Method and device for electrolyzing water, and method for determining driving potential for electrolyzing water
By using the first transition metal oxidation catalyst in the PEM electrolytic device and controlling the driving potential, the problem of unstable iridium oxide catalyst in the acidic environment is solved, and the stability and efficiency of catalyzing oxygen generation in the acidic environment are achieved for a long time.
Patent Information
- Application Number
- CN201980052832.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-09
- Filing Date
- 2019-08-09
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2039-08-09
AI Technical Summary
The iridium oxide catalyst used in existing PEM electrolytic devices is unstable in an acidic environment, resulting in catalyst deactivation, and the development of stable non-precious metal oxidants is difficult to achieve, affecting the efficiency and sustainability of electrolyzed water.
By using an oxidation catalyst containing the first transition metal in the electrolytic cell, such as oxides or hydroxides of manganese, iron, cobalt, and controlling the driving potential within a specific range (P1
The stability of the first transition metal oxidation catalyst is achieved, and the catalytic oxygen generation can be continuously catalyzed in an acidic environment for a long time (more than 8000 hours), improving the efficiency of electrolyzed water and the stability of the catalyst.
Smart Images

Figure CN114040996B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for electrolyzing water and an apparatus for electrolyzing water. In addition, the present invention relates to a method for determining a driving potential when electrolyzing water. Background Art
[0002] In order to meet the increasing energy demand, it is important to develop technologies that efficiently utilize renewable energy. Hydrogen generated by water electrolysis (2H2O→2H2+O2) is not only an ideal energy carrier for storing renewable energy, but also an important raw material in chemical industries such as ammonia synthesis.
[0003] A particularly promising mechanism for electrolyzing water is the proton exchange membrane (PEM) electrolysis device. However, PEM generates an acidic environment locally. Therefore, the reaction to generate oxygen (OER; 2H2O→O2+4H + +4e - ) Catalysts that maintain stable catalytic activity include iridium oxides, but iridium is one of the rarest elements in the earth's crust. For example, if a PEM electrolyzer is used on a megawatt scale using an iridium oxide catalyst, an amount more than 10 times the annual iridium production is required. In view of this, the development of acid-stable non-precious metal OER catalysts is an important issue in water electrolysis using a PEM electrolyzer.
[0004] In order to develop 3d transition metal OER catalysts that can be used in a wide pH range, extensive research has been conducted. However, a large number of experimental studies have shown that oxides of abundant metals (iron, cobalt, nickel, manganese) are unstable due to their solubility in acidic media (non-patent literature 1 to 6). Since it is impossible to reasonably form currently stable materials, the lack of stability of these materials has become a particularly urgent issue. On the other hand, it has been demonstrated that the activity of 3d transition metal (first transition metal) catalysts can be predicted and screened by d-band theory (non-patent literature 7).
[0005] Prior art literature
[0006] Non-patent literature
[0007] Non-patent literature 1: CC McCrory, S. Jung, IM Ferrer, SM Chatman, JC Peters, TF Jaramillo, J. Am. Chem. Soc. 2015, 137, 4347-4357
[0008] Non-patent document 2: M. Pourbaix, Atlas of electrochemical equilibria in aqueous solutions, Pergamon, New York, 1966, pp. 286-292
[0009] Non-patent document 3: IA Moreno-Hernandez, CA MacFarland, CG Read, KM Papadantonakis, BS Brunschwig, NS Lewis, Energy Environ. Sci. 2017, 10, 2103-2108
[0010] Non-patent document 4: JS Mondschein, JF Callejas, CG Read, JYC Chen, CF Holder, CK Badding, RES Chaak, Chem. Mater. 2017, 29, 950-957
[0011] Non-patent document 5: R. Frydendal, EA Paoli, I. Chorkendorff, J. Rossmeisl, IEL Stephens, Adv. Energy Mater. 2015, 5, 1500991
[0012] Non-patent document 6: M. Huynh, T. Ozel, C. Liu, E.C. Lau, D.G. Nocera, Chem. Sci. 2017, 8, 4779-4794
[0013] Non-patent document 7: JK Norskov, T. Bligaard, J. Rossmeisl, CH Christensen, Nat. Chem. 2009, 1, 37-46 Summary of the invention
[0014] Problems to be solved by the invention
[0015] The present invention has been made in view of the above-mentioned problems in the prior art, and an object of the present invention is to provide a method for electrolyzing water by stabilizing an oxidation catalyst containing a 3d transition metal (first transition metal).
[0016] Means of solving problems
[0017] The present inventors have repeatedly studied to achieve the above object and have found that there is a potential window in which the driving potential is stabilized, which allows the first transition metal oxide or the like to efficiently promote OER while suppressing the catalyst deactivation pathway of the metal oxide or the like, thereby completing the present invention.
[0018] That is, the present invention relates to a method and apparatus capable of stabilizing an oxidation catalyst containing a first transition metal and electrolyzing water. In addition, the present invention relates to a method for determining a driving potential capable of stabilizing an oxidation catalyst containing a first transition metal and electrolyzing water. More specifically, the present invention is the following aspects.
[0019] <1> A method for electrolyzing water, comprising the following steps: a step of supplying at least water to an electrolytic cell having a solid polymer electrolyte membrane, an anode and a cathode, and a step of applying a potential P between the anode and the cathode to generate oxygen gas from the anode, wherein the anode and the cathode are arranged in a manner of sandwiching the solid polymer electrolyte membrane, an oxidation catalyst containing at least one first transition metal (for example, an oxide or hydroxide of the first transition metal, or a single oxide or hydroxide of the first transition metal, or a composite oxide or composite hydroxide of two or more first transition metals, preferably a single oxide of the first transition metal or a composite oxide of two or more first transition metals) is present on at least a portion of the surface of the anode, and the potential P satisfies P1<P<P2 (wherein P1 represents the lowest potential at which oxygen gas is generated from the anode, and P2 represents the lowest potential P2 at which an indicator of the amount of dissolved chemical substances originating from the oxidation catalyst begins to show potential dependence).
[0020] <2> The method according to <1>, comprising the step of measuring P1 and P2 separately in advance.
[0021] <3> A method for determining a driving potential P of an electrolytic cell for electrolyzing water, the electrolytic cell for electrolyzing water comprising a solid polymer electrolyte membrane, an anode and a cathode, the anode having an oxidation catalyst containing at least one first transition metal, the method comprising the following steps: predetermining a minimum potential P1 between the anode and the cathode when oxygen begins to be generated from the anode; predetermining a minimum potential P2 between the anode and the cathode when an indicator of the amount of dissolved chemical substances originating from the oxidation catalyst begins to show potential dependence; and determining the driving potential P to a value that satisfies the condition P1<P<P2.
[0022] <4> A method for determining a driving potential P of an electrolytic cell for electrolyzing water, the electrolytic cell for electrolyzing water comprising a solid polymer electrolyte membrane, an anode and a cathode, the anode comprising an oxidation catalyst containing at least one first transition metal (for example, an oxide or hydroxide of the first transition metal, or an oxide or hydroxide of a single first transition metal, or a composite oxide or composite hydroxide of two or more first transition metals, preferably an oxide of a single first transition metal or a composite oxide of two or more first transition metals), the method comprising the following steps: plotting the amount of oxygen generated from the anode against the potential between the anode and the cathode to obtain a first curve; plotting an index of the amount of dissolved chemical substances derived from the oxidation catalyst against the potential between the anode and the cathode to obtain a second curve; and determining the driving potential P based on a comparison between the first curve and the second curve.
[0023] <5> The method according to any one of <1> to <4>, wherein the index of the amount is an intensity I of an absorption peak attributable to the chemical substance.
[0024] <6> The method according to any one of <1> to <4>, wherein the first transition metal is at least one metal selected from the group consisting of manganese, iron, cobalt, and nickel.
[0025] <7> The method according to any one of <1> to <4>, wherein the oxidation catalyst is an oxide or hydroxide of at least one metal selected from the first transition metal.
[0026] <8> According to any one of the methods <1> to <4>, the oxidation catalyst is at least one metal oxide or metal hydroxide selected from manganese oxide (2+, 3+, 4+), iron oxide (2+, 3+), cobalt hydroxide (2+, 3+) and nickel oxide (2+, 3+, 4+).
[0027] <9> The method according to any one of <1> to <4>, wherein the oxidation catalyst is manganese oxide, and P satisfies 1.65 V < P < 1.75 V relative to a hydrogen electrode (RHE).
[0028] <10> A device for electrolyzing water, comprising a solid polymer electrolyte membrane, an anode and a cathode arranged in a manner to clamp the solid polymer electrolyte membrane, a power supply unit for applying a potential between the anode and the cathode, and a control unit for controlling the potential to P satisfying P1<P<P2, wherein at least a portion of the surface of the anode has an oxidation catalyst containing at least one first transition metal (for example, an oxide or hydroxide of a first transition metal (it can be an oxide or hydroxide of a single first transition metal, or it can be a composite oxide or composite hydroxide of two or more first transition metals, preferably an oxide of a single first transition metal or a composite oxide of two or more first transition metals.), P1 is the minimum potential at which oxygen gas is generated from the anode, and P2 represents the minimum potential P2 at which an indicator of the amount of dissolved chemical substances originating from the oxidation catalyst begins to show potential dependence.
