymer are free or substantially free of vinyl acetate and non-polar vinyl monomers. As used herein to describe vinyl acetate and non-polar vinyl monomers, the term "substantially free" means that the polymerizable components contain less than 1 wt%, less than 0.5 wt%, less than 0.2 wt%, or less than 0.1 wt% of these monomers.

[0048] The (meth)acrylate copolymers typically have a glass transition temperature no greater than -15°C as determined by dynamic mechanical analysis.

[0049] For example, the glass transition temperature may be no greater than -20° C., no greater than -25° C., no greater than -30° C., no greater than -35° C., or no greater than -40° C. The glass transition temperature is typically greater than -50° C., greater than -40° C., or greater than -30° C. The (meth)acrylate copolymer preferably has a single glass transition temperature when measured using dynamic mechanical analysis.

[0050] (Meth)acrylate macromonomer

[0051] The (meth)acrylate macromonomer contained in the polymerizable components used to form the (meth)acrylate copolymer has a (meth)acryloyloxy group plus a poly(ethylene oxide) group, a poly(propylene oxide) group, or a poly(ethylene oxide-co-propylene oxide) group, the latter three of which may also be referred to as poly(ethylene glycol), poly(propylene glycol), or poly(ethylene oxide-co-propylene oxide) groups, respectively. If the macromonomer contains a poly(ethylene oxide) group, it may be referred to as poly(ethylene oxide)(meth)acrylate. If the macromonomer contains a poly(propylene oxide) group, it may be referred to as poly(propylene oxide)(meth)acrylate. If the macromonomer contains a poly(ethylene oxide-co-propylene oxide) group, it may be referred to as poly(ethylene oxide-co-propylene oxide)(meth)acrylate, which is a copolymer.

[0052] The (meth)acrylate macromonomers typically have a number average molecular weight in the range of 350 to 900 Daltons. For example, the (meth)acrylate macromonomers have a number average molecular weight of no greater than 900 Daltons, no greater than 850 Daltons, no greater than 800 Daltons, no greater than 750 Daltons, no greater than 700 Daltons, no greater than 650 Daltons, no greater than 600 Daltons, no greater than 550 Daltons, no greater than 500 Daltons, or no greater than 400 Daltons, and at least 350 Daltons, at least 400 Daltons, at least 450 Daltons, or at least 500 Daltons.

[0053] The (meth)acrylate macromonomer is typically selected to be non-waxy at room temperature. That is, a (meth)acrylate macromonomer is selected that is non-crystalline and liquid at room temperature. The (meth)acrylate macromonomer typically has a glass transition temperature of no greater than -20°C (as measured using a homopolymer of the macromonomer). For example, the glass transition temperature may be no greater than -30°C, no greater than -40°C, no greater than -50°C, or no greater than -60°C. Such a low macromonomer glass transition temperature imparts conformability and flexibility to the (meth)acrylate copolymer and the adhesive composition containing the (meth)acrylate copolymer.

[0054] Examples of such commercially available (meth)acrylate macromonomers include poly(ethylene glycol) methyl ether acrylates, such as those having a reported number average molecular weight (Mn) of 480 Daltons (available from Sigma-Aldrich), and poly(propylene glycol) acrylates, such as those having a reported number average molecular weight of 475 Daltons (available from Sigma-Aldrich). Other suitable macromonomers are available from Geo Specialty Chemicals, Ambler, PA, under the tradename BISOMER, such as BISOMER PPA6 (poly(propylene glycol) acrylate having a reported number average molecular weight of 420 Daltons), BISOMER PEM63P HD (a mixture of poly(ethylene glycol) methacrylate and poly(propylene glycol) having a reported number average molecular weight of 524 Daltons), BISOMER PPM5 LI (poly(propylene glycol) methacrylate having a reported number average molecular weight of 376 Daltons), BISOMER PEM6 LD (poly(ethylene glycol) methacrylate having a reported number average molecular weight of 350 Daltons), BISOMER MPEG350MA (methoxy poly(ethylene glycol) methacrylate having a reported number average molecular weight of 430 Daltons), and BISOMER MPEG550MA (methoxy poly(ethylene glycol) methacrylate having a reported number average molecular weight of 628 Daltons). Other suitable macromonomers are available from Miwon Specialty Chemical Company, Gyeonggi-do, Korea, under the trade designation MIRAMER, such as MIRAMER M193MPEG600MA (methoxy poly(ethylene glycol) methacrylate having a reported number average molecular weight of 668 Daltons), MIRAMER M164 (nonylphenol poly(ethylene glycol) acrylate having a reported number average molecular weight of 450 Daltons), MIRAMER M1602 (nonylphenol poly(ethylene glycol) acrylate having a reported number average molecular weight of 390 Daltons), and MIRAMER M166 (nonylphenol poly(ethylene glycol) acrylate having a reported number average molecular weight of 626 Daltons). Other suitable macromonomers are available from Sans Esters Corporation, New York, NY, such as MPEG-A400 (methoxy poly(ethylene glycol) acrylate having a reported number average molecular weight of 400 Daltons) and MPEG-A550 (methoxy poly(ethylene glycol) acrylate having a reported number average molecular weight of 550 Daltons). Various combinations of such macromonomers may be used if desired.

[0055] The polymerizable components used to form the (meth)acrylate copolymers typically include at least 5 wt%, at least 10 wt%, at least 15 wt%, at least 20 wt%, at least 25 wt%, at least 30 wt%, at least 35 wt%, at least 40 wt% and up to 60 wt%, up to 55 wt%, up to 50 wt%, up to 45 wt%, or up to 40 wt% of (meth)acrylate macromers, based on the total weight of the polymerizable components.

[0056] Alkyl (meth)acrylate

[0057] The polymerizable component also includes an alkyl (meth)acrylate monomer. Any suitable alkyl (meth)acrylate or mixture of alkyl (meth)acrylates may be used, provided that the glass transition temperature of the final (meth)acrylate copolymer is sufficiently low (e.g., not greater than -15°C). Some alkyl (meth)acrylate monomers may be classified as low T based on the glass transition temperature of the corresponding homopolymer. g Monomer. Low T measured from the corresponding homopolymer g The monomers generally have a T of no greater than 20°C, no greater than 10°C, no greater than 0°C, or no greater than -10°C. g .

[0058] Suitable low T g The (meth) alkyl acrylate monomer includes, but is not limited to, non-tertiary alkyl acrylates, but may be alkyl methacrylates having a linear alkyl group of at least 4 carbon atoms. Specific examples of (meth) alkyl acrylates include, but are not limited to, methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, n-butyl methacrylate, isobutyl acrylate, sec-butyl acrylate, n-pentyl acrylate, 2-methylbutyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 4-methyl-2-pentyl acrylate, 2-methylhexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, 2-octyl acrylate, isooctyl acrylate, isononyl acrylate, isopentyl acrylate, n-decyl acrylate, isodecyl acrylate, n-decyl methacrylate, lauryl acrylate, isotridecyl acrylate, n-octadecyl acrylate, isostearyl acrylate, n-dodecyl acrylate, and combinations thereof. In some embodiments, low T g The alkyl (meth)acrylate is selected from the group consisting of 2-ethylhexyl acrylate, isooctyl acrylate, n-butyl acrylate, 2-methylbutyl acrylate, 2-octyl acrylate, and combinations thereof.

[0059] Other alkyl (meth)acrylates that may be included in the polymerizable component are classified as high T based on the glass transition temperature of the corresponding homopolymer. g Monomer. High T gThe monomers generally have a T greater than 30°C, greater than 40°C, or greater than 50°C when homopolymerized. g (i.e., the homopolymer formed from the monomer has a T greater than 30°C, greater than 40°C, or greater than 50°C g ). Some suitable high T g The alkyl (meth)acrylate monomer includes, for example, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl (meth)acrylate, cyclohexyl methacrylate, isobornyl (meth)acrylate, stearyl (meth)acrylate, and 3,3,5-trimethylcyclohexyl (meth)acrylate.

[0060] The amount of alkyl (meth)acrylate can be any suitable amount up to 95 wt %, based on the total weight of the polymerizable components. The amount can be, for example, up to 90 wt %, up to 85 wt %, up to 80 wt %, up to 75 wt %, up to 70 wt %, up to 65 wt %, up to 60 wt %, up to 55 wt %, up to 50 wt %, up to 45 wt %, or up to 40 wt %. The amount is typically at least 25 wt %, at least 30 wt %, at least 35 wt %, at least 40 wt %, at least 45 wt %, or at least 50 wt %.

