A modified acrylic emulsion and preparation method thereof

By introducing silicone polyurea dispersion into acrylic emulsion, the problems of insufficient ductility, adhesion and corrosion resistance of acrylic emulsion in industrial anti-corrosion coatings are solved, and the high water resistance and salt spray resistance of the modified acrylic emulsion are achieved. and improved mechanical properties, suitable for coatings with high protective requirements.

CN114085330BActive Publication Date: 2024-10-18GUANGZHOU JOINTAS CHEM
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111371656.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-18
Publication Date
2024-10-18
Estimated Expiration
2041-11-18

AI Technical Summary

Technical Problem

Existing acrylic emulsions have insufficient ductility, adhesion, wear resistance and corrosion resistance in the field of industrial anti-corrosion coatings. In addition, pre-emulsion instability, excessive alkali thickening, poor solvent compatibility and storage problems exist during resin preparation and performance optimization. Poor stability problem.

Method used

Using silicone polyurea modified acrylic emulsion, by introducing silicone polyurea dispersion, using its hydrophobic polysiloxane, polyether segment, urea group and thiourea group characteristics to improve the density and adhesion of the paint film , water resistance and chemical resistance, enhanced adhesion to metal substrates.

Benefits of technology

It significantly improves the water resistance, salt spray resistance, adhesion, mechanical properties and chemical resistance of the paint, enhances the cohesive strength and water repellency of the paint film, and is suitable for single-component water-based paints with high protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure BDA0003362540750000041
    Figure BDA0003362540750000041
  • Figure BDA0003362540750000171
    Figure BDA0003362540750000171
Patent Text Reader

Abstract

The invention discloses a modified acrylic emulsion and a preparation method thereof. The modified acrylic emulsion comprises the following raw materials in terms of mass percentage: 10% to 35% of alkyl acrylate, 2% to 25% of alkyl methacrylate, 0.2% to 2% of methacrylic acid, 5% to 30% of non-acrylate vinyl monomer, 1% to 10% of organosilicon polyurea dispersion, 0.1% to 1.5% of emulsifier, 0.1% to 1.5% of initiator, 30% to 75% of water, 0.02% to 0.5% of buffer, and 0.5% to 6% of pH regulator. The organosilicon polyurea dispersion of the invention has amphiphilicity and has carbon-carbon double bonds, which helps to reduce the amount of emulsifier used in emulsion polymerization and improve the water resistance and salt spray resistance of the paint film. In addition, silicone polyurea is introduced into the acrylic resin molecule, and the characteristics of polysiloxane, polyether segment, urea group, thiourea group and sulfonic acid group in the silicone polyurea structure are utilized to make the paint film have excellent adhesion, salt spray resistance, impact resistance, water resistance and acetone wiping resistance. It is suitable for one-component water-based paint with high anti-corrosion requirements (C3) and has high cost performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of industrial anticorrosive coatings, and particularly relates to a modified acrylic emulsion and a preparation method thereof. Background Art

[0002] Faced with the increasingly severe environmental situation and changes in market demand, the research and development technology of water-based resins has become more mature, and the performance of water-based coatings has become more multifunctional and high-performance. Among them, water-based industrial anti-corrosion coatings have developed rapidly, and their performance can meet the requirements of light anti-corrosion paints. The market share has gradually increased and has become an indispensable coating product in industrial fields such as steel structures, machinery, bridges, and petrochemical equipment, especially in the field of light anti-corrosion.

[0003] Due to its high cost-effectiveness, acrylic emulsions have gradually entered the field of industrial anti-corrosion coatings. Single-component acrylic emulsions have good gloss, hardness, water resistance and stain resistance, but their ductility, adhesion, wear resistance and corrosion resistance are average. How to improve the film density and adhesion to metal substrates is the key problem that acrylic emulsions for anti-corrosion coatings must solve. At present, in addition to the design of latex particle structure and glass transition temperature, some functional monomers are often selected to improve the adhesion and cross-linking density of the paint film, such as N-hydroxymethyl acrylamide, phosphate esters, glycidyl methacrylate, vinyl siloxane and ketone hydrazine. However, the effects of these technical solutions are not very good, and usually have some negative effects on the preparation and performance of the resin, such as pre-emulsion instability, excessive alkali thickening, poor compatibility with solvents, poor water resistance and storage stability, etc. To improve the protective performance of the coating, it is necessary not only to ensure that the resin forms a dense paint film during the film-forming process, with good cross-linking density and good adhesion to the metal substrate, but also to increase the effective contact interface between the resin and the metal substrate, reduce the internal stress generated by the resin during the film-forming process, and improve the water repellency of the paint film. Summary of the invention

[0004] The present invention aims to provide a modified acrylic emulsion and a preparation method thereof to solve the above-mentioned deficiencies of the prior art. The present invention utilizes silicone polyurea to modify acrylic emulsion to improve the water resistance, salt spray resistance, density, adhesion, mechanical properties, chemical resistance and acetone wiping resistance of the paint film.

[0005] To achieve the above-mentioned purpose, the technical scheme adopted by the present invention is as follows: a modified acrylic emulsion comprises the following component raw materials in percentage by weight: 10% to 35% of alkyl acrylate, 2% to 25% of alkyl methacrylate, 0.2% to 2% of methacrylic acid, 5% to 30% of non-acrylate vinyl monomer, 1% to 10% of silicone polyurea dispersion, 0.1% to 1.5% of emulsifier, 0.1% to 1.5% of initiator, 30% to 75% of water, 0.02% to 0.5% of buffer, and 0.5% to 6% of pH adjuster.

[0006] The organosilicon polyurea dispersion of the present invention is amphiphilic and has carbon-carbon double bonds. It is a reactive functional polymer that helps reduce the amount of emulsifier used in emulsion polymerization and improves the water resistance and salt spray resistance of the paint film. The present invention introduces organosilicon polyurea into the molecular skeleton of acrylic resin, and utilizes the characteristics of polysiloxane, polyether segment, urea group, thiourea group and sulfonic acid group in the structure of organosilicon polyurea dispersion to give the emulsion unique wetting ability and excellent cohesive strength and film-forming density of the paint film, so that the paint film has excellent adhesion, salt spray resistance, impact resistance, water resistance and acetone wiping resistance, etc., and is suitable for single-component water-based paints with high anti-corrosion requirements (C3), and has high cost performance.

[0007] As a preferred embodiment of the present invention, the modified acrylic emulsion includes the following component raw materials in percentage by weight: 15% to 25% of alkyl acrylate, 5% to 20% of alkyl methacrylate, 0.2% to 1% of methacrylic acid, 10% to 25% of non-acrylate vinyl monomer, 1% to 6% of silicone polyurea dispersion, 0.1% to 1% of emulsifier, 0.1% to 0.8% of initiator, 40% to 65% of deionized water, 0.02% to 0.2% of buffer, and 1% to 5% of pH adjuster.

