Aluminum alloy grain remover and preparation method and application thereof

By using a specific composition aluminum alloy texture remover and appropriate immersion time and temperature treatment, the problem of removing aluminum alloy surface texture is solved, the production efficiency and product quality are improved, and the defect rate is reduced. It is suitable for various aluminum alloys Products.

CN114016032BActive Publication Date: 2024-11-19GUANGZHOU BOER CHEM MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111305161.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-04
Publication Date
2024-11-19
Estimated Expiration
2041-11-04

AI Technical Summary

Technical Problem

During the extrusion and forming of aluminum alloys, surface textures are easily formed due to improper process control or impurities. The existing mechanical grinding methods are large in losses and have high defect rate, especially for special shapes and curved surfaces.

Method used

Provide an aluminum alloy texture removal agent, consisting of phosphoric acid, sulfuric acid, copper sulfate, iron sulfate, nickel sulfate, aluminum sulfate, water and glycerin, and forms a suitable solution through different A and B agent ratios and heating temperature control. , used for soaking and sandblasting to remove texture.

Benefits of technology

This method has a short process time for removing textures, which improves production efficiency and reduces the defect rate. It is suitable for flat and non-planar products, especially special-shaped and curved aluminum parts, and has good safety performance, will not cause excessive corrosion and reduces defects Rate below 5%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The present invention belongs to the technical field of aluminum alloys, and specifically relates to an aluminum alloy grain remover, a preparation method thereof, and an application thereof. The aluminum alloy grain remover of the present invention is composed of the following raw materials in percentage by mass: 40%-70% phosphoric acid, 16%-33% sulfuric acid, 3%-11% copper sulfate, 0.1%-2% iron sulfate, 0.1%-2% nickel sulfate, 0.5%-6% aluminum sulfate, 5%-10% water, 0.1%-1% nitric acid, and 1%-4% glycerol. The aluminum alloy grain remover of the present invention can reduce the mechanical grinding intensity and reduce the grinding cost. Moreover, the grain removal treatment time is short, and a large number of products can be processed simultaneously per unit time, which can improve production efficiency. The present invention is suitable for processing planar and non-planar products, especially defective grains of special-shaped profiles, and can greatly reduce the defective rate caused by grains. The defective rate of aluminum products processed by the present invention is less than 5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum alloys, and in particular to an aluminum alloy grain remover and a preparation method and application thereof. Background Art

[0002] In recent years, aluminum alloys have been widely used in the electronics industry, not only for the back covers of smartphones, but also for tablet computers, all-in-one desktop stands, mobile power supply casings, etc. It has a wide range of applications and huge market demand.

[0003] Due to improper process control or the influence of impurities during extrusion molding, it is easy to form voids on the surface of aluminum products, resulting in lines and other material patterns, commonly known as "extrusion lines / black lines" in the industry. Figure 1-2 As shown. Although the thickness of the grain is generally only a few microns to a few hundred microns, it seriously affects the appearance of the finished aluminum products and reduces the product yield. To address this problem, mechanical grinding is currently the main method used, that is, mechanical grinding is used to remove the grain on the surface of aluminum products. However, the method of removing grain by mechanical grinding not only causes a large loss of aluminum products, is labor-intensive, and has a high product defect rate (up to 10%-20%), but also for the surface of special-shaped and curved aluminum products, mechanical grinding is inconvenient to operate and often fails to achieve the ideal effect of removing grain. Summary of the invention

[0004] According to a first aspect of the present invention, there is provided an aluminum alloy grain remover, which is composed of the following raw materials in percentage by mass: 40%-70% phosphoric acid, 16%-33% sulfuric acid, 3%-11% copper sulfate, 0.1%-2% iron sulfate, 0.1%-2% nickel sulfate, 0.5%-6% aluminum sulfate, 5%-10% water, 0.1%-1% nitric acid, and 1%-4% glycerol.