[0029] <11> The device according to <10>, wherein P1 and P2 are pre-input values.
[0030] <12> The device according to <10>, further comprising a measuring means for measuring in situ an index of the amount of dissolved chemical substances derived from the oxidation catalyst, wherein the control means controls P based on a value of the index of the amount detected by the measuring means.
[0031] <13> In the device according to <10>, the index of the quantity is an intensity I of an absorption peak attributable to the chemical substance.
[0032] <14> In the device according to <10>, the first transition metal is at least one metal selected from the group consisting of manganese, iron, cobalt, and nickel.
[0033] <15> The device according to <10>, wherein the oxidation catalyst is an oxide or hydroxide of at least one metal selected from the first transition metal.
[0034] <16> According to the device described in <10>, the oxidation catalyst is at least one metal oxide or metal hydroxide selected from manganese oxide (2+, 3+, 4+), iron oxide (2+, 3+), cobalt hydroxide (2+, 3+) and nickel oxide (2+, 3+, 4+).
[0035] <17> The device according to <10>, wherein the oxidation catalyst is manganese oxide, and P satisfies 1.65V<P<1.75V relative to a hydrogen electrode (RHE).
[0036] <18> A device for electrolyzing water, comprising a solid polymer electrolyte membrane, an anode and a cathode arranged in a manner of clamping the solid polymer electrolyte membrane, a power supply unit for applying a potential between the anode and the cathode, and a control unit for controlling the potential to be P satisfying P1<P<P2, an oxidation catalyst is present on at least a portion of the surface of the anode, the spinel-type composite oxide containing cobalt and manganese, P1 is the minimum potential at which oxygen is generated from the anode, and P2 represents the minimum potential P2 at which an indicator of the amount of dissolved chemical substances originating from the oxidation catalyst begins to show potential dependence.
[0037] <19> A device for electrolyzing water, comprising a solid polymer electrolyte membrane, an anode and a cathode arranged in a manner to clamp the solid polymer electrolyte membrane, and a power supply unit for applying a potential between the anode and the cathode, wherein an oxidation catalyst exists on at least a portion of the surface of the anode, and the oxidation catalyst contains a spinel-type composite oxide of cobalt and manganese.
[0038] Effects of the Invention
[0039] According to the present invention, water can be stably electrolyzed by an oxidation catalyst containing a first transition metal. For example, as shown in the examples described below, according to the present invention, γ-MnO2 can be electrolyzed at 10 mA cm-1 for more than 8000 hours in an electrolyte at pH 2 without significant decrease in activity. -2 Promotes the reaction that produces oxygen. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] [ Figure 1 A] is a diagram showing the structure of γ-MnO2. In the figure, (a) shows a TEM image of γ-MnO2. (b) shows an HRTEM image of γ-MnO2. (c) is a schematic diagram showing the eutectic structure of pyrolusite (1×1 tunnel) matrix and ramsdellite (1×2 tunnel) matrix.
[0041] [ Figure 1B ] is a diagram showing a representative XRD pattern of γ-MnO2.
[0042] [ Figure 1C ] is a diagram showing a representative Raman spectrum of γ-MnO2.
[0043] [ Figure 2A ] is a graph showing the linear sweep voltammogram of FTO and γ-MnO2 on carbon paper in 1.0M H2SO4 (scan rate: 1 mVs -1 ).
[0044] [ Figure 2B ] is a graph showing the Tafel plots of γ-MnO2 on FTO and carbon paper.
[0045] [ Figure 3A] is a diagram showing a schematic diagram of the experimental setup for in-situ UV-Vis measurement. The working electrode is placed just in front of the detector window, and the reference electrode and the counter electrode are placed adjacent to the wall of the electrochemical cell.
[0046] [ Figure 3B ] is a graph showing the UV / Vis absorption spectrum of the electrolyte after electrolysis for 1 hour at the indicated potential. The measurement was performed on γ-MnO2 on FTO at pH 2.
[0047] [ Figure 3C ] is to show Mn 3+ Potential dependence of accumulation (squares), current of oxygen generation (black line), and generation of MnO4 - (circles) The measurements were performed on γ-MnO2 on FTO at pH 2.
[0048] [ Figure 3D ] is shown as 10mAcm -2 (curve a) and 100mAcm -2 (curve b) is a graph of the time dependence of the anode potential in electrolysis at a constant current density. The measurement was performed on γ-MnO2 on FTO at pH 2.
[0049] [ Figure 4 ] is the Bourbaix diagram of the Mn-H2O system calculated using the CHNOSZ program package [see reference 19]. The formation (ΔG0) free energy used, MnO2, Mn 2+ 、MnO4 - 、MnO4 2- , Mn2O3, Mn3O4, Mn(OH)2 and Mn are -465.15 kJmol -1 、-227.76kJmol -1 、-449.66kJmol -1 、-504.09kJmol -1 、-888.857kJmol -1 、-1281.16kJmol -1 、-615.04kJmol -1 and 0 kJmol -1 . Solution substance (MnO4 - 、MnO4 2- , Mn 2+ 、HMnO2 - ) activity from T = 25 ° C 10 -7 Change to 10 0 molL -1 .
[0050] [ Figure 5A] is a schematic diagram showing the preparation sequence of the anode (γ-MnO2 / carbon paper).
[0051] [ Figure 5B ] is a diagram showing a schematic structure of a PEM electrolysis device.
[0052] [ Figure 5C ] is a photo showing a PEM water electrolysis system. Electrolysis was performed using a single stack PEM water electrolysis device unit. Milli-Q ultrapure water was pressed into the anode part of the electrolysis device. The PEM water electrolysis device used a 2-electrode system and was controlled by a potentiometer.
[0053] [ Fig. 6A ] is a graph showing the linear sweep voltammogram of γ-MnO2 on carbon paper at 25°C.
[0054] [ Figure 6B ] is shown as 10mAcm 2 and 100mAcm 2 Graph of the time dependence of the cell voltage under (25°C, without ohmic resistance correction).
[0055] [ Fig. 7A ] is 100 mA cm at pH 1 -2 Spinel Cobalt Manganese Oxide Co 3-X A graph showing the stability of MnXO4.
[0056] [ Figure 7B ] is shown as 100mAcm -2 Curve diagram of the stability of Co2MnO4 under H2SO4 (pH 1) and H3PO4 (pH 1).
[0057] [ Figure 7C ] is shown as 100mAcm -2 The stability of γ-MnO2 under H2SO4 (pH1, pH2) and H3PO4 (pH1) is shown in the graph. It shows that the 100mAcm -2 The stability curve of γ-MnO2 is shown below.
[0058] [ Figure 8 ] is a schematic diagram showing the chemical species derived from the OER cycle under acidic conditions and the γ-MnO2 generated in its side reactions. DETAILED DESCRIPTION
[0059] (Method and device for electrolyzing water)
[0060] As shown in the examples described below, the present inventors have found that there is a potential window in which the driving potential is stable, which can efficiently promote the oxygen evolution reaction (OER) by a catalyst containing a first transition metal while suppressing the deactivation path of the metal. The present invention is based on these insights and specifically provides the following method and device for electrolyzing water.
[0061] A method for electrolyzing water, comprising supplying at least water to an electrolytic cell having a solid polymer electrolyte membrane, and an anode and a cathode arranged in a manner to clamp the solid polymer electrolyte membrane; applying a potential P between the anode and the cathode to generate oxygen from the anode, wherein an oxidation catalyst containing at least one first transition metal exists on at least a portion of the surface of the anode, and the potential P satisfies P1<P<P2 (wherein P1 represents the lowest potential at which oxygen is generated from the anode, and P2 represents the lowest potential P2 at which an indicator of the amount of dissolved chemical substances originating from the oxidation catalyst begins to show potential dependence).
[0062] A device for electrolyzing water, comprising a solid polymer electrolyte membrane, an anode and a cathode arranged in a manner of clamping the solid polymer electrolyte membrane, a power supply unit for applying a potential between the anode and the cathode, and a control unit for controlling the potential to be P satisfying P1<P<P2, wherein an oxidation catalyst containing at least one first transition metal exists on at least a portion of the surface of the anode, P1 is the minimum potential at which oxygen is generated from the anode, and P2 represents the minimum potential P2 at which an indicator of the amount of dissolved chemical substances originating from the oxidation catalyst begins to show potential dependence.
[0063] In the present invention, the anode is connected to the positive electrode of the power supply unit and is an electrode that undergoes an oxidation reaction to generate oxygen in water electrolysis, and an oxidation catalyst containing at least one first transition metal exists on at least a portion of its surface.
