Positive electrode active material for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and method for producing positive electrode active material for non-aqueous electrolyte secondary battery
By adjusting the ratio of Ni and Nb in the lithium transition metal compound and performing the firing process under specific conditions, the problem of high reaction resistance in non-aqueous electrolyte secondary batteries is solved and the performance and economy of the battery are improved.
Patent Information
- Application Number
- CN202080044979.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-06-16
AI Technical Summary
In existing non-aqueous electrolyte secondary batteries, the proportion of Ni in the lithium transition metal compound is too high, which increases the reaction resistance, and the content of Co is too low, which increases the manufacturing cost and fails to effectively reduce the reaction resistance of the battery.
By adjusting the proportion of Ni and Nb in the lithium transition metal compound, the proportion of Ni in moles of the total metal elements is more than 80%, and the proportion of Co is less than 10%, and the firing process is performed in an oxygen atmosphere to control the heating rate and temperature range. , to reduce the reaction resistance of the battery.
It effectively reduces the reaction resistance of the battery, improves the cycle characteristics and thermal stability of the battery, and controls the manufacturing cost at the same time.
Smart Images

Figure BDA0003420306790000151 
Figure BDA0003420306790000171 
Figure BDA0003420306790000172
Abstract
Description
Technical Field
[0001] The present disclosure relates to a positive electrode active material for a non-aqueous electrolyte secondary battery, a non-aqueous electrolyte secondary battery, and a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery. Background Art
[0002] In recent years, as a high-output, high-energy-density secondary battery, a nonaqueous electrolyte secondary battery having a positive electrode, a negative electrode and a nonaqueous electrolyte, and in which lithium ions are moved between the positive electrode and the negative electrode for charge and discharge, has been widely used. From the viewpoints of low resistance, high capacity, high reliability, etc. of the battery, it is required that the characteristics of the positive electrode active material contained in the positive electrode of the battery be improved.
[0003] For example, Patent Document 1 discloses a positive electrode active material for a non-aqueous electrolyte secondary battery, which is a lithium nickel manganese composite oxide containing 2 mol % to 8 mol % of Nb, and a lithium niobium compound is present on the surface of the primary particles, and a portion of the Nb is solid dissolved in the primary particles, thereby having a high capacity and improved cycle characteristics and thermal stability.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2018 / 123951 Summary of the invention
[0007] However, for the lithium transition metal compound contained in the positive electrode active material, it is possible to consider increasing the content of Ni in order to obtain a high battery capacity, and reducing the content of Co in order to reduce the manufacturing cost. However, in a lithium transition metal compound in which the ratio of Ni is 80 mol% or more and the ratio of Co is 10 mol% or less relative to the total molar number of metal elements other than Li, the reaction resistance of the battery sometimes increases. The technology of Patent Document 1 does not take into account the reaction resistance of the battery, and there is still room for improvement.
[0008] Therefore, the purpose of the present disclosure is to provide a positive electrode active material, which contains a lithium transition metal compound, for which the proportion of Ni is greater than 80 mol% and the proportion of Co is less than 10 mol% relative to the total molar number of metal elements other than Li, and the reaction resistance of the battery is reduced.
[0009] A positive electrode active material for a non-aqueous electrolyte secondary battery as one embodiment of the present invention is characterized in that it contains a lithium transition metal compound, wherein the lithium transition metal compound contains Ni at a ratio of 80 mol% to 94 mol% relative to the total molar number of metal elements other than Li, and contains Nb at a ratio of 0.1 mol% to 0.6 mol% relative to the total molar number of metal elements other than Li; in terms of molar amount, n1 and n2 satisfy the condition of 50%≤n1 / (n1+n2)<75%, and n1 is a mixture of 5 mL of pure water and 5 mL of 35% hydrochloric acid. The amount of Nb is determined by inductively coupled plasma emission spectrometry analysis in the first filtrate obtained by filtering and extracting the first sample solution obtained by adding 0.2 g of a lithium transition metal compound to an aqueous hydrochloric acid solution of 100 μg / mL and dissolving the solution under violent boiling for 120 minutes; the amount of Nb is determined by inductively coupled plasma emission spectrometry analysis in the second filtrate obtained by filtering and extracting the first sample solution obtained by immersing the filter used for filtering the first sample solution in 5 mL of 46% hydrofluoric acid / 5 mL of 63% nitric acid; the amount of Nb is determined by inductively coupled plasma emission spectrometry analysis in the second filtrate obtained by filtering and extracting the second sample solution obtained by violent boiling for 180 minutes.
[0010] A nonaqueous electrolyte secondary battery as one embodiment of the present disclosure is characterized by comprising a positive electrode, a negative electrode, and a nonaqueous electrolyte, wherein the positive electrode includes the positive electrode active material.