[0005] In some embodiments, it is composed of agent A and agent B, and the mass ratio of agent A to agent B is 1:1 to 6:1; wherein,

[0006] Agent A is composed of the following raw materials: phosphoric acid, sulfuric acid, iron sulfate, nickel sulfate, aluminum sulfate, glycerol and water; the amount of phosphoric acid in Agent A is 60%-90% of the total mass of phosphoric acid, the amount of sulfuric acid is 60%-90% of the total mass of sulfuric acid, and the amount of water is 30%-70% of the total mass of water;

[0007] Agent B is composed of the following raw materials: phosphoric acid, sulfuric acid, copper sulfate, water and nitric acid; the amount of phosphoric acid in Agent B is 10%-40% of the total mass of phosphoric acid, the amount of sulfuric acid is 10%-40% of the total mass of sulfuric acid, and the amount of water is 30%-70% of the total mass of water.

[0008] In some embodiments, the mass volume concentration of phosphoric acid is 1500-1800 g / L, the mass volume concentration of sulfuric acid is 1600-2000 g / L, and the mass volume concentration of nitric acid is 1200-1500 g / L.

[0009] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned aluminum alloy grain removing agent, comprising the following steps:

[0010] Add nickel sulfate, iron sulfate, and aluminum sulfate to water accounting for 30% to 70% of the total mass of water, heat until dissolved, and then add phosphoric acid accounting for 60% to 90% of the total mass of phosphoric acid, sulfuric acid accounting for 60% to 90% of the total mass of sulfuric acid, and glycerol to the mixed solution to obtain Agent A;

[0011] Add copper sulfate to the remaining water, heat until dissolved, then add nitric acid, remaining sulfuric acid and remaining phosphoric acid to the copper sulfate solution to obtain Agent B;

[0012] Mix agent A and agent B to obtain an aluminum alloy grain remover.

[0013] In some embodiments, when preparing agent A, the heating temperature is 60-80° C.; when preparing agent B, the heating temperature is 60-80° C. By heating appropriately, the solid raw material can be quickly dissolved in water.

[0014] In some embodiments, the mass ratio of agent A to agent B is 1:1 to 6:1. The mass ratio of agent A to agent B is different, and the texture of the surface of the obtained aluminum product is also different. When the mass ratio of agent A to agent B is 1:1, the surface of the obtained aluminum product has a rough and smooth sandy feel; when the mass ratio of agent A to agent B is 6:1, the surface of the obtained aluminum product has a uniform and fine sandy feel. Therefore, the mass ratio of agent A to agent B can be controlled according to the demand for the surface texture of the aluminum product.

[0015] According to a third aspect of the present invention, there is provided an application of the aluminum alloy grain removing agent in removing grain from aluminum products. Specifically, when used, the aluminum alloy grain removing agent is heated to 80-110° C., and then the cleaned aluminum alloy workpiece is placed in the aluminum alloy grain removing agent, soaked for 60-300 seconds, taken out, and subjected to a sandblasting process.

[0016] When the aluminum alloy grain removing agent is heated to different temperatures during use, the texture of the surface of the obtained aluminum product is also different. Therefore, the heating temperature of the aluminum alloy grain removing agent during use can be controlled according to the demand for the surface texture of the aluminum product.

[0017] When used, the aluminum product is immersed in the aluminum alloy grain remover for different time periods, and the surface size of the obtained aluminum product is reduced. Specifically, the longer the aluminum product is immersed in the aluminum alloy grain remover, the greater the reduction in the surface size of the aluminum product, but the reduction is within 100 microns. Therefore, the immersion time of the aluminum product in the aluminum alloy grain remover can be flexibly controlled according to actual needs.

[0018] Due to the special composition of aluminum alloy, the present invention is mainly used to remove grain from 5 series or 6 series aluminum alloy products. Specifically, the aluminum alloy products include profiles, desktop frames, tablet back covers, smart phone back covers, tablet computer bodies, mobile computer shells, and mobile power supply shells.

[0019] The 5 series aluminum alloy referred to in the present invention is an aluminum alloy with Mg as the main alloying element, and the 6 series aluminum alloy is an aluminum alloy with Mg and Si as the main alloying elements.