[0064] The first transition metal (3d transition metal) in the present invention is not particularly limited, and examples thereof include manganese, iron, cobalt, and nickel. Manganese is preferred from the viewpoints of abundance in nature, durability of the catalyst, and ease of synthesis.
[0065] In addition, the oxidation catalyst used in the present invention may not contain precious metals. Even if it is an embodiment containing precious metals, the molar ratio of the precious metal relative to the total molar ratio of all metals in the catalyst can be 10% or less, 5% or less, 1% or less, 0.1% or less, or 0.
[0066] The oxidation catalyst in the present invention may contain an oxide or hydroxide of a first transition metal, for example, at least one metal oxide or metal hydroxide selected from manganese oxide (2+, 3+, 4+), iron oxide (2+, 3+), cobalt hydroxide (2+, 3+) and nickel oxide (2+, 3+, 4+).
[0067] As compounds containing manganese, for example, pyrolusite (β-MnO2), ramsdellite (RMnO2), and enastarite (γ-MnO2) [see reference 25]. Pyrolusite is one of the most abundant manganese ores, and its structure is formed by lattice unit parameters and [See Reference 26], which is composed of a chain of [MnO6] octahedrons that share corners and edges and are connected in a 1×1 tunnel framework. Ramsdellite is a relatively rare mineral, and its structure is composed of a unit lattice parameter and The 1×2 tunnel framework of [see Reference 27] is composed of two chains of asymmetric [MnO6] with two edges. Among them, the oxidation catalyst in the present invention preferably contains γ-MnO2.
[0068] The oxidation catalyst in the present invention may be a composite oxide or composite hydroxide of multiple first transition metals. Examples of the multiple first transition metal oxides or hydroxides include composite oxides of cobalt and manganese (spinel cobalt-manganese oxides, etc.), and more specifically, Co 3-x Mn x O4(Co 0.1 Mn 0.9 O4, CoMn2O4, Co 1.5 Mn 1.5 O4, Co2MnO4), among which, from the viewpoint of easily showing higher stability, it is preferred that the oxidation catalyst in the present invention contains Co2MnO4. From other viewpoints, according to this embodiment, that is, in an embodiment using a composite oxide of manganese and cobalt as a catalyst, in an embodiment using manganese oxide as a catalyst, the width of the potential window capable of stable driving determined by the method of the present invention can be widened (more specifically, the upper limit potential P2 of the potential window is increased).
[0069] The form of the oxidation catalyst of the present invention is not particularly limited, and generally, it can be in the form of a catalyst supported on an anode (support). As a support for the supported catalyst, for example, conductive ceramics such as FTO (fluorine-doped tin oxide) and ITO (indium tin oxide), metals such as nickel and platinum, and carbon (conductive carbon materials) such as acetylene black and Ketjen black can be cited.
[0070] The method for preparing the catalyst of the present invention is not particularly limited, and the catalyst of the present invention can be easily prepared by a known method. In addition, as a method for supporting the catalyst of the present invention on a carrier, for example, thermal decomposition, spraying, mixing, impregnation, adsorption, and ion exchange methods can be cited. In addition, the oxidation catalyst may be present in at least a portion of the surface of the carrier (anode), for example, the oxidation catalyst may be present in more than 10%, more than 20%, more than 30%, more than 40%, more than 50%, more than 60%, more than 70%, more than 80%, more than 90%, or 100% of its surface.
[0071] The specific surface area of the catalyst of the present invention is not particularly limited, but is usually 5 to 200 m 2 / g, preferably 10m 2 / g or more, more preferably 20m 2 / g or more, more preferably 50m 2 / g or more, more preferably 70m 2 As a method for measuring the specific surface area of the catalyst, as shown in the examples described later, the BET (Brunauer-Emett-Teller) method of analyzing nitrogen adsorption can be used.
[0072] In addition, the catalyst of the present invention may also contain components other than the first transition element, alkali and carbonate as appropriate. As these components, for example, polymer electrolytes such as perfluorosulfonic acid polymers (NAFION; trade name) and conductive carbon materials such as acetylene black and Ketjen black can be cited.
[0073] In the present invention, the cathode (cathode) is connected to the cathode of the power supply unit, and a reduction reaction occurs. It can be an electrode that produces hydrogen in water electrolysis, and for example, a platinum electrode can be cited. In addition, as a solid polymer electrolyte membrane disposed between the anode and the cathode, it is a membrane composed of a water-insoluble polymer electrolyte, as long as it is a polymer electrolyte membrane called an ion exchange membrane. As the polymer electrolyte, for example, perfluorosulfonic acid polymers (NAFION; trade name, etc.) can be cited. In addition, there is no particular limitation on the electrolytic cell having a solid polymer electrolyte membrane and an anode and a cathode configured in a manner to clamp the solid polymer electrolyte membrane, and an electrolytic cell known in the art (especially the proton exchange membrane (PEM) electrolysis field) can be appropriately used.
[0074] In the present invention, the water supplied to the electrolytic cell for electrolysis may be only water (so-called pure water) or may be in the form of an aqueous solution containing an electrolyte. As the electrolyte, phosphate ion, sulfate ion, carbonate ion, arsenate ion, phosphite ion, silicate ion, borate ion may be cited, wherein, from the viewpoint of being more likely to improve the stability of the first transition metal, preferably phosphate ion, sulfate ion, more preferably phosphate ion. If phosphate ion is used in particular, the width of the potential window that can be stably driven determined by the method of the present invention can be expanded (more specifically, the upper limit potential P2 can be improved).
[0075] The pH of water is not particularly limited, but is usually acidic near the anode. Examples of the acidic conditions include pH less than 7 (pH 6, pH 5, pH 4, pH 3, pH 2, pH 1).
[0076] Generally, a potential is applied between the anode and the cathode for electrolysis of water. In the present invention, the potential (P) is adjusted to satisfy a predetermined range. The range (P1<P<P2) can be determined by the method described below.
[0077] The "control unit for processing the potential control to satisfy P1<P<P2" provided in the water electrolysis device of the present invention may be any device that can adjust the potential to be applied by inputting P1 and P2 predetermined by the method described later, and examples thereof include a potentiometer and a potential programmer. In addition, the water electrolysis device of the present invention further includes a measuring means for in-situ measuring an index of the amount of dissolved chemical substances described later, and the control means controls P based on the value of the index of the amount detected by the measuring means. As the measuring means for the in-situ measurement, for example, a UV-Vis spectrometer using in-situ spectroscopy described later can be mentioned.
[0078] (Method for determining driving potential)
[0079] As shown in the examples described below, the present inventors have found that there is a potential window in which a catalyst containing a first transition metal can efficiently promote the oxygen evolution reaction (OER) while suppressing the deactivation path of the metal and stabilize the driving potential. Therefore, the present invention provides the following method for determining the driving potential.
[0080] A method for determining a driving potential P of an electrolytic cell for electrolyzing water, the electrolytic cell for electrolyzing water comprising a solid polymer electrolyte membrane, an anode and a cathode, the anode having an oxidation catalyst containing at least one first transition metal, the method comprising: predetermining a minimum potential P1 between the anode and the cathode when oxygen begins to be generated from the anode; predetermining a minimum potential P2 between the anode and the cathode at which an indicator of the amount of dissolved chemical substances originating from the electrolytic catalyst begins to show potential dependence; and determining the driving potential P to a value that satisfies the condition P1<P<P2.
[0081] As "the lowest potential P1 between the anode and the cathode when oxygen starts to be generated from the anode", those skilled in the art can appropriately determine it using a known method according to the type of oxidation catalyst used, water, the type of electrolyte contained in the water, and the pH of the water. As the known method, as shown in the embodiments described below, a method of detecting the amount of oxygen generated in the electrolytic cell for electrolysis using a thermal conductivity detector (TCD) and / or a gas chromatograph while changing the applied potential can be cited.
[0082] The lowest potential P2 between the anode and the cathode at which the index of the amount of dissolved chemical substances originating from the oxidation catalyst begins to show potential dependence, the "index of the amount of dissolved chemical substances originating from the oxidation catalyst" may be any index reflecting the amount of chemical substances dissolved (eluted) from the oxidation catalyst, for example, the intensity of the absorption peak attributable to the chemical substance. In addition, as to whether the intensity of the absorption peak begins to show potential dependence, for example, in-situ spectroscopy (more specifically, in-situ UV / Vis spectroelectrochemical measurement) may be used as shown in the examples described later.
[0083] In the present invention, in addition, regarding the driving potential P, the first curve can be obtained by plotting the amount of oxygen generated from the anode against the potential between the anode and the cathode, and the second curve can be obtained by plotting the index of the amount of dissolved chemical substances derived from the oxidation catalyst against the potential between the anode and the cathode, and the driving potential P can be determined based on the comparison between the first curve and the second curve.
