A method for quickly determining the composition window of molten iron for producing high-quality ductile iron parts
By establishing a database of solidification characteristics of iron and liquid components and high-quality iron and liquid components sorting algorithm, the problem of difficult control of iron and liquid components in ductile cast iron production is solved, the high spheroidization rate and excellent mechanical properties of ductile iron parts are achieved, and the production efficiency and qualification rate are improved. .
Patent Information
- Application Number
- CN202111303084.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-11-04
AI Technical Summary
In the existing ductile cast iron production, it is difficult to accurately control the iron composition, resulting in low spheroidization rate and spherical shape, affecting the mechanical properties and production stability of ductile iron parts, lacking methods to quickly determine the window of high-quality iron composition, affecting the pass rate and Process stability.
By considering the addition amount of inoculant and spheroidizer and its relationship with insulation temperature and time, a database of iron ingredient solidification characteristics is established, a high-quality iron ingredient selection algorithm is developed, and an appropriate ingredient window is calculated to meet spheroidization rate and spheroidal shape Requirements for degree and mechanical properties, including determining the ratio of spheroidizer/iron and inoculant, solidification characteristics parameters and production conditions.
The window for quickly determining the iron composition of high-quality pivotal iron parts is realized, which improves production efficiency and pass rate, and ensures the high spheroidization rate, spherical shape and excellent mechanical properties of pivotal iron parts.
Smart Images

Figure BDA0003337135710000031
Abstract
Description
[0001] Fields of involvement
[0002] The invention relates to the field of ductile iron casting, and in particular to a method for quickly determining a molten iron composition window for use in the production of high-quality ductile iron parts. Technical Background
[0003] Ductile iron has good toughness, its maximum tensile strength can reach 1600MPa, and its maximum elongation is as high as 24%. Compared with steel, it also has good casting performance, simple production process and equipment, and low production cost, which is only 1 / 3 to 1 / 2 of cast steel or forged steel. Therefore, ductile iron has a wide range of applications and high output. It has successfully replaced some forged steel and cast steel, becoming one of the metal structural materials with broad application prospects. The production of ductile iron often requires the process of proportioning furnace charge, spheroidization and inoculation. During this process, complex physical and chemical processes occur in the molten iron, which can easily cause the burning or loss of active elements such as magnesium or silicon in the inoculation and spheroidization, resulting in reduced quality of the molten iron. After forming, the graphite sphericity and spheroidization rate of the solidified structure of ductile iron are low, the mechanical properties of the material are poor, and the product quality is poor. Even if the active elements can be supplemented through secondary inoculation or spheroidization to improve the quality of the molten iron, the amount of spheroidizer or inoculant added is difficult to accurately control, resulting in poor consistency of the quality of the molten iron, and it is difficult to obtain ductile iron parts with process stability, which is not conducive to the improvement of ductile iron productivity and part quality. Therefore, the composition window suitable for molten iron before leaving the furnace is particularly important, which is directly related to the quality of ductile iron parts and the process stability of production. Unfortunately, there is currently no method for quickly determining the composition window suitable for molten iron for the production of high-quality ductile iron parts, which greatly affects the qualification rate and process stability of ductile iron parts, and is not conducive to large-scale production. Summary of the invention
[0004] In view of the above-mentioned status of the industry, the purpose of the present invention is to provide a method for quickly determining the composition window of molten iron for producing high-quality ductile iron parts, so as to quickly determine the composition window of molten iron suitable for actual production and process conditions, and realize the production of cast iron parts with high spheroidization rate, high sphericity organizational characteristics and excellent mechanical properties. The implementation of the technical solution of the present invention includes the following steps:
[0005] 1) Considering the addition equivalent of inoculant and spheroidizer, and the functional relationship between the burnout amount of active elements of spheroidizer and the holding temperature and time, the thermodynamic and solidification characteristics of high-throughput materials of the molten iron are calculated:
[0006] 2) Based on step 1), a database of solidification characteristics of different molten iron components is established:
[0007] 3) Based on step 2) and combined with actual production casting conditions, develop a high-quality iron liquid composition selection algorithm:
[0008] 4) Based on step 3), the composition of the molten iron of high-quality cast iron parts is calculated to form a composition window suitable for production casting process conditions.