[0020] The aluminum alloy grain removing agent of the present invention has a short grain removing treatment time, can simultaneously treat a large number of products per unit time, and can improve production efficiency.

[0021] The aluminum alloy grain remover of the present invention will not cause excessive corrosion to the surface of the aluminum alloy and has good safety performance.

[0022] The present invention is suitable for processing flat and non-flat products, especially defective grains of special-shaped and curved aluminum parts, and can greatly reduce the defective rate caused by grains. The defective rate of aluminum products processed by the present invention is less than 5%. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1-2 It is a material grain defect formed on the surface of aluminum products.

[0024] Figure 2 yes Figure 1 The microscopic view of the grain defect shown is under a microscope.

[0025] Figure 3 It is the material texture on the surface of the aluminum alloy workpiece to be processed.

[0026] Figure 4-5 yes Figure 3 Schematic diagram of the surface treatment process of aluminum alloy workpiece shown.

[0027] Figure 6 yes Figure 3 The effect diagram of material handling after processing.

[0028] Figure 7 This is a diagram showing the effect of processing a special-shaped aluminum alloy workpiece in Example 2. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below in conjunction with the accompanying drawings. It is worth noting that the following examples are only for better explanation of the present invention and are not intended to limit the scope of protection of the present invention. The undisclosed process steps in the examples are prior art. Unless otherwise specified, the following reagents are commercially available, and the acid described in the present examples refers to an aqueous solution of an acid.

[0030] In the following examples, the mass volume concentration of phosphoric acid is 1680 g / L, the mass volume concentration of sulfuric acid is 1840 g / L, and the mass volume concentration of nitric acid is 1330 g / L.

[0031] Example 1

[0032] The aluminum alloy grain remover of this embodiment is composed of the following raw materials in percentage by mass: 800 kg of phosphoric acid, 450 kg of sulfuric acid, 120 kg of copper sulfate, 30 kg of iron sulfate, 30 kg of nickel sulfate, 85 kg of aluminum sulfate, 120 kg of water, 2 kg of nitric acid, and 30 kg of glycerol.

[0033] Agent A consists of nickel sulfate, iron sulfate, aluminum sulfate, 60 kg water, 533 kg phosphoric acid, 315 kg sulfuric acid and glycerol;

[0034] Agent B consists of: copper sulfate, remaining water, nitric acid, remaining phosphoric acid, and remaining sulfuric acid.

[0035] The preparation method thereof comprises the following steps:

[0036] Add nickel sulfate, iron sulfate and aluminum sulfate to 60 kg of water, heat until dissolved, the heating temperature is 70°C, then add 533 kg of phosphoric acid, 315 kg of sulfuric acid and glycerol to the mixed solution to obtain Agent A;

[0037] Add copper sulfate to the remaining water and heat until dissolved at 70°C, then add nitric acid, remaining phosphoric acid and remaining sulfuric acid to the copper sulfate solution to obtain Agent B;

[0038] Mix agent A and agent B in a mass ratio of 6:1 to obtain an aluminum alloy grain remover.

[0039] Example 2

[0040] The aluminum alloy grain remover of this embodiment is composed of the following raw materials in percentage by mass: 900 kg of phosphoric acid, 350 kg of sulfuric acid, 120 kg of copper sulfate, 30 kg of iron sulfate, 30 kg of nickel sulfate, 85 kg of aluminum sulfate, 120 kg of water, 2 kg of nitric acid, and 30 kg of glycerol.

[0041] Agent A consists of nickel sulfate, iron sulfate, aluminum sulfate, 60 kg water, 600 kg phosphoric acid, 252 kg sulfuric acid and glycerol;

[0042] Agent B consists of: copper sulfate, remaining water, nitric acid, remaining phosphoric acid, and remaining sulfuric acid.

