A wear-resistant coating with strong bonding
By combining the microstructure and occlusive design of metal and ceramic materials in the waste incinerator coating, the problem of insufficient binding force of the existing coating is solved, and stronger high temperature and wear resistance is achieved, and suitable for waste incinerators. high temperature protection.
Patent Information
- Application Number
- CN202011142222.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-10-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-10-23
AI Technical Summary
The existing metal and ceramic coatings have poor bonding power in high-temperature corrosion environments, resulting in a short service life in waste incinerators, and the toughness of the ceramic coatings is poor and it is difficult to withstand impact loads.
Using metal materials as the basecoat and ceramic materials as the surface coating, microstructures such as grooves are formed on the surface of the basecoat, laser etching or chemical mask etching is used to form an occlusion structure, and combined with metal-coated thermal decomposition materials as the fabrication The pore agent produces gas during spraying, forming a stronger interface structure.
It improves the bonding power between metal and ceramic coating, enhances high temperature resistance, wear resistance and corrosion resistance, and is suitable for high temperature protection of waste incinerators, extends service life and improves protection effect.
Smart Images

Figure CN113969387B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of garbage incinerator equipment protection, and in particular relates to a wear-resistant coating with strong bonding force. Background Art
[0002] The world produces about 8 to 10 billion tons of solid waste each year, and this number is increasing year by year with industrial development and population growth. As waste has a severe impact on the environment, how to dispose of it has become an important part of current environmental protection. Waste incineration has developed rapidly due to its large processing capacity, large capacity reduction, and heat recovery.
[0003] In the recycling of heat energy resources from waste incineration, the waste contains high levels of salt and plastic. Compared with other fuels, its combustion gas products contain a large amount of corrosive gases such as hydrogen chloride and ash. When the steam temperature of the waste incineration boiler exceeds 300°C, the superheater tubes made of carbon steel will be rapidly corroded by high-temperature chlorine and chlorides. Therefore, the steam temperature usually does not exceed 300°C. When generating electricity under such low steam parameters, the maximum power generation efficiency is about 12%. If the steam temperature can be increased to 400°C, the power generation efficiency can reach 21%, which is more conducive to the promotion and application of waste incinerator power generation technology.
[0004] As a fuel, domestic waste has the characteristics of high water content, low calorific value, low components, and large composition changes. During operation, its unique combustion conditions cause corrosion to the metal heating surface of the boiler. There are mainly the following reasons: During the combustion of domestic waste in the furnace, it decomposes high-concentration nitrides, alkaline metals, pyrosulfates, some heavy metals related to corrosion, and mixtures with lower melting points. Under the conditions of high-temperature flue gas and high metal pipe wall temperature, its combined effect mainly causes high-temperature corrosion to the metal heating surface at the superheater position. Among them, the solid particles carried in the flue gas and frequent soot blowing cause erosion and corrosion wear on the inner wall of the waste incinerator, which may require shutdown for inspection and maintenance at the least, or may lead to safety accidents at the worst.
[0005] Metal coating is a wear-resistant coating that has been studied and applied earlier. Commonly used coatings include metal (Mo, Ni), carbon steel and low alloy steel, stainless steel and Ni-Cr alloy series coatings. Generally, flame spraying, arc spraying, plasma spraying, HVOF and explosion spraying processes are used. The coating has the advantages of high bonding strength with the substrate, good wear resistance, corrosion resistance and toughness. However, the service life of metal coatings is short in high temperature corrosive environments.
[0006] Ceramic coating is another widely used wear-resistant coating, including oxides, carbides, borides, nitrides and silicides, which are crystalline or amorphous compounds composed of metal elements and non-metallic elements. Ceramic coating has the characteristics of high melting point, high hardness, good wear resistance, corrosion resistance and high temperature stability. However, the spraying process of ceramic coating is complicated and the cost is high. In addition, cracks are prone to appear on the surface of the coating, and the thermal fatigue resistance is not as good as that of metal coating. In addition, the toughness of the coating is poor and cannot be used to withstand large impact loads. Currently, commonly used ceramic coatings include Al2O3, TiO2, Cr2O3, ZrO2, WC, TiC, Cr3C2, TiB2, etc., which are generally prepared by plasma spraying, flame spraying, HVOF and explosion spraying technology.