[0061] If the (meth)acrylate alkyl ester is selected to include a high T g If the monomer is used in an amount greater than 20 wt % based on the total weight of the polymerizable components, the amount of the monomer is generally not greater than 20 wt % based on the total weight of the polymerizable components. That is, the amount may be in the range of 0 wt % to 20 wt % based on the total weight of the curable components. If a higher amount is used, the total T of the (meth)acrylate copolymer may be greater than 20 wt %. g May be too high. High T g The amount of alkyl (meth)acrylate monomer is typically no greater than 15 wt%, no greater than 10 wt%, or no greater than 5 wt%. If present, the amount of high Tg alkyl (meth)acrylate monomer is often at least 0.1 wt%, at least 0.2 wt%, at least 0.3 wt%, at least 0.5 wt%, or at least 1 wt%. If the polymerizable components include high Tg alkyl (meth)acrylate monomer, a sufficiently low Tg alkyl (meth)acrylate monomer is typically added. g (Meth) alkyl acrylate monomer to form T g (Meth)acrylate copolymers not exceeding -15°C.

[0062] The alkyl (meth)acrylate monomers are typically selected to include low Tg monomers, such as Tg 200, 200, 200, 300, 400, 500, 600, 700, 800, 900, 1000, 1000, 2000, 3000, 4000, 5000, 6000, 7000, 8000, 9000, 10000, 20000, 30000, 40000, 50000, 60000, 70000, 80000, 90000, 100000, 300000, 400000, 500000, 600000, 700000, 800000, gFor example, the polymerizable component often comprises at least 40 wt%, at least 45 wt%, at least 50 wt%, at least 55 wt%, at least 60 wt%, at least 65 wt%, or at least 70 wt%, and at most 95 wt%, at most 90 wt%, at most 85 wt%, at most 80 wt%, at most 75 wt%, or at most 70 wt% when measured as a homopolymer. g Low T not more than -10℃ g Monomer. This amount is based on the total weight of the polymerizable components.

[0063] When measured as a homopolymer, T g Suitable alkyl monomers having a temperature no greater than -10°C include, but are not limited to, 2-ethylhexyl acrylate, isooctyl acrylate, n-butyl acrylate, 2-methylbutyl acrylate, 2-octyl acrylate, and combinations thereof.

[0064] (Meth)acrylate-containing carboxylic acid

[0065] The polymerizable components used to form the (meth)acrylate copolymer include a (meth)acrylate-containing carboxylic acid. Exemplary (meth)acrylate-containing carboxylic acids include those selected from (meth)acrylic acid, β-carboxyethyl (meth)acrylate, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxysuccinic acid, and combinations thereof. In many embodiments, the (meth)acrylate-containing carboxylic acid is (meth)acrylic acid, and in some embodiments, acrylic acid.

[0066] The carboxylic acid containing (meth) acrylate is used in an amount not more than 15 % by weight based on the total weight of polymerizable components. Usually, if more than 15 % by weight of this acidic component is used, the adhesive composition of gained may be too hard. Based on the total weight of polymerizable components, this amount is usually not more than 12 % by weight, not more than 10 % by weight, not more than 8 % by weight, not more than 6 % by weight, not more than 5 % by weight, not more than 4 % by weight, not more than 3 % by weight or not more than 2 % by weight. Based on the total weight of polymerizable components, this amount is usually at least 0.1 % by weight, at least 0.2 % by weight, at least 0.5 % by weight or at least 1.0 % by weight.

[0067] Optional cross-linking agent

[0068] In some embodiments, (meth) acrylate copolymer is crosslinked. Generally, such crosslinking improves the durability and cohesive properties of (meth) acrylate copolymer. In some embodiments, a crosslinking agent (crosslinkingagent / crosslinker) such as a multifunctional (meth) acrylate monomer, a multifunctional aziridine or a combination thereof is used to crosslink the (meth) acrylate copolymer. As used with respect to a crosslinking agent, the term "multifunctional" means that there are at least two groups that can react to crosslink the (meth) acrylate copolymer. Examples of multifunctional (meth) acrylate monomer crosslinkers include, but are not limited to, 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, poly (ethylene glycol) diacrylate (e.g., Mw in the range of 100 daltons to 1,000 daltons), ethoxylated bisphenol A diacrylate, tetraethylene glycol diacrylate, trimethylolpropane triacrylate and 1,6-hexanediol diacrylate. Examples of aziridine crosslinkers include 1,1'-isophthaloyl-bis (2-methylaziridine). Crosslinking can also be achieved using electron beam radiation without the addition of chemical crosslinking agents.

[0069] The polymerizable component typically includes 0 to 5 weight percent of an optional crosslinking agent. Based on the total weight of the polymerizable component, the amount may be at least 0.1 weight percent, at least 0.2 weight percent, at least 0.3 weight percent, at least 0.5 weight percent, or at least 1 weight percent, and up to 5 weight percent, up to 4 weight percent, up to 3 weight percent, up to 2 weight percent, or up to 1 weight percent. The amount of crosslinking agent included depends on well-known factors, such as the desired degree of crosslinking and / or the relative effectiveness of the crosslinking agent in a specific system, as measured by well-known tests such as shear adhesion. Any conventional technique such as thermal initiation or actinic radiation initiation may be used to initiate polymer crosslinking using such crosslinking agents.

[0070] Optional non-acidic polar monomer

[0071] Other optional polar monomers may be included in the non-acidic polymerizable component. For example, the non-acidic polar monomer may have a hydroxyl group, an ether (or polyether) group, or a nitrogen-containing group. Suitable nitrogen-containing groups are typically primary acylamino groups, secondary acylamino groups, tertiary acylamino groups, or amino groups.

[0072] Exemplary polar monomers containing hydroxyl groups include, but are not limited to, hydroxyalkyl (meth)acrylates (e.g., 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate), hydroxyalkyl (meth)acrylamides (e.g., 2-hydroxyethyl (meth)acrylamide or 3-hydroxypropyl (meth)acrylamide), ethoxylated hydroxyethyl (meth)acrylates (e.g., monomers commercially available under the trade names CD570, CD571, and CD572 from Sartomer (Exton, PA, USA)), aryloxy-substituted hydroxyalkyl (meth)acrylates (e.g., 2-hydroxy-2-phenoxypropyl (meth)acrylate), 4-vinylphenol, and hydroxypropyl-urethane acrylate.

[0073] Exemplary ether-containing (meth)acrylate monomers include those selected from 2-ethoxyethyl (meth)acrylate, 2-methoxyethoxyethyl (meth)acrylate, di(ethylene glycol)-2-ethylhexyl ether acrylate, ethylene glycol-methyl ether acrylate, and combinations thereof. Suitable ether-containing (meth)acrylate monomers have a number average molecular weight of less than 350 Daltons, less than 300 Daltons, or less than 250 Daltons.

[0074] Exemplary polar monomers containing primary amido groups include (meth)acrylamide. Exemplary polar monomers containing secondary amido groups include, but are not limited to, N-alkyl (meth)acrylamide or N-alkoxyalkyl (meth)acrylamide, such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, or N-octyl (meth)acrylamide. N-(3-methoxypropyl)acrylamide or N-(isobutoxymethyl)acrylamide. Exemplary polar monomers containing tertiary acylamino groups include, but are not limited to, N-vinyl carbazole, N-vinyl caprolactam, N-vinyl-2-pyrrolidone, N-vinyl azlactone, 4-(meth)acryloylmorpholine, N-vinylimidazole, urea (meth)acrylates, and N,N-dialkyl (meth)acrylamides, such as N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, and N,N-dibutyl (meth)acrylamide.

[0075] Polar monomers having amino groups include various N,N-dialkylaminoalkyl (meth)acrylates and N,N-dialkylaminoalkyl (meth)acrylamides. Examples include, but are not limited to: N,N-dimethylaminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylamide, N,N-dimethylaminopropyl (meth)acrylate, N,N-dimethylaminopropyl (meth)acrylamide, N,N-diethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylamide, N,N-diethylaminopropyl (meth)acrylate, and N,N-diethylaminopropyl (meth)acrylamide.

[0076] In some embodiments, the polymer of the adhesive composition of the present disclosure includes monomer units derived from carboxylic acids containing (meth) acrylates and monomers containing N polar monomers (e.g., monomers containing primary acylamino groups, secondary acylamino groups, tertiary acylamino groups, or amino groups). This combination of monomers can provide an adhesive composition having excellent high impact resistance or drop resistance and excellent bonding formation ability (i.e., good viscosity, instant bonding formation). These performance criteria are often highly desired for applications within the electronic bonding and industrial market segments.