[0084] If we use the example of γ-MnO2 on FTO at pH 2 ( Figure 3C ) is used to illustrate that the first curve (oxygen evolution) obtained by plotting the amount of oxygen generated on the surface of the oxidation catalyst containing γ-MnO2 against the potential starts to rise at 1.60 V relative to the potential of the hydrogen electrode (vs. RHE). On the other hand, the MO4 derived from the dissolution of the oxidation catalyst -The second curve obtained by plotting the absorption peak intensity of the potential starts to rise at 1.75 V. Therefore, those skilled in the art can determine from this curve that the driving potential is 1.60 V to 1.75 V (preferably 1.65 V to 1.75 V) relative to the hydrogen electrode when the oxidation catalyst is manganese oxide.
[0085] in addition, Figure 8 The figure shows the schematic diagram of the OER cycle and the changes of γ-MnO2 generated in its side reactions under acidic conditions. The solid line in the figure represents the OER cycle. The dotted line represents the dissolution / reaccumulation of manganese oxides, Mn III The heterogeneity and MnO4 - The potential in the figure is the value determined by the above method. The chemical substance surrounded by the gray circle is considered to be stable on the γ-MnO2 electrode.
[0086] In addition, as shown in the examples described below, in experiments using manganese oxide as a catalyst, the potential window for stable driving obtained by in-situ analysis is Figure 4 The range shown is about 220 mV wider than the range expected based on the Pourbaix plot of manganese.
[0087] Therefore, based on the determination method of the present invention and the above-mentioned new insights into manganese, according to the properties of the solid polymer electrolyte membrane (anode side pH, etc.) further combined as needed, even if it is believed that in a water oxidation decomposition system using other metals (iron, cobalt, nickel, etc.) as catalysts, when predicted from the Pourbaix diagram of the metal, the potential range that can be stably driven is very narrow or does not exist, it is possible to determine the potential window (potential range) that can be stably driven.
[0088] Example
[0089] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to the following examples. In addition, this example was carried out using the materials and methods shown below.
[0090] (Formation of γ-MnO2 on FTO substrate)
[0091] γ-MnO2 is directly generated by thermal decomposition on glass coated with fluorinated tin oxide (FTO) (SPD Research Institute Co., Ltd.) [see reference 18]. That is, 0.5 mL of 4M Mn(NO3)2 is dripped on the cleaned FTO-coated glass (JIS reagent special grade, ≧98.0%, シグマアルドリッチ), and calcined at 220°C for 6 hours in air on a hot plate. The input of Mn is controlled by the number of dripping and calcining cycles. The obtained electrode is cleaned with Milli-Q ultrapure water (18.2MΩcm at 25°C, メルクミリポア) and ultrasonicated for 10 seconds. Finally, the electrode is dried in an oven at 40°C for several hours before the measurement.
[0092] (Growth of γ-MnO2 on Carbon Paper Substrate)
[0093] γ-MnO2 was generated on hydrophilic carbon paper (HGP-H-060, thickness 190 μm, Toray). Figure 5A As shown in the figure, first, a 2.2×2.2 cm 2 The hydrophilic carbon paper was placed on a 2.4×2.4 cm 2 The center of the hydrophobic carbon paper (EC-TP1-060T, treated with Teflon (registered trademark), thickness 190μm, Toray). Then, use polyethylene cloth adhesive tape (Teraoka Tape) to mount the hydrophilic carbon paper and the hydrophobic carbon paper to the center of the stainless steel sample holder. Pre-treat the structure at 220°C for 10 minutes on a hot plate to obtain better adhesion. After cooling to room temperature, drop 0.5mL of 4M Mn(NO3)2 on the exposed hydrophilic carbon paper and sinter it at 220°C in air on a hot plate for 6 hours. The obtained electrode was cleaned with Milli-Q ultrapure water and decomposed by ultrasound for 10 seconds. Finally, the electrode was dried in an oven at 40°C for several hours before use.
[0094] (Characteristics evaluation)
[0095] After generation, the properties of the catalysts were evaluated by XRD, XPS, Raman spectroscopy, TEM, HRTEM and N2 adsorption-desorption isotherms.
[0096] The operating voltage was set to 40 kV, the current was set to 200 mA, and Cu-Kα radiation was used. XRD patterns were collected using a SmartLab (リガク) device. The patterns were recorded in the range of 10 to 90° (2θ) using a low scanning speed of 0.05° / min and a measurement step of 0.01°. No characteristic peaks were observed for α-MnO2, δ-MnO2, Mn3O4, and MnO.
[0097] XPS was performed using a surface analysis device (PHI 5000 Versa Probe II, ULVAC-PHI). Monochromatic Al Kα (1486.6 eV) radiation was used in all XPS measurements.
[0098] Raman spectra were collected by a Raman microscope system (Senterra, Bruker) using an excitation wavelength of 532 nm (0.02 mW) and a metallurgical objective lens (MPlan 50×, NA=0.75, Orion Pass, Tokyo, Japan). Raman spectra were obtained by integrating 100 times with an exposure time of 15 seconds. A low power of 0.02 mW was used to avoid damage caused by laser irradiation.
[0099] TEM images were obtained using a Hitachi HT7700 microscope. For TEM samples, the sample suspension was dropped onto a copper grid and dried in air. HRTEM images were obtained using a JEM-2100 microscope at 200 kV. For HRTEM samples, the processed sample suspension was dropped onto a lace carbon support and dried in air.
[0100] The surface area and pore structure of bulk manganese oxide were examined by measuring nitrogen adsorption and desorption isotherms at liquid nitrogen temperature (77 K) using a surface area analyzer (Micromeritics ASAP2000 device). The sample was degassed at 373 K for 9 hours before measurement. The specific surface area of manganese oxide was evaluated as 71.2 m according to the Brunauer-Emmett-Teller (BET) equation [see reference 19] 2 g -1 The average pore width of manganese oxide adsorption was estimated to be 10.3 nm based on fitting analysis using the Barrett-Joyner-Halenda (BJH) method [see Reference 20].
[0101] (Evaluation of electrolytic catalyst characteristics)
[0102] The electrochemical behavior of γ-MnO2 was evaluated in a three-electrode electrochemical cell using 30 mL of electrolyte. -2 The electrode was pretreated with sulfuric acid solution (1.0M H2SO4) (Wako Junyaku Kogyo Co., Ltd.) for 2 hours at a current density of 1.0M H2SO4. Then, a Pt wire (99.98%, PT-351325, Φ0.30mm, Niraco) was used as the counter electrode and Ag / AgCl / KCl (saturated KCl, World Precision Instruments) was used as the reference electrode at 1mVs -1The current density (j) versus potential (U) curve was obtained using a commercially available potentiometer and potential programmer (HZ-5000, Hokuto Denko) at a sweep rate of 1000 Hz and room temperature (25±2°C). In the electrochemical measurement at pH 2, a sulfuric acid electrolyte containing 0.5 M Na2SO4 (Wako Pure Chemical Industries, Ltd.) was used as a supporting electrolyte. The iR correction value of the working electrode and the reference electrode was measured by electrochemical impedance spectroscopy (i, current; R, resistance). The electrode potential after iR correction was recalibrated as a reversible hydrogen electrode (RHE). All measurements used an Ag / AgCl / KCl reference electrode, so the potential conversion vs. Ag / AgCl or vs. RHE was performed using the following formula.
[0103] E(vs.RHE)=E(vs.Ag / AgCl)+0.199V+0.0591V×pH.
[0104] (Faraday efficiency)
[0105] In a pH 2 electrolyte (anode: γ-MnO2 / FTO, cathode: Pt) at 10 mA cm -2 Hydrogen and oxygen are generated by electrolyzing water at a constant current density of . The generated H2 and O2 are analyzed by an online gas chromatograph (GC-7890A) equipped with a thermal conductivity detector (TCD) and a stainless steel column filled with molecular sieves. Argon is used as the carrier gas.
[0106] (Time-dependent change of Mn dissolution)
[0107] The amount of elements leached into the electrolyte during OER was analyzed by induced bonding plasma atomic emission spectroscopy (ICP-AES, Shimadzu Model ICPS8100). Samples were collected at various time points during the OER process.
[0108] (Electrochemical UV-Vis spectroscopy)
[0109] UV-Vis absorption spectra were obtained using a UV-Vis spectrometer (UV-2550, Shimadzu) in diffuse transmission mode with a built-in integrating sphere (MPC-2200, Shimadzu). To obtain the spectrum in situ, a manganese oxide thin film electrode mounted in a quartz electrochemical cell (2 cm × 2 cm × 2.5 cm high) filled with 7 mL of electrolyte was placed just in front of the integrating sphere.
[0110] (Proton Exchange Membrane (PEM) Electrolyzer)
[0111] A membrane-electrode assembly (MEA) was made using Nafion (registered trademark) 117 polymer membrane (Dupont, thickness 177.8 μm, N117). Before making the MEA, the N117 membrane was boiled in the following solutions for 1 hour to remove possible contaminants and ensure that the membrane was completely protonated. First, 3 wt% H2O2, then Milli-Q ultrapure water, then 1.0 M H2SO4, and finally Milli-Q ultrapure water again. Finally, the N117 membrane was dried in an oven at 40°C for several hours before use.