[0011] As one embodiment of the present invention, a method for manufacturing a positive electrode active material for a non-aqueous electrolyte secondary battery is characterized in that it includes: a mixing step of mixing a composite oxide containing at least Ni, a Li compound and a Nb compound to obtain a mixture; and a calcining step of heating a calcining furnace in an oxygen atmosphere at a heating rate of 450°C to 680°C in a range of greater than 3.5°C / min and less than 5.5°C / min, and reaching a maximum temperature in a range of 700°C to 780°C, thereby calcining the mixture, and the holding time to reach the maximum temperature is 1 hour to 10 hours.
[0012] According to the positive electrode active material for a nonaqueous electrolyte secondary battery as one embodiment of the present disclosure, a nonaqueous electrolyte secondary battery with low reaction resistance can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 It is a cross-sectional view of a nonaqueous electrolyte secondary battery as an example of the embodiment. DETAILED DESCRIPTION
[0014] In the layered structure of the lithium transition metal compound, there are transition metal layers such as Ni, Li layers, and oxygen layers, and the Li ions present in the Li layer reversibly enter and exit, thereby performing the charge and discharge reaction of the battery. In the lithium transition metal compound contained in the positive electrode active material, when the ratio of Ni is 80 mol% or more and the ratio of Co is 10 mol% or less relative to the total molar number of metal elements other than Li, the formation of the NiO layer on the surface of the primary particles and secondary particles of the lithium transition metal compound and the decomposition of the electrolyte are promoted, so that the reaction resistance of the battery is sometimes increased.
[0015] The inventors conducted in-depth research and found that the reaction resistance of the battery can be reduced by suppressing the Nb content to less than 0.6 mol% and adjusting the distribution state of Nb. It is speculated that by allowing a specified amount of Nb compound to exist on the surface of the primary particles and secondary particles of the lithium ion transition metal compound, the interface resistance can be reduced and the reaction resistance of the battery can be reduced.
[0016] Hereinafter, an example of an embodiment of the non-aqueous electrolyte secondary battery of the present disclosure is described in detail. Hereinafter, a cylindrical battery in which a wound electrode body is housed in a cylindrical battery case is exemplified, but the electrode body is not limited to a wound type, and may also be a stacked type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one through a separator. In addition, the battery case is not limited to a cylindrical shape, and may be, for example, a square, a coin shape, etc., or may be a battery case composed of a laminate sheet including a metal layer and a resin layer.
[0017] Figure 1 FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 as an example of an embodiment. Figure 1 As shown, the nonaqueous electrolyte secondary battery 10 includes an electrode body 14, a nonaqueous electrolyte (not shown), and a battery case 15 that accommodates the electrode body 14 and the nonaqueous electrolyte. The electrode body 14 has a winding structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. The battery case 15 is composed of an outer can 16 having a bottomed cylindrical shape and a sealing body 17 that seals the opening of the outer can 16.
[0018] The electrode body 14 is composed of a long positive electrode 11, a long negative electrode 12, two long separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. In order to prevent the precipitation of lithium, the negative electrode 12 is formed to be one size larger than the positive electrode 11. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the length direction and the width direction (short side direction). The two separators 13 are formed to be at least one size larger than the positive electrode 11, and are arranged in a manner of sandwiching the positive electrode 11, for example.
[0019] The nonaqueous electrolyte secondary battery 10 includes insulating plates 18 and 19 disposed above and below the electrode body 14 , respectively. Figure 1 In the example shown, the positive electrode tab 20 mounted on the positive electrode 11 passes through the through hole of the insulating plate 18 and extends to the sealing body 17 side, and the negative electrode tab 21 mounted on the negative electrode 12 passes through the outside of the insulating plate 19 and extends to the bottom side of the outer can 16. The positive electrode tab 20 is connected to the lower surface of the bottom plate 23 of the sealing body 17 by welding or the like, and the cover 27 of the sealing body 17 electrically connected to the bottom plate 23 becomes the positive terminal. The negative electrode tab 21 is connected to the inner surface of the bottom of the outer can 16 by welding or the like, and the outer can 16 becomes the negative terminal.
[0020] The outer can 16 is, for example, a metal container in a cylindrical shape with a bottom. A gasket 28 is provided between the outer can 16 and the sealing body 17, and the internal space of the battery case 15 is sealed. The outer can 16 has, for example, a groove portion 22 for supporting the sealing body 17 formed by pressing the side portion from the outside. The groove portion 22 is preferably formed in an annular shape along the circumferential direction of the outer can 16, and supports the sealing body 17 with its upper surface.
[0021] The sealing body 17 has a structure in which a bottom plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26 and a cover 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective central portions, and the insulating member 25 is inserted between the peripheral portions. When the internal pressure of the battery rises due to abnormal heat, the lower valve body 24 is deformed and broken in a manner that pushes the upper valve body 26 toward the cover 27 side, and the current path between the lower valve body 24 and the upper valve body 26 is cut off. Furthermore, when the internal pressure rises, the upper valve body 26 will break, and the gas will be discharged from the opening of the cover 27.
[0022] Hereinafter, the positive electrode 11 , the negative electrode 12 , the separator 13 , and the nonaqueous electrolyte constituting the nonaqueous electrolyte secondary battery 10 , and in particular, the positive electrode active material contained in the positive electrode active material layer 31 constituting the positive electrode 11 will be described in detail.