[0007] Metal and ceramic coatings each have their own unique excellent properties and obvious performance weaknesses. How to combine the respective advantages of metal and ceramic materials, realize the combination of the advantages of metal and ceramics, prepare composite materials that have both metal strength and toughness and ceramic high temperature resistance, wear resistance, corrosion resistance and other advantages, and broaden the application range of metal and ceramic materials has always been a popular research direction and has broad application prospects in industrial protection fields such as aviation, aerospace, chemical industry, machinery, and electric power.
[0008] However, due to the differences in the physical and chemical properties of metals and ceramics, such as chemical bonding methods (metallic bonds / covalent bonds), thermal expansion coefficients, thermal conductivity, etc., directly compounding the two often results in problems such as weak interface bonding and easy detachment. Summary of the invention
[0009] In order to overcome the shortcomings of the prior art, the present invention provides a wear-resistant coating with strong bonding strength, which has a metal material base coating and a ceramic material surface coating. The base coating and the surface coating form a bite by means of a special interface structure generated between the base coating and the surface coating, thereby improving the bonding strength between the metal material base coating and the ceramic material surface coating.
[0010] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a wear-resistant coating with strong bonding force, comprising a base coating formed on a substrate, and a top coating formed on the base coating; the base coating is a metal material, and the top coating is a ceramic material; wherein the surface of the base coating facing the top coating has a microstructure capable of embedding the top coating, and a bite is formed with the top coating through the microstructure.
[0011] Furthermore, the metal material is an alloy formed by at least two elements selected from Fe, Ti, Ni, Cr, and Al, such as Ni-Cr, Ni-Cr-Ti, Ni-Cr-Al, Fe-Ti, Fe-Cr, Fe-Al alloys, etc. The alloy may also contain other elements besides Fe, Ti, Ni, Cr, and Al to enhance its performance.
[0012] Furthermore, the ceramic material includes hard ceramic particles and a high temperature binder, wherein the hard ceramic particles are one or more of aluminum oxide, zirconium oxide, chromium oxide, cerium oxide, silicon carbide, silicon nitride, boron nitride, and chromium carbide, and the average particle size is 10nm-20μm; the high temperature binder includes one or more of water glass, aluminum dihydrogen phosphate, silica sol, aluminum sol, and zirconium sol. In addition, the ceramic material may also contain other fillers, solvents, and additives to improve the comprehensive performance of the formed coating.
[0013] Furthermore, the microstructure is a groove formed by laser etching or chemical mask etching, the cross-sectional shape of the groove is one or more of square, V-shaped, semicircular, and inverted trapezoidal, and the length of the groove cross-sectional opening is more than 1.5 times the average particle size of the ceramic material forming the surface coating.
[0014] Forming microscopic patterns by laser etching or chemical mask etching is a mature prior art that can accurately form the required groove distribution and shape, which will not be described here. However, laser etching or chemical mask etching is limited by the process and has high requirements for equipment or environment. Small construction spaces cannot be used for laser etching, and parts that are difficult to disassemble or large in size are not suitable for chemical mask etching. In this regard, in order to broaden the scope of application of the present invention, the inventor creatively proposes another method for forming the microstructure required by the present invention:
[0015] The pore-forming agent is mixed with the metal material, and the pore-forming agent generates gas escape when forming the base coating, thereby generating a microstructure on the surface of the base coating. This method is simple to operate and can be implemented in most protective occasions in theory.
[0016] Since the metal material forming the base coating has a high melting point, flame spraying, arc spraying, plasma spraying, HVOF and explosion spraying are generally used. Usually, the organic or inorganic pore-forming agent has been decomposed early in the spraying process and cannot play a pore-forming role after the metal coating is formed. In order to adapt to the process requirements of the present invention, further, the pore-forming agent can be selected from a metal-coated thermal decomposition material, and the thermal decomposition material is selected from carbonates, carbon materials, etc. In the thermal spraying process, the metal used for coating plays a temporary protective role for the thermal decomposition material, ensuring that the pore-forming agent will not decompose in advance and lose its effect before reaching the surface of the substrate. The metal used for coating is preferably selected from a metal close to the base coating. For example, when the base coating is a Ni-Cr alloy, the coated metal can be Ni, Cr or Ni-Cr, so that when the thermal decomposition material is released, the residual coated metal is integrated with the metal of the base coating at high temperature, which will not substantially affect the performance of the base coating. In order to avoid introducing additional impurities, carbon is an ideal thermal decomposition material. When the coated metal melts or breaks, carbon can directly generate carbon dioxide in the high-temperature oxidizing atmosphere of thermal spraying without producing any residue. There is no special restriction on the process of preparing metal-coated carbon materials. Usually, a metal shell layer can be directly deposited on the outer surface of carbon by chemical plating. Other methods also include hydrothermal reduction method.