[0043] The preparation method thereof comprises the following steps:

[0044] Add nickel sulfate, iron sulfate and aluminum sulfate to 60 kg of water, heat until dissolved, the heating temperature is 70°C, then add 600 kg of phosphoric acid, 252 kg of sulfuric acid and glycerol to the mixed solution to obtain agent A;

[0045] Add copper sulfate to the remaining water and heat until dissolved at 70°C, then add nitric acid, remaining phosphoric acid and remaining sulfuric acid to the copper sulfate solution to obtain Agent B;

[0046] Mix agent A and agent B in a mass ratio of 5:1 to obtain an aluminum alloy grain remover.

[0047] Example 3

[0048] The aluminum alloy grain remover of this embodiment is composed of the following raw materials in percentage by mass: 1000 kg of phosphoric acid, 350 kg of sulfuric acid, 120 kg of copper sulfate, 30 kg of iron sulfate, 30 kg of nickel sulfate, 85 kg of aluminum sulfate, 120 kg of water, 2 kg of nitric acid, and 60 kg of glycerol.

[0049] Agent A consists of nickel sulfate, iron sulfate, aluminum sulfate, 104 kg water, 870 kg phosphoric acid, 252 kg sulfuric acid and glycerol;

[0050] Agent B consists of: copper sulfate, remaining water, nitric acid, remaining phosphoric acid, and remaining sulfuric acid.

[0051] The preparation method thereof comprises the following steps:

[0052] Add nickel sulfate, iron sulfate and aluminum sulfate to 104 kg of water, heat until dissolved, the heating temperature is 70°C, then add 870 kg of phosphoric acid, 252 kg of sulfuric acid and glycerol to the mixed solution to obtain Agent A;

[0053] Add copper sulfate to the remaining water and heat until dissolved at 70°C, then add nitric acid, remaining phosphoric acid and remaining sulfuric acid to the copper sulfate solution to obtain Agent B;

[0054] Mix agent A and agent B in a mass ratio of 4:1 to obtain an aluminum alloy grain remover.

[0055] Example 4

[0056] The aluminum alloy grain remover of this embodiment is composed of the following raw materials in percentage by mass: 1100 kg of phosphoric acid, 350 kg of sulfuric acid, 120 kg of copper sulfate, 30 kg of iron sulfate, 30 kg of nickel sulfate, 85 kg of aluminum sulfate, 120 kg of water, 2 kg of nitric acid, and 60 kg of glycerol.

[0057] Agent A consists of nickel sulfate, iron sulfate, aluminum sulfate, 104 kg water, 957 kg phosphoric acid, 252 kg sulfuric acid and glycerol;

[0058] Agent B consists of: copper sulfate, remaining water, nitric acid, remaining phosphoric acid, and remaining sulfuric acid.

[0059] The preparation method thereof comprises the following steps:

[0060] Add nickel sulfate, iron sulfate and aluminum sulfate to 104 kg of water, heat until dissolved, the heating temperature is 70°C, then add 957 kg of phosphoric acid, 252 kg of sulfuric acid and glycerol to the mixed solution to obtain Agent A;

[0061] Add copper sulfate to the remaining water and heat until dissolved at 70°C, then add nitric acid, remaining phosphoric acid and remaining sulfuric acid to the copper sulfate solution to obtain Agent B;

[0062] Mix agent A and agent B in a mass ratio of 3:1 to obtain an aluminum alloy grain remover.

[0063] Example 5

[0064] The aluminum alloy grain remover of this embodiment is composed of the following raw materials in percentage by mass: 1200 kg of phosphoric acid, 350 kg of sulfuric acid, 120 kg of copper sulfate, 30 kg of iron sulfate, 30 kg of nickel sulfate, 85 kg of aluminum sulfate, 120 kg of water, 2 kg of nitric acid, and 60 kg of glycerol.

[0065] Agent A consists of nickel sulfate, iron sulfate, aluminum sulfate, 104 kg water, 1044 kg phosphoric acid, 304 kg sulfuric acid and glycerol;

[0066] Agent B consists of: copper sulfate, remaining water, nitric acid, remaining phosphoric acid, and remaining sulfuric acid.