[0077] The amount of optional non-acidic polar monomer is typically no greater than 20 weight percent, no greater than 15 weight percent, no greater than 10 weight percent, or no greater than 5 weight percent, based on the total weight of the polymerizable components. If present, the amount of the monomer is often at least 0.1 weight percent, at least 0.5 weight percent, at least 1 weight percent, at least 2 weight percent, or at least 5 weight percent.

[0078] In many embodiments, the total combined weight of the acidic monomer (i.e., carboxylic acid containing (meth)acrylate) and the optional non-acidic polar monomer is no greater than 35 wt%, no greater than 30 wt%, no greater than 25 wt%, no greater than 20 wt%, no greater than 15 wt%, no greater than 10 wt%, or no greater than 5 wt%, based on the total weight of the polymerizable components. The amount of such monomer is often at least 0.2 wt%, at least 0.5 wt%, at least 1 wt%, at least 2 wt%, or at least 5 wt%.

[0079] Aggregation methods

[0080] The (meth)acrylate copolymers can be prepared from the polymerizable components using any known polymerization method, including those activated thermally or by actinic radiation (e.g., actinic radiation in the visible and / or ultraviolet regions of the electromagnetic spectrum). A free radical initiator is typically combined with the polymerizable components. Other optional components such as chain transfer agents, antioxidants, solvents, etc. may be included in the polymerizable composition.

[0081] The free radical initiator, which may be a photoinitiator or a thermal initiator, is generally used to form a (meth) acrylate copolymer. A variety of photoinitiators or a variety of thermal initiators may be used. The amount of the free radical initiator may affect the weight average molecular weight, wherein a larger amount generally produces a copolymer material of lower molecular weight. Based on the total weight of the polymerizable components, the amount of the free radical initiator is generally at least 0.001 wt %, at least 0.005 wt %, at least 0.01 wt %, at least 0.05 wt % or at least 0.1 wt %. Based on the total weight of the polymerizable components, the amount may be at most 5 wt %, at most 4 wt %, at most 3 wt %, at most 2 wt %, at most 1.5 wt %, at most 1 wt %, at most 0.5 wt %, at most 0.3 wt %, at most 0.2 wt % or at most 0.1 wt %.

[0082] Suitable thermal initiators include various azo compounds such as those commercially available under the trade name VAZO from The Chemours Co. (Wilmington, DE, USA), including VAZO 67 (which is 2,2'-azobis(2-methylbutyronitrile)), VAZO 64 (which is 2,2'-azobis(isobutyronitrile)), VAZO 52 (which is 2,2'-azobis(2,4-dimethylvaleronitrile)), and VAZO 88 (which is 1,1'-azobis(cyclohexanecarbonitrile)); various peroxides such as benzoyl peroxide, cyclohexane peroxide, lauroyl peroxide, di-tert-amyl peroxide, t-butyl perbenzoate, dicumyl peroxide, and the like under the trade name LUPERSOL from Atofina Chemical Company (Philadelphia, Pennsylvania, USA). Peroxides commercially available from LUPERSOL Chemical, Inc. (Philadelphia, PA, USA) (e.g., LUPERSOL 101, which is 2,5-bis(tert-butylperoxy)-2,5-dimethylhexane, and LUPERSOL 130, which is 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne); various hydroperoxides, such as tert-amyl hydroperoxide and tert-butyl hydroperoxide; and mixtures thereof.

[0083] In many embodiments, a photoinitiator is used to form a (meth)acrylate copolymer. Some exemplary photoinitiators are benzoin ethers (e.g., benzoin methyl ether or benzoin isopropyl ether) or substituted benzoin ethers (e.g., anisole methyl ether). Other exemplary photoinitiators are substituted acetophenones, such as 2,2-diethoxyacetophenone or 2,2-dimethoxy-2-phenylacetophenone (commercially available under the trade name IRGACURE 651 from BASF Corp., Florham Park, NJ, USA or under the trade name ESACURE KB-1 from Sartomer, Exton, PA, USA). Still other exemplary photoinitiators are substituted α-keto alcohols (such as 2-methyl-2-hydroxypropiophenone), aromatic sulfonyl chlorides (such as 2-naphthalenesulfonyl chloride), and photoactive oximes (such as 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)oxime). Other suitable photoinitiators include, for example, 1-hydroxycyclohexyl phenyl ketone (available under the trade name IRGACURE 184), bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide (available under the trade name IRGACURE 819), 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one (available under the trade name IRGACURE 2959), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone (available under the trade name IRGACURE 369), 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one (available under the trade name IRGACURE 907), and 2-hydroxy-2-methyl-1-phenylpropan-1-one (available under the trade name DAROCUR 1173 from Ciba Specialty Chemicals, Tarrytown, NY, USA). (Commercially available from Efficacy Chemicals Corp. (Tarrytown, NY, USA)).

[0084] Chain transfer agents are generally included in the polymerizable composition to control the molecular weight of the (meth)acrylate copolymer. Suitable chain transfer agents include, but are not limited to, those selected from the following: carbon tetrabromide, hexabromoethane, bromotrichloromethane, 2-mercaptoethanol, tert-dodecyl mercaptan, isooctylthioglycolate, 3-mercapto-1,2-propylene glycol, cumene, pentaerythritol tetrakis (3-mercaptobutyrate) (available under the trade name KARENZ MT PE1 from Showa Denko), ethylene glycol dithioglycolate, and mixtures thereof. Depending on the reactivity of the selected chain transfer agent, the amount of the chain transfer agent is generally in the range of 0 wt % to 5 wt % based on the total weight of the monomers in the polymerizable composition. In some embodiments, the amount of chain transfer agent is at least 0.05 wt%, at least 0.1 wt%, at least 0.2 wt%, at least 0.3 wt%, or at least 0.5 wt%, and can be up to 5 wt%, up to 4.5 wt%, up to 4 wt%, up to 3.5 wt%, up to 3 wt%, up to 2.5 wt%, up to 2 wt%, up to 1.5 wt%, or up to 1 wt%. The weight percentage values ​​are based on the total weight of the polymerizable components used to form the (meth)acrylate copolymer.

[0085] The reaction of the polymerizable composition to form the (meth)acrylate copolymer can occur in the presence or absence of an organic solvent. If an organic solvent is included in the polymerizable composition, the amount is often selected to provide a desired viscosity. Examples of suitable organic solvents include, but are not limited to, methanol, tetrahydrofuran, ethanol, isopropanol, pentane, hexane, heptane, acetone, methyl ethyl ketone, methyl acetate, ethyl acetate, toluene, xylene, and ethylene glycol alkyl ethers. Those organic solvents can be used alone or as mixtures thereof.

[0086] In some embodiments, based on the total weight of the polymerizable composition, polymerization occurs in the presence of at least 10 wt % organic solvent. For example, the amount can be at least 20 weight percents, at least 30 weight percents, at least 40 weight percents, and at most 70 weight percents, at most 60 weight percents, at most 50 weight percents. In other embodiments, polymerization is carried out in the presence of less or no organic solvent. That is, the polymerizable composition does not contain organic solvent or contains a minimum amount of organic solvent. If an organic solvent is used, then based on the total weight of the polymerizable composition, the organic solvent is generally present in an amount less than 10 weight %, less than 5 weight %, less than 4 weight %, less than 3 weight %, less than 2 weight % or less than 1 weight %.

[0087] The (meth)acrylate copolymer can be formed from the polymerizable composition using any suitable method. The polymerization can be carried out in a single step or in multiple steps. That is, all or a portion of the monomers and / or free radical initiators can be charged into a suitable reaction vessel and polymerized. For example, a polymerizable composition comprising an organic solvent and a thermal initiator can be mixed and heated at an elevated temperature, such as in the range of 50° C. to 100° C. for several hours.

[0088] In one possible method for preparing (meth)acrylate copolymers, little or no organic solvent is included in the polymeric composition. This free radical polymerization process can be carried out in a continuous manner as described, for example, in U.S. Pat. Nos. 4,619,979 (Kotnour et al.) and 4,843,134 (Kotnour et al.). In an alternative method for preparing (meth)acrylate copolymers, an adiabatic method such as described in U.S. Pat. Nos. 5,986,011 (Ellis et al.) and 5,637,646 (Ellis) can be used. In another method for preparing (meth)acrylate copolymers, the polymerization reaction can occur in a polymer package, as described in U.S. Pat. No. 5,804,610 (Hamer et al.).

[0089] Depending on the composition of the polymerizable composition, the resulting (meth)acrylate copolymer may be non-crosslinked or crosslinked. In many embodiments, the (meth)acrylate copolymer is crosslinked.

