Semiconductor manufacturing method

By forming a multi-layer dielectric structure on the substrate and separating the deposition and etching processes, the trench size is gradually reduced, which solves the problems of high cost and complex process of small-sized deep trench isolation in the existing technology, and achieves efficient and low-cost Deep trench isolation improves the imaging quality of the image sensor.

CN114093763BActive Publication Date: 2024-10-18WUHAN XINXIN SEMICON MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111397145.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-23
Publication Date
2024-10-18
Estimated Expiration
2041-11-23

AI Technical Summary

Technical Problem

The existing technology has high costs and complicated process control when manufacturing small-sized deep trench isolation (DTI). It is difficult to effectively reduce the critical dimensions of the trench, which affects the imaging quality of the image sensor.

Method used

By forming a multi-layer dielectric structure on the substrate, layer-by-layer deposition and etching processes are separated, and the critical dimensions of the trench are gradually reduced. Gases such as C4F8, CF4, CO, O2, Ar2, and SF6 are used for deposition. and etching, combining O2 plasma ashing and oxalic acid wet etching to achieve low-cost, small-sized deep trench isolation.

Benefits of technology

It effectively reduces the critical dimensions of the trench, improves the pixel density and imaging quality of the image sensor, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114093763B_ABST
    Figure CN114093763B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a semiconductor, comprising: providing a substrate, sequentially forming a first dielectric layer, a second dielectric layer and a third dielectric layer on the substrate, wherein the third dielectric layer has an initial opening; forming a first deposition layer, wherein the first deposition layer at least covers the sidewall surface of the initial opening; etching the second dielectric layer directly below the first opening until the sidewall of the second dielectric layer is exposed; forming a second deposition layer, wherein the second deposition layer at least covers the sidewall of the first opening and the exposed sidewall of the second dielectric layer; etching the first dielectric layer directly below the second opening until the substrate is exposed; etching the substrate to form a groove. The present invention separates deposition and etching processes, forms a first deposition layer to reduce the width of the second dielectric layer to be etched; forms a second deposition layer to reduce the width of the first dielectric layer to be etched, and transfers layer by layer to reduce the critical size of the groove finally formed; forms a small-sized deep trench isolation (DTI) at a relatively low cost, thereby improving imaging quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of integrated circuit manufacturing, and in particular relates to a method for manufacturing a semiconductor. Background Art

[0002] Image sensors are widely used in digital still cameras, cellular phones, security cameras, and in medical, automotive, and other applications. The device architecture of image sensors has continued to evolve rapidly due to the ever-increasing demands for higher resolution, lower power consumption, increased dynamic range, etc. These demands have also promoted further miniaturization and integration of image sensors in these devices.

[0003] The image sensor includes a plurality of photosensitive elements, and image light from an external scene is incident on the image sensor, so that each photosensitive element absorbs a portion of the incident image light. The photosensitive elements (e.g., photodiodes) included in the image sensor each generate image charges after absorbing the image light. The amount of the generated image charge is proportional to the intensity of the image light. The generated image charge can be used to represent an image of the external scene.

[0004] Image sensors add deep trench isolation (DTI) between photosensitive elements to avoid crosstalk between adjacent photosensitive elements, improve the electronic isolation function of image sensors, and thus improve the quality of imaging. The quality of image sensor imaging can be improved by making the DTI process smaller in size, and more photosensitive elements can be made in the same area, thereby increasing the number of pixels. The miniaturization of image sensors can reduce the distance between adjacent photosensitive elements, thus placing an urgent demand on the small size of deep trench isolation (DTI).

[0005] However, making small-sized deep trench isolation, that is, reducing the critical dimension (CD) of deep trench isolation (DTI), requires more expensive photoresist and more precise process control, which greatly increases the cost, and it is necessary to find a more suitable manufacturing method. Summary of the invention

[0006] The purpose of the present invention is to form a small-sized deep trench isolation (DTI) semiconductor device at a relatively low cost, thereby improving the imaging quality of the semiconductor device.