[0112] MEA was made using Pt as the cathode for hydrogen generation reaction and MnO2 as the anode for oxygen generation reaction. First, Pt slurry was made by mixing Pt / C (20wt% Pt in carbon black, Fuel Cell Earth), water, ethanol, and Nafion (registered trademark) solution (5wt% in H2O, Sigma Aldrich) as a binder. The catalyst ink mixture was then added with 0.1mgcm of Pt and 0.1mgcm of Nafion (registered trademark) respectively. -2 and 0.03mgcm -2 The mass supply amount was supplied to the hydrophobic Toray carbon paper and dried in an oven at 40°C for several hours. As described in the above item "γ-MnO2 formation on carbon paper substrate", the amount of 3.5±0.5mgcm -2 After the catalyst material was deposited, the surface was coated with an additional amount of Nafion (registered trademark) (0.6 mg / cm for the cathode and anode, respectively). -2 and 1.0mgcm -2 The obtained Pt / carbon and MnO2 / carbon samples were dried in an oven at 40°C for 24 hours. Then, Pt / carbon paper and MnO2 / carbon paper were heat-pressed on both sides of a commercially available N117 membrane at 135°C with a clamping force of 5 MPa for 10 minutes to produce an MEA. The effective area of the MEA is 2 cm×2 cm (4 cm 2 ).
[0113] The electrolysis test was carried out using a single-cell PEM electrolysis device (FC-R&D, PEM-3036, Kanagawa, Japan). A stainless steel mesh was used as a gas diffusion layer for both the anode and the cathode. The MEA was mounted on the PEM electrolysis device using a rubber gasket. The measurement was carried out using a potentiometer (HZ-7000, Hokuto Electric). During the PEM electrolysis operation, deionized water was supplied to the anode side of the electrolyte in the electrolytic cell. The current-voltage curve and constant current stability of the electrolytic cell at 40mA and 400mA were tested at 25°C. The voltage efficiency was calculated using the following formula [see reference 21].
[0114] η voltage =E eq / E cell ×100%=1.23V / E cell ×100%(25℃)
[0115] Where, E cell is the cell voltage, E eq is the balanced voltage.
[0116] (Example 1)
[0117] γ-MnO2 is known as a cathode material for dry cells, and its industrial-scale synthesis has historically been carried out in concentrated sulfuric acid (pH <1), indicating its inherent chemical stability in acidic environments [see Reference 9]. In this example, γ-MnO2 was generated on a fluorinated tin oxide (FTO) or carbon-based substrate by thermally decomposing manganese nitrate at 220°C in air. Although not shown in the figure, transmission electron microscopy (TEM) images show that MnO2 nanoparticles with a diameter of approximately 15 nm are bonded within the porous aggregate. N2 adsorption-desorption isotherms showed that the γ-MnO2 generated from the mesoporous porous structure (average pore size: 10.3 nm) had a high surface area (71.2 m 2 g -1 ).
[0118] The significant structural feature of γ-MnO2 is the eutectic of pyrolusite (β-MnO2 composed of symmetrical octahedral units) and rhombusite (R-MnO2 composed of symmetrical octahedral units). From the high-resolution transmission electron microscopy (HRTEM) image, it can be seen that an alternating structure of single and double [MnO6] unit cells is generated ( Figure 1 A) [See reference 10]. The ratio of the XRD peaks of (110) and (130) faces ( Figure 1B ), and, 400~800cm -1 Raman shift of Mn-O stretching vibration in the region ( Figure 1C ) shows that the proportion of pyrolusite (Pr ratio) is about 70% [see references 9b, 11].
[0119] In 1.0M sulfuric acid, at 1mVs -1 The electrochemical behavior of γ-MnO2 was evaluated by linear sweep voltammetry (LSV) at a potential sweep rate of Figure 2A and B). γ-MnO2 in order to achieve 10 mA cm on FTO substrate -2The current density (geometric area) requires an overvoltage of 489±5mV. The Faradaic efficiency and H2 / O2 ratio of oxygen generation were determined by online gas chromatography to be approximately 100% and 2, respectively, which proves that the oxidation current is only caused by the oxidation of water. By simply changing the substrate to porous carbon paper, the overvoltage dropped to 428±5mV. This is the lowest value reported so far among 3d-metal OER catalysts in an acidic environment [see references 3b, 7b-e, 12]. The Tafel slope is approximately 80mVdec -1 ( Figure 2B ), from which it can be predicted that the 5-fold increase in current density is caused by the increase in surface area.
[0120] (Example 2)
[0121] It is well known that manganese oxide dissolves in water electrolysis, especially under acidic conditions. Electrodeposited manganese oxide is reported to be stable and has been shown to dissolve at relatively low current densities (less than 1 mA cm -2 ) in a short time overvoltage increases significantly [see references 12a, b]. Manganese oxide doped with titanium, ternary oxide Ni 0.5 Mn 0.5 Sb 1.7 O y Manganese dissolution has also been observed in MgO2O3 [see citations 7d, 7b]. Currently, there are no reports of Mn oxides that are stable under OER conditions in acidic electrolytes over a period of months.
[0122] To clarify the mechanism by which MnO2 becomes unstable under acidic conditions, the present inventors conducted in situ UV / Vis spectroelectrochemical measurements of both the γ-MnO2 electrode and the electrolyte in water electrolysis at pH 2 ( Figure 3A Although not shown in the figure, the in situ UV / Vis spectrum of the electrode is consistent with the inventors' previous studies using other phases of manganese oxide, and a kinetic energy that is believed to be caused by the surface-attached Mn 3+ The absorption peak of OER (480 nm) is shown in Figure 13, 14. In contrast, in the UV / Vis spectrum of the electrolyte, no change in absorption was observed near the onset potential of OER, showing a significantly different potential dependence ( Figure 3B Only when the potential was raised to about 1.8 V vs. RHE (hereinafter, all potentials are expressed as vs. RHE), the peaks believed to be caused by MnO4 were observed at 525 and 545 nm. - new absorption properties [see reference 15].
[0123] Figure 3CThe figure shows how the potential affects the activity and stability of γ-MnO2 as an OER catalyst. If the potential is scanned on the positive side, a MnO2 peak characterized by a 480 nm peak is generated at 1.4 V in the UV / Vis spectrum of the electrode. 3+ [See cited document 14]. The generation of this intermediate, like other Mn oxides, starts to generate OER current at 1.6V [See cited documents 13, 16]. It should be noted that there is a third potential-dependent process that becomes significant from 1.8V. This process is MnO4 in the UV / Vis spectrum of the electrolyte. - The absorption peak of - Therefore, these results indicate that there is a stable potential window between 1.6 V and 1.75 V that can sustainably promote OER by γ-MnO2. It should be noted that the experimentally determined potential window is different from the overvoltage for dissolution (MnO4 - formed by Figure 4 The potential window predicted by the Pourbaix diagram (thermodynamic Pourbaix diagram) shown [see references 7a, 17] is only 220 mV wider.
[0124] In view of these insights, the present inventors, in order to explore the possibility of acid-stabilized MnO2, carried out water electrolysis at a constant current density ( Figure 5A ~C). The electrode potential of electrolysis is 10mAcm -2 The current density is about 1.73Vvs.RHE. This is higher than the start of the production of MnO4 - In fact, the catalyst shows no significant decrease in activity even after more than 8000 hours of operation (>11 months), demonstrating the unexpected stability of γ-MnO2 under these electrochemical conditions ( Figure 3D , curve a). Long-term water electrolysis was also confirmed at pH 1. Mn was detected by induced bonding plasma atomic emission spectroscopy (ICP-AES). 2+ ions into the electrolyte, but no soluble Mn was observed after 250 hours. 2+ ions. This is because, as demonstrated by Raman spectroscopy, XRD, and XPS, the Mn ions in the solution were redeposited in the form of γ-MnO2. 2+ This is consistent with the existing view that γ-MnO2 is preferentially deposited in H2SO4 [see references 9a, b].
[0125] As a control, at 100 mA cm -2 Under this condition, MnO2 is completely deactivated within 120 hours ( Figure 3D , curve b), the electrolyte forms MnO4 -This is because, although the initial electrolysis potential of 1.8V slightly exceeds the aforementioned potential window by only 50mV, it is still not enough to produce MnO4. - is sufficiently anodic, ultimately leading to dissolution and deactivation of the electrode. These results therefore show that γ-MnO2 can be used as a long-term OER catalyst under highly acidic conditions simply by keeping the applied electrochemical potential within a specific operating window. Oxygen was produced continuously in this system for 8000 hours, which is 50 times longer than the value reported so far for the best performing earth-abundant metal oxides [see citations 7b-e, 12d] and exceeds the benchmark of approximately 3000 hours in 1 year of operation assuming 8 hours of operation per day. The upper potential limit obtained by in situ spectroscopy is about 220 mV higher than the value calculated thermodynamically from the Pourbaix plot ( Figure 4 )[See references 7a, 17]. If we consider that the Tafel slope is 80 mV dec -1 ( Figure 2B ), this difference is important, and the additional driving force corresponds to an approximately 3-digit increase in the OER current. Therefore, both the highest levels of stability and activity reported so far can be achieved simultaneously.