[0090] Adhesive composition

[0091] Provided is an adhesive composition comprising a (meth)acrylate copolymer. The adhesive composition is a pressure-sensitive adhesive. The (meth)acrylate copolymer itself may have adhesive properties suitable for use as a pressure-sensitive adhesive. Alternatively, an optional additive (such as a tackifier) ​​may be combined with the (meth)acrylate copolymer to provide a composition with suitable adhesive properties. Available tackifiers include, for example, rosin ester resins and terpene phenol resins. Tackifiers are typically mixed in an amount less than or equal to the amount of the (meth)acrylate-based polymer material contained in the core. Based on the gross weight of the polymerizable composition, the amount of the optional tackifier is often in the range of 0 wt % to 25 wt %, 0 wt % to 20 wt %, 0 wt % to 15 wt %, 0 wt % to 10 wt %, or 0 wt % to 5 wt %.

[0092] Optional antioxidants and / or stabilizers, such as hydroquinone monoethyl ether (p-methoxyphenol, MeHQ), available under the trade name IRGANOX 1010 (pentaerythritol tetrakis (3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) from BASF Corp., Florham Park, NJ, USA, may be added to increase the temperature stability of the polymeric material. If used, antioxidants and / or stabilizers are typically added in the range of 0.01 wt % to 1.0 wt %, based on the total weight of the polymerizable components used to form the (meth)acrylate copolymer.

[0093] Various other optional components may be added to the polymerizable composition, such as adhesion promoters (e.g., (3-glycidoxypropyl)trimethoxysilane or (3-glycidoxypropyl)triethoxysilane), colorants (e.g., titanium dioxide or carbon black), dyes, corrosion inhibitors (e.g., benzotriazole), antistatic agents, plasticizers, thickeners, thixotropic agents, processing aids, nanoparticles, fibers, and combinations thereof. Generally, the amount of each additive will depend on the use of the adhesive composition.

[0094] In some embodiments, the adhesive composition may have a viscosity of at least 0.6 g / cm3. 3 ), at least 0.8g / cm 3 , or at least 1.0g / cm 3 The adhesive composition is generally not a foam.

[0095] In some embodiments, the adhesive composition (which may be only a cross-linked polymer) exhibits desired adhesion properties. For example, in some embodiments, the adhesive composition exhibits 180 degree peel adhesion of at least 0.3 N / mm on polyethylene terephthalate, at least 0.3 N / mm on glass, at least 0.3 N / mm on polycarbonate, and at least 0.5 N / mm on stainless steel at 12.6 inches / minute (32 centimeters / minute (cm / min)) at 23°C, wherein the adhesive thickness is 35 microns. 180 degree peel adhesion can generally be regarded as a measure of the ability of the adhesive composition to resist debonding from the substrate by adhesive / interface or cohesive / internal failure mode. 180 degree peeling is measured according to the method described in the examples (Test Method 3).

[0096] In some embodiments, the adhesive composition (which may be only an optionally crosslinked (meth) acrylate copolymer) exhibits: at a frequency of 1 Hz, at a temperature of 23° C., a shear storage modulus (G') of typically not more than 50 kPa, not more than 40 kPa, not more than 30 kPa, or not more than 20 kPa; and at a temperature of -20° C., at a frequency of 1 Hz, a shear storage modulus (G') of typically not more than 2000 kPa, not more than 1600 kPa, not more than 1200 kPa, not more than 1000 kPa, not more than 800 kPa, not more than 600 kPa, not more than 500 kPa, not more than 400 kPa, or not more than 200 kPa. The shear modulus indicates the elastic and viscous response of the material to the applied shear stress. These relatively low shear storage modulus values ​​indicate that the pressure-sensitive adhesive is soft enough to bond well to the substrate. If the shear storage modulus is no greater than 2000 kPa at -20°C and no greater than 50 kPa at 23°C, the adhesive can generally undergo sufficient deformation to be folded. The shear storage modulus is determined according to the method described in the Examples (Test Method 1).

[0097] In some embodiments, the adhesive composition (which may be only an optionally cross-linked (meth)acrylate copolymer) exhibits: a maximum shear strain percentage of at least 300%, at least 400%, at least 500%, or at least 600% under an applied shear stress of 40 kPa; and a strain recovery of at least 60% within 1 minute after removing the applied shear stress of 40 kPa. Shear strain and strain recovery demonstrate the conformability and recovery of the composition, which is important for flexible and / or foldable articles. Shear strain and recovery are measured according to the method described in the examples (Test Method 2).

[0098] In some embodiments, using 35 μ m thick adhesive, the adhesive composition (which can be only an optionally cross-linked (meth) acrylate copolymer) shows an impact resistance of at least 250 mJ for the total energy absorbed, and shows an impact resistance greater than 3 MPa for the peak force. The total energy absorbed is generally at least 275 mJ, at least 300 mJ, at least 325 mJ, at least 350 mJ, at least 375 mJ or at least 400 mJ. This is generally considered to be a measure of the ability of the composition to absorb impact energy at a relevant rate and temperature under a tensile deformation mode. Impact resistance is measured according to the method described in the examples (Test Method 4).

[0099] In some embodiments, the adhesive composition (which may be only the optionally crosslinked (meth)acrylate copolymer) has a haze value of less than 5%, less than 2%, or less than 1%. This is important for articles where an optically clear adhesive is desired. The haze value is determined according to the method described in the Examples (Test Method 5).

[0100] For use in foldable or flexible articles, it may be desirable for the adhesive composition to have a combination of good adhesive properties, good impact resistance, and good foldability. That is, the adhesive composition typically exhibits the following properties: (1) a 180 degree peel adhesion of at least 0.5 N / mm on stainless steel (alternatively or additionally, at least 0.3 N / mm on polyethylene terephthalate and / or at least 0.3 N / mm on glass and / or at least 0.3 N / mm on polycarbonate) at 12.6 inches / minute (32 centimeters / minute (cm / min)) at 23°C, where the adhesive thickness is 35 microns and (2) a shear storage modulus of no more than 2000 kPa at -20°C and no more than 50 kPa at 23°C. Using a 35 μm thick adhesive, the impact resistance is typically at least 250 mJ for total energy absorbed and greater than 3 MPa for peak force.

[0101] Products

[0102] Provided are articles comprising an adhesive composition and a substrate. Any suitable substrate can be used. In many embodiments, the layer of the adhesive composition is positioned adjacent to the substrate. The adhesive composition can be in direct contact with the substrate or can be separated from the substrate by a layer (such as a primer layer) in the multilayer.

[0103] Any suitable substrate can be used. In some embodiments, the substrate is flexible. Examples of flexible substrate materials include, but are not limited to, polymer films, woven or nonwoven fabrics; metal foil, foam (e.g., polyacrylic acid, polyethylene, polyurethane) and combinations thereof (e.g., metallized polymer films). Polymer films include, for example, polypropylene (e.g., biaxially oriented), polyethylene (e.g., high density or low density), polyvinyl chloride, polyurethane (e.g., thermoplastic polyurethane), polyester (e.g., polyethylene terephthalate (PET), polyethylene naphthalate (PEN) and polylactic acid copolymer), polycarbonate, polyacrylate, poly(methyl)acrylate (PMMA), polyvinyl butyral, polyimide, polyamide, fluoropolymer, cellulose acetate, triacetyl cellulose (TAC), ethyl cellulose and polycyclic olefin polymer (COP). Woven or nonwoven fabrics may include fibers or filaments of synthetic or natural materials such as cellulose, cotton, nylon, rayon, glass, ceramic materials, etc.

[0104] In some embodiments, the article is or comprises an adhesive tape. Examples of such tapes include transfer tapes, single-sided tapes, double-sided tapes (i.e., a core substrate having an adhesive layer on each side of the substrate) or a die-cut adhesive article (e.g., an article having an adhesive layer positioned adjacent to a release liner or positioned between two release liners). Such tapes may include a variety of substrates used as backings or release liners. Examples include woven and nonwoven materials, plastic films, metal foils, etc.

[0105] Adhesive tape is usually prepared by applying adhesive composition to various flexible or non-flexible backing materials and / or release liner using conventional coating techniques to produce single-sided tape or double-sided tape. With regard to single-sided tape, adhesive composition can be applied to the backing material layer, and the side of the backing material opposite to the place where the adhesive is set can be coated with suitable release material (for example, release layer or release liner). Release material is known, and includes materials such as, for example, silicone, polyethylene, polyurethane, polyacrylic acid. For double-sided tape, the first adhesive composition is applied to the backing material layer, and the second layer of adhesive composition is arranged on the opposite surface of the backing material. The second layer can include adhesive composition as described herein or different adhesive compositions. For die-cut adhesive products or for transfer tape, the adhesive composition is usually positioned between two release liners.