[0023] [positive electrode]
[0024] The positive electrode 11 has a positive electrode collector 30 and a positive electrode active material layer 31 formed on both sides of the positive electrode collector 30. The positive electrode collector 30 can use a foil of a metal such as aluminum or aluminum alloy that is stable within the potential range of the positive electrode 11, a thin film of the metal configured on the surface, etc. The positive electrode active material layer 31 contains a positive electrode active material, a conductive material, and a binding material. The thickness of the positive electrode active material layer 31 is, for example, 10 μm or more and 150 μm or less on one side of the positive electrode collector 30. The positive electrode 11 can be made as follows: a positive electrode slurry containing a positive electrode active material, a conductive material, a binding material, etc. is applied to the surface of the positive electrode collector 30, and the coating is dried and then compressed to form a positive electrode active material layer 31 on both sides of the positive electrode collector 30.
[0025] As the conductive material contained in the positive electrode active material layer 31, carbon materials such as carbon black, acetylene black, Ketjen black, and graphite can be exemplified. As the binding material contained in the positive electrode active material layer 31, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, polyolefin, etc. can be exemplified. These resins can also be used in combination with carboxymethyl cellulose (CMC) or its salt, polyethylene oxide (PEO), etc.
[0026] The positive electrode active material includes a lithium transition metal compound, wherein the lithium transition metal compound comprises 80 mol% or more and 94 mol% or less of Ni relative to the total molar number of metal elements other than Li, and comprises 0.1 mol% or more and 0.6 mol% or less of Nb relative to the total molar number of metal elements other than Li. The lithium transition metal compound has a layered structure, and the layered structure comprises a transition metal layer, a Li layer, and an oxygen layer such as Ni. The layered structure of the lithium transition metal compound can include, for example, a layered structure belonging to the space group R-3m, a layered structure belonging to the space group C2 / m, and the like. Among these, from the perspectives of high capacity, stability of the crystal structure, etc., a layered structure belonging to the space group R-3m is preferred.
[0027] Lithium transition metal compounds can be represented by the general formula Li a Ni x Co y M z Nb α O2 (0.95≤a≤1.10, 0.80≤x≤0.94, 0≤y≤0.02, 0.04≤z≤0.20, 0.001≤α≤0.006, x+y+z+α=1, M contains at least one element selected from Al, W, Mg, Ti, Mn and Mo).
[0028] a, which represents the ratio of Li in the lithium transition metal compound to the total molar number of metal elements other than Li, satisfies 0.95≤a≤1.10, more preferably satisfies 0.95≤a≤1.05, and particularly preferably satisfies 0.97≤a≤1.03. When a is less than 0.95, the battery capacity may be reduced compared to the case where a satisfies the above range. When a is 1.10 or more, more Li compound needs to be added compared to the case where a satisfies the above range, which is sometimes uneconomical from the perspective of manufacturing cost.
[0029] In order to achieve a high capacity of the battery and to add other metal elements, x representing the ratio of Ni to the total number of moles of metal elements excluding Li and Nb in the lithium transition metal compound satisfies 0.80≤x≤0.94.
[0030] y, which represents the ratio of Co in the lithium transition metal compound to the total number of moles of metal elements other than Li, satisfies 0≤y≤0.02. Co is an optional component. In addition, Co is expensive, so from the perspective of reducing manufacturing costs, y≤0.02 is satisfied.
[0031] The ratio z of M (M includes at least one element selected from Al, Mn, Ti, Mo, W and Mg) in the lithium transition metal compound to the total number of moles of metal elements other than Li satisfies 0.04≤z≤0.20. M may be Al or Mn.
[0032] The ratio α representing the total molar number of Nb in the lithium transition metal compound relative to the metal elements other than Li satisfies 0.001≤α≤0.006, and more preferably satisfies 0.001≤α≤0.003. Nb is an essential component. When α<0.001, it is difficult to obtain the effect of reducing the reaction resistance of the battery. On the other hand, when Nb>0.006, the initial capacity of the battery becomes low.
[0033] In addition, the reaction resistance of the battery can be reduced by the distribution state of Nb contained in the lithium transition metal compound. Specifically, the Nb compound exists on the primary particle surface and the secondary particle surface of the lithium transition metal compound in a manner that satisfies the condition of 50%≤n1 / (n1+n2)<75% as calculated below, thereby reducing the reaction resistance of the battery.
[0034] (1) A first sample solution prepared by adding 0.2 g of a lithium transition metal compound to an aqueous hydrochloric acid solution of 5 mL of pure water / 5 mL of 35% hydrochloric acid was dissolved under bumping for 120 minutes, and then the first sample solution was filtered.
[0035] (2) The amount of Nb n1 in the first filtrate obtained by filtering and extracting the first sample solution is quantified by inductively coupled plasma emission spectrometry.
[0036] (3) The filter used for filtering the first sample solution was immersed in a second sample solution prepared by immersing the filter in 5 mL of 46% hydrofluoric acid / 5 mL of 63% nitric acid under bumping for 180 minutes to dissolve the solution, and then the second sample solution was filtered.