[0067] The preparation method thereof comprises the following steps:

[0068] Add nickel sulfate, iron sulfate and aluminum sulfate to 104 kg of water, heat until dissolved, the heating temperature is 70°C, then add 1044 kg of phosphoric acid, 304 kg of sulfuric acid and glycerol to the mixed solution to obtain Agent A;

[0069] Add copper sulfate to the remaining water and heat until dissolved at 70°C, then add nitric acid, remaining phosphoric acid and remaining sulfuric acid to the copper sulfate solution to obtain Agent B;

[0070] Mix agent A and agent B in a mass ratio of 2:1 to obtain an aluminum alloy grain remover.

[0071] Example 6

[0072] The aluminum alloy grain remover of this embodiment is composed of the following raw materials in percentage by mass: 1300 kg of phosphoric acid, 350 kg of sulfuric acid, 120 kg of copper sulfate, 30 kg of iron sulfate, 30 kg of nickel sulfate, 85 kg of aluminum sulfate, 120 kg of water, 2 kg of nitric acid, and 60 kg of glycerol.

[0073] Agent A consists of nickel sulfate, iron sulfate, aluminum sulfate, 104 kg water, 1131 kg phosphoric acid, 288 kg sulfuric acid and glycerol;

[0074] Agent B consists of: copper sulfate, remaining water, nitric acid, remaining phosphoric acid, and remaining sulfuric acid.

[0075] The preparation method thereof comprises the following steps:

[0076] Add nickel sulfate, iron sulfate and aluminum sulfate to 104 kg of water, heat until dissolved, the heating temperature is 70°C, then add 1131 kg of phosphoric acid, 288 kg of sulfuric acid and glycerol to the mixed solution to obtain Agent A;

[0077] Add copper sulfate to the remaining water and heat until dissolved at 70°C, then add nitric acid, remaining phosphoric acid and remaining sulfuric acid to the copper sulfate solution to obtain Agent B;

[0078] Agent A and agent B are mixed in a mass ratio of 1:1 to obtain an aluminum alloy grain removing agent.

[0079] In order to prove the grain removal effect of the aluminum alloy grain remover of the present invention and to explore the influence of the use temperature and immersion time on the grain removal effect of the aluminum alloy grain remover of the present invention, grain removal effect tests, grain removal effect tests at different action temperatures, and grain removal effect tests at different action times were carried out respectively, as follows:

[0080] 1. Material removal effect test

[0081] Pour the aluminum alloy grain remover prepared in Example 1 into the treatment tank, maintain the temperature in the tank at about 90°C, first clean the surface of the aluminum alloy workpiece to remove dirt and scale, then clamp the aluminum alloy workpiece and immerse it in the tank, aerate the tank (aerate according to the aeration amount in the prior art), swing the workpiece at a frequency of 35 times per minute, take out the workpiece after 65 seconds, perform the sandblasting process, and observe with the naked eye whether there are grain defects such as black lines on the surface of the aluminum workpiece after washing. For the comparison of aluminum alloy workpieces before and after treatment, please refer to Figure 3 and Figure 6 For the processing process, see Figure 4-5 ,It can be seen from the figure that before treatment, the surface of the aluminum alloy workpiece has obvious ,material grain defects, and after treatment, the surface of the workpiece is smooth and ,free of material grain defects.

[0082] The same method as above was adopted to treat the special-shaped aluminum profiles used to manufacture the desktop all-in-one machine frame with the aluminum alloy grain remover prepared in Example 2. Figure 7 As shown, the effect of removing grain is also very obvious.

[0083] 2. The influence of the ratio of agent A to agent B on the surface of aluminum alloy workpiece

[0084] Based on the agent A and agent B prepared in Example 1, the mass ratio of agent A to agent B was changed (6:1, 1:1) to form two groups of grain removers, which were poured into two treatment tanks respectively and maintained at about 90°C. The same batch of 5 series aluminum profiles with grain were randomly divided into two parts, and placed in the two groups of grain removers for surface treatment. The 5 series aluminum profiles were taken out after being immersed for about 65 seconds.