[0008] The present invention is verified through a large number of experiments that when the components of the modified acrylic emulsion are in the above ratios, the coating prepared from the modified acrylic emulsion has optimal adhesion, salt spray resistance, impact resistance, water resistance, acetone wiping resistance and stability.

[0009] As a preferred embodiment of the present invention, the silicone polyurea dispersion comprises the following component raw materials in percentage by weight: 5% to 35% polyisocyanate, 10% to 45% aminopropyl polysiloxane, 3% to 25% terminal amino polyether, 0.2% to 10% small molecule diamine, 1% to 10% monoamino-terminated monomer, 5% to 30% solvent, and 30% to 70% deionized water.

[0010] The organosilicon polyurea dispersion of the present invention is prepared by the above raw materials, and contains polysiloxane with excellent hydrophobicity, polyether segments with high flexibility, polar urea groups and thiourea groups, and hydrophilic sulfonic acid groups in the molecular structure. Therefore, the acrylic emulsion is grafted with organopolysiloxane segments and polyether segments, which reduces the surface tension of the emulsion, improves the wettability of the emulsion to the metal substrate, increases the effective contact area between the paint film and the metal substrate, and is conducive to improving the compactness and adhesion of the paint film. At the same time, the hydrophobic organopolysiloxane segment also improves the water repellency and water resistance of the paint film. In the film-forming process of the emulsion, the urea group and the thiourea group can not only form hydrogen bonds within and between molecules, making the network structure of the polymer more solid and the cohesive strength of the paint film greater, but also can generate interaction forces with the polar groups on the metal substrate, improve the adhesion of the paint film to the metal substrate, thereby improving the physical and mechanical properties and chemical resistance of the paint film, especially the adhesion and acetone wiping resistance.

[0011] As a preferred embodiment of the present invention, the organosilicon polyurea dispersion comprises the following component raw materials in percentage by weight: 8% to 20% polyisocyanate, 15% to 35% aminopropyl polysiloxane, 5% to 18% terminal amino polyether, 0.5% to 5% small molecule diamine, 1.5% to 5% monoamino-terminated monomer, 5% to 20% solvent, and 35% to 60% deionized water.

[0012] As a preferred embodiment of the present invention, the method for preparing the silicone polyurea dispersion comprises the following steps:

[0013] (1) adding a solvent, aminopropyl polysiloxane, terminal amino polyether and a small molecule diamine into different containers, heating to 95-100° C., and vacuum dehydrating for 60-90 minutes;

[0014] (2) adding the solvent obtained in step (1), aminopropyl polysiloxane, amino-terminated polyetheramine and small molecule diamine to the reactor in sequence, and dropping polyisocyanate under nitrogen atmosphere and stirring at room temperature, and reacting for 30 to 60 minutes after the dropwise addition is completed to obtain a silicone polyurea prepolymer;

[0015] (3) After mixing the monoamino-terminated monomer with 10% water, add it to the silicone polyurea prepolymer and react at room temperature for 60 minutes. Then, add 90% water while stirring and continue stirring for 15 minutes to 20 minutes to obtain the silicone polyurea dispersion.

[0016] As a preferred embodiment of the present invention, the polyisocyanate is a difunctional isocyanate or a mixture of a difunctional isocyanate and a trifunctional isocyanate; the difunctional isocyanate is at least one of isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane dimethylene diisocyanate, toluene diisocyanate, 1,4-cyclohexane diisocyanate, xylylene diisocyanate, and tetramethylxylylene diisocyanate; the trifunctional isocyanate is at least one of hexamethylene diisocyanate trimer and isophorone diisocyanate trimer; the molar ratio of the polyisocyanate to aminopropyl polysiloxane is 2:1 to 4.5:1, and the trifunctional isocyanate is not more than 2% of the total mass of the polyisocyanate, aminopropyl polysiloxane, amino-terminated polyether, small molecule diamine and monoamino-terminated monomer.

[0017] More preferably, the trifunctional isocyanate is not higher than 1.5% of the total mass of the polyisocyanate, aminopropyl polysiloxane, amino-terminated polyether, small molecule diamine and monoamino-terminated monomer.

[0018] As a preferred embodiment of the present invention, the molar ratio of the polyisocyanate to the aminopropyl polysiloxane is 2:1 to 4.5:1; more preferably, the molar ratio of the polyisocyanate to the aminopropyl polysiloxane is 2:1 to 4:1.

[0019] As a preferred embodiment of the present invention, the number average molecular weight of the aminopropyl polysiloxane is 1000-2000; the number average molecular weight of the amino-terminated polyether is 300-1000, and the structural unit formula of the amino-terminated polyether is as follows:

[0020]

[0021] As a preferred embodiment of the present invention, the small molecule diamine is ethylenediamine, isophoronediamine, hexamethylenediamine, trimethylhexamethylenediamine, or 1,3-cyclohexylamine.

[0022] As a preferred embodiment of the present invention, the monoamino-terminated monomer is a mixture A or a mixture B, wherein the mixture A is a mixture of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and allylthiourea, and the mixture B is a mixture of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt, allylthiourea and a monoamino-terminated monomer A, wherein the monoamino-terminated monomer A is at least one of n-hexylamine and cyclohexylamine.

[0023] The 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and allylthiourea are functional monomers, and hydrophilic sulfonic acid groups and unsaturated carbon-carbon double bonds are introduced into the molecular skeleton of the silicone polyurea dispersion respectively. The 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and allylthiourea are added into the reaction system in the form of aqueous solution.

[0024] As a preferred embodiment of the method for preparing the silicone polyurea dispersion of the present invention, in the step (3), if the monoamino-terminated monomer is mixture A, mixture A is mixed with 10% of water and then added to the silicone polyurea prepolymer for reaction at room temperature; if the monoamino-terminated monomer is mixture B, the monoamino-terminated monomer A is first added to the silicone polyurea prepolymer, and then 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and 10% of allylthiourea water are mixed and then added to the silicone polyurea prepolymer for reaction.

[0025] As a preferred embodiment of the present invention, the molar amount of the allylthiourea is 30% to 60% of the molar amount of -NCO in the silicone polyurea prepolymer; more preferably, the molar amount of the allylthiourea is 30% to 50% of the molar amount of -NCO in the silicone polyurea prepolymer.

[0026] As a preferred embodiment of the present invention, the solvent is at least one of ethylene glycol butyl ether acetate, ethylene glycol ethyl ether acetate, propylene glycol methyl ether acetate, and propylene glycol diacetate.

[0027] The solvent used in the synthesis of silicone polyurea is a commonly used film-forming aid for water-based coatings and has low toxicity. The use of the silicone polyurea to modify acrylic emulsion reduces the amount of organic solvent used in the paint making stage.