[0106] The adhesive article can be part of another article. For example, the adhesive composition can bond two parts of an article together. In some such articles, the adhesive is positioned adjacent to a flexible and / or foldable substrate and is used in another flexible and / or foldable article, such as in a flexible and / or foldable electronic device.

[0107] In some embodiments, the article comprising the adhesive composition is a part of an electronic device. In such devices, the adhesive composition is usually formed into a layer between two substrates for bonding the two substrates together. Examples of suitable substrates include materials such as polyacrylates, polymethyl methacrylates, polycarbonates, polyamides, polyimides, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polycyclic olefin polymers (COP), thermoplastic polyurethanes, triacetyl cellulose (TAC) and metal foils.

[0108] A common application of adhesives in the electronics industry today is the manufacture of various displays, such as computer monitors, televisions, mobile phones, and small displays (in cars, appliances, wearables, electronic devices, etc.). Flexible electronic displays (wherein the display can be bent freely without cracking or breaking) are a rapidly emerging technology field for making electronic devices using, for example, flexible plastic substrates. This technology allows electronic functions to be integrated into non-planar objects, conforming to desired designs, and flexibility during use, which can generate a large number of new applications. Therefore, in some embodiments, the electronic device includes a flexible display.

[0109] With the advent of flexible electronic displays, there is an increasing demand for adhesives, and in particular for optically transparent adhesives (OCAs), to be used as an assembly layer or gap filling layer between an outer cover lens or sheet (based on glass, polyethylene terephthalate (PET), polycarbonate (PC), polymethyl methacrylate (PMMA), polyimide, polyethylene naphthalate (PEN), cyclic olefin copolymer, etc.) of an electronic display assembly and a display module below. The presence of OCA improves the performance of the display by increasing brightness and contrast, while also providing structural support for the assembly. In flexible assemblies, OCA will also be used as an assembly layer, which, in addition to typical OCA functions, can also absorb most of the stress caused by folding to prevent damage to the fragile components of the display panel and protect the electronic assembly from breaking under folding stress. The OCA layer can also be used to configure and retain the neutral bending axis at or at least near the fragile components of the display, such as, for example, a barrier layer, a drive electrode, or a thin film transistor of an organic light emitting display (OLED). The adhesive composition described herein can be prepared as an OCA.

[0110] In some embodiments, the electronic device includes a photovoltaic device. The performance and device configuration of photovoltaic devices are developing rapidly. The ability to roll or fold portable arrays is an attractive design for off-grid uses such as long-distance regional travel or living, camping, and mobile applications. As photovoltaic (PV) modules become more efficient, the number of modules required to generate sufficient power is reduced, thereby reducing size and weight. Integrating organic PV cells or inorganic PV cells onto or into flexible forms provides an advantageous design.

[0111] Other flexible articles that may include the adhesive compositions described herein include, for example, rollable keyboards, electronic game sensors, lighting elements, and articles of clothing.

[0112] The article is usually formed by positioning the adhesive layer adjacent to the substrate. Conventional coating techniques can be used to coat the adhesive composition on the substrate (for example backing or release liner). For example, the adhesive composition can be applied by methods such as roller coating, flow coating, dip coating, spin coating, spray coating, scraping and die coating. Based on the gross weight of the adhesive composition, the applied adhesive composition can have any required solid weight percentage, but usually in the scope of 10 solid weight percentages to 100 solid weight percentages. Required solid content can be realized by further diluting the coating composition or by partial drying.

[0113] The adhesive composition that is arranged on substrate as a layer or is arranged between two release liners as a layer generally has a thickness of up to 100 microns (i.e., microns or μm), up to 50 microns, up to 35 microns or up to 25 microns. In some embodiments, the adhesive composition may have an overall (average) thickness of up to 400 microns, up to 300 microns or up to 200 microns of the adhesive composition arranged on the substrate in the layer (e.g., in the form of a coating placed between the liners). The desired thickness depends on the specific use of the adhesive layer. A thinner layer may be desirable for applications where the adhesive composition will be folded, and a thicker layer may be desirable for applications where the adhesive composition will be folded.

[0114] Implementation

[0115] Various embodiments are provided, such as (meth)acrylate copolymers, adhesive compositions comprising the (meth)acrylate copolymers, and articles comprising the adhesive compositions.

[0116] Embodiment 1A is a (meth)acrylate copolymer comprising monomer units derived from a polymerizable component comprising (1) a (meth)acrylate macromonomer comprising a poly(ethylene oxide) group, a poly(propylene oxide) group, or a poly(ethylene oxide-co-propylene oxide) group, (2) an alkyl (meth)acrylate, and (3) a (meth)acrylate-containing carboxylic acid. The (meth)acrylate macromonomer has a number average molecular weight of no greater than 900 g / mole and is present in an amount of at least 5 wt % based on the total weight of the polymerizable component. The (meth)acrylate-containing carboxylic acid is present in an amount of no greater than 15 wt % based on the total weight of the polymerizable component. The (meth)acrylate copolymer has a glass transition temperature of no greater than -15°C.

[0117] Embodiment 2A is the (meth)acrylate copolymer of embodiment 1A, wherein the polymerizable component comprises 5 wt % to 60 wt % of the (meth)acrylate macromonomer.

[0118] Embodiment 3A is the (meth)acrylate copolymer of embodiment 1A or 2A, wherein the (meth)acrylate macromonomer has a weight average molecular weight in a range of 350 g / mol to 900 g / mol.

[0119] Embodiment 4A is a (meth)acrylate copolymer according to any one of embodiments 1A to 3A, wherein the (meth)acrylate macromonomer has a poly(ethylene oxide) group.

[0120] Embodiment 5A is a (meth)acrylate copolymer according to any one of Embodiments 1A to 4A, wherein the (meth)acrylate macromonomer has a T of no greater than -20°C when measured as a homopolymer. g .

[0121] Embodiment 6A is the (meth)acrylate copolymer of any one of embodiments 1A to 5A, wherein the polymerizable component comprises 25 wt% to 95 wt% of the alkyl (meth)acrylate, based on the total weight of the polymerizable component.

[0122] Embodiment 7A is a (meth)acrylate copolymer according to embodiment 6A, wherein the polymerizable component comprises no more than 20 wt % of the (meth)acrylate copolymer as a homopolymer. g Alkyl (meth)acrylates above 30°C.

[0123] Embodiment 8A is a (meth)acrylate copolymer according to any one of Embodiments 1A to 7A, wherein the polymerizable component comprises a mixture of alkyl (meth)acrylates, and the mixture of alkyl (meth)acrylates comprises at least one g Low T not more than -10℃ g Alkyl (meth)acrylate.

[0124] Embodiment 9A is a (meth)acrylate copolymer according to embodiment 6A, wherein the polymerizable component comprises 40 wt % to 95 wt % of a (meth)acrylate copolymer having a molecular weight of 100 Å and a molecular weight of 100 Å. g Low T not more than -10℃ g Alkyl (meth)acrylate, the weight percentage is based on the total weight of the polymerizable components.

[0125] Embodiment 10A is a (meth)acrylate copolymer according to embodiment 8A or 9A, wherein the low T g The monomer is selected from the group consisting of 2-ethylhexyl acrylate, isooctyl acrylate, n-butyl acrylate, 2-methylbutyl acrylate, 2-octyl acrylate, and combinations thereof.

[0126] Embodiment 11A is the (meth)acrylate copolymer of any of Embodiments 1A to 10A, wherein the polymerizable components comprise 0.1 wt% to 15 wt% of the (meth)acrylate-containing carboxylic acid, based on the total weight of the polymerizable components.

[0127] Embodiment 12A is a (meth)acrylate copolymer according to any one of embodiments 1A to 11A, wherein the (meth)acrylate-containing carboxylic acid is selected from (meth)acrylic acid, β-carboxyethyl (meth)acrylate, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxysuccinic acid, and combinations thereof.

[0128] Embodiment 13A is a (meth)acrylate copolymer according to any one of Embodiments 1A to 12A, wherein the (meth)acrylate-containing carboxylic acid is (meth)acrylic acid.

[0129] Embodiment 14A is a (meth)acrylate copolymer according to any one of embodiments 1A to 13A, wherein the polar component comprises 5 wt% to 60 wt% of the (meth)acrylate macromonomer, 25 wt% to 95 wt% of the (meth)acrylate alkyl ester, and 0.1 wt% to 15 wt% of the (meth)acrylate-containing carboxylic acid, based on the total weight of the polymerizable components.