[0085] The surface texture of the aluminum profiles obtained by each experimental group is slightly different, as shown in Table 1. As can be seen from Table 1, when the mass ratio of agent A to agent B is 1:1, the surface of the obtained aluminum profile has a sandy feel and presents a rough and flat feeling; when the mass ratio of agent A to agent B is 6:1, the surface of the obtained aluminum profile presents a uniform and fine sandy feeling and a bright color. Therefore, the mass ratio of agent A to agent B can be controlled according to the demand for the surface texture of aluminum products.

[0086] Table 1 Effect of the ratio of agent A to agent B on the surface of aluminum alloy workpiece

[0087] Experimental Group The mass ratio of A and B Texture 1 6∶1 The surface is evenly sandy and bright in color 2 1∶1 Surface sandy, rough and smooth

[0088] 3. Experiment on the effect of grain removal by grain removers at different action temperatures

[0089] Pour the aluminum alloy grain remover prepared in Example 1 into four treatment tanks respectively, and maintain the temperature in the tank at 80°C, 88°C, 100°C, and 110°C respectively. First, clean the surface of the aluminum alloy workpiece to remove dirt and scale, then clamp the aluminum alloy workpiece, immerse it in the tank, aerate the tank (at the aeration rate in the prior art), swing the workpiece at a frequency of 35 times per minute, take out the workpiece after 100 seconds, perform sandblasting, and observe with the naked eye whether there are grain defects such as black lines on the surface of the aluminum workpiece after washing with water.

[0090] The surface condition results of aluminum alloy workpieces treated with aluminum alloy grain remover at different use temperatures are shown in Table 2. It can be seen from Table 2 that the surface texture of aluminum products obtained by aluminum alloy grain remover at different use temperatures is different. As the use temperature increases, the surface texture of the aluminum alloy workpiece changes from sparse bright sand feeling to uniform fine sand feeling and then to three-dimensional sand feeling. Therefore, the heating temperature of the aluminum alloy grain remover during use can be controlled according to the demand for the surface texture of the aluminum product.

[0091] Table 2 Effect of grain removal by grain removers at different action temperatures

[0092] Operating temperature Texture 80℃ Sparse, bright sand feeling, weak covering power 88℃ Uniform and fine sand feeling, high gloss and good covering power 100℃ Uniform and fine sand feeling, high gloss and good covering power 110℃ Strong three-dimensional sand feeling and high gloss

[0093] 4. Test on the effect of grain removal agent on grain removal with different action time

[0094] Based on the agent A and agent B prepared in Example 1, the mass ratio of agent A to agent B was changed (6:1, 5:1, 4:1, 3:1, 2:1, 1:1) to form six groups of grain removing agents, and the same batch of 5 series aluminum profiles with grain were randomly divided into thirty parts to study the surface treatment effects of grain removing agents with different mass ratios on aluminum alloy workpieces at different immersion times (60 seconds, 120 seconds, 180 seconds, 240 seconds, 300 seconds).

[0095] Before treatment, three workpieces in each slot were randomly selected to measure the workpiece thickness (unit: micron) and mark them. After immersion, the thickness of the marked workpieces in each slot was measured again to detect the surface size reduction of the workpiece (size reduction = thickness before treatment - thickness after treatment). The average value was taken to obtain the surface size reduction of the aluminum alloy workpiece at different immersion times. The results are shown in Table 3.

[0096] It can be seen from Table 3 that the surface size of the aluminum alloy workpiece is reduced when the aluminum alloy workpiece is immersed in the aluminum alloy grain remover for different time periods. Specifically, when the mass ratio of agent A to agent B is constant, the longer the aluminum alloy workpiece is immersed in the aluminum alloy grain remover, the greater the reduction in the surface size of the aluminum product; under the same immersion time, the greater the mass ratio of agent A to agent B, the smaller the reduction in the surface size of the aluminum alloy workpiece; but the reduction in the surface size of the aluminum alloy workpiece is within 100 microns. Therefore, the immersion time of the aluminum product in the aluminum alloy grain remover can be flexibly controlled according to actual needs.

