A HJT photovoltaic silver paste and preparation method thereof
By using silver paste blended with low melting point metal powder and conductive silver powder in HJT solar cells, the problem of difficult sintering of silver powder at low temperatures is solved, the conductivity and adhesion are improved, the overlap resistance is reduced, and a stable welding process is achieved. .
Patent Information
- Application Number
- CN202111244567.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-26
AI Technical Summary
In HJT solar cells, it is difficult to sinter silver powder to form metallized grid lines under low-temperature process conditions, resulting in a large overlap resistance between the silver paste and the TCO film, which affects the welding tension and conductivity of the battery.
A HJT photovoltaic silver paste is prepared by blending low-melting-point metal powder and conductive silver powder to form solder joints through melting characteristics, and combining polymer resin and solvent to reduce resistivity and improve adhesion and welding pullout force.
It achieves effective silver paste solidification at low temperature, improves conductivity and adhesion, reduces the overlap resistance between silver paste and Si wafer TCO film, and ensures the stability of the welding process and the welding pull-out force.
Smart Images

Figure CN114023487B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar cell pastes, and in particular relates to a HJT photovoltaic silver paste and a preparation method thereof. Background Art
[0002] High-efficiency silicon heterojunction solar cells (HJT) combine the characteristics and advantages of crystalline silicon and thin-film solar cells, and have the advantages of high efficiency, bifaciality, low attenuation and high temperature, strong weak light power generation capability, simple manufacturing process, low temperature process, thin Si wafer, etc. Its conversion efficiency has exceeded 26% so far. It has better taken into account the performance and cost factors in the existing silicon high-efficiency cell technology, so it has been widely valued by photovoltaic research and industry, and will become the mainstream technology of the third-generation cell.
[0003] Traditional crystalline silicon cell paste is sintered at high temperature. The silver powders are connected to each other by surface melting. The glass phase melts the silver powders to a certain extent and etches the silicon plate to form a reliable bond and ohmic contact with the Si wafer. However, the process temperature of HJT solar cells is below 250°C, and low-temperature curing silver paste is required, which is currently mainly imported. It is difficult for the curing silver paste to sinter the silver powder to form metallized grid lines at this temperature. The silver powders and the TCO (transparent conductive film) on the surface of the Si wafer are mainly bonded by organic resin. Therefore, the technology of HJT battery silver paste mainly revolves around how to reduce the intrinsic resistivity of the curing conductive silver paste, reduce the lap impedance between the silver paste and the TCO film, and increase the welding tension of the silver paste on the TCO. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:
[0005] A HJT photovoltaic silver paste, comprising the following components by mass percentage:
[0006] Curing agent: 1-3%;
[0007] Polymer resin: 4-6%;
[0008] Solvent: 3-6%;
[0009] Thixotropic agent: 0.2-0.5%;
[0010] Conductive silver powder: 80-85%;
[0011] Metal powder: 3-6%;
[0012] The metal powder is selected from one or a combination of two of low melting point indium powder, tin-bismuth alloy powder, bismuth-lead-tin alloy powder, lead-tin-cadmium alloy powder, bismuth-lead alloy powder, tin-bismuth-cadmium alloy powder, bismuth-cadmium alloy powder, and tin-cadmium alloy powder.
[0013] Preferably, the curing agent is selected from one or more of blocked isocyanate curing agent, phthalate, silane coupling agent, dicyandiamide, modified dicyandiamide, imidazole, modified imidazole, acid anhydride, boron trifluoride monoethylamine, and amino resin.
[0014] Preferably, the polymer resin is selected from two or more of bisphenol A epoxy resin, bisphenol F epoxy resin, ester ring epoxy resin, silicone modified epoxy resin, phenoxy resin, thermosetting acrylic resin, polyester resin, etc.; more preferably, it is a small molecule liquid epoxy resin.
[0015] Preferably, the solvent is a combination of two or more of DBE, ethylene glycol ethyl ether acetate, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, diethylene glycol ethyl ether acetate, diethylene glycol butyl ether, terpineol, and propylene carbonate.
[0016] Preferably, the thixotropic agent is selected from one of fumed silica, organic bentonite, castor oil, polyamide, and polyamide wax, and more preferably polyamide wax.
[0017] Preferably, the conductive silver powder is selected from a mixture of two or three of flaky silver powder, quasi-spherical silver powder and nano silver powder. Further preferably, the flaky silver powder has a D50 of 4-7 μm and a tap density of 5-6 g / mL, the quasi-spherical silver powder has a D50 of 0.8-1.5 μm and a tap density of 4.5-6 g / mL, and the nano silver powder has a D50 of 200-500 nm and a tap density of 2.5-4 g / mL.