[0017] The metal-coated carbon material can be in the form of particles, rods or other shapes. In order to form a microstructure with sufficiently large openings after carbon decomposition, the average particle size of the metal-coated carbon material should be set to be more than 2 times, preferably more than 5 times, or even more than 10 times the average particle size of the ceramic particles, so that the openings of the microstructure formed after the carbon material generates and releases gas can accommodate more ceramic particles to form an occlusion. The average particle size of the metal-coated carbon material is, for example, 50-200 μm.
[0018] The present invention also relates to a method for preparing a wear-resistant coating with strong bonding force, comprising the following steps:
[0019] (1) Grinding or sandblasting the substrate to form a pre-treated substrate with a rough surface;
[0020] (2) spraying a metal material containing a pore-forming agent on the surface of the pretreated substrate to form a base coating having a microstructure;
[0021] (3) Spraying ceramic material on the base coating having a microstructure to form a top coating.
[0022] Furthermore, in step (2), the pore former is metal-coated carbon, wherein the metal used for coating is selected from one or more metal elements in the metal material components forming the base coating.
[0023] Furthermore, in step (2), the feed amount or carrier gas amount of the spraying is controlled so that the metal-coated carbon material will not decompose prematurely before reaching the surface of the substrate. At present, the temperature control accuracy of various thermal spraying processes is generally not high, and it is only necessary to ensure that the metal-coated carbon will not decompose prematurely before reaching the surface of the substrate. Although the actual operating temperature of the thermal spraying process may be above 2000°C, and the melting point of the metal material is usually only more than 1000°C, the melting of the metal material can still be slowed down by increasing the feed amount or carrier gas amount, as long as the heat received by the metal material in the extremely short time of spraying is low. In this case, the initially formed base coating is not actually completely melted, so further, the initially formed base coating is subjected to flame or laser surface treatment to remelt the surface, and more importantly, the metal-coated carbon is completely formed into gas and released, thereby producing the desired microstructure. This surface treatment also has the additional advantage that, due to the secondary melting, the originally formed microstructure openings will be closed to a certain extent, which is more conducive to forming a bite structure with higher bonding strength. In addition, when the ceramic material is subsequently sprayed, the closure of the microstructure openings can also reduce the chance of solid particles rebounding to a certain extent.
[0024] Furthermore, the spraying in step (3) is cold spraying to avoid the formation of ceramic melt and destruction of the formed microstructure.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) In order to overcome the problem of low bonding strength of metal-ceramic composite coatings in the prior art, the present invention uses a special interface structure generated between the base coating and the top coating to form a bite, thereby improving the bonding strength between the metal material base coating and the ceramic material top coating.
[0027] (2) The pore-forming agent is mixed with the metal material. When the base coating is formed, the pore-forming agent produces gas escape, thereby producing a microstructure on the surface of the base coating. This method is simple to operate and can theoretically be implemented in most protective occasions.
[0028] (3) Using metal-coated carbon as a pore-forming agent can avoid premature decomposition of carbon during spraying, facilitate the formation of a microstructure, and have no impurities remaining, without affecting the performance of the original metal base coating.
[0029] (4) After the initial formation of the base coating, further flame or laser remelting can completely release the metal-encapsulated carbon into gas, thereby producing the desired microstructure. This surface treatment also has the additional advantage that due to the secondary melting, the original microstructure openings will be closed to a certain extent, which is more conducive to forming a bite structure with higher bonding strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The structure and form process diagram of the wear-resistant coating of the present invention. The meanings of the reference numerals are as follows:
[0031] 1: substrate; 2: base coating; 3: top coating; 4: metal-coated carbon; 5: microstructure. DETAILED DESCRIPTION
[0032] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with the examples, but it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention. All raw materials of the present invention are not particularly limited to their sources, and can be purchased on the market or prepared according to conventional methods well known to those skilled in the art.