[0126] (Example 3)
[0127] The advantages of accurately determining the potential window stabilized using spectroscopic techniques are shown in PEM electrolysis ( Figure 5A ~C). This mechanism is accompanied by a two-electrode system with a naphthon layer between them during the period when the electrode produces an acidic environment [see references 2c, 18]. Although various factors such as unit resistance and catalyst loading have not yet been optimized, Fig. 6A It can be clearly seen from the current-voltage curves shown that γ-MnO2 can be used as an efficient OER catalyst in the PEM mechanism as long as the driving potential is within the stable potential window. -2 The total overvoltage of the anode and cathode when operating at a current density of 2.5 is about 480 mV at room temperature after ohm correction, which is consistent with the results of the three-electrode system ( Figure 2A The increase in operating voltage observed after 350 hours is only 30 mV for 10 mA cm -2 The high stability of γ-MnO2 can also be seen from the time dependence of the cell voltage in the electrolysis under Figure 6B , curve a). After 350 hours of operation, the average voltage efficiency is 70.12%. -2 If electrolysis is carried out under this condition, the voltage efficiency will decrease immediately within 12 hours ( Figure 6B , curve b), confirms the importance of maintaining within the potential window in order to inhibit the deactivation of γ-MnO2.
[0128] So far, only 4d / 5d rare metals have been reported to be sufficiently stable to function as catalysts for OER, but the inventors have shown here that γ-MnO2 can operate continuously for more than 8000 hours under acidic conditions. On the other hand, small deviations in the driving potential of 50-mV can lead to complete deactivation of γ-MnO2 within 120 hours, highlighting why MnO2, which is abundant on Earth, is difficult to use as a stable OER catalyst in acidic electrolytes. In state-of-the-art solar fuel generation systems combining Ir-based PEM electrolyzers with 3-junction photovoltaic cells (PV), average sunlight-to-hydrogen (STH) conversion efficiencies of more than 30% have been reported [see citation 2e], and therefore PV-electrically driven water electrolysis is one of the most feasible means of producing renewable hydrogen. The inventors expect that the spectroelectrochemical approach to determine the stable potential window for OER in acid is a reasonable starting point for the development of precious metal-free PEM systems for renewable hydrogen production.
[0129] In a water oxidation decomposition system using other metals (iron, cobalt, nickel, etc.) as catalysts, the potential window (potential range) that can be stably driven can be determined by the same method as in the above embodiment according to the properties of the solid polymer electrolyte membrane that needs to be combined (anode side pH, etc.).
[0130] (Example 4)
[0131] The molar ratio of Co to Mn was varied and the -1 , produced by SPD Laboratory, Inc.) are respectively formed with cobalt manganese oxide layers. Specifically, it is as follows.
[0132] <Fabrication of FTO electrode with Co2MnO4 layer>
[0133] Co(NO3)2·6H2O (JIS special grade, ≧98.0%, purchased from Fujifilm Wako Pure Chemical Industries, Ltd.) and Mn(NO3)2·6H2O (JIS special grade, ≧98.0%, purchased from シグマ-アルドリッチ) were dissolved in water at a molar ratio of Co:Mn of 2:1, and a precursor solution with a total cation concentration of 2.5 M was prepared. 25 μL of the precursor solution was dropped onto a clean FTO substrate (hereinafter referred to as the "drop casting process"), and fired on a hot plate in the atmosphere for 12 hours (hereinafter referred to as the "firing process") to form a layer. It was rinsed with Milli-Q ultrapure water (18.2MΩcm at 25°C, purchased from Melku Millipore) and ultrasonically cleaned for 10 seconds to remove particles such as impurities slightly attached to the surface (hereinafter referred to as the "cleaning process"). The above-mentioned drop casting process, sintering process, and cleaning process were repeated again to form a layer that completely covered the surface of the FTO substrate. The electrode substrate was dried in an oven at 40°C for several hours before the measurement.
[0134] The following analysis confirmed that the obtained layer was composed of spinel cobalt manganese oxide having a Co / Mn molar ratio of 2:1 (hereinafter, this layer is referred to as "Co2MnO4 layer"). Thus, a FTO electrode with Co2MnO4 was produced.
[0135] The X-ray diffraction (XRD) pattern of the layer formed above was measured. The measurement conditions were Cu-Kα radiation. Irradiation, working voltage 40kV, and current 200mA. In addition, the measurement uses a fully automatic multi-purpose X-ray diffraction device SmartLab (Likagaku Co., Ltd.). The scanning speed is 0.5° / min in the range of 10-80° (2θ), and the measurement is performed at a scanning speed of 0.5° / min for every 0.01°. It can be understood from the obtained XRD pattern that the obtained cobalt manganese oxide forms a crystal system of a cubic spinel structure.
[0136] In addition, the produced catalyst layer was subjected to X-ray photoelectron spectroscopy (XPS) measurement using a ULVAC-PHI spectrometer (PHI 5000 Versa Probe II) equipped with an AlKα (1486.6 eV) irradiation device.
[0137] XPS results show that there is Co 2+ and Co 3+ The average valence of these two is about 2.5, and there is Mn 3+ and Mn 4+ The average valence of these two is about 3.6. Generally, the chemical formula of cobalt manganese spinel oxide with a Co / Mn ratio of 2:1 is (Co 2+ ) tet (Mn x+Co 3+ ) oct O 4+δ (δ = 0.1 ~ 0.4) indicates that Co 2+ Existing in tetrahedral sites, Mn x+ and Co 3+ The XPS results show that x is about 3.6 and δ is about 0.3, which is consistent with the values of cobalt-manganese spinel oxide with a Co / Mn ratio of 2:1 reported previously.
[0138] In addition, the elemental spectrum of the catalyst layer was measured using an energy dispersive X-ray (EDX) spectrometer equipped with a TEM (JEM-2100F), and the results confirmed that the catalyst layer existed uniformly in the form of Co2MnO4 nanoparticles.
[0139] In addition, the TEM image was obtained using a field emission electron microscope (JSF-7800F; 5 kV scanning). The primary particle size of Co2MnO4 was confirmed to be 10 to 15 nm at 200 kV.
[0140] <With Co 1.5 Mn 1.5 O4 layer, CoMn2O4 layer, or Co 0.1 Mn 0.9 Fabrication of FTO electrode with O4 layer>
[0141] Precursor solutions were prepared with a molar ratio of Co to Mn of 1:1, 1:2, and 1:9, and Co was formed on FTO in the same manner as above except that the respective precursor solutions were used. 1.5 Mn 1.5 O4 layer, CoMn2O4 layer and Co 0.1 Mn 0.9 In addition, in the same manner as the Co2MnO4 layer, it was confirmed that the composite oxide in each layer was a spinel-type cobalt-manganese composite oxide in which the molar ratios of Co to Mn were 1:1, 1:2, and 1:9, respectively.
[0142] Thus, they were made into 1.5 Mn 1.5 FTO electrode with CoO4 layer, FTO electrode with CoMn2O4 layer, and FTO electrode with Co 0.1 Mn 0.9 O4 layer of FTO electrode.
[0143] <Evaluation of the stability of OER catalyst function under strong acidic conditions>
[0144] The stability of the oxygen evolution reaction (OER) catalytic function of each layer under strong acidic conditions was evaluated by chronopotentiometry. Specifically, the following is described.
[0145] For the FTO electrodes with various layers prepared above, the 100 mA cm -2 The chronopotentiometry at a current density of . The measurement was performed using a commercially available three-electrode potentiostat (HZ-7000; produced by Hokuto Denko Co., Ltd.). The counter electrode was a Pt wire electrode (99.98%, PT-351325, Φ0.30 mm, produced by Niraco), and the reference electrode was Ag / AgCl (3.5 M KCl, produced by World Precision Instruments, 0.205 V vs. NHE at 25°C). The current density was based on the area of the FTO substrate exposed to the electrolyte (0.28 cm 2 In addition, all measurements were performed at a temperature of 25°C.
[0146] In addition, an FTO electrode with a γ-MnO2 layer prepared by the same operation as above (generation of γ-MnO2 on FTO substrate) and an FTO electrode with Co3O4 prepared by a known method were prepared, and the chronopotentiometry was measured under the same conditions. The results are shown in Fig. 7A .
[0147] Depend on Fig. 7A The results shown show that the stability of the OER catalyst function under strong acidic conditions is significantly improved by using a composite oxide of cobalt and manganese as manganese oxide. This result is unpredictable if one considers that the cobalt oxide catalyst can be deactivated in a short time under strong acidic conditions (refer to the data of Co3O4).