[0037] (4) The amount of Nb n2 in the second filtrate obtained by filtering and extracting the second sample solution is quantified by inductively coupled plasma emission spectrometry.
[0038] (5) Based on the above quantitative n1 and n2, calculate n1 / (n1+n2) in terms of molar amount.
[0039] It is believed that n1 represents the amount of Nb contained in the lattice of the lithium transition metal compound, especially the Li layer. In addition, it is believed that n2 represents the amount of Nb present on the surface of the primary particles and the secondary particles of the lithium transition metal compound. Therefore, n1 / (n1+n2) is an index representing the approximate proportion of Nb contained in the lattice of the lithium transition metal compound. It is speculated that by allowing Nb compounds to exist on the surface of the primary particles and the secondary particles of the lithium transition metal compound to a degree that satisfies the condition of 50%≤n1 / (n1+n2)<75%, the reaction resistance of the battery can be suppressed.
[0040] The content of elements constituting the lithium transition metal compound can be measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron beam microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), etc. For example, for the content of Nb, a sample solution prepared by adding 0.2 g of a lithium transition metal compound to 5 mL of 46% hydrofluoric acid / 5 mL of 63% nitric acid in fluorine nitric acid can be dissolved under boiling for 180 minutes, and then the sample solution can be filtered and the filtrate extracted can be quantitatively analyzed using inductively coupled plasma atomic emission spectrometer.
[0041] From the perspective of increasing the capacity of the battery and efficiently suppressing the reduction in charge and discharge cycle characteristics, for example, the content of the lithium transition metal compound in the positive electrode active material is preferably 90% by mass or more, and more preferably 99% by mass or more, relative to the total mass of the positive electrode active material.
[0042] In addition, the positive electrode active material of the present embodiment may include other lithium transition metal compounds in addition to the lithium transition metal compound of the present embodiment. As other lithium transition metal compounds, for example, lithium transition metal compounds having a Ni content of 0 mol % or more and less than 80 mol % may be cited.
[0043] Hereinafter, an example of a method for producing a lithium transition metal compound will be described.
[0044] The manufacturing method of the lithium transition metal compound comprises the following steps: a mixing step, mixing a composite oxide containing at least Ni, a Li compound and a Nb compound to obtain a mixture; and a calcining step, in an oxygen atmosphere, heating the calcining furnace at a heating rate of 450°C to 680°C in a range of greater than 3.5°C / min and less than 5.5°C / min, and reaching a maximum temperature in a range of 700°C to 780°C, thereby calcining the mixture, and the holding time to reach the maximum temperature is 1 hour to 10 hours.
[0045] The composite oxide containing at least Ni may be a composite oxide in which the ratio of Ni in the composite oxide is 80 mol % or more and 94 mol % or less, and preferably a composite oxide of the general formula Ni x Co y M z A composite oxide represented by O2 (0.80≤x≤0.94, 0≤y≤0.02, 0.04≤z≤0.20, x+y+z=1, M contains at least one element selected from Al, W, Mg, Ti, Mn and Mo). The method for producing the composite oxide is not particularly limited. For example, while stirring a solution of a metal salt containing Ni and other metal elements (Co, Al, Mn, etc.), an alkaline solution such as sodium hydroxide is added dropwise, and the pH is adjusted to the alkaline side (for example, 8.5 to 12.5), so that a composite hydroxide containing Ni and other metal elements is precipitated (coprecipitated), and the composite hydroxide is calcined, thereby obtaining a composite oxide containing Ni and other metal elements. The calcination temperature is not particularly limited, for example, in the range of 500°C to 600°C.
[0046] In the mixing step, the mixing ratio of the above-mentioned composite oxide, Li compound and Nb compound can be appropriately determined in such a way that each element in the finally obtained Li transition metal oxide becomes a desired ratio. The molar ratio of Li to metal elements other than Li and Nb is 0.95 mol% or more and 1.10 mol% or less, more preferably 0.95 mol% or more and 1.05 mol% or less, and particularly preferably 0.97 mol% or more and 1.03 mol% or less. In addition, the molar ratio of Nb to metal elements other than Li and Nb is 0.001 mol% or more and 0.006 mol% or less, more preferably 0.0025 mol% or more and 0.005 mol% or less. As the Li compound, for example, Li2CO3, LiOH, Li2O3, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, LiF, etc. can be cited. In addition, as Nb compounds, Nb2O5, Nb2O5·nH2O, LiNbO3, NbCl5, etc. can be cited, and Nb2O5 is particularly preferred. In the mixing step, when the composite oxide, Li compound and Nb compound are mixed, other metal raw materials can also be added as needed. Other metal raw materials are oxides of metal elements other than metal elements constituting the composite oxide and Li and Nb.