[0009] Preferably, a method for quickly determining the molten iron composition window for producing high-quality ductile iron parts, the inoculant is a Si-containing system, the spheroidizer is a Mg-containing system, and the added amounts of the spheroidizer and the inoculant satisfy the mass relationship: spheroidizer / molten iron × 100 = 0.5-2%, inoculant / molten iron × 100 = 0.6-1.5%.
[0010] Preferably, a method for quickly determining the molten iron composition window for producing high-quality ductile iron parts is provided, wherein the solidification characteristic database comprises the following parameters: primary austenite temperature, graphite starting formation temperature, Fe-C eutectic equilibrium temperature, latent heat of crystallization, and solidification curve.
[0011] Preferably, a method for quickly determining the molten iron composition window for producing high-quality ductile iron parts is provided, wherein the production casting conditions include information on molten iron quality, insulation process, casting temperature, and cooling rate.
[0012] Preferably, a method for quickly determining the molten iron composition window for producing high-quality ductile iron parts is provided, wherein the high-quality molten iron composition selection algorithm is based on a solidification characteristic database and a solidification cooling curve constructed under production casting conditions, and the preferred criteria are:
[0013] 1) Inoculation index: αINO=SU∶SEI∶SE2∈{(16-30)∶(15-28)∶(15∶21)}, SU is the area enclosed by the horizontal line passing the highest eutectic temperature point and the solidification cooling curve, SE1 is the area enclosed by the solidification cooling curve from the starting eutectic temperature to the highest eutectic temperature, the horizontal line passing the starting eutectic temperature, and the vertical line passing the highest eutectic temperature, and SE2 is the area enclosed by the solidification cooling curve from the highest eutectic temperature to the termination eutectic temperature, the vertical line passing the highest eutectic temperature, and the horizontal line passing the termination eutectic temperature;
[0014] 2) Spheroidization rate: β = -350-50.2 (dT / dt) max +3.3Δt≥80, Δt is the fluctuation time of the second differential curve of the solidification cooling curve at the end of solidification:
[0015] 3) Magnesium effect index:
[0016] γ=22-0.02T EMIN -0.42(T EMAX -T EMIN )+0.5(SE1+SE2) / SU∈[0.15, 0.6]
[0017] Preferably, a method for quickly determining a molten iron composition window for producing high-quality ductile iron parts is provided, wherein the high-quality molten iron composition window involves the content ranges of C, Si, Mn, S, P, and Mg.
[0018] The present invention has the following beneficial effects:
[0019] The method for quickly determining the molten iron composition window for producing high-quality ductile iron parts described in the present invention can quickly determine the molten iron composition window required for producing high-quality ductile iron parts, improve production efficiency, and has a high pass rate and stable process. In the solidified structure of the ductile iron parts produced as described in this patent, the graphite spheroidization rate and sphericity are high, and the ductile iron parts have high yield and tensile strength. DETAILED DESCRIPTION
[0020] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0021] Example 1
[0022] This embodiment provides a method for quickly determining the composition window of molten iron for producing high-quality ductile iron parts, specifically:
[0023] 1) FeSi75 is selected as the inoculant and the spheroidizer with Mg content of 5wt.%, considering that the index ratio of the inoculant and the spheroidizer to the molten iron is 1wt.%, the relationship between the consumption of Mg in the spheroidizer with the holding time t(min) and the temperature T(℃) is L(Mg)%=1-0.15(TT E ) 0.4 -0.2log(t-5), the thermodynamic and solidification characteristics of high-throughput materials are calculated based on the molten iron composition in Table 1, and the Si and Mg contents introduced by the addition of inoculants and refiners are added, and the loss of Mg due to heat preservation is subtracted to obtain the range of iron composition: For the range of iron composition, the content of the elements listed in Table 1 is changed in turn by the single factor method, and the thermodynamic and solidification characteristics of high-throughput materials are calculated based on Thermo-Calc by Python, and the number of calculated components is required to be ≥10 6 .