[0148] In addition, it is believed that the catalytic function of γ-MnO2 deactivates rapidly because it is driven at a potential of 1.8 V outside the potential window that can be stably driven. Therefore, it can be understood that by using cobalt and composite cobalt manganese oxide as manganese oxide, the potential window that can be stably driven can be expanded (specifically, the upper limit potential P2 can be increased).
[0149] As can be seen from the above results, the FTO electrode with a Co2MnO4 layer has the highest stability under strong acidic conditions. The same operation was performed except that the electrolyzed water was replaced from H2SO4 (pH = 1) to H3PO4 (pH = 1). The chronopotentiometry results showed that it could be driven stably for more than 1200 hours. The results are shown in Figure 7B In addition, as a reference, the Fig. 7A Results for the curves of the FTO electrode with the Co2MnO4 layer removed.
[0150] In addition, for the FTO electrode with γ-MnO2 layer, in order to confirm the effect of electrolytic water on stability, the electrolytic water was replaced from H2SO4 (pH = 1) to H3PO4 (pH = 1) and H2SO4 (pH = 2), and the same operation was performed except that the electrolytic water was replaced from H2SO4 (pH = 1) to H3PO4 (pH = 1) and H2SO4 (pH = 2), and the chronopotentiometry was measured. The results are shown in Figure 7C In addition, as a reference, the Fig. 7A The curve of the FTO electrode with γ-MnO2 is removed.
[0151] Depend on Figure 7B and 7C It can be understood from the results that the presence of phosphate ions in electrolyzed water can also expand the potential window that enables stable driving.
[0152] (Citations) [1]
[0154] a)RESmalley, Bull.Mater.Res.Soc.2005, 30, 412-417;
[0155] b)NSLewis, DGNocera, Proc.Natl.Acad.Sci.USA2006, 103, 15729-15735;
[0156] c) N.Muradov, T.Veziroglu, Int.J.Hydrogen Energy 2008, 33, 68046839;
[0157] d)M.Gotz, J.Lefebvre, F.Mors, A.McDaniel Koch, F.Graf, S.Bajohr, R.Reimert, T.Kolb, Renew.Energy 2016, 85, 1371-1390;
[0158] e) B. Pivovar, N. Rustagi, S. Satyapal, Electrochem.Soc.Interface 2018, 27, 47-52. [2]
[0160] a) JATurner, Science 2004, 305, 972-974;
[0161] b) A. Ursua, LMGandia, P. Sanchis, Proc. IEEE 2012, 100, 410-426;
[0162] c)M.Carmo,DLFritz,J.Mergel,D.Stolten,Int.J.Hydrogen Energy 2013,38,4901-4934;
[0163] d)K.Fujii,S.Nakamura,M.Sugiyama,K.Watanabe,B.Bagheri,Y.Nakano,Int.J.Hydrogen Energy 2013,38,14424–14432;
[0164] e)J.Jia,LCSeitz,JDBenck,Y.Huo,Y.Chen,JWNg,T.Bilir,JSHarris,TFJaramillo,Nat.Commun.2016,7,13237.
[0165] f)C.Tang,N.Cheng,Z.Pu,W.Xing,X.Sun,Angew.Chem.Int.Ed.2015,54,9351-9355;Angew.Chem.2015,18783,949
[0166] g)C.Tang,R.Zhang,W.Lu,L.He,X.Jiang,AMAsiri,X.Sun,Angew.Chem.Int.Ed.2017,56,1064-1068,Angew.14,1024,20817,
[0167] h)G.Maayan,N.Gluz,G.Christou,Nat.Catal.2018,1,48-54;
[0168] i)H.Liu,X.Gao,X.Yao,M.Chen,G.Zhou,J.Qi,X.Zhao,W.Wang,W.Zhang,R.Cao,Chem.Sci.2019,10–19.19. [3]
[0170] a)JRMcKone,NSLewis,HBGray,Chem.Mater.2014,26,407-414;
[0171] b)CCMcCrory,S.Jung,IMFerrer,SMChatman,JCPeters,TFJaramillo,J.Am.Chem.Soc.2015,137,4347-4357;
[0172] c)LCSeitz,CFDickens,K.Nishio,Y.Hikita,J.Montoya,A.Doyle,C.Kirk,A.Vojvodic,HYHwang,JKNorskov,TFJaramillo,Science 2016,101-1014;
[0173] d)S.Geiger,O.Kasian,M.Ledendecker,E.Pizzutilo,AMMingers,WTFu,O.Diaz-Morales,Z.Li,T.O ellers,L.Fruchter,A.Ludwig,KJJMayrhofer,MTMKoper,S.Cherevko,Nat.Catal.2018,1,508-515.
[0174] e)O.Kasian,J.-P.Grote,S.Geiger,S.Cherevko,KJJMayrhofer,Angew.Chem.Int.Ed.2018,57,2488-2491;
[0175] [4]PCKVesborg,TFJaramillo,RSC Adv.2012,2,7933.
[0176] [5]EAPaoli,F.Masini,R.Frydendal,D.Deiana,C.Schlaup,M.Malizia,TWHansen,S.Horch,IELStephens,I.Chorkendorff,Chem.Sci.2015,601-96. [6]
[0178] a)I.Roger,MAShipman,MDSymes,Nat.Rev.Chem.2017,1,0003;
[0179] b)C.Spori,JTHKwan,A.Bonakdarpour,DPWilkinson,P.Strasser,Angew.Chem.Int.Ed.2017,56,5994-6021.Angew.Chem.2017,1298-617. [7]
[0181] a)M.Pourbaix,Atlas of electrochemical equilibria in aqueoussolutions,Pergamon,New York,1966,pp.286-292.
[0182] b)IAMoreno-Hernandez,CAMacFarland,CGRead,KMPadantonakis,BSBrunschwig,NSLewis,Energy Environ.Sci.2017,10,2103-2108;
[0183] c)JSMondschein,JFCallejas,CGRead,JYCChen,CFHolder,CKBadding,RESchaak,Chem.Mater.2017,29,950-957;
[0184] d)R.Frydendal,EAPaoli,I.Chorkendorff,J.Rossmeisl,IELStephens,Adv.Energy Mater.2015,5,1500991;
[0185] e)M.Huynh,T.Ozel,C.Liu,ECLau,DGNocera,Chem.Sci.2017,8,4779-4794;
[0186] f)R.Pokhrel,MKGoetz,SEShaner,X.Wu,SSStahl,J.Am.Chem.Soc.2015,137,8384-8387;
[0187] g)M.Blasco-Ahicart,J.Soriano-Lopez,JJCarbo,JMPoblet,JRGalan-Mascaros,Nat.Chem.2018,10,24-30. [8]
[0189] JKNorskov,T.Bligaard,J.Rossmeisl,CHChristensen,Nat.Chem.2009,1,37-46. [9]
[0191] a)S.Bodoardo,J.Brenet,M.Maja,P.Spinelli,Electrochim.Acta 1994,39,1999-2004;
[0192] b)Y.Chabre,J.Pannetier,Prog.Solid State Chem.1995,23,1-130;
[0193] c)DKWalanda,GALawrance,SWDonne,J.Power Sources 2005,139,325-341.
[10]
[0195] a)PMde Wolff,Acta Crystallogr.1959,12,341-345;
[0196] b)S.Turner,PRBuseck,Nature 1983,304,143146.
[11]
[0198] C.Julien,M.Massot,S.Rangan,M.Lemal,D.Guyomard,J.Raman Spectrosc.2002,33,223-228.
[12]
[0200] a)M.Huynh,DKBediako,DGNocera,J.Am.Chem.Soc.2014,136,6002-6010;
[0201] b)M.Huynh,C.Shi,SJBillinge,DGNocera,J.Am.Chem.Soc.2015,137,14887–14904;
[0202] c)L.Han,P.Tang,A.ReyesCarmona,B.Rodriguez-Garcia,M.Torrens,JRMorante,J.Arbiol,JRGalan-Mascaros,J.Am.Chem.Soc.2016,1603,1348
[0203] d)M.Blasco-Ahicart,J.Soriano-Lopez,JJCarbo,JMPoblet,JRGalanMascaros,Nature chemistry 2018,10,24-30.
[13]
[0205] a)T.Tashima,K.Hashimoto,R.Nakamura,J.Am.Chem.Soc.2012,134,1519–1527;
[0206] b)K.Jin,H.Seo,T.Hayashi,M.Balamurugan,D.Jeong,YKGo,JSHong,KHCho,H.Kakizaki,N. Bonnet-Mercier,MGKim,SHKim,R.Nakamura,KTNam,J.Am.Chem.Soc.2017,139,2277-2285.
[14]
[0208] G.Davies,Coord.Chem.Rev.1969,4,199-224.
[15]
[0210] NVKlassen,D.Marchington,HCEMcGowan,Anal.Chem.1994,66,2921-2925.