[0018] In order to meet the lead-free requirements of the photovoltaic industry, it is further preferred that the metal powder is a lead-free metal powder.
[0019] Preferably, the melting point of the alloy powder is in the range of 90-200°C.
[0020] Preferably, the particle size of the metal powder is preferably above 400 mesh.
[0021] The present application also provides a method for preparing HJT photovoltaic silver paste with fusion welding characteristics, the method comprising the following steps:
[0022] Step 1: Preparation of organic carrier
[0023] Weigh a curing agent, a polymer resin, a thixotropic agent and an organic solvent according to mass percentage, and disperse them evenly to obtain an organic carrier mixture;
[0024] Step 2: Premixing of Conductive Silver Paste
[0025] Add the metal powder in the formula amount to the organic carrier mixture, add the conductive silver powder after evenly dispersing, stir to obtain the premixed HJT silver paste, and then disperse again and cool;
[0026] Step 3: Grinding and sieving
[0027] The premixed silver paste is ground and dispersed to a fineness that meets the requirements, and the impurities and uneven large particles in the paste are filtered out to obtain the finished silver paste.
[0028] Preferably, in step 1, a high-speed centrifugal disperser is used for dispersion, and the power of the disperser is 1000-1600 rpm.
[0029] More preferably, the dispersion time is 2-3 min.
[0030] Preferably, after adding the conductive silver powder in step 2, stirring is performed by gradient stirring with gradually increasing speed, the stirring rate range is 800-1600 rpm, and stirring is performed for 2 minutes at each speed.
[0031] Preferably, in step three, sieving refers to sieving through a 500-mesh sieve.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The HJT photovoltaic silver paste provided by the present invention is prepared by mixing low-melting-point metal powder that can melt at a certain temperature with silver powder. The metal powder with melting characteristics of the HJT silver paste can play a role in melting with the silver powder during the curing and baking process, and can also form solder joints between the silver particles, which not only improves the conductivity of the paste, but also reduces the intrinsic resistivity; at the same time, under the action of temperature, the molten metal or alloy liquid can penetrate into the velvet inverted pyramid structure of the Si sheet, so that the HJT silver paste has strong adhesion on the one hand, effectively reducing the overlap impedance between the silver paste and the Si sheet TCO film. In addition, the stability of the overlap impedance during the ring test can also be guaranteed. Moreover, it helps to improve the tinning property of the silver paste surface and the welding pull-out force. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the SEM image of Example 1 after baking at 200℃*30min
[0035] Figure 2 This is the SEM image of Example 2 after baking at 200℃*30min
[0036] Figure 3 This is the SEM image of Example 3 after baking at 200℃*30min
[0037] Figure 4 Schematic diagram of the test lines made by silver paste printing. DETAILED DESCRIPTION
[0038] Examples 1-3
[0039] A HJT photovoltaic silver paste is composed of the following components, as shown in Table 1, and the unit of each value is g.
[0040] Its preparation method is:
[0041] Step 1: Preparation of organic carrier
[0042] Weigh the curing agent, polymer resin, thixotropic agent and organic solvent according to mass percentage, and use a high-speed centrifugal disperser to centrifuge and disperse for 2-3 minutes at 1000-1600 rpm to obtain an organic carrier mixture;
[0043] Step 2: Premixing of Conductive Silver Paste
[0044] Add 3-6% of other metal powders to the above organic carrier mixture by mass percentage. Use a centrifugal disperser again to centrifuge and disperse at 1000-1600rpm. Add 80-85% of conductive silver powder to the above mixture by mass percentage, manually stir to slowly mix the silver powder into it to obtain the premixed HJT silver paste, and then use a high-speed centrifugal disperser again, centrifugally stir at 800rpm, 1000rpm, 1400rpm, and 1600rpm for 2 minutes respectively. After centrifugation at each speed, take out the slurry and cool it properly before continuing to the next centrifugation step to prevent the slurry from heating up during continuous centrifugation;
[0045] Step 3: Grinding and sieving
[0046] The premixed silver paste is ground and dispersed to a fineness that meets the requirements (the fourth line is less than 6um, 50% is less than 2.5um), and is passed through a 500 sieve to remove impurities and uneven large particles in the paste to obtain a finished silver paste.
[0047] Examples 2-3 use different silver powder combinations and different powder ratios, as shown in Table 1. Figure 1-3 Shown is a SEM image of the silver paste provided in Examples 1-3 after baking at 200° C.*30 min. Figure 1 , Figure 2 , Figure 3 The HJT silver paste formula uses a combination of different types of silver flakes, spherical silver or nano silver powder. Figure 1-Figure 3 They can also be clearly distinguished in the SEM image after fusion welding.