[0024] Table 1 Initial composition of molten iron
[0025]
[0026] 2) The primary austenite temperature, graphite initial formation temperature, Fe-C eutectic equilibrium temperature, crystallization latent heat, and solidification curve calculated in step 1) are stored and compiled into a database according to the solidification process index of the component through an interface program:
[0027] 3) Based on the database in step 2), the solidification curve is corrected by the actual production molten iron quality, pouring temperature, and cooling rate parameters to form a cooling curve data set:
[0028] 4) Through the gestation index: α INO =S U :S E1 :S E2 ∈{(16~30)∶(15~28)∶115∶21)}, spheroidization rate:
[0029] β=-350-50.2·(dT / dt) max +3.3Δt≥80, magnesium action index:
[0030] γ=22-0.02T EMIN -0.42(T EMAX -T EMIN )+0.5(SE1+SE2) / SU∈[0.15, 0.6]
[0031] The cooling curve data set in step 3) is screened to obtain a composition window containing C, Si, Mn, S, P, and Mg and suitable for production casting process conditions.
[0032] In this embodiment, after the molten iron within the composition window is formed, the graphite spheroidization rate and sphericity in the solidified structure are high, and the ductile iron parts have excellent yield and tensile properties.
[0033] Comparative Example 1
[0034] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, step 1) spheroidizing agent / molten iron × 100 = 0.3%, inoculant / molten iron × 100 = 2.6%, both are not within the scope of claim 2, and other processes are the same.
[0035] In this example, no component satisfying the screening condition in step 4) of Example 1 was screened out.
[0036] Comparative Example 2
[0037] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, step 1) spheroidizing agent / molten iron × 100 = 5%, which is not within the range described in claim 2, and inoculant / molten iron × 100 = 1.2%, both of which are not within the range described in claim 2, and other processes are the same.
[0038] In this example, no component satisfying the screening condition in step 4) of Example 1 was screened out.
[0039] Comparative Example 3
[0040] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, step 1) spheroidizing agent / molten iron × 100 = 1.5%, inoculant / molten iron × 100 = 1.2%, both are not within the scope of claim 2, and other processes are the same.
[0041] In this example, no component satisfying the screening condition in step 4) of Example 1 was screened out.
[0042] Comparative Example 4
[0043] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, the Fe-C eutectic equilibrium temperature and crystallization latent heat are not taken into account in step 2.
[0044] In this embodiment, it is difficult to form the cooling curve data set in step 3) of embodiment 1.
[0045] Comparative Example 5
[0046] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, the solidification curve is not corrected in step 3.
[0047] In this example, no component satisfying the screening condition in step 4) of Example 1 was screened out.
[0048] Comparative Example 6
[0049] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, the inoculation index in step 4 is not considered.
[0050] In this embodiment, after the molten iron with some components screened out is formed, the graphite spheroidization rate and sphericity in the solidified structure are low, and the yield and tensile properties of the ductile iron parts are poor.
[0051] Comparative Example 7
[0052] This comparative example provides a method for producing high-quality ductile iron parts by using a molten iron composition window. Compared with Example 1, the α INO =S u :S E1 :S E2 ∈{(10~15)∶(15~28)∶(15∶21)}.
[0053] In this embodiment, after the molten iron with some components screened out is formed, the graphite spheroidization rate and sphericity in the solidified structure are low, and the yield and tensile properties of the ductile iron parts are poor.
[0054] Comparative Example 9
[0055] This comparative example provides a method for producing high-quality ductile iron parts by using a molten iron composition window. Compared with Example 1, the α INO =S U :S E1 :S E2 ∈{(16~30)∶(30~50)∶(15∶21)}.
[0056] In this example, no component satisfying the screening condition in step 4) of Example 1 was screened out.
[0057] Comparison Feed 9
[0058] This comparative example provides a method for producing high-quality ductile iron parts by using a molten iron composition window. Compared with Example 1, the α INO =S U :S E1 :S E2 ∈{(18~35)∶(15~28)∶(5∶10)}.
[0059] In this example, no component satisfying the screening condition in step 4) of Example 1 was screened out.