[0028] As a preferred embodiment of the present invention, the alkyl acrylate is at least one of butyl acrylate, isooctyl acrylate, cyclohexyl acrylate, lauryl acrylate, and isobornyl acrylate; the alkyl methacrylate is at least one of methyl methacrylate, glycidyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, acetoacetoxyethyl methacrylate, and butyl methacrylate.

[0029] As a preferred embodiment of the present invention, the non-acrylic vinyl monomer is at least one of styrene, vinyl versatate, vinyl siloxane, acrylamide, diacetone acrylamide, and N-hydroxyethyl acrylamide.

[0030] As a preferred embodiment of the present invention, the emulsifier is at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, and sodium dodecyl diphenyl ether disulfonate; the initiator is ammonium persulfate; the buffer is sodium bicarbonate; and the pH adjuster is at least one of ammonia water, N,N-dimethylethanolamine, and AMP-95.

[0031] The preparation method of the modified acrylic emulsion of the present invention comprises the following steps:

[0032] (1) 23% to 47% of alkyl methacrylate, 7% to 13% of alkyl acrylate, 15% to 32% of non-acrylate vinyl monomer, 31% of emulsifier and 16% of deionized water are mixed and stirred to obtain a core pre-emulsion; silicone polyurea dispersion, 31% of emulsifier, 53% to 77% of alkyl methacrylate, 87% to 93% of alkyl acrylate, 68% to 85% of non-acrylate vinyl monomer and 42% of water are mixed and stirred to obtain a shell pre-emulsion; 40% of initiator and 10% of water are mixed and stirred to obtain an initiator solution;

[0033] (2) Add 30% water, buffer and 38% emulsifier to the reactor and stir evenly. When the temperature is raised to 40°C, take 2% to 6% of the nuclear pre-emulsion as the seed emulsion and add it to the reactor. Continue to raise the temperature to 85°C, then add 60% of the initiator and 2% of the mixture to the reactor. After the solution in the reactor turns blue, keep it warm for 20 minutes, then start to add the nuclear pre-emulsion and 20% of the initiator solution, and keep it warm for 30 minutes.

[0034] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added and kept warm for 120 minutes, then the temperature is lowered to 50° C., a pH adjuster is added to adjust the pH value of the emulsion to 8-9, and the modified acrylic emulsion is obtained by filtration.

[0035] As a preferred embodiment of the present invention, in the step (2), the core pre-emulsion and the initiator solution are added dropwise for 50-70 min; in the step (3), the shell pre-emulsion and the initiator solution are added dropwise for 120-170 min.

[0036] Compared with the prior art, the present invention has the following beneficial effects: the molecular structure of the organosilicon polyurea dispersion of the present invention contains polysiloxane with excellent hydrophobicity, polyether segments with high flexibility, polar urea groups and thiourea groups, and hydrophilic sulfonic acid groups. Therefore, the acrylic emulsion of the present invention is grafted with organopolysiloxane segments and polyether segments, which reduces the surface tension of the emulsion, improves the wettability of the emulsion to the metal substrate, increases the effective contact area between the paint film and the metal substrate, and is conducive to improving the compactness and adhesion of the paint film. At the same time, the hydrophobic organopolysiloxane segment also improves the water repellency and water resistance of the paint film. In the film-forming process of the emulsion, the urea group and the thiourea group can not only form hydrogen bonds within and between molecules, making the network structure of the polymer more solid and the cohesive strength of the paint film greater, but also can generate interaction forces with the polar groups on the metal substrate, improve the adhesion of the paint film to the metal substrate, thereby improving the physical and mechanical properties and chemical resistance of the paint film, especially the adhesion and acetone wiping resistance. DETAILED DESCRIPTION

[0037] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0038] In the embodiments and comparative examples, the aminopropyl polysiloxane 1000 is an aminopropyl polysiloxane with a number average molecular weight of 1000; the aminopropyl polysiloxane 1500 is an aminopropyl polysiloxane with a number average molecular weight of 1500; the aminopropyl polysiloxane 2000 is an aminopropyl polysiloxane with a number average molecular weight of 2000; the amino-terminated polyether 700 is an amino-terminated polyether with a number average molecular weight of 700; the amino-terminated polyether 400 is an amino-terminated polyether with a number average molecular weight of 400; the amino-terminated polyether 600 is an amino-terminated polyether with a number average molecular weight of 600; and the amino-terminated polyether 500 is an amino-terminated polyether with a number average molecular weight of 500.

[0039] Example 1

[0040] The preparation method of the silicone polyurea dispersion described in this embodiment comprises the following steps:

[0041] (1) Ethylene glycol butyl ether acetate, aminopropyl polysiloxane 1000, amino-terminated polyether 700 and 1,3-cyclohexylamine were added into four different flasks respectively, heated to 100°C, and vacuum dehydrated for 60 minutes;

[0042] (2) 54.2 g of ethylene glycol butyl ether acetate, 150 g of aminopropyl polysiloxane 1000, 52.5 g of amino-terminated polyether 700 and 5 g of 1,3-cyclohexylamine obtained in step (2) were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium-speed stirring, 50.7 g of hexamethylene diisocyanate was slowly added dropwise, and the reaction was allowed to proceed for 40 minutes after the addition was completed;

[0043] (3) 4.7 g of allylthiourea and 8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.8 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0044] (4) Under high-speed stirring, 249.2 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0045] The preparation method of the modified acrylic emulsion comprises the following steps:

[0046] (1) 5.8 g of methyl methacrylate, 3.4 g of isooctyl acrylate, 10.8 g of styrene, 0.2 g of sodium dodecylbenzene sulfonate and 16.8 g of deionized water are used to prepare a core pre-emulsion; 5 g of silicone polyurea dispersion, 0.2 g of sodium dodecylbenzene sulfonate, 5 g of methyl methacrylate, 26 g of butyl acrylate, 9 g of isooctyl acrylate, 0.5 g of methacrylic acid, 37.5 g of styrene, 2 g of acetoacetoxyethyl methacrylate and 44.1 g of deionized water are used to prepare a shell pre-emulsion; 0.14 g of ammonium persulfate and 10.5 g of deionized water are added to prepare an initiator solution;

[0047] (2) Add 31.5 g of deionized water, NaHCO3 and 0.25 g of sodium dodecylbenzene sulfonate to the reactor, stir evenly, and when the temperature is raised to 40° C., take part of the nuclear pre-emulsion as the seed emulsion and add it to the reactor, continue to raise the temperature to 85° C., add 0.2 g of ammonium persulfate and 2.1 g of deionized water, and keep the temperature for 20 min after the seeds turn blue. Then, start to drop the nuclear pre-emulsion and 20% initiator solution, and add them all over in 60 min. Keep the temperature for 30 min.