[0047] In the calcining step, the mixture obtained in the mixing step is calcined under an oxygen atmosphere to obtain the lithium transition metal compound of the present embodiment. In the calcining step, the heating rate from 450°C to 680°C is greater than 3.5°C / minute and less than 5.5°C / minute, and the maximum temperature reaches a range of 700°C to 780°C. The heating rate from greater than 680°C to the maximum temperature is, for example, 0.5 to 2°C / minute. In addition, the holding time to the maximum temperature is greater than 1 hour and less than 10 hours. The calcining step is carried out, for example, in a calcining furnace, and the maximum pressure applied to the calcining furnace during calcining is preferably: greater than 0.55kPa and less than 1.0kPa higher than the pressure outside the calcining furnace. In addition, from the perspective of easily adjusting the distribution state of Nb, the calcining step is preferably calcined in two stages, for example. The calcining temperature of the first stage is preferably in the range of 450°C to 680°C. The second stage calcination temperature is preferably in the range of, for example, 700° C. to 780° C. The Nb distribution state of the finally obtained lithium transition metal compound is adjusted by controlling the temperature increase rate, the maximum temperature reached, the maximum pressure in the calcination furnace, and the like in the calcination step.
[0048] [negative electrode]
[0049] The negative electrode 12 has a negative electrode collector 40 and a negative electrode active material layer 41 formed on both sides of the negative electrode collector 40. The negative electrode collector 40 can use a foil of a metal such as copper or a copper alloy that is stable within the potential range of the negative electrode 12, a thin film of the metal configured on the surface, etc. The negative electrode active material layer 41 contains a negative electrode active material and a binding material. The thickness of the negative electrode active material layer 41 is, for example, 10 μm or more and 150 μm or less on one side of the negative electrode collector 40. The negative electrode 12 can be made as follows: a negative electrode slurry containing a negative electrode active material, a binding material, etc. is applied to the surface of the negative electrode collector 40, and the coating is dried and then rolled to form a negative electrode active material layer 41 on both sides of the negative electrode collector 40.
[0050] The negative electrode active material contained in the negative electrode active material layer 41 is not particularly limited as long as it can reversibly absorb and release lithium ions, and generally, carbon materials such as graphite can be used. The graphite can be natural graphite such as flaky graphite, blocky graphite, and earthy graphite, blocky artificial graphite, and artificial graphite such as graphitized mesophase carbon microbeads. In addition, metals alloyed with Li such as Si and Sn, metal compounds containing Si, Sn, etc., lithium-titanium composite oxides, etc. can also be used as the negative electrode active material. In addition, those provided with a carbon coating can also be used. For example, SiO x (0.5≤x≤1.6) or in the case of a Si-containing compound represented by 2y SiO (2+y)A Si-containing compound in which Si fine particles are dispersed in a lithium silicate phase represented by (0<y<2) or the like can also be used together with graphite.
[0051] The binder contained in the negative electrode active material layer 41 is the same as that in the positive electrode 11, and can be PTFE, PVdF and other fluorine-containing resins, PAN, polyimide, acrylic resin, polyolefin, etc., preferably styrene-butadiene rubber (SBR). In addition, the negative electrode active material layer 41 may also contain CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc.
[0052] [Separator]
[0053] The separator 13 may be, for example, a porous sheet having ion permeability and insulation. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, and the like. Suitable materials for the separator include polyolefins such as polyethylene and polypropylene, and cellulose. The separator 13 may be a single-layer structure or a laminated structure. In addition, a resin layer having high heat resistance such as aramid resin or a filler layer containing a filler of an inorganic compound may be provided on the surface of the separator 13.
[0054] [Non-aqueous electrolyte]
[0055] The non-aqueous electrolyte, for example, comprises a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent may use, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more thereof. The non-aqueous solvent may contain a halogen substituted body in which at least a portion of the hydrogen of these solvents is substituted by a halogen atom such as fluorine. As the halogen substituted body, fluorinated cyclic carbonates such as fluorinated ethylene carbonate (FEC), fluorinated chain carbonates, fluorinated chain carboxylates such as methyl fluoropropionate (FMP), etc. may be cited.
[0056] Examples of the above-mentioned esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate, chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate, cyclic carboxylates such as γ-butyrolactone (GBL) and γ-valerolactone (GVL), and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0057] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, Chain ethers such as dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0058] The electrolyte salt is preferably a lithium salt. Examples of lithium salts include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1<x<6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, Li2B4O7, Li(B(C2O4)F2) and other borates, LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1 SO2) {l, m is an integer greater than 0} and other imide salts. Lithium salts can be used alone or in combination. Among these, LiPF6 is preferably used from the viewpoints of ion conductivity and electrochemical stability. The concentration of the lithium salt is preferably set to 0.8 to 1.8 mol per 1L of non-aqueous solvent, for example. In addition, vinylene carbonate and propane sultone additives can also be added.
[0059] Example
[0060] Hereinafter, the present disclosure will be further described using examples and comparative examples, but the present disclosure is not limited to the following examples.