[0048] Table 1 HJT photovoltaic silver paste formula provided in Examples 1-3
[0049]
[0050] Experimental Example 1 Resistivity Test:
[0051] Resistivity is mainly calculated by the following formula
[0052] ρ=RS / L
[0053] ρ is the resistivity, L is the length of the material, S is the cross-sectional area of the material, and R is the resistance value.
[0054] Before the resistivity test, the silver paste prepared in each embodiment was printed into the following Figure 4 The test lines shown are cured at 200°C for 30 minutes. The line width is 1.5mm and the length is 100mm. A laser microscope is used to test the film thickness of the lines at multiple points on the silver paste lines to obtain the average film thickness data. Secondly, the average film thickness data is multiplied by the line width (1.5mm) to obtain the cross-sectional area of the line. The line length is a fixed value (100mm), and the R data is measured by a multimeter. By calculation and unit conversion, the resistivity of the printed lines can be obtained. After averaging multiple lines, the average resistivity of the sample can be obtained. The test results of each embodiment and comparative example are shown in Table 1.
[0055] Experimental Example 2 Welding Tensile Test
[0056] Method steps:
[0057] 1. Soak the solder strip (specifications: strip width 1.5mm, strip thickness 0.2mm) in flux for more than 1 minute to remove surface oxides. Set the soldering iron temperature to 260℃ and preheat.
[0058] 2. Silver paste is printed on the surface of TCO silicon wafer by screen printing. Figure 4 The line pattern shown (length 100mm, width 1.5mm) is baked and cured at 200℃*30min for use.
[0059] 3. Take out the soldering tape, align it with the line, and use the soldering iron to dip a small amount of 305 solder to solder the soldering tape head and the top of the wire together.
[0060] 4. After one end is fixed, straighten the other end and overlap it with the printed line, use the soldering iron to touch the surface of the solder ribbon and push it quickly along the solder ribbon. At this time, the 305 solder on the surface of the solder ribbon will also melt and wet the solder ribbon and the silver layer as the soldering iron pushes.
[0061] 5. When the soldering iron is pushed to the end of the line, bend the excess solder strip and use solder to spot weld it to form a tensile test buckle.
[0062] 6. Use a handheld tensile testing machine, reset the instrument data to zero, pull horizontally at a constant speed to test the tensile force, and read the test peak value after each pulling.
[0063] 7. Remove the maximum and minimum values from the series of data read, and take the average value of the remaining data to obtain the welding tensile test data. The test results of each embodiment and comparative example are shown in Table 1.
Claims
1. A HJT photovoltaic silver paste, comprising the following components by mass percentage: Curing agent: 1-3%; Polymer resin: 4-6%; Organic solvent: 3-6%; Thixotropic agent: 0.2-0.5%; Conductive silver powder: 80-85%; Metal powder: 3-6%; The metal powder is tin-bismuth alloy powder, indium powder or bismuth-cadmium alloy powder; The curing agent is a mixture of Asahi Kasei MF-K60X and 2-ethyl-4-methylimidazole; The polymer resin is a mixture of Hansen 240 epoxy, ester ring epoxy resin 2021P, and thermosetting acrylic resin; The organic solvent is a mixture of diethylene glycol butyl ether acetate and terpineol; The thixotropic agent is polyamide wax; The conductive silver powder is a mixture of at least two of flaky silver powder, spherical silver powder and nano silver powder.
2. The HJT photovoltaic silver paste according to claim 1, is composed of the following components by mass percentage: Curing agent: 2-3%; Polymer resin: 4.5-5.5%; Organic solvent: 4-5.5%; Thixotropic agent: 0.3-0.5%; Conductive silver powder: 82-85%; Metal powder: 3-5%.
3. According to the HJT photovoltaic silver paste according to claim 1, the D50 of the flaky silver powder is 4-7 μm; and / or the tap density is 5-6 g / mL; and / or the D50 of the spherical silver powder is 0.8-1.5 μm; and / or the tap density is 4.5-6 g / mL; and / or the D50 of the nano silver powder is 200-500 nm; and / or the tap density is 2.5-4 g / mL.
4. A method for preparing a HJT photovoltaic silver paste as claimed in any one of claims 1 to 3, comprising the following steps: Step 1: Preparation of organic carrier Weigh a curing agent, a polymer resin, a thixotropic agent and an organic solvent according to mass percentage, and disperse them evenly to obtain an organic carrier mixture; Step 2: Premixing of Conductive Silver Paste Add the metal powder in the formula amount to the organic carrier mixture, add the conductive silver powder after evenly dispersing, stir to obtain the premixed HJT silver paste, and then disperse again and cool; Step 3: Grinding and sieving The premixed silver paste is ground and dispersed to a fineness that meets the requirements, and the impurities and uneven large particles in the paste are filtered out to obtain the finished silver paste.