[16]
[0212] a)CHKuo,W.Li,L.Pahalagedara,AMEl-Sawy,D.Kriz,N.Genz,C.Guild,T.Ressler,SLSuib,J.He,Angew.Chem.,Int.Ed.2015-2015-3255;
[0213] b) I. Zaharieva, P. Chernev, M. Risch, K. Klingan, M. Kohlhoff, A. Fischer, H. Dau, Energy Environ. Sci. 2012, 5, 7081;
[0214] c) B. Zhang, H. Chen, Q. Daniel, B. Philippe, F. Yu, M. Valvo, Y. Li, RBAmbre, P. Zhang, F. Li, H. Rensmo, L. Sun, ACS Catal.
[17]
[0216] a)AJBard,R.Parsons,J.Jordan,Standard Potentials in AqueousSolution,CRC Press,New York,1985,pp.429-439.
[0217] b)JMDick,Geochem.Trans.,2008,9,10.
[18]
[0219] NFBunkin,PSIgnatiev,VAKozlov,AVShkirin,SDZakharov,AAZinchenko,Water 2013,4,129-154.
[19]
[0221] M.Maneva,N.Petroff,J.Therm.nal.1990,36,2511-2520.
[20]
[0223] S.Brunauer,PHEmmett,E.Teller,J.Am.Chem.Soc.1938,60,309-319.
[21]
[0225] EPBarrett,LGJoyner,PPHalenda,J.Am.Chem.Soc.1951,73,373-380.
[22]
[0227] K.Zeng,D.Zhang,Pror.Energy Combust.Sci.2010,36,307-326.
[23]
[0229] a)T.Takashima,K.Hashimoto,R.Nakamura,J.Am.Chem.Soc.2012,134,18153-18156;
[0230] b) Y. Gorlin, B. Lassalle-Kaiser, JDBenck, S. Gul, SMWebb, VKYachandra, J. Yano, TF Jaramillo, J. Am.Chem.Soc.2013,135,8525-8534;
[0231] c)Z.Morgan Chan,DAKitchaev,J.Nelson Weker,C.Schnedermann,K.Lim,G.Ceder,W.Thomas,MFToney,DGNocera,Proc.Natl.Acad.Sci.USA2018,1528,E526.
[24]
[0233] G.Mattioli,I.Zaharieva,H.Dau,L.Guidoni,J.Am.Chem.Soc.2015,137,10254-10267.
[25]
[0235] O.Schilling,JRDahn,J.Appl.Crystallogr.1998,31,396-406.
[26]
[0237] JEPost,Proc.Natl.Acad.Sci.USA1999,96,3447-3454.
[27]
[0239] WHBaur, Acta Crystallogr., Sect.B: Struct.Crystallogr.Cryst.Chem.1976, 32, 2200-2204.
[28]
[0241] JE Post, PJ Heaney, Am. Mineral. 2004, 89, 969-975.
[29]
[0243] a) E.Silvester, A.Manceau, VADrits, Am.Mineral.1997, 82, 962-978;
[0244] b) Y. Tanaka, M. Tsuji, Y. Tamaura, Phys. Chem. Chem. Phys. 2000, 2, 1473-1479; c) S. Tu, GJ Racz, TBGoh, Clays Clay Miner. 1994, 42, 321-330.
[30]
[0246] a) JSMondschein, et al., Inorg.Chem.2018, 57, 6010-6015.
[0247] b)Delgado et al.Sci.Rep.2015, 5, 15208.
[31]
[0249] JGVos, TAWezendonk, AWJeremiasse, MTMKoper, J.Am.Chem.Soc., 2018, 140, 10270-10281
[0250] Industrial Applicability
[0251] As described above, according to the present invention, water can be stably electrolyzed using an oxidation catalyst containing a first transition metal.
Claims
1. A method for electrolyzing water, comprising: At least water is supplied to an electrolytic cell including a solid polymer electrolyte membrane and an anode and a cathode, wherein the anode and the cathode are arranged so as to sandwich the solid polymer electrolyte membrane. applying a driving potential P between the anode and the cathode, thereby generating oxygen from the anode, An oxidation catalyst containing at least one first transition metal is present on at least a portion of the surface of the anode, The amount of oxygen generated from the anode is plotted against the potential between the anode and the cathode to obtain a first curve. The second curve is obtained by plotting the index of the amount of dissolved chemical substances originating from the oxidation catalyst against the potential between the anode and the cathode. The driving potential P is determined based on the comparison between the first curve and the second curve. The driving potential P satisfies P1<P<P2, where P1 represents the lowest potential at which oxygen is generated from the anode, and P2 represents the lowest potential P2 at which an indicator of the amount of dissolved chemical substances derived from the oxidation catalyst begins to show potential dependence.
2. A method for determining a driving potential P of an electrolytic cell for electrolysis of water, the electrolytic cell for electrolysis of water comprising a solid polymer electrolyte membrane, an anode and a cathode, the anode having an oxidation catalyst containing at least one first transition metal, the method comprising: The amount of oxygen generated from the anode is plotted against the potential between the anode and the cathode to obtain a first curve. The second curve is obtained by plotting the index of the amount of dissolved chemical substances originating from the oxidation catalyst against the potential between the anode and the cathode. The driving potential P is determined based on the comparison between the first curve and the second curve. The driving potential P satisfies P1<P<P2, where P1 represents the lowest potential at which oxygen is generated from the anode, and P2 represents the lowest potential P2 at which an indicator of the amount of dissolved chemical substances derived from the oxidation catalyst begins to show potential dependence.
3. The method according to claim 1 or 2, wherein the indicator of the quantity is the intensity I of the absorption peak attributable to the chemical substance.
4. The method according to claim 1 or 2, wherein the first transition metal is at least one metal selected from the group consisting of manganese, iron, cobalt and nickel. 5 . The method according to claim 1 , wherein the oxidation catalyst is an oxide or hydroxide of at least one metal selected from the first transition metal.
6. The method according to claim 1 or 2, wherein the oxidation catalyst is at least one metal oxide or metal hydroxide selected from manganese oxide +2, manganese oxide +3, manganese oxide +4, iron oxide +2, iron oxide +3, cobalt hydroxide +2, cobalt hydroxide +3 and nickel oxide +2, nickel oxide +3, nickel oxide +4.
7. A method for electrolyzing water, comprising: At least water is supplied to an electrolytic cell including a solid polymer electrolyte membrane and an anode and a cathode, wherein the anode and the cathode are arranged so as to sandwich the solid polymer electrolyte membrane. applying a driving potential P between the anode and the cathode, thereby generating oxygen from the anode, An oxidation catalyst containing at least one first transition metal is present on at least a portion of the surface of the anode, The oxidation catalyst is manganese oxide, and P satisfies 1.65V<P<1.75V relative to the hydrogen electrode, ie, RHE.
8. A device for electrolyzing water, comprising: Solid polymer electrolyte membrane, an anode and a cathode arranged so as to sandwich the solid polymer electrolyte membrane, a power supply unit for applying a driving potential between the anode and the cathode, and A control unit for controlling the driving potential to be P, An oxidation catalyst containing at least one first transition metal is present on at least a portion of the surface of the anode, The amount of oxygen generated from the anode is plotted against the potential between the anode and the cathode to obtain a first curve. The second curve is obtained by plotting the index of the amount of dissolved chemical substances originating from the oxidation catalyst against the potential between the anode and the cathode. The driving potential P is determined based on the comparison between the first curve and the second curve. The driving potential P satisfies P1<P<P2, where P1 represents the lowest potential at which oxygen is generated from the anode, P2 represents the lowest potential P2 at which the indicator of the amount of dissolved chemical substances originating from the oxidation catalyst begins to show potential dependence, The water electrolysis device further includes a measuring means for measuring in-situ an index of the amount of dissolved chemical substances derived from the oxidation catalyst, and the control unit controls P based on the index value of the amount detected by the measuring means.
9. The device according to claim 8, wherein the indicator of the quantity is an intensity I of an absorption peak attributable to the chemical substance. 10 . The device according to claim 8 , wherein the first transition metal is at least one metal selected from the group consisting of manganese, iron, cobalt, and nickel. 11 . The device according to claim 8 , wherein the oxidation catalyst is an oxide or hydroxide of at least one metal selected from the first transition metal.
12. The device according to claim 8, wherein the oxidation catalyst is at least one metal oxide or metal hydroxide selected from manganese oxide +2, manganese oxide +3, manganese oxide +4, iron oxide +2, iron oxide +3, cobalt hydroxide +2, cobalt hydroxide +3 and nickel oxide +2, nickel oxide +3, nickel oxide +4.
13. The device according to claim 8 or 9, The oxidation catalyst is an oxidation catalyst of a spinel-type composite oxide containing cobalt and manganese.
Citation Information
Patent Citations
Process for isolating rubbers
EP0002015A1
Apparatus for recovering the waste heat of a supercharged internal combustion engine
EP0015208A1
Porous MnCo2O4 and preparation method and application
CN105396599A
Oxygen evolution with improved Mn stabilized catalyst
US4289591A