[0061] [Preparation of positive electrode active material]
[0062] <Example 1-1>
[0063] The [Ni 0.90 Co 0.01 Al 0.05 Mn 0.04 The composite hydroxide represented by ](OH)2 was calcined for 2 hours to obtain a composite oxide (Ni 0.90 Co 0.01 Al 0.05 Mn 0.04 O2). LiOH, the above-mentioned composite oxide and Nb2O5 are mixed in such a way that the molar ratio of Li to the total amount of Ni, Co, Al, Mn and Nb is 1.01:1 to obtain a mixture. The molar ratio of Nb to the total mole of metals other than Li is set to 0.0025. In an oxygen gas flow, the mixture is heated to 680°C at a heating rate of 3.8°C / min in a temperature range of above 450°C and below 680°C, and then the heating rate is set to 1°C / min. After calcining at a maximum temperature of 720°C for 5 hours, impurities are removed by water washing to obtain a lithium transition metal compound. The composition of the lithium transition metal compound obtained above was determined using an inductively coupled plasma emission spectrometer (manufactured by Seiko Instruments Inc., trade name "SPS3100"), and the result was a composition of LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.0025 O2 was used as the positive electrode active material of Example 1-1.
[0064] <Example 1-2>
[0065] A lithium transition metal compound was obtained in the same manner as in Example 1-1 except that the heating rate in the temperature range of 450° C. to 680° C. was changed to 5.5° C. / min. This was used as the positive electrode active material of Example 1-2.
[0066] <Examples 1-3>
[0067] Nb2O5 was mixed in such a way that the molar ratio of Nb to the total molar ratio of metals other than Li was 0.00125 to obtain a mixture, and a lithium transition metal compound was obtained in the same manner as in Example 1-1. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.00125 O2 was used as the positive electrode active material of Example 1-3.
[0068] <Comparative Example 1-1>
[0069] A lithium transition metal compound was obtained in the same manner as in Example 1-1 except that the heating rate in the temperature range of 450°C to 680°C was changed to 3.2°C / min. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.0025 O2 was used as the positive electrode active material of Comparative Example 1-1.
[0070] <Comparative Example 1-2>
[0071] A lithium transition metal compound was obtained in the same manner as in Example 1-1 except that the heating rate in the temperature range of 450° C. to 680° C. was changed to 1.2° C. / min. This was used as the positive electrode active material of Comparative Example 1-2.
[0072] <Comparative Examples 1-3>
[0073] Nb2O5 was mixed in such a manner that the molar ratio of Nb to the total molar ratio of metals other than Li was 0.00125, thereby obtaining a mixture; and a lithium transition metal compound was obtained in the same manner as in Example 1-1 except that the heating rate in the temperature range of 450°C to 680°C was changed to 1.2°C / min. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.00125 O2 was used as the positive electrode active material of Comparative Example 1-3.
[0074] <Comparative Examples 1-4>
[0075] A lithium transition metal compound was obtained in the same manner as in Example 1-1 except that Nb2O5 was not mixed to obtain a mixture. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 O2 was used as the positive electrode active material of Comparative Example 1-4.
[0076] <Comparative Examples 1-5>
[0077] Nb2O5 was mixed in such a way that the molar ratio of Nb to the total molar ratio of metals other than Li was 0.00025 to obtain a mixture, and a lithium transition metal compound was obtained in the same manner as in Example 1-1. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn0.04 Nb 0.00025 O2 was used as the positive electrode active material of Comparative Example 1-5.
[0078] <Comparative Examples 1-6>
[0079] Nb2O5 was mixed in such a way that the molar ratio of Nb to the total molar ratio of metals other than Li was 0.0100 to obtain a mixture, and a lithium transition metal compound was obtained in the same manner as in Example 1-1. The composition of the obtained lithium transition metal compound was LiNi 0.90 Co 0.01 Al 0.05 Mn 0.04 Nb 0.0098 O2 was used as the positive electrode active material of Comparative Example 1-6.
[0080] <Comparative Examples 1-7>
[0081] A lithium transition metal compound was obtained in the same manner as in Example 1-1 except that the heating rate in the temperature range of 450° C. to 680° C. was changed to 6.0° C. / min.
[0082] <Example 2>
[0083] The [Ni 0.85 Al 0.05 Mn 0.10 The composite hydroxide represented by ](OH)2 was calcined for 2 hours to obtain a composite oxide (Ni 0.85 Al 0.05 Mn 0.10 O2). LiOH, the above-mentioned composite oxide and Nb2O5 are mixed in such a way that the molar ratio of Li to Ni, Al, Mn and Nb becomes 1.01:1 to obtain a mixture. The molar ratio of Nb to the total mole of metals other than Li is set to 0.0025. In an oxygen gas flow, the mixture is heated to 680°C at a heating rate of 3.8°C / min in a temperature range of above 450°C and below 680°C, and then the heating rate is set to 1°C / min. After calcining at a maximum temperature of 750°C for 5 hours, impurities are removed by water washing to obtain a lithium transition metal compound. The composition of the lithium transition metal compound obtained above was determined using an inductively coupled plasma emission spectrometer (manufactured by Seiko Instruments Inc., trade name "SPS3100"), and the result was a composition of LiNi 0.85 Al 0.05 Mn 0.10 Nb 0.0025 O2 was used as the positive electrode active material in Example 2.