[0060] Comparative Example 10
[0061] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, the spheroidization rate β in step 4 has a value range of [30, 60].
[0062] In this embodiment, after the molten iron within the composition window is formed, the graphite spheroidization rate in the solidified structure is low and the sphericity is high, and the yield and tensile properties of the ductile iron parts are poor.
[0063] Comparative Example 11
[0064] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, the value range of the magnesium action index γ in step 4 is [0.05, 0.13].
[0065] In this embodiment, after the molten iron within the composition window is formed, the graphite spheroidization rate and sphericity in the solidified structure are low, and the yield and tensile properties of the ductile iron parts are poor.
[0066] Comparative Example 12
[0067] This comparative example provides a molten iron composition window method for producing high-quality ductile iron parts. Compared with Example 1, the value range of the magnesium action index γ in step 4 is [0.6, 0.8].
[0068] In this embodiment, after the molten iron within the composition window is formed, the sphericity in the solidified structure is low, and the yield and tensile properties of the ductile iron parts are poor.
Claims
1. A method for quickly determining the composition window of molten iron for producing high-quality ductile iron parts, characterized in that It contains the following steps: 1) Considering the addition equivalent of inoculant and spheroidizer, and the functional relationship between the burnout amount of active elements of spheroidizer and the holding temperature and time, the thermodynamic and solidification characteristics of high-throughput materials of the molten iron are calculated: 2) establishing a solidification characteristic database of different molten iron components based on step 1); 3) Based on step 2) and combined with actual production casting conditions, develop a high-quality iron liquid composition selection algorithm; 4) Based on step 3), the composition of the molten iron of the high-quality cast iron is calculated to form a composition window suitable for production casting process conditions; Step 1) the inoculant is a Si-containing system, the spheroidizer is a Mg-containing system, and the addition amounts of the spheroidizer and the inoculant satisfy the mass relationship: spheroidizer / molten iron × 100 = 0.5-2%, inoculant / molten iron × 100 = 0.6-1.5%; Step 2) the solidification characteristics database includes the following parameters: primary austenite temperature, graphite initial formation temperature, Fe-C eutectic equilibrium temperature, crystallization latent heat, and solidification curve; Step 3) the production pouring conditions include molten iron quality, insulation process, pouring temperature, and cooling rate information; Step 3) The high-quality molten iron component selection algorithm, the preferred algorithm is based on the solidification cooling curve constructed by the solidification characteristic database and the production casting conditions, and the preferred criteria are: 1) Pregnancy index: α INO =S U :S E1 :S E2 ∈{(16~30):(15~28):(15:21)}, S U is the area enclosed by the horizontal line passing through the highest eutectic temperature point and the solidification cooling curve, SE1 is the area enclosed by the solidification cooling curve from the starting eutectic temperature to the highest eutectic temperature, the horizontal line passing through the starting eutectic temperature, and the vertical line passing through the highest eutectic temperature, and SE2 is the area enclosed by the solidification cooling curve from the highest eutectic temperature to the termination eutectic temperature, the vertical line passing through the highest eutectic temperature, and the horizontal line passing through the termination eutectic temperature; 2) Spheroidization rate: β = -350-50.2 (dT / dt) max +3.3Δt≥80, Δt is the fluctuation time of the second differential curve of the solidification cooling curve at the end of solidification; 3) Magnesium effect index: γ=22-0.02T EMIN -0.42(T EMAX -T EMIN )+0.5(S E1 +S E2 ) / S U ∈[0.15,0.6]。 2. The method for quickly determining the molten iron composition window for producing high-quality ductile iron parts according to claim 1, characterized in that: Step 4) The molten iron composition window is characterized in that the window involves the content range of C, Si, Mn, S, P, and Mg.
Citation Information
Patent Citations
High-strength low stress cast nodular cast iron with high elasticity modulus and manufacturing method thereof
CN103614612A
Large-section nodular cast iron melt mass stokehole control method
CN104156569A
Method and system for dynamic regulation and control of nodulizing inoculation processing of nodular cast iron
CN105785882A
A method to control ausferritic as-cast microstructure in ductile iron parts
EP3026128A1