[0048] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added dropwise, and the addition is completed within 150 minutes, and the heat preservation is carried out for 120 minutes;

[0049] (4) Cooling to 50° C., adding ammonia water until the pH value of the emulsion is 8-9, and filtering to obtain a silicone polyurea modified acrylic emulsion.

[0050] Example 2

[0051] The preparation method of the silicone polyurea dispersion described in this embodiment comprises the following steps:

[0052] (1) A certain amount of propylene glycol methyl ether acetate, aminopropyl polysiloxane 1500, amino-terminated polyether 400, trimethylhexanediamine and 1,3-cyclohexylamine were added to 5 different flasks respectively, heated to 100°C, and vacuum dehydrated for 60 minutes;

[0053] (2) 54.7 g of propylene glycol methyl ether acetate, 150 g of aminopropyl polysiloxane 1500, 30 g of amino-terminated polyether 400, 7.9 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium speed stirring, 65.2 g of isophorone diisocyanate and 3 g of hexamethylene diisocyanate trimer were slowly added dropwise, and the reaction was carried out for 40 minutes after the addition was completed;

[0054] (3) 4.7 g of allyl thiourea and 8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 14 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0055] (4) Under high-speed stirring, 251.9 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0056] The preparation method of the modified acrylic emulsion comprises the following steps:

[0057] (1) 5 g of methyl methacrylate, 4 g of butyl acrylate, 11 g of styrene, 0.2 g of sodium dodecylbenzene sulfonate and 16.8 g of deionized water are used to prepare a core pre-emulsion; 5 g of silicone polyurea dispersion, 0.2 g of sodium dodecylbenzene sulfonate, 4.5 g of methyl methacrylate, 26 g of butyl acrylate, 9 g of isooctyl acrylate, 0.5 g of methacrylic acid, 38 g of styrene, 2 g of acetoacetoxyethyl methacrylate and 44.1 g of deionized water are used to prepare a shell pre-emulsion; 0.14 g of ammonium persulfate and 10.5 g of deionized water are added to prepare an initiator solution;

[0058] (2) Add 31.5 g of deionized water, NaHCO3 and 0.25 g of sodium dodecylbenzene sulfonate to the reactor, stir evenly, and when the temperature is raised to 40° C., take part of the nuclear pre-emulsion as the seed emulsion and add it to the reactor, continue to raise the temperature to 85° C., add 0.2 g of ammonium persulfate and 2.1 g of deionized water, and keep the temperature for 20 min after the seeds turn blue. Then, start to drop the nuclear pre-emulsion and 20% initiator solution, and add them all over in 60 min. Keep the temperature for 30 min.

[0059] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added dropwise, and the addition is completed within 150 minutes, and the heat preservation is carried out for 120 minutes;

[0060] (4) Cooling to 50° C., adding ammonia water until the pH value of the emulsion is 8-9, and filtering to obtain a silicone polyurea modified acrylic emulsion.

[0061] Example 3

[0062] The preparation method of the silicone polyurea dispersion described in this embodiment comprises the following steps:

[0063] (1) A certain amount of ethylene glycol ethyl ether acetate, aminopropyl polysiloxane 2000, amino-terminated polyether 400, trimethylhexanediamine and 1,3-cyclohexylamine were added to 5 different flasks respectively, heated to 100°C, and vacuum dehydrated for 60 minutes;

[0064] (2) 52.4 g of ethylene glycol ethyl ether acetate, 150 g of aminopropyl polysiloxane 2000, 30 g of amino-terminated polyether 400, 11.9 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium-speed stirring, 52.5 g of toluene diisocyanate was slowly added dropwise, and the reaction was allowed to proceed for 40 min after the addition was completed;

[0065] (3) 8 g of allylthiourea and 4.7 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.4 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0066] (4) Under high-speed stirring, 241.1 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0067] The preparation method of the modified acrylic emulsion comprises the following steps:

[0068] (1) 10 g of methyl methacrylate, 2 g of butyl acrylate, 6.2 g of styrene, 1.8 g of isooctyl acrylate, 0.2 g of sodium dodecylbenzene sulfonate and 16.8 g of deionized water are used to prepare a core pre-emulsion; 5 g of silicone polyurea dispersion, 0.2 g of sodium dodecylbenzene sulfonate, 19.5 g of methyl methacrylate, 25 g of butyl acrylate, 10 g of isooctyl acrylate, 0.5 g of methacrylic acid, 20 g of styrene, 3 g of tert-butyl carbonate, 2 g of acetoacetoxyethyl methacrylate and 44.1 g of deionized water are used to prepare a shell pre-emulsion; 0.14 g of ammonium persulfate is added to 10.5 g of deionized water to prepare an initiator solution;

[0069] (2) Add 31.5 g of deionized water, NaHCO3 and 0.25 g of sodium dodecylbenzene sulfonate to the reactor, stir evenly, and when the temperature is raised to 40° C., take part of the nuclear pre-emulsion as the seed emulsion and add it to the reactor, continue to raise the temperature to 85° C., add 0.2 g of ammonium persulfate and 2.1 g of deionized water, and keep the temperature for 20 min after the seeds turn blue. Then, start to drop the nuclear pre-emulsion and 20% initiator solution, and add them all over in 60 min. Keep the temperature for 30 min.

[0070] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added dropwise, and the addition is completed within 150 minutes, and the heat preservation is carried out for 120 minutes;

[0071] (4) Cooling to 50° C., adding ammonia water until the pH value of the emulsion is 8-9, and filtering to obtain a silicone polyurea modified acrylic emulsion.

[0072] Example 4

[0073] The preparation method of the silicone polyurea dispersion described in this embodiment comprises the following steps:

[0074] (1) A certain amount of propylene glycol methyl ether acetate, aminopropyl polysiloxane 2000, amino-terminated polyether 600, trimethylhexanediamine and 1,3-cyclohexylamine were added to 5 different flasks respectively, the temperature was raised to 100°C, and vacuum dehydration was performed for 60 minutes;

[0075] (2) 56.9 g of propylene glycol methyl ether acetate, 133.4 g of aminopropyl polysiloxane 2000, 40 g of amino-terminated polyether 600, 14.4 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium-speed stirring, 78.9 g of dicyclohexylmethane diisocyanate was slowly added dropwise, and the reaction was allowed to proceed for 40 min after the addition was completed;

[0076] (3) 4.7 g of allylthiourea, 8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and 14.5 g of deionized water were mixed and added to the reactor in sequence, and reacted at room temperature for 60 min;

[0077] (4) Under high-speed stirring, 261.6 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0078] The preparation method of the modified acrylic emulsion comprises the following steps:

[0079] (1) 8.1 g of methyl methacrylate, 2.4 g of butyl acrylate, 8.1 g of styrene, 1.4 g of isooctyl acrylate, 0.2 g of sodium dodecylbenzene sulfonate and 16.8 g of deionized water are used to prepare a core pre-emulsion; 5 g of silicone polyurea dispersion, 0.2 g of sodium dodecylbenzene sulfonate, 19 g of methyl methacrylate, 36.5 g of butyl acrylate, 0.5 g of methacrylic acid, 19 g of styrene, 3 g of versatate, 2 g of acetoacetoxyethyl methacrylate and 44.1 g of deionized water are used to prepare a shell pre-emulsion; 0.14 g of ammonium persulfate and 10.5 g of deionized water are added to prepare an initiator solution;

[0080] (2) Add 31.5 g of deionized water, NaHCO3 and 0.25 g of sodium dodecylbenzene sulfonate to the reactor, stir evenly, and when the temperature is raised to 40° C., take part of the nuclear pre-emulsion as the seed emulsion and add it to the reactor, continue to raise the temperature to 85° C., add 0.2 g of ammonium persulfate and 2.1 g of deionized water, and keep the temperature for 20 min after the seeds turn blue. Then, start to drop the nuclear pre-emulsion and 20% initiator solution, and add them in about 60 min. Keep the temperature for 30 min.

[0081] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added dropwise, and the addition is completed in about 150 minutes, and the heat preservation is carried out for 120 minutes;

[0082] (4) Cooling to 50° C., adding ammonia water until the pH value of the emulsion is 8-9, and filtering to obtain a silicone polyurea modified acrylic emulsion.

[0083] Example 5

[0084] The preparation method of the silicone polyurea dispersion described in this embodiment comprises the following steps:

[0085] (1) A certain amount of propylene glycol methyl ether acetate, aminopropyl polysiloxane 1000, amino-terminated polyether 1000, trimethylhexanediamine, 1,3-cyclohexylamine and n-hexylamine were added to 6 different flasks respectively, the temperature was raised to 100°C, and vacuum dehydration was performed for 60 minutes;

[0086] (2) 53.5 g of propylene glycol methyl ether acetate, 100 g of aminopropyl polysiloxane 1000, 75 g of amino-terminated polyether 1000, 7.9 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium speed stirring, 67 g of isophorone diisocyanate was slowly added dropwise, and the reaction was allowed to proceed for 40 min after the addition was completed;

[0087] (3) 1.6 g of n-hexylamine was first added to the reactor, and 2.9 g of allyl thiourea and 8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.7 g of deionized water, and then water was added to the reactor in sequence, and the reaction was carried out at room temperature for 60 min;

[0088] (4) Under high-speed stirring, 246 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0089] The preparation method of the modified acrylic emulsion comprises the following steps:

[0090] (1) 7.5 g of methyl methacrylate, 1.8 g of butyl acrylate, 7.5 g of styrene, 1.8 g of isooctyl acrylate, 1.4 g of tert-butylene carbonate, 0.2 g of sodium dodecylbenzene sulfonate and 16.8 g of deionized water are used to prepare a core pre-emulsion; 5 g of silicone polyurea dispersion, 0.2 g of sodium dodecylbenzene sulfonate, 19 g of methyl methacrylate, 35 g of butyl acrylate, 0.5 g of methacrylic acid, 20.5 g of styrene, 1 g of isooctyl acrylate, 2 g of cyclohexyl methacrylate, 2 g of acetoacetoxyethyl methacrylate and 44.1 g of deionized water are used to prepare a shell pre-emulsion; 0.14 g of ammonium persulfate and 10.5 g of deionized water are added to prepare an initiator solution;

[0091] (2) Add 31.5 g of deionized water, NaHCO3 and 0.25 g of sodium dodecylbenzene sulfonate to the reactor, stir evenly, and when the temperature is raised to 40° C., take part of the nuclear pre-emulsion as the seed emulsion and add it to the reactor, continue to raise the temperature to 85° C., add 0.2 g of ammonium persulfate and 2.1 g of deionized water, and keep the temperature for 20 min after the seeds turn blue. Then, start to drop the nuclear pre-emulsion and 20% initiator solution, and add them all over in 60 min. Keep the temperature for 30 min.

[0092] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added dropwise, and the addition is completed within 150 minutes, and the heat preservation is carried out for 120 minutes;

[0093] (4) Cooling to 50° C., adding ammonia water until the pH value of the emulsion is 8-9, and filtering to obtain a silicone polyurea modified acrylic emulsion.

[0094] Example 6

[0095] The preparation method of the silicone polyurea dispersion described in this embodiment comprises the following steps:

[0096] (1) A certain amount of propylene glycol methyl ether acetate, aminopropyl polysiloxane 1000, amino-terminated polyether 500, trimethylhexanediamine, 1,3-cyclohexylamine and n-hexylamine were added to 6 different flasks respectively, the temperature was raised to 100°C, and vacuum dehydration was performed for 60 minutes;

[0097] (2) 56 g of propylene glycol methyl ether acetate, 150 g of aminopropyl polysiloxane 1000, 37.5 g of amino-terminated polyether 500, 7.9 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium speed stirring, 67 g of isophorone diisocyanate was slowly added dropwise, and the reaction was carried out for 40 minutes after the addition was completed;

[0098] (3) 0.7 g of n-hexylamine was first added to the reactor, and 3.9 g of allyl thiourea and 8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 14.3 g of deionized water, and then water was added to the reactor in sequence, and the reaction was carried out at room temperature for 60 min;

[0099] (4) Under high-speed stirring, 257.6 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0100] The preparation method of the modified acrylic emulsion comprises the following steps:

[0101] (1) 10.2 g of methyl methacrylate, 1.9 g of butyl acrylate, 6 g of styrene, 1.9 g of isooctyl acrylate, 0.2 g of sodium dodecylbenzene sulfonate and 16.8 g of deionized water are used to prepare a core pre-emulsion; 5 g of silicone polyurea dispersion, 0.2 g of sodium dodecylbenzene sulfonate, 20 g of methyl methacrylate, 0.5 g of methacrylic acid, 24.3 g of styrene, 31.2 g of isooctyl acrylate, 2 g of cyclohexyl methacrylate, 2 g of acetoacetoxyethyl methacrylate and 44.1 g of deionized water are used to prepare a shell pre-emulsion; 0.14 g of ammonium persulfate and 10.5 g of deionized water are added to prepare an initiator solution;

[0102] (2) Add 31.5 g of deionized water, NaHCO3 and 0.25 g of sodium dodecylbenzene sulfonate to the reactor, stir evenly, and when the temperature is raised to 40° C., take part of the nuclear pre-emulsion as the seed emulsion and add it to the reactor, continue to raise the temperature to 85° C., add 0.2 g of ammonium persulfate and 2.1 g of deionized water, and keep the temperature for 20 min after the seeds turn blue. Then, start to drop the nuclear pre-emulsion and 20% initiator solution, and add them all over in 60 min. Keep the temperature for 30 min.