[0084] <Comparative Example 2>
[0085] A lithium transition metal compound was obtained in the same manner as in Example 2 except that the heating rate in the temperature range of 450°C to 680°C was changed to 1.2°C / min. The composition of the obtained lithium transition metal compound was LiNi 0.85 Al 0.05 Mn 0.10 Nb 0.0025 O2 was used as the positive electrode active material of Comparative Example 2.
[0086] <Example 3>
[0087] The [Ni 0.93 Al 0.04 Mn 0.03 The composite hydroxide represented by ](OH)2 was calcined for 2 hours to obtain a composite oxide (Ni 0.93 Al 0.04 Mn 0.03 O2). LiOH, the above-mentioned composite oxide and Nb2O5 are mixed in such a way that the molar ratio of Li to the total amount of Ni, Al, Mn and Nb is 1.01:1 to obtain a mixture. The molar ratio of Nb to the total mole of metals other than Li is set to 0.0025. In an oxygen gas flow, the mixture is heated to 680°C at a heating rate of 3.8°C / min in a temperature range of above 450°C and below 680°C, and then the heating rate is set to 1°C / min. After calcining at a maximum temperature of 710°C for 5 hours, impurities are removed by water washing to obtain a lithium transition metal compound. The composition of the lithium transition metal compound obtained above was determined using an inductively coupled plasma emission spectrometer (manufactured by Seiko Instruments Inc., trade name "SPS3100"), and the result was a composition of LiNi 0.93 Al 0.04 Mn 0.03 Nb 0.0025 O2 was used as the positive electrode active material in Example 3.
[0088] <Comparative Example 3>
[0089] A lithium transition metal compound was obtained in the same manner as in Example 3 except that the heating rate in the temperature range of 450°C to 680°C was changed to 1.2°C / min. The composition of the obtained lithium transition metal compound was LiNi 0.93 Al 0.04 Mn 0.03 Nb 0.0025 O2 was used as the positive electrode active material of Comparative Example 3.
[0090] The value of the index n1 / (n1+n2) indicating the distribution state of Nb was calculated for the lithium transition metal compounds (positive electrode active materials) of Examples and Comparative Examples under the above conditions. Table 1 shows the values of n1, n2 and n1 / (n1+n2)×100(%).
[0091] [Table 1]
[0092]
[0093] Using the lithium transition metal compounds (positive electrode active materials) of Examples and Comparative Examples, test cells were prepared as follows.
[0094] [Production of positive electrode]
[0095] The positive electrode slurry was prepared by mixing 91 parts by mass of the positive electrode active material of Example 1, 7 parts by mass of acetylene black as a conductive material, and 2 parts by mass of polyvinylidene fluoride as a binder, and mixing them with N-methyl-2-pyrrolidone (NMP). Then, the slurry was applied to both sides of the positive electrode collector formed by an aluminum foil with a thickness of 15 μm, and after the coating was dried, the coating was rolled with a roller to produce a positive electrode having a positive electrode active material layer formed on both sides of the positive electrode collector. The packing density of the positive electrode active material layer is 3.55 g / cm 3 The positive electrodes of other examples and comparative examples were prepared in the same manner.
[0096] [Production of negative electrode]
[0097] As the negative electrode active material, 96 parts by mass of graphite and 4 parts by mass of SiO2 having a carbon coating were used. x (x=0.94). 100 parts by mass of the negative electrode active material, 1 part by mass of the SBR dispersion, and 1 part by mass of the sodium salt of CMC were mixed, and mixed with water to prepare a negative electrode slurry. Then, the slurry was applied to both sides of a negative electrode collector formed of copper foil, and after the coating was dried, the coating was rolled with a roller to produce a negative electrode having a negative electrode active material layer formed on both sides of the negative electrode collector.
[0098] [Preparation of non-aqueous electrolyte]
[0099] Ethylene carbonate (EC), ethyl methyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed at a volume ratio of 3:3:4, and lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0100] [Production of test battery cells]
[0101] The positive electrode and negative electrode of Example 1 were stacked in a manner facing each other with a separator interposed therebetween and wound to produce an electrode body. Then, the electrode body and the nonaqueous electrolyte were inserted into an aluminum outer casing to produce a test battery cell. Test battery cells were also produced in the same manner in other Examples and Comparative Examples.
[0102] [Measurement of initial battery capacity]
[0103] The test cell was charged at a constant current of 120 mA at 25° C. until the cell voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current value reached 8 mA. The charge capacity at this time was defined as the battery capacity.
[0104] [Measurement of reaction resistance]
[0105] After the above-mentioned battery capacity measurement, the above-mentioned test battery cell was again charged at a constant current of 120 mA at a temperature of 25° C. until the battery cell voltage reached 4.2 V, and then charged at a constant voltage of 4.2 V until the current value reached 8 mA. Then, the AC impedance of the test battery cell was measured at 20 kHz to 0.01 Hz using an AC impedance meter, and a Cole-Cole plot was drawn based on the measured data, and the reaction resistance was calculated based on the size of the arc between 10 Hz and 0.1 Hz.