[0007] The present invention provides a method for manufacturing a semiconductor, comprising:

[0008] Providing a substrate, and sequentially forming a first dielectric layer, a second dielectric layer, and a third dielectric layer on the substrate, wherein the third dielectric layer has an initial opening;

[0009] forming a first deposition layer, wherein the first deposition layer at least covers the sidewall surface of the initial opening to form a first mask layer having a first opening;

[0010] Performing a first etching process using the first mask layer as a mask to remove the second dielectric layer directly below the first opening until a side wall of the second dielectric layer is exposed;

[0011] forming a second deposition layer, wherein the second deposition layer at least covers the sidewalls of the first opening and the exposed sidewalls of the second dielectric layer, so as to form a second mask layer having a second opening;

[0012] Performing a second etching process using the second mask layer as a mask to remove the first dielectric layer directly below the second opening until the substrate is exposed;

[0013] The second mask layer is removed, and the substrate is etched using the first dielectric layer having the second opening as a mask to form a trench.

[0014] Further, the steps of forming the first mask layer, performing the first etching, forming the second mask layer, and performing the second etching are all completed in the same etching machine. Further, the process parameters for forming the first deposition layer are: deposition gas includes C4F8, source power: 800-1200W, bias voltage: 250-400V, and deposition gas flow rate is 100-500sccm.

[0015] Furthermore, the thickness of the first deposition layer formed on the sidewall of the initial opening is greater than or equal to 200 nm.

[0016] Furthermore, the process parameters for etching the second dielectric layer directly below the first opening are as follows: etching gas includes CF4, source power: 600-800W, bias voltage: 250-400V.

[0017] Furthermore, the process for forming the second deposition layer is as follows: the deposition gas includes C4F8, the source power is 800-1200W, the bias voltage is 250-400V, and the flow rate of the deposition gas is 200-600sccm.

[0018] Furthermore, the process parameters for etching the first dielectric layer directly below the second opening are as follows: etching gases include CO, O2, Ar2, source power: 800-1500W, bias voltage: 200-400V.

[0019] Furthermore, removing the second mask layer includes: removing the second deposition layer, the first deposition layer and the third dielectric layer by using O2 plasma ashing or stripping solution immersion, and removing the second dielectric layer by using oxalic acid wet etching.

[0020] Furthermore, etching the substrate is performed alternately by etching and passivation, the etching gas includes SF6, and the passivation gas includes C4F8.

[0021] Furthermore, in the process of etching the substrate, the passivation process parameters include: passivation gas C4F8, passivation time 10-30s, power supply power 450-600W, C4F8 flow rate 10-20sccm, pressure 3-10mtor, temperature 30-50°C, bias voltage: 60~100V; the etching process parameters specifically include: etching gas SF6, etching time 30-50s, power supply power 300-400W, SF6 flow rate 30-50sccm, pressure 3-10mtor, temperature 30-50°C.

[0022] Furthermore, the first dielectric layer is a bottom anti-reflection layer, the second dielectric layer is a low-temperature oxidation layer, and the third dielectric layer is a photoresist layer.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The present invention provides a method for manufacturing a semiconductor, comprising: providing a substrate, sequentially forming a first dielectric layer, a second dielectric layer and a third dielectric layer on the substrate, wherein the third dielectric layer has an initial opening; forming a first deposition layer, wherein the first deposition layer at least covers the side wall surface of the initial opening, so as to form a first mask layer having a first opening; performing a first etching with the first mask layer as a mask, removing the second dielectric layer directly below the first opening until the side wall of the second dielectric layer is exposed; forming a second deposition layer, wherein the second deposition layer at least covers the side wall of the first opening and the exposed side wall of the second dielectric layer, so as to form a second mask layer having a second opening; performing a second etching with the second mask layer as a mask, removing the first dielectric layer directly below the second opening until the substrate is exposed; removing the second mask layer, and etching the substrate with the first dielectric layer having the second opening as a mask, so as to form a groove.

[0025] The present invention separates the deposition and etching processes, forms a first deposition layer to reduce the width of the second dielectric layer to be etched; forms a second deposition layer to reduce the width of the first dielectric layer to be etched, and transfers the critical dimension (CD) of the final groove layer layer by layer; that is, inserting two-step deposition processes in the three-layer structure of the first dielectric layer, the second dielectric layer and the third dielectric layer effectively reduces the critical dimension (CD) of the groove. A small-sized deep trench isolation (DTI) is formed at a lower cost, and more photosensitive elements can be made in the same area, thereby increasing the pixel and improving the imaging quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The figure is a schematic flow chart of a method for manufacturing a semiconductor according to an embodiment of the present invention.