[0103] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added dropwise, and the addition is completed within 150 minutes, and the heat preservation is carried out for 120 minutes;

[0104] (4) Cooling to 50° C., adding ammonia water until the pH value of the emulsion is 8-9, and filtering to obtain a silicone polyurea modified acrylic emulsion.

[0105] Example 7

[0106] The preparation method of the silicone polyurea dispersion described in this embodiment comprises the following steps:

[0107] (1) A certain amount of ethylene glycol butyl ether acetate, aminopropyl polysiloxane 1500, amino-terminated polyether 400, trimethylhexanediamine and 1,3-cyclohexylamine were added to 5 different flasks respectively, heated to 100°C, and vacuum dehydrated for 60 minutes;

[0108] (2) 54.6 g of ethylene glycol butyl ether acetate, 150 g of aminopropyl polysiloxane 1500, 30 g of amino-terminated polyether 400, 7.2 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium-speed stirring, 67 g of isophorone diisocyanate was slowly added dropwise, and the reaction was carried out for 40 minutes after the addition was completed;

[0109] (3) 5.9 g of allyl thiourea and 7.8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.9 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0110] (4) Under high-speed stirring, 251.1 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0111] The preparation method of the modified acrylic emulsion comprises the following steps:

[0112] (1) 11 g of methyl methacrylate, 4 g of butyl acrylate, 5 g of styrene, 0.2 g of sodium dodecylbenzene sulfonate and 16.8 g of deionized water are used to prepare a core pre-emulsion; 5 g of silicone polyurea dispersion, 0.2 g of sodium dodecylbenzene sulfonate, 18 g of methyl methacrylate, 20.7 g of butyl acrylate, 0.5 g of methacrylic acid, 22.3 g of styrene, 13.5 g of isooctyl acrylate, 2 g of isobornyl methacrylate, 2 g of acetoacetoxyethyl methacrylate, 1 g of vinyl versatate, and 44.1 g of deionized water are used to prepare a shell pre-emulsion; 0.14 g of ammonium persulfate and 10.5 g of deionized water are added to prepare an initiator solution;

[0113] (2) Add 31.5 g of deionized water, NaHCO3 and 0.25 g of sodium dodecylbenzene sulfonate to the reactor, stir evenly, and when the temperature is raised to 40° C., take part of the nuclear pre-emulsion as the seed emulsion and add it to the reactor, continue to raise the temperature to 85° C., add 0.2 g of ammonium persulfate and 2.1 g of deionized water, and keep the temperature for 20 min after the seeds turn blue. Then, start to drop the nuclear pre-emulsion and 20% initiator solution, and add them all over in 60 min. Keep the temperature for 30 min.

[0114] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added dropwise, and the addition is completed within 150 minutes, and the heat preservation is carried out for 120 minutes;

[0115] (4) Cooling to 50° C., adding ammonia water until the pH value of the emulsion is 8-9, and filtering to obtain a silicone polyurea modified acrylic emulsion.

[0116] Example 8

[0117] The preparation method of the silicone polyurea dispersion described in this embodiment comprises the following steps:

[0118] (1) A certain amount of ethylene glycol ethyl ether acetate, aminopropyl polysiloxane 1500, amino-terminated polyether 400, trimethylhexanediamine and 1,3-cyclohexylamine were added to 5 different flasks respectively, heated to 100°C, and vacuum dehydrated for 60 minutes;

[0119] (2) 54.5 g of ethylene glycol ethyl ether acetate, 150 g of aminopropyl polysiloxane 1500, 30 g of amino-terminated polyether 400, 7.4 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium speed stirring, 67 g of isophorone diisocyanate was slowly added dropwise, and the reaction was carried out for 40 minutes after the addition was completed;

[0120] (3) 6.2 g of allyl thiourea and 6.8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.9 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0121] (4) Under high-speed stirring, 250.6 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0122] The preparation method of the modified acrylic emulsion comprises the following steps:

[0123] (1) 8 g of methyl methacrylate, 2 g of butyl acrylate, 7.8 g of styrene, 1.7 g of isooctyl acrylate, 0.5 g of isobornyl methacrylate, 0.2 g of sodium dodecylbenzene sulfonate, and 16.8 g of deionized water are used to prepare a core pre-emulsion; 5 g of silicone polyurea dispersion, 0.2 g of sodium dodecylbenzene sulfonate, 10.5 g of methyl methacrylate, 19.5 g of butyl acrylate, 0.5 g of methacrylic acid, 31 g of styrene, 14.5 g of isooctyl acrylate, 2 g of isobornyl methacrylate, 2 g of acetoacetoxyethyl methacrylate, and 44.1 g of deionized water are used to prepare a shell pre-emulsion; 0.14 g of ammonium persulfate and 10.5 g of deionized water are added to prepare an initiator solution;

[0124] (2) Add 31.5 g of deionized water, NaHCO3 and 0.25 g of sodium dodecylbenzene sulfonate to the reactor, stir evenly, and when the temperature is raised to 40° C., take part of the nuclear pre-emulsion as the seed emulsion and add it to the reactor, continue to raise the temperature to 85° C., add 0.2 g of ammonium persulfate and 2.1 g of deionized water, and keep the temperature for 20 min after the seeds turn blue. Then, start to drop the nuclear pre-emulsion and 20% initiator solution, and add them all over in 60 min. Keep the temperature for 30 min.

[0125] (3) After the heat preservation is completed, the shell pre-emulsion and 80% initiator solution are added dropwise, and the addition is completed within 150 minutes, and the heat preservation is carried out for 120 minutes;

[0126] (4) Cooling to 50° C., adding ammonia water until the pH value of the emulsion is 8-9, and filtering to obtain a silicone polyurea modified acrylic emulsion.

[0127] Comparative Example 1

[0128] The preparation method of the silicone polyurea dispersion in this comparative example comprises the following steps:

[0129] (1) A certain amount of propylene glycol diacetate, aminopropyl polysiloxane 1000 and amino-terminated polyether 400 were added to three different flasks respectively, heated to 100°C, and vacuum dehydrated for 60 minutes;

[0130] (2) 60.7 g of propylene glycol diacetate, 200 g of aminopropyl polysiloxane 1000 and 24.1 g of amino-terminated polyether 400 obtained in step (1) were added to the reactor in sequence, and then N2 was introduced. Under room temperature and medium-speed stirring, 67 g of isophorone diisocyanate was slowly added dropwise, and the reaction was allowed to proceed for 40 min after the addition was completed;

[0131] (3) 4.8 g of allyl thiourea and 7.8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 15.5 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0132] (4) Under high-speed stirring, 279.4 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0133] The preparation method of the modified acrylic emulsion in this comparative example is the same as that in Example 1.