[0097] Table 3 Surface size reduction of aluminum alloy workpiece (unit: micron)

[0098]

[0099] When the temperature in the tank is maintained at 95, 100, and 110°C, respectively, the above experiment is repeated, and the obtained results are similar to the above results, wherein when the use temperature is 95°C, the surface size reduction of the aluminum alloy workpiece in the corresponding immersion time is about 1.1 times that at 88°C; when the use temperature is 100°C, the surface size reduction of the aluminum alloy workpiece in the corresponding immersion time is about 1.16 times that at 88°C; when the use temperature is 110°C, the surface size reduction of the aluminum alloy workpiece in the corresponding immersion time is about 1.24 times that at 88°C. This shows that the aluminum alloy grain remover of the present invention is heated to 80-110°C for use, which will not cause excessive corrosion to the aluminum alloy surface and has good safety performance.

[0100] The above are only some specific embodiments of the present invention. For those skilled in the art, several modifications and improvements can be made without departing from the creative concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. Aluminum alloy grain remover, characterized in that: It is composed of the following raw materials in percentage by mass: 40%-70% phosphoric acid, 16%-33% sulfuric acid, 3%-11% copper sulfate, 0.1%-2% iron sulfate, 0.1%-2% nickel sulfate, 0.5%-6% aluminum sulfate, 5%-10% water, 0.1%-1% nitric acid, and 1%-4% glycerol; The mass volume concentration of the phosphoric acid is 1500-1800 g / L, the mass volume concentration of the sulfuric acid is 1600-2000 g / L, and the mass volume concentration of the nitric acid is 1200-1500 g / L; The aluminum alloy grain remover is composed of agent A and agent B, and the mass ratio of agent A to agent B is 1:1 to 6:1; wherein, Agent A is composed of the following raw materials: phosphoric acid, sulfuric acid, iron sulfate, nickel sulfate, aluminum sulfate, glycerol and water; the amount of phosphoric acid in Agent A is 60%-90% of the total mass of phosphoric acid, the amount of sulfuric acid is 60%-90% of the total mass of sulfuric acid, and the amount of water is 30%-70% of the total mass of water; Agent B is composed of the following raw materials: phosphoric acid, sulfuric acid, copper sulfate, water and nitric acid; the amount of phosphoric acid in Agent B is 10%-40% of the total mass of phosphoric acid, the amount of sulfuric acid is 10%-40% of the total mass of sulfuric acid, and the amount of water is 30%-70% of the total mass of water.

2. The method for preparing the aluminum alloy grain removing agent according to claim 1, characterized in that: The following steps are involved: Add nickel sulfate, iron sulfate, and aluminum sulfate to water accounting for 30% to 70% of the total mass of water, heat until dissolved, and then add phosphoric acid accounting for 60% to 90% of the total mass of phosphoric acid, sulfuric acid accounting for 60% to 90% of the total mass of sulfuric acid, and glycerol to the mixed solution to obtain Agent A; Add copper sulfate to the remaining water, heat until dissolved, then add nitric acid, remaining sulfuric acid and remaining phosphoric acid to the copper sulfate solution to obtain Agent B; Mix agent A and agent B to obtain an aluminum alloy grain remover.

3. The method for preparing the aluminum alloy grain removing agent according to claim 2, characterized in that: When preparing agent A, the heating temperature is 60-80°C; when preparing agent B, the heating temperature is 60-80°C.

4. Use of the aluminum alloy grain removing agent according to claim 1 in removing grain from aluminum products.

5. The use according to claim 4, characterized in that: Heat the aluminum alloy grain remover to 80-110°C, then put the cleaned aluminum alloy workpiece into the aluminum alloy grain remover, soak for 60-300 seconds, and take it out.

6. The use according to claim 4, characterized in that: The aluminum product is one or more of a profile, a desktop frame, a tablet back cover, a smart phone back cover, a tablet computer body, a mobile computer housing, and a mobile power supply housing.