[0027] Figure 2It is a schematic diagram after forming a third dielectric layer in the manufacturing method according to an embodiment of the present invention.

[0028] Figure 3 It is a schematic diagram after forming the first deposition layer in the manufacturing method of an embodiment of the present invention.

[0029] Figure 4 It is a schematic diagram after etching the second dielectric layer in the manufacturing method of an embodiment of the present invention.

[0030] Figure 5 It is a schematic diagram after forming the second deposition layer in the manufacturing method of an embodiment of the present invention.

[0031] Figure 6 It is a schematic diagram after etching the first dielectric layer in the manufacturing method of an embodiment of the present invention.

[0032] Figure 7 It is a schematic diagram after removing the second dielectric layer and the third dielectric layer in the manufacturing method of an embodiment of the present invention.

[0033] Figure 8 It is a schematic diagram after etching the substrate in the manufacturing method of an embodiment of the present invention.

[0034] Fig. 9 It is a schematic diagram after removing the first dielectric layer in the manufacturing method of an embodiment of the present invention.

[0035] The reference numerals are as follows:

[0036] 11 - substrate; 12 - oxide layer; 13 - first dielectric layer; 14 - second dielectric layer; 15 - third dielectric layer; 16 - first deposition layer; 17 - second deposition layer. DETAILED DESCRIPTION

[0037] Based on the above research, an embodiment of the present invention provides a method for manufacturing a semiconductor. The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. According to the following description, the advantages and features of the present invention will become clearer. It should be noted that the drawings are all in a very simplified form and use an inaccurate scale, which is only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0038] The present invention provides a method for manufacturing a semiconductor. Figure 1 As shown, including:

[0039] S1. providing a substrate, and sequentially forming a first dielectric layer, a second dielectric layer and a third dielectric layer on the substrate, wherein the third dielectric layer has an initial opening;

[0040] S2, forming a first deposition layer, wherein the first deposition layer at least covers the sidewall surface of the initial opening to form a first mask layer having a first opening;

[0041] S3, performing a first etching process using the first mask layer as a mask to remove the second dielectric layer directly below the first opening until a side wall of the second dielectric layer is exposed;

[0042] S4, forming a second deposition layer, wherein the second deposition layer at least covers the sidewalls of the first opening and the exposed sidewalls of the second dielectric layer to form a second mask layer having a second opening;

[0043] S5, performing a second etching process using the second mask layer as a mask to remove the first dielectric layer directly below the second opening until the substrate is exposed;

[0044] S6. Remove the second mask layer, and etch the substrate using the first dielectric layer having the second opening as a mask to form a trench.

[0045] Combine the following Figures 2 to 9 Each step of the semiconductor manufacturing method according to the embodiment of the present invention is described in detail.

[0046] like Figure 2 As shown, in step S1, a substrate 11 is provided, an oxide layer 12 may be formed on the substrate 11, a first dielectric layer 13, a second dielectric layer 14 and a third dielectric layer 15 are sequentially formed on the oxide layer 12, and the third dielectric layer 15 has an initial opening K0, and the initial opening K0 exposes the second dielectric layer 14. The number of initial openings K0 is set according to actual needs, and the cross-sectional width of the initial opening K0 on the cross section perpendicular to the substrate is D0, and the cross-sectional width D0 of the initial opening K0 is the minimum width that can be produced by a photolithography machine.

[0047] In one embodiment, the first dielectric layer 13 is, for example, a bottom anti-reflective coating (BARC); the second dielectric layer 14 is, for example, a low temperature oxide layer (LTO), a silicon nitride layer, a silicon carbide layer, a titanium nitride layer, a tantalum nitride layer, a titanium oxide layer, and a tantalum oxide layer, or a combination of two or more thereof. The third dielectric layer 15 is, for example, a photoresist layer, which is patterned by exposure and development steps to form a pattern with a predetermined shape, forming an initial opening K0 that penetrates the photoresist layer. The first dielectric layer 13 is, for example, a bottom anti-reflective coating, which can reduce light reflection when patterning the photoresist layer. Alternatively, the third dielectric layer 15 can also be a polysilicon layer, a silicon oxide layer, a silicon nitride layer, and a silicon carbide layer, or a combination of two or more thereof. The third dielectric layer 15 can