[0130] Embodiment 15A is the (meth)acrylate copolymer of any one of embodiments 1A to 14A, wherein the polymerizable component further comprises an optional non-acidic polar monomer.

[0131] Embodiment 16A is the (meth)acrylate copolymer of embodiment 15A, wherein the non-acidic polar monomer is a hydroxyl-containing monomer, an ether-containing monomer, or a nitrogen-containing monomer.

[0132] Embodiment 17A is a (meth)acrylate copolymer according to embodiment 16A, wherein the nitrogen-containing monomer has a primary amido group, a secondary amido group, a tertiary amido group, or an amino group.

[0133] Embodiment 18A is the (meth)acrylate copolymer of any one of embodiments 15A to 19A, wherein the non-acidic polar monomer is a nitrogen-containing monomer.

[0134] Embodiment 19A is a (meth)acrylate copolymer according to embodiment 18A, wherein the nitrogen-containing monomer is selected from acrylamide, N,N-dimethylacrylamide, N,N-diethylacrylamide, N-vinylcarbazole, N-vinyl 2-pyrrolidone, N-vinylimidazole, ureido (meth)acrylate, hydroxypropyl-urethane acrylate, 4-acryloylmorpholine, N-isopropylacrylamide, N-(3-methoxypropyl)acrylamide, alkylacrylamide, N-(isobutoxymethyl)acrylamide, N-vinylcaprolactam, and combinations thereof.

[0135] Embodiment 20A is the (meth)acrylate copolymer of any of embodiments 15A to 19A, wherein the amount of the optional non-acidic polar monomer ranges from 0 wt % to 20 wt % based on the total weight of the polymerizable components.

[0136] Embodiment 21A is a (meth)acrylate copolymer according to any one of embodiments 15A to 20A, wherein the polymerizable components comprise no greater than 35 weight percent of the (meth)acrylate-containing carboxylic acid plus the non-acidic polar monomer, based on the total weight of the polymerizable components.

[0137] Embodiment 22A is the (meth)acrylate copolymer of any one of embodiments 1A to 21A, wherein the (meth)acrylate copolymer is cross-linked.

[0138] Embodiment 23A is the (meth)acrylate copolymer according to embodiment 22A, wherein the (meth)acrylate copolymer is crosslinked using electron beam radiation or a crosslinking agent.

[0139] Embodiment 24A is the (meth)acrylate copolymer of any of embodiments 1A to 23A, wherein the polymerizable components further comprise 0 wt % to 5 wt % of an optional crosslinker, based on the total weight of the polymerizable components.

[0140] Embodiment 25A is the (meth)acrylate copolymer according to embodiment 24A, wherein the crosslinking agent is a multifunctional (meth)acrylate monomer or a multifunctional aziridine compound.

[0141] Embodiment 26A is a (meth)acrylate copolymer according to any one of Embodiments 1A to 25A, wherein the (meth)acrylate copolymer has a T g Not more than -20℃.

[0142] Embodiment 27A is a (meth)acrylate copolymer according to any one of embodiments 1A to 26A, wherein the (meth)acrylate copolymer contains no hydroxyl-containing monomer or contains no greater than 5 weight percent of hydroxyl-containing monomer based on the total weight of the polymerizable components.

[0143] Embodiment 28A is a (meth)acrylate copolymer according to any one of embodiments 1A to 27A, wherein the (meth)acrylate copolymer does not contain a vinyl monomer selected from vinyl acetate and a non-polar vinyl monomer, or contains no more than 5 weight percent of the vinyl monomer based on the total weight of the polymerizable components.

[0144] Embodiment 1B is an adhesive composition, wherein the adhesive composition comprises the (meth)acrylate copolymer according to embodiment 1A.

[0145] Embodiment 2B is the adhesive composition of embodiment 1B, wherein the adhesive composition comprises the (meth)acrylate copolymer of any one of embodiments 2A to 28A.

[0146] Embodiment 3B is the adhesive composition of embodiment 1B or 2B, wherein the adhesive composition further comprises an optional plasticizer and / or an optional tackifier.

[0147] Embodiment 4B is the adhesive composition of any one of Embodiments 1B to 3B, wherein the adhesive composition further comprises a filler, an adhesion promoter, a colorant, a UV absorber, an antioxidant, a stabilizer, or a combination thereof.

[0148] Embodiment 5B is the adhesive composition of any one of Embodiments 1B to 4B, wherein the adhesive composition is a pressure sensitive adhesive.

[0149] Embodiment 6B is the adhesive composition of any one of Embodiments 1B to 5B, wherein the adhesive composition exhibits a 180 degree peel adhesion of at least 0.3 N / mm on polyethylene terephthalate, at least 0.3 N / mm on glass, at least 0.3 N / mm on polycarbonate, and at least 0.5 N / mm on stainless steel at 12.6 inches / minute (32 centimeters / minute (cm / min)) at 23°C, wherein the adhesive thickness is 35 microns.

[0150] Embodiment 7B is the adhesive composition of any one of Embodiments 1B to 6B, wherein the adhesive composition exhibits a shear storage modulus of no greater than 2000 kPa at -20°C and no greater than 50 kPa at 23°C.

[0151] Embodiment 8B is the adhesive composition of any one of Embodiments 1B to 7B, wherein a 35 μm thick adhesive is used, and the adhesive composition exhibits an impact resistance of at least 250 mJ for total energy absorbed and an impact resistance of greater than 3 MPa for peak force.

[0152] Embodiment 9B is an adhesive composition according to any one of Embodiments 1B to 8B, wherein the adhesive composition exhibits a maximum shear strain percentage of at least 300% under an applied shear stress of 40 kPa and a strain recovery of at least 60% within 1 minute after removal of the applied shear stress of 40 kPa.

[0153] Embodiment 10B is the adhesive composition of any one of embodiments 1B to 9B, wherein the haze is less than 5% (or less than 2% or less than 1%) based on the Optical Durability Test.

[0154] Embodiment 1C is an article comprising a substrate and the adhesive composition according to embodiment 1B positioned adjacent to the substrate.

[0155] Embodiment 2C is the article of embodiment 1C, wherein the adhesive composition is the adhesive composition of any one of embodiments 2B to 10B.

[0156] Embodiment 3C is the article of embodiment 1C or 2C, wherein the article is a transfer tape, a single-sided tape, a double-sided tape, or a die-cut adhesive article.

[0157] Embodiment 4C is an article according to embodiment 1C or 2C, wherein the article is an electronic device comprising the adhesive composition.

[0158] Embodiment 5C is an article according to Embodiment 4C, wherein the electronic device comprises a flexible display or a photovoltaic device.

[0159] Embodiment 6C is an article according to embodiment 1C or 2C, wherein the article is a flexible article.

[0160] Embodiment 7C is an article according to embodiment 6C, wherein the flexible article is an electronic device.

[0161] Embodiment 8C is an article according to embodiment 1C or 2C, wherein the article is a foldable article.

[0162] Embodiment 9C is the article of embodiment 8C, wherein the foldable article is an electronic display device.

[0163] Embodiment 10C is the article of embodiment 8C or 9C, wherein the foldable article is flexible.

[0164] Example

[0165] While objects and advantages of this disclosure are further illustrated by the following examples, the materials and amounts thereof recited in these examples, as well as other conditions and details, should not be construed to unduly limit this disclosure.

[0166] Unless otherwise indicated, all parts, percentages, ratios, etc. used in the examples and other parts of the specification are by weight, and all reagents used in the examples are obtained from or can be purchased from general chemical suppliers, such as, for example, Sigma-Aldrich, St. Louis, MO, or can be synthesized by conventional methods.

[0167] The following abbreviations are used in this section: mL = milliliter, min = minute, h = hour, sec = second, g = gram, mg = milligram, Kg = kilogram, J = joule, mJ = millijoule, mmol = millimole, m = meter, cm = centimeter, mm = millimeter, μm = micrometer or micrometer, ms -1 = meter / second, °C = degrees Celsius, cP = centipoise, mmHg = millimeters of mercury, kPa = kilopascals, lb = pounds, N = Newton, oz = ounces, rpm = revolutions per minute, mW / cm 2 = milliwatt per square centimeter, mJ / cm 2 = millijoules per square centimeter, Hz = Hertz, Da = Daltons, phr = parts per hundred parts of resin (ie, total polymer mass).