[0134] Comparative Example 2

[0135] The preparation method of the silicone polyurea dispersion in this comparative example comprises the following steps:

[0136] (1) A certain amount of propylene glycol diacetate, aminopropyl polysiloxane 2000, amino-terminated polyether 600, trimethylhexanediamine and 1,3-cyclohexylamine were added to 5 different flasks respectively, heated to 100°C, and vacuum dehydrated for 60 minutes;

[0137] (2) 54.2 g of propylene glycol diacetate, 120 g of aminopropyl polysiloxane 2000, 45 g of amino-terminated polyether 600, 14.4 g of trimethylhexanediamine and 12 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium speed stirring, 67 g of isophorone diisocyanate was slowly added dropwise, and the reaction was carried out for 40 minutes after the addition was completed;

[0138] (3) 4.8 g of allyl thiourea and 7.8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.9 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0139] (4) Under high-speed stirring, 249.3 g of deionized water was slowly added to the reactor. After the addition of water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0140] The preparation method of the modified acrylic emulsion in this comparative example is the same as that in Example 4.

[0141] Comparative Example 3

[0142] The preparation method of the silicone polyurea dispersion in this comparative example comprises the following steps:

[0143] (1) A certain amount of propylene glycol methyl ether acetate, aminopropyl polysiloxane 1500, amino-terminated polyether 4000, trimethylhexanediamine, 1,3-cyclohexylamine and n-hexylamine were added to 6 different flasks respectively, the temperature was raised to 100°C, and vacuum dehydration was performed for 60 minutes;

[0144] (2) 54.4 g of propylene glycol methyl ether acetate, 150 g of aminopropyl polysiloxane 1500, 30 g of amino-terminated polyether 400, 7.9 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium speed stirring, 67 g of isophorone diisocyanate was slowly added dropwise, and the reaction was carried out for 40 minutes after the addition was completed;

[0145] (3) 2.15 g of n-hexylamine was first added to the reactor, and 2.4 g of allyl thiourea and 7.8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.9 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0146] (4) Slowly add 250.5% deionized water into the reactor under high-speed stirring. Continue stirring for 20 minutes after adding the water to obtain a silicone polyurea dispersion.

[0147] The preparation method of the modified acrylic emulsion in this comparative example is the same as that in Example 5.

[0148] Comparative Example 4

[0149] The preparation method of the silicone polyurea dispersion in this comparative example comprises the following steps:

[0150] (1) A certain amount of ethylene glycol ethyl ether acetate, aminopropyl polysiloxane 2000, amino-terminated polyether 400, trimethylhexanediamine and 1,3-cyclohexylamine were added to 5 different flasks respectively, heated to 100°C, and vacuum dehydrated for 60 minutes;

[0151] (2) 52.5 g of ethylene glycol ethyl ether acetate, 150 g of aminopropyl polysiloxane 2000, 30 g of amino-terminated polyether 400, 10.3 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium speed stirring, 52.5 g of toluene diisocyanate was slowly added dropwise, and the reaction was allowed to proceed for 40 min after the addition was completed;

[0152] (3) 7.6 g of allyl thiourea and 7.1 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.4 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0153] (4) Under high-speed stirring, 241.5 deionized water was slowly added to the reactor. After adding the water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0154] The preparation method of the modified acrylic emulsion in this comparative example is the same as that in Example 3.

[0155] Comparative Example 5

[0156] The preparation method of the silicone polyurea dispersion in this comparative example comprises the following steps:

[0157] (1) A certain amount of propylene glycol methyl ether acetate, aminopropyl polysiloxane 1500, amino-terminated polyether 400, trimethylhexanediamine and 1,3-cyclohexylamine were added to four different flasks respectively, the temperature was raised to 100°C, and vacuum dehydration was performed for 60 minutes;

[0158] (2) 55.1 g of propylene glycol methyl ether acetate, 150 g of aminopropyl polysiloxane 1500, 30 g of amino-terminated polyether 400, 7.9 g of trimethylhexanediamine and 5 g of 1,3-cyclohexylamine were added to the reactor in sequence, and then N2 was introduced. At room temperature and medium speed stirring, 63 g of isophorone diisocyanate and 6.8 g of hexamethylene diisocyanate trimer were slowly added dropwise, and the reaction was carried out for 40 minutes after the addition was completed;

[0159] (3) 4.8 g of allyl thiourea and 7.8 g of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt were mixed with 13.9 g of deionized water, and then added to the reactor in sequence, and reacted at room temperature for 60 min;

[0160] (4) Under high-speed stirring, 250.1 deionized water was slowly added to the reactor. After adding the water, stirring was continued for 20 minutes to obtain a silicone polyurea dispersion.

[0161] The preparation method of the modified acrylic emulsion in this comparative example is the same as that in Example 2.

[0162] Comparative Example 6

[0163] The only difference between the preparation method of the modified acrylic emulsion described in this comparative example and that of Example 1 is that no silicone polyurea dispersion is added to the shell pre-emulsion, and 0.8 g of sodium dodecylbenzene sulfonate is added to the shell emulsion.

[0164] Test example: performance test

[0165] The modified acrylic emulsions prepared in Examples 1-8 and Comparative Examples 1-6 were respectively formulated into bottom and top combined coatings according to Table 1 below, and then the performance tests were performed.

[0166] Table 1 Composition of coatings

[0167]

[0168]

[0169] Performance testing method:

[0170] Impact resistance test method: Determined in accordance with GB / T 1732-1993;

[0171] Cross-cut adhesion test method: Determined in accordance with GB / T9286-1998;

[0172] Pull-off adhesion test method: Determined in accordance with GB / T 5210-2006;

[0173] Early water resistance test method: Determined in accordance with HG / T 5176-2017;

[0174] Water resistance test method: Determined in accordance with GB / T 1733-1993;

[0175] Neutral salt spray resistance test method: Determined in accordance with GB / T 1771-2007;

[0176] Acetone wiping resistance test method: Determined in accordance with GB / T 23989-2009.

[0177] Table 2 Performance test results of coatings prepared from modified acrylic emulsions described in Examples 1-8

[0178]

[0179] Table 3 Performance test results of coatings prepared from modified acrylic emulsions described in Comparative Examples 1-6

[0180]

[0181]

[0182] According to the data comparison of Table 2 and Table 3, it is shown that the coating prepared by the modified acrylic emulsion of the present invention has excellent adhesion, salt spray resistance, impact resistance, water resistance and acetone wiping resistance, and also has storage stability. According to Comparative Example 1 compared with the embodiment, it is shown that the organosilicon polyurea dispersion prepared by the molar ratio of diisocyanate to aminopropyl polysiloxane is not within the scope of the present invention, which reduces the impact resistance, adhesion, water resistance, salt spray resistance and acetone wiping resistance of the coating. According to Comparative Examples 2-5, it is shown that the addition amount of polyisocyanate, allyl thiourea and aminopropyl polysiloxane has a great influence on the performance of the coating prepared by the present invention. Comparative Example 6 compared with Example 1, the organosilicon polyurea dispersion can improve the impact resistance, adhesion, water resistance and neutral salt spray resistance of the coating prepared by the modified acrylic emulsion.