[0033] See also Figure 1 a-1d, the wear-resistant coating of the present invention comprises a base coating 2 formed on a substrate 1, and a top coating 3 formed on the base coating 2; the base coating 2 is a metal material, and the top coating 3 is a ceramic material; wherein the surface of the base coating 2 facing the top coating 3 has a microstructure 5 capable of embedding the top coating 3, and the microstructure 5 forms an engagement with the top coating 3. The coating preparation process is:
[0034] (1) Grinding or sandblasting the substrate 1 to form a pre-treated substrate 1 with a rough surface, such as Figure 1 As shown in a;
[0035] (2) Spraying a metal material containing metal-coated carbon 4 on the surface of the pretreated substrate 1 to form a primer layer 2 having a microstructure 5, such as Figure 1 As shown in b;
[0036] Among them, in order to fully release the carbon in the metal-coated carbon 4, the melting of the metal material can be slowed down by increasing the feed amount or the carrier gas amount, as long as the heat received by the metal material in the extremely short time of spraying is low. In this case, the initially formed base coating 2 and the metal-coated carbon 4 are not actually completely melted, so further, the initially formed base coating 2 is subjected to flame or laser surface treatment to remelt the surface, and more importantly, to allow the metal-coated carbon to more fully form gas and release, thereby producing more desired microstructures 5. This surface treatment also has an additional advantage. Due to the secondary melting, the opening of the originally formed microstructure 5 will be closed or retracted to a certain extent after being impacted by the flame or laser cladding, which is more conducive to forming a occlusal structure with higher bonding strength, such as Figure 1 As shown in c.
[0037] (3) Spraying a ceramic material onto the base coating 2 having the microstructure 5 to form a top coating 3, such as Figure 1d. Since the melting point of the ceramic material is relatively high, much higher than the melting point of the metal material of the base coating, if thermal spraying is used, the formed microstructure 5 may be destroyed. Therefore, step (3) is preferably formed by cold spraying. At this time, in order to allow the ceramic material to fully occupy the microstructure, it is necessary to control the average particle size of the ceramic material and the average opening diameter of the microstructure 5, so that the average opening diameter of the microstructure 5 is more than 1.5 times the average particle size of the ceramic material, preferably more than 2 times.
[0038] Example 1
[0039] Ordinary carbon steel was used as the substrate. The metal material Ni-Cr-Al and Ni-coated carbon powder were sprayed onto the substrate by HVOF to form a base coating. The Ni-coated carbon powder accounted for 3% of the mass of the Ni-Cr-Al powder. The average particle size of the Ni-Cr-Al powder was 90nm, and the average particle size of the Ni-coated carbon powder was 80μm. The ceramic material was sprayed onto the base coating by cold spraying to form a top coating. The ceramic material included 45wt% of high-temperature binder aluminum dihydrogen phosphate, 40wt% of hard ceramic particle alumina and 15wt% of water. The average particle size of the hard ceramic particle alumina was 80 nm. After the top coating was cured at room temperature, flame treatment was applied to the surface for further sintering and curing. The final thickness of the base coating was 200μm, and the thickness of the top coating was 180μm.
[0040] Example 2
[0041] Referring to Example 1, before the ceramic material is sprayed onto the base coating layer by cold spraying to form the top coating layer, the base coating layer is subjected to a surface flame treatment and secondary remelting, and the rest is the same as Example 1.
[0042] Example 3
[0043] Ordinary carbon steel is used as the substrate. The metal material Ni-Cr and Ni-coated carbon powder are sprayed onto the substrate by HVOF to form a base coating. The Ni-coated carbon powder accounts for 5% of the mass of the Ni-Cr powder. The average particle size of the Ni-Cr powder is 75nm, and the average particle size of the Ni-coated carbon powder is 50μm. The ceramic material is sprayed onto the base coating by cold spraying to form a top coating. The ceramic material includes 50wt% of high-temperature binder silica sol, 40wt% of hard ceramic particle zirconium oxide and 10wt% of water. The average particle size of the hard ceramic particle zirconium oxide is 55nm. After the top coating is cured at room temperature, flame treatment is applied to the surface for further sintering and curing. The final base coating thickness is 200μm and the top coating thickness is 180μm.