[0106] The battery capacity and reaction resistance of the examples and comparative examples are shown in Tables 2 to 4. Table 2 shows the measured values of the battery capacity and reaction resistance of the test battery cells of Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-7.
[0107] Table 3 shows the measured values of the battery capacity of the test cells of Example 2 and Comparative Example 2. The reaction resistance of the test cell of Example 2 is data shown relative to the reaction resistance of the test cell of Comparative Example 2 being 100.
[0108] Table 4 shows the measured values of the battery capacity of the test cells of Example 3 and Comparative Example 3. The reaction resistance of the test cell of Example 3 is shown relative to the reaction resistance of the test cell of Comparative Example 3 being 100.
[0109] [Table 2]
[0110]
[0111] [Table 3]
[0112]
[0113] [Table 4]
[0114]
[0115] In Table 2, the reaction resistances of Examples 1-1 to 1-3 satisfying the condition of 50% ≤ n1 / (n1+n2) < 75% are all lower than those of Comparative Examples 1-1 to 1-6. In addition, the Nb content of Comparative Example 1-6 is too high, and the heating rate of Comparative Example 1-7 is too fast, and it is estimated that the battery capacity is reduced.
[0116] In Tables 3 and 4, regardless of the Ni content, the reaction resistances of Examples 2 and 3 satisfying the condition of 50%≤n1 / (n1+n2)<75% are lower than those of Comparative Examples 2 and 3, respectively.
[0117] Description of Reference Numerals
[0118] 10 Non-aqueous electrolyte secondary battery
[0119] 11 Positive electrode
[0120] 12 Negative electrode
[0121] 13 Divider
[0122] 14 Electrode body
[0123] 15 Battery housing
[0124] 16 Outer can
[0125] 17 Sealing body
[0126] 18, 19 Insulation board
[0127] 20 positive electrode tab
[0128] 21. Negative electrode tab
[0129] 22 Groove
[0130] 23 Base Plate
[0131] 24 Lower valve body
[0132] 25 Insulation components
[0133] 26 Upper valve body
[0134] 27 Cover
[0135] 28 Gasket
[0136] 30 Positive electrode collector
[0137] 31. Positive electrode active material layer
[0138] 40 Negative electrode collector
[0139] 41 Negative electrode active material layer
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium transition metal compound, The lithium transition metal compound contains Ni in a ratio of 80 mol% to 94 mol% relative to the total molar number of metal elements other than Li, and contains Nb in a ratio of 0.1 mol% to 0.6 mol% relative to the total molar number of metal elements other than Li, In terms of molar conversion, n1 and n2 satisfy the condition of 50%≤n1 / (n1+n2)<75%, The n1 is the amount of Nb determined by inductively coupled plasma emission spectrometry in a first filtrate obtained by filtering and extracting a first sample solution prepared by adding 0.2 g of the lithium transition metal compound to a hydrochloric acid aqueous solution of 5 mL pure water / 5 mL 35% hydrochloric acid, dissolving the solution under boiling for 120 minutes, and then analyzing the first filtrate by inductively coupled plasma emission spectrometry. The n2 is the amount of Nb determined by inductively coupled plasma emission spectrometry in a second filtrate obtained by filtering and extracting a filter used for filtering the first sample solution and then dissolving the second sample solution for 180 minutes in a second sample solution prepared by immersing the filter in 5 mL of 46% hydrofluoric acid / 5 mL of 63% nitric acid under boiling. The lithium transition metal compound is of the general formula Li a Ni x Co y M z Nb α O2 represents, 0.95≤a≤1.10, 0.80≤x≤0.94, 0≤y≤0.02, 0.04≤z≤0.20, 0.001≤α≤0.006, x+y+z+α=1, and M contains at least one element selected from Al, W, Mg, Ti, Mn and Mo. 2 . A non-aqueous electrolyte secondary battery comprising: a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode comprises the positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 .
3. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, comprising: a mixing step of mixing a composite oxide containing at least Ni, a Li compound, and a Nb compound to obtain a mixture; and The calcining step comprises: calcining the mixture in an oxygen atmosphere at a temperature range of 450° C. to 680° C. at a temperature increasing rate of 3.5° C. / min to 5.5° C. / min to a maximum temperature of 700° C. to 780° C., The holding time to reach the maximum temperature is 1 hour or more and 10 hours or less.
4. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 3, wherein: In the calcining step, the maximum pressure applied to the inside of the calcining furnace is within a range of 0.55 kPa or more and 1.0 kPa or less than the pressure outside the calcining furnace.
Citation Information
Patent Citations
Positive electrode active material for non-aqueous electrolyte secondary cell and method for manufacturing same, and non-aqueous electrolyte secondary cell
WO2018123951A1
Positive electrode active material for nonaqueous electrolyte secondary batteries, method for producing same, and nonaqueous electrolyte secondary battery