[0183] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A modified acrylic emulsion, characterized in that: The raw materials include the following components in percentage by weight: alkyl acrylate 10%~35%, alkyl methacrylate 2%~25%, methacrylic acid 0.2%~2%, non-acrylate vinyl monomer 5%~30%, silicone polyurea dispersion 1%~10%, emulsifier 0.1%~1.5%, initiator 0.1%~1.5%, water 30%~75%, buffer 0.02%~0.5%, pH adjuster 0.5%~6%; The organosilicon polyurea dispersion comprises the following raw materials in percentage by weight: 5% to 35% polyisocyanate, 10% to 45% aminopropyl polysiloxane, 3% to 25% amino-terminated polyether, 0.2% to 10% small molecule diamine, 1% to 10% monoamino-terminated monomer, 5% to 30% solvent, and 30% to 70% deionized water; The molar ratio of the polyisocyanate to the aminopropyl polysiloxane is 2:1 to 4.5:1; The preparation method of the silicone polyurea dispersion comprises the following steps: (1) Add the solvent, aminopropyl polysiloxane, terminal amino polyether and small molecule diamine into different containers respectively, heat to 95-100°C, and vacuum dehydrate for 60-90 minutes; (2) adding the solvent obtained in step (1), aminopropyl polysiloxane, amino-terminated polyetheramine and small molecule diamine into the reactor in sequence, adding polyisocyanate dropwise under nitrogen atmosphere and stirring at room temperature, and reacting for 30 min to 60 min after the addition is completed to obtain silicone polyurea prepolymer; (3) After mixing the monoamino-terminated monomer with 10% deionized water, add it to the silicone polyurea prepolymer and react at room temperature for 60 minutes. Then, add 90% deionized water while stirring and continue stirring for 15 minutes to 20 minutes to obtain the silicone polyurea dispersion.

2. The modified acrylic emulsion according to claim 1, characterized in that The polyisocyanate is a difunctional isocyanate or a mixture of a difunctional isocyanate and a trifunctional isocyanate; the difunctional isocyanate is at least one of isophorone diisocyanate, hexamethylene diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane dimethylene diisocyanate, toluene diisocyanate, 1,4-cyclohexane diisocyanate, xylylene diisocyanate, and tetramethylxylylene diisocyanate; the trifunctional isocyanate is at least one of hexamethylene diisocyanate trimer and isophorone diisocyanate trimer; the trifunctional isocyanate is not more than 2% of the total mass of the polyisocyanate, aminopropyl polysiloxane, amino-terminated polyether, small molecule diamine, and monoamino-terminated monomer.

3. The modified acrylic emulsion according to claim 1, characterized in that The solvent is at least one of ethylene glycol butyl ether acetate, ethylene glycol ethyl ether acetate, propylene glycol methyl ether acetate, and propylene glycol diacetate; the number average molecular weight of the aminopropyl polysiloxane is 1000-2000; the number average molecular weight of the amino-terminated polyether is 300-1000, and the structural unit formula of the amino-terminated polyether is as follows: 。 4. The modified acrylic emulsion according to claim 1, characterized in that The small molecule diamine is ethylenediamine, isophoronediamine, hexamethylenediamine, trimethylhexamethylenediamine, and 1,3-cyclohexylamine; the monoamino-terminated monomer is a mixture A or a mixture B, wherein the mixture A is a mixture of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt and allylthiourea, and the mixture B is a mixture of 2-[(2-aminoethyl)amino]ethanesulfonic acid sodium salt, allylthiourea and monoamino-terminated monomer A, wherein the monoamino-terminated monomer A is at least one of n-hexylamine and cyclohexylamine; and the molar amount of the allylthiourea is 30% to 60% of the molar amount of -NCO in the silicone polyurea prepolymer.

5. The modified acrylic emulsion according to claim 1, characterized in that, The alkyl acrylate is at least one of butyl acrylate, isooctyl acrylate, cyclohexyl acrylate, lauryl acrylate, and isobornyl acrylate; the alkyl methacrylate is at least one of methyl methacrylate, glycidyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, acetoacetoxyethyl methacrylate, and butyl methacrylate; and the non-acrylic ester vinyl monomer is at least one of styrene, versatate vinyl carbonate, vinyl siloxane, acrylamide, diacetone acrylamide, and N-hydroxyethyl acrylamide.

6. The modified acrylic emulsion according to claim 1, characterized in that: The emulsifier is at least one of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, and sodium dodecyl diphenyl ether disulfonate; the initiator is ammonium persulfate; the buffer is sodium bicarbonate; and the pH adjuster is at least one of ammonia water, N,N-dimethylethanolamine, and AMP-95.

7. The method for preparing the modified acrylic emulsion according to claim 1, characterized in that: The steps include: (1) 23% to 47% of alkyl methacrylate, 7% to 13% of alkyl acrylate, 15% to 32% of non-acrylate vinyl monomer, 31% of emulsifier and 16% of water are mixed and stirred to obtain a core pre-emulsion; silicone polyurea dispersion, 31% of emulsifier, 53% to 77% of alkyl methacrylate, 87% to 93% of alkyl acrylate, 0.2% to 2% of methacrylic acid, 68% to 85% of non-acrylate vinyl monomer and 42% of water are mixed and stirred to obtain a shell pre-emulsion; 40% of initiator and 10% of water are mixed and stirred to obtain an initiator solution; (2) Add 30% water, buffer and 38% emulsifier to the reactor and stir evenly. When the temperature reaches 40°C, take 2%~6% of the nuclear pre-emulsion as the seed emulsion and add it to the reactor. Continue to heat it to 85°C, then mix 60% of the initiator and 2% of the water and add them to the reactor. After the solution in the reactor turns blue, keep it warm for 20 minutes, then start adding the nuclear pre-emulsion and 20% of the initiator solution, and keep it warm for 30 minutes. (3) After the heat preservation is completed, add the shell pre-emulsion and 80% initiator solution and keep the temperature for 120 minutes, then cool to 50°C, add pH adjuster to the pH value of the emulsion to 8-9, and filter to obtain the modified acrylic emulsion.

Citation Information

Patent Citations

  • Silicone modified acrylate hybrid emulsion and preparation method and application thereof

    CN102977253A

  • Polyuria-acrylate emulsion and aqueous gravure ink prepared from same

    CN103641962A