[0044] Comparative Example 1
[0045] Referring to Example 1, ordinary carbon steel is used as a substrate, and a metal material Ni-Cr-Al is sprayed onto the substrate by HVOF to form a primer, and the average particle size of the Ni-Cr-Al powder is 90 nm. A ceramic material is sprayed onto the primer by cold spraying to form a topcoat, and the ceramic material includes 45 wt% of a high-temperature binder aluminum dihydrogen phosphate, 40 wt% of hard ceramic particle alumina, and 15 wt% of water, and the average particle size of the hard ceramic particle alumina is 80 nm. After the topcoat is cured at room temperature, flame treatment is applied to the surface for further sintering and curing. The final thickness of the primer is 200 μm, and the thickness of the topcoat is 180 μm.
[0046] The experimental results are shown in Table 1:
[0047] Table 1
[0048]
[0049] From the experimental results in Table 1, it can be seen that the wear-resistant coating of the present invention has good properties such as high temperature resistance, wear resistance and thermal shock resistance, and the ceramic layer is well combined with the metal layer, and can be suitable for use in parts of a waste incinerator that require high temperature protection.
[0050] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A wear-resistant coating with strong bonding strength, comprising a base coating formed on a substrate, and a top coating formed on the base coating; the base coating is a metal material, and the top coating is a ceramic material; characterized in that: The surface of the primer layer facing the top coating layer has a microstructure capable of being embedded with the top coating layer, and an interlocking is formed between the microstructure and the top coating layer; the microstructure formation process is as follows: a pore-forming agent is mixed with a metal material, and the pore-forming agent generates gas escape when the primer layer is formed, thereby generating a microstructure on the surface of the primer layer; the pore-forming agent is a metal-coated thermal decomposition material, and the thermal decomposition material is selected from a carbon material; the initially formed primer layer is subjected to flame or laser surface treatment again to remelt the surface, and due to the secondary melting, the opening of the originally formed microstructure is closed to a certain extent, forming an interlocking structure with higher bonding strength.
2. A wear-resistant coating with strong bonding force according to claim 1, characterized in that: The metal material is an alloy formed by at least two elements selected from Fe, Ti, Ni, Cr and Al.
3. The wear-resistant coating with strong bonding force according to claim 1, characterized in that: The ceramic material includes hard ceramic particles and a high-temperature binder, wherein the hard ceramic particles are one or more of aluminum oxide, zirconium oxide, chromium oxide, cerium oxide, silicon carbide, silicon nitride, boron nitride, and chromium carbide, and the average particle size is 10nm-20μm; the high-temperature binder includes one or more of water glass, aluminum dihydrogen phosphate, silica sol, aluminum sol, and zirconium sol.
4. A method for preparing a coating, which is used to prepare a wear-resistant coating with strong bonding force as claimed in claim 1, characterized in that The following steps are involved: (1) grinding or sandblasting the substrate to form a pre-treated substrate with a rough surface; (2) spraying a metal material containing a pore-forming agent on the surface of the pretreated substrate to form a primer layer having a microstructure; (3) Spraying ceramic material on the surface of the base coating with microstructure to form a top coating.
5. The preparation method according to claim 4, characterized in that: The average particle size of the metal-coated carbon material is more than twice the average particle size of the ceramic particles.
6. The preparation method according to claim 4, characterized in that: The metal used for coating is selected from one or more metal elements in the metal material components forming the base coating.
Citation Information
Patent Citations
Coating structure with micropore transition layer and preparation method thereof
CN101748404A
Preparation process for ceramic oxidation film resistant to fused salt corrosion
CN105420659A
Ceramic alloy coating and coating layer
CN108793929A
High-bonding-strength high-temperature-oxidation-resistant porous MCrAlY abradable coating and preparation method of high-bonding-strength high-temperature-oxidation-resistant porous MCrAlY abradable coating
CN110527940A
Method for preparing composite coating of waste incineration power generating boiler tube by inductive remelting and injecting integration
CN110541137A