[0168] Table 1: Materials

[0169]

[0170]

[0171] Test Method

[0172] Test Method 1: Dynamic Mechanical Analysis (DMA) Test

[0173] The transfer tapes for DMA testing were laminated together to form a stack with a total thickness of 1 mm by removing the RF02N release liner and repeatedly folding the sticky side over on itself (using a 15-cm rubberized hand roller (Polymag Tek, NY)) to ensure that no air bubbles were trapped within the adhesive. Dynamic mechanical analysis was used to probe the shear storage modulus (G') and loss modulus (G") as a function of temperature and / or frequency and to determine the glass transition temperature (T) of the material. g ). An 8-mm diameter x 1-mm thick disk of adhesive without liner was placed between the 8-mm probes of a DHR-3 parallel plate shear rheometer (TA Instruments, New Castle, DE). A temperature sweep was performed by ramping from -30°C to 160°C at 3°C / min at 1 Hz and ≤5% strain. Shear storage modulus was recorded at selected temperatures of -20°C and 23°C. T of the material g It is determined as the peak value in the loss tangent versus temperature curve (ie maxtan(δ)).

[0174] Test Method 2: Creep Compliance by Dynamic Mechanical Analysis (DMA)

[0175] The creep compliance of adhesive is further evaluated using the DHR-3 rheometer with the Peltier platform equipped with 8-mm parallel plate geometry. Sample temperature is maintained at 25 ℃, and the stress of 40kPa is applied to sample for a period of 5 seconds simultaneously, and the stress applied now recovers to 0kPa.The maximum strain of each sample during the period of the stress applied is recorded, to provide the measurement (maximum strain % in table 6) of adhesive ductility.Record the recovery strain % at 10 seconds and 60 seconds after stress is reduced to 0kPa, to indicate the high strain recoverability of adhesive when stress is applied.

[0176] Test method 3: 180 degree peel adhesion test

[0177] The peel adhesion of PSA transfer tape (Adhesive Transfer Tape, ATT) was measured at an angle of 180°. For peel adhesion testing to rigid substrates such as annealed 18 gauge, 304 stainless steel (SS), polycarbonate (PC) (all available from Chem. Instruments, Fairfield, OH)) and glass (made of float glass using the air side, available from 3M Glass Laboratories), ATT was laminated directly to a 2 inch x 6 inch (5.08 cm x 15.24 cm) substrate. For peel adhesion to flexible substrates such as PET (5 mil thick, biaxially oriented, no surface treatment, from Mitsubishi Polyester Film, Greer, SC) and PI (2 mil (50 μm) thick, no surface treatment, KAPTON film from Dupont, Midland MI), the substrate was first adhered to 2 inch by 6 inch (5.08 cm by 15.24 cm) glass using double-sided adhesive transfer tape. The method followed ASTM D3330 Test Method E, Liner Side, and TM-613 (180° Peel Adhesion to Stainless Steel or Backing) Procedure F. PSAATT was laminated to the plasma treated side of a 2 mil (50 μm) biaxially oriented polyethylene terephthalate (PET) film used as a backing material (3M, processing conditions described in U.S. Pat. No. 10,134,566). Prior to testing, all samples and substrates were conditioned in a temperature and humidity (CTH) controlled room (70°F (21°C), 50% RH) for a period of not less than 24 hours. Before and after testing, the test panels were cleaned with methyl ethyl ketone (MEK) solvent. The PET strips were laminated to the panels using a rubberized 4.5-lb (2.04Kg) roller (4×3 second rolling). Peel tests were performed using an Instron Universal Testing Instrument in a CTH room equipped with an environmental chamber. The peel tests were performed at a temperature of 23°C with a grip speed of 12 inches / minute (0.3m / min). Each sample was peeled off from the same SS substrate at least three times, and the average of all three measurements was recorded.

[0178] Test Method 4: Tensile Impact Test

[0179] Tensile impact test is a destructive test to measure the tensile impact resistance of adhesive materials in dynamic events (e.g., falling). The PSA ATT between the liner is cut into a predetermined geometry (see Table 2) and laminated between two unused and clean (MEK) stainless steel coupons of a specified geometry (see Table 2). Before testing, the coupon-ATT stack is kept pressurized for a specified time (e.g., 48 hours under CTH conditions), and repeated (greater than 5 times) and tested. Instron CEAST 9340 drop tower (0.3J-450J energy delivery) is used to test the coupon-adhesive stack with a drop height of 115mm and a drop weight of 3Kg. The total energy absorbed and peak force of each adhesive tested in this configuration are recorded.

[0180] The test method for tensile impact strength of adhesive bonds is a modified version of the ISO 9653:1998 shear impact test method. Impact is tested by adhering two surfaces together and subjecting the bond to impact (but in tension mode) using the substrate geometry and assembly procedure outlined in Table 2 and Test Method 4. All substrates and instruments are commercially available.

[0181] Table 2: Tensile impact test parameters

[0182]

[0183] Test Method 5: Optical Durability Test

[0184] Transmittance / haze / clarity (THC) measurements were performed using a BYK-Chemie (Wesel, Germany) Hazegard i. The ATT was cut into approximately 5 cm wide by 10 cm long. The RF02N liner was removed and the adhesive with the second liner was laminated to a 1 mm thick optically clear glass sheet (Eagle Glass, Corning Glass, Corning, NY). The second liner was then removed and a 2 mil (50 μm) thick layer of optically clear polyethylene terephthalate (PET, Skyrol SH-81 purchased from SKC Haas, Seoul, Korea) was laminated to the assembly. The samples were placed in the Hazegard to measure the THC that passed through the PET / PSA / glass assembly. The samples were then aged for at least 500 hours in an oven chamber set to 65°C and 90% relative humidity. Haze measurements are remeasured after the samples are removed from the heat / humidity chamber and allowed to equilibrate for at least 1 hour at 50% relative humidity (RH) and 23° C. Typically, samples acceptable for optically clear applications will retain haze values ​​of less than about 2%, or more desirably less than 1%, after being subjected to these aging conditions.

[0185] Test method 6: Number average molecular weight determination

[0186] Reversed-phase HPLC can be used to determine the number average molecular weight (Mn) of macromonomers. This technique provides superior oligomer resolution to conventional GPC. Conventional polymer distribution calculations can be applied to determine number average molecular weight, weight average molecular weight, and polydispersity.

[0187] Separation can be performed on an Agilent 1290 UHPLC / MS, which consists of a quaternary gradient pump, an autosampler, a heated column chamber, a diode array with a 10 mm path length unit, and a 6130 mass selective detector (MSD). Separation can be performed using a 100 mm×2 mm WatersAcquity CSH 1.7 μm C18 column equilibrated with 75 / 25 v / v (volume / volume) of water (H2O) / acetonitrile (ACN) at 0.50 mL / min and 50° C. After injecting 0.50 microliters (μL) of a macromonomer sample dissolved in a suitable solvent at an appropriate concentration, a 10.0 min linear gradient to 60 / 40 H2O / ACN, then a 2.0 min linear gradient to pure ACN isocratic hold for 1.0 min, and then re-equilibrated in the starting eluent to separate the sample components. Substances can be detected by UV absorbance (200 ± 1 nm relative to a 400 ± 50 nm signal). Electrospray ionization (ESI) mass spectrometry detection can be performed using nebulization with 11 L / min N2 at 325°C and 45 pounds per square inch (psi). Positive ion spectra are scanned from m / z 75-1350 using a 100 V fragmentation potential.

[0188] Examples E1-E14 and Comparative Examples CE5-CE11: Preparation of Adhesive Tapes

[0189] Each reaction mixture was prepared in a 16 ounce (120 mL) amber glass bottle. The monomers were combined in appropriate weight % ratios (shown in Table 3 below) to achieve the desired final copolymer composition target, wherein the total weight % was 100% by mass. V67 (0.1 phr-0.2 phr, wherein the total amount of resin was the total mass of 100 weight % monomers) and TDDM (0.1 phr-0.2 phr, wherein the total amount of resin was the total mass of 100 weight % monomers) were added. The samples were made into monomer solutions according to Tables 3 and 4. Nitrogen was bubbled through the reaction mixture for 7 minutes. The bottles were sealed and placed in a 67° C. hot water bath while gently stirring. The bottles were removed after continuous mixing and heating for 20 hours and quenched with cold water. The solution was diluted to 30% solids with the solvent used during polymerization, and 0.10-0.20 phr (relative to 100 wt% total mass of monomers) of BisA crosslinker (1,1'-isophthaloyl-bis(2-methylaziridine) crosslinker, CAS No. 7652-64-4) was mixed into the solution using a high shear mixing device (1660 rpm) less than 1 hour before coating. The uniformly mixed solution was coated onto RF22N PET release liner (SKC Haas, Seoul, Korea, 2 mil (50 μm)) using a notched bar coater set to a total gap of 175 μm between the RF22N liner and the notched bar (to achieve a nominal dry adhesive thickness of 35 μm). The coated PSA film was dried in an oven at 80°C for 15 minutes. Once removed and cooled to room temperature, the tacky adhesive transfer tape (ATT) was covered with a second PET release liner having a lower and different release force than the first release liner (RF02N, SKC Haas, Korea, 2 mil, (50 μm)) used for protection. For adhesive performance testing, the RF02N liner was removed and the exposed side of the tacky tape was rolled onto a 6 inch (15 cm) wide primed polyester film (3M, 2 mil (50 μm) biaxially oriented PET film under plasma treatment conditions as described in U.S. Pat. No. 10,134,566 (David et al.)) by hand lamination (using a 6 inch (15 cm) rubberized hand roller (Polymag Tek, Rochester, NY)), ensuring that there were no air bubbles trapped between the adhesive and the primed polyester film.

[0190] Examples E15-E21 and Comparative Examples CE1-CE4 and CE12-CE15: Preparation of Adhesive Tapes

[0191] The monomers were combined in appropriate weight % ratios (shown in Table 3 below) to achieve the desired final copolymer composition target, where the total weight % is 100 mass %. The initial monomer mixtures for Examples E18-E21 and Comparative Examples CE12-CE15 were formulated without macromonomer; macromonomer was added after the first reaction step at the phr levels shown in Tables 3 and 4. In Tables 3 and 4, E18 to E21 and CE12 to CE15 with a plus sign indicate that the macromonomer was added in parts per hundred parts of resin (phr).

[0192] To this mixture was added 0.025 phr (relative to 100 wt% total mass of monomers) of I651. The monomer mixture was degassed with nitrogen for 10 minutes and then exposed to low intensity (0.3 mW / cm 2 ) UVA irradiation while stirring until a viscosity of approximately 1000 cP-2000 cP is obtained. Additional I651 (0.2 phr, relative to 100 wt% total mass of monomers) and SR344 (0.10 phr, relative to 100 wt% total mass of monomers) are added, and the solution is mixed thoroughly. The solution is then coated on a PET release liner (RF22N and RF02N, SKC Haas, Seoul, Korea), 2 mil (Examples E15-E17 and Comparative Examples CE1-CE10, 50 μm)) (Examples E18-E23, 200 μm and Comparative Examples CE13-CE14, 180 μm) and irradiated with 1,600 mJ / cm 2 The adhesive was cured by UVA radiation to produce a tacky adhesive film. For adhesive performance testing, the RF02N liner was removed and the exposed side of the tacky tape was rolled onto a 6 inch (15 cm) wide primed polyester film (3M, 2 mil (50 μm) biaxially oriented PET film under plasma treatment conditions as described in U.S. Patent No. 10,134,566) by hand lamination (using a 6 inch (15 cm) rubberized hand roller (Polymag Tek, NY)), ensuring that there were no air bubbles trapped between the adhesive and the primed polyester film.

[0193] Table 3: Composition of Examples and Comparative Examples

[0194]

[0195]

[0196] Table 4: Solid percentage and solvent percentage in the compositions of the examples and comparative examples

[0197]

[0198]

[0199] Table 5: Test results of test method 1

[0200]

[0201]

[0202] Table 6: Test results of test method 2

[0203]

[0204]

[0205] Table 7: Test results of test method 3

[0206]

[0207]

[0208] *1 day stay

[0209] Table 8: Test results of test method 4

[0210]

[0211]

[0212] Table 9: Test results of test method 5

[0213]

[0214] *Aging time, t for these samples at 65°C / 90%RH is 135h.

[0215] All disclosures of the patents, patent documents and publications cited herein are incorporated by reference in their entirety, as if each file were cited separately. If there is any conflict or contradiction between the disclosures in this specification as written and any document incorporated by reference herein, the specification as written shall prevail. Various modifications and changes made to the disclosure will become apparent to those skilled in the art without departing from the scope and substance of the disclosure. It should be understood that the disclosure is not intended to be improperly limited by the exemplary embodiments and embodiments shown herein, and such embodiments and embodiments are presented only by way of example, and the scope of the disclosure is intended to be limited only by the claims shown below herein.

Claims

1. A (meth)acrylate copolymer, comprising monomer units derived from a polymerizable component, wherein the polymerizable component comprises: a (meth)acrylate macromonomer comprising 1) a single (meth)acryloyloxy group and 2) a poly(ethylene oxide) group, a poly(propylene oxide) group, or a poly(ethylene oxide-co-propylene oxide) group, the (meth)acrylate macromonomer having a number average molecular weight of no greater than 900 Daltons and being present in an amount of at least 5 weight percent, based on the total weight of the polymerizable components; Alkyl (meth)acrylates; and a (meth)acrylate-containing carboxylic acid, the (meth)acrylate-containing carboxylic acid being present in an amount of no greater than 15 weight percent, based on the total weight of the polymerizable components; and a crosslinking agent, the crosslinking agent being a multifunctional (meth)acrylate monomer, a multifunctional aziridine or a combination thereof, the amount of the crosslinking agent being in a range of 0.1 wt % to 5 wt % based on the total weight of the polymerizable components, and The (meth)acrylate copolymer has a glass transition temperature of not greater than -15°C.

2. The (meth)acrylate copolymer of claim 1, wherein the polymerizable component comprises up to 60 wt% of the (meth)acrylate macromonomer. 3 . The (meth)acrylate copolymer of claim 1 , wherein the (meth)acrylate copolymer has a number average molecular weight ranging from 350 Daltons to 900 Daltons. 4 . The (meth)acrylate copolymer of claim 1 , wherein the (meth)acrylate macromonomer has a poly(ethylene oxide) group. 5 . The (meth)acrylate copolymer of claim 1 , wherein the polymerizable component comprises 25 to 95 wt % of an alkyl (meth)acrylate based on the total weight of the polymerizable component.

6. The (meth)acrylate copolymer according to claim 1, wherein the (meth)acrylate-containing carboxylic acid is selected from (meth)acrylic acid, β-carboxyethyl acrylate, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxysuccinic acid, or a mixture thereof.

7. The (meth)acrylate copolymer of claim 1, wherein the polymerizable component comprises 5 to 60 wt% of the (meth)acrylate macromonomer, 25 to 95 wt% of an alkyl (meth)acrylate, 0.1 to 15 wt% of a (meth)acrylate-containing carboxylic acid, and 0.1 to 5 wt% of a crosslinking agent, based on the total weight of the polymerizable component. 8 . The (meth)acrylate copolymer according to claim 1 , further comprising a monomer unit derived from a non-acidic polar monomer. 9 . The (meth)acrylate copolymer according to claim 8 , wherein the non-acidic polar monomer is a nitrogen-containing monomer having a primary acylamino group, a secondary acylamino group, a tertiary acylamino group or an amino group.

10. The (meth)acrylate copolymer of claim 8, wherein the amount of the non-acidic polar monomer is no greater than 20 wt% based on the total weight of the polymerizable components. 11 . An adhesive composition comprising the (meth)acrylate copolymer according to any one of claims 1 to 10. 12 . The adhesive composition according to claim 11 , wherein the adhesive composition is a pressure sensitive adhesive.

13. The adhesive composition according to claim 12, wherein the adhesive composition exhibits (1) 180 degree peel adhesion of at least 0.3 N / mm on polyethylene terephthalate, at least 0.3 N / mm on glass, at least 0.3 N / mm on polycarbonate, and at least 0.5 N / mm on stainless steel at 12.6 inches / minute (32 centimeters / minute (cm / min)) at 23°C, with an adhesive thickness of 35 microns; and (2) Shear storage modulus of not more than 2000 kPa at -20°C and not more than 50 kPa at 23°C.

14. The adhesive composition according to claim 13, wherein the adhesive composition also exhibits A maximum shear strain percentage of at least 300% under an applied shear stress of 40 kPa and a strain recovery of at least 60% within 1 minute after removal of the applied shear stress of 40 kPa.

15. The adhesive composition of claim 13 or 14, wherein the haze is less than 5% based on an optical durability test.

16. An article comprising a substrate and the adhesive composition of any one of claims 11 to 15 positioned adjacent to the substrate.

17. The article of claim 16, wherein the article is a transfer tape, a single-sided tape, a double-sided tape, or a die-cut adhesive article.

18. The article of claim 16, wherein the article is an electronic device comprising the adhesive composition.

19. The article of claim 18, wherein the electronic device is flexible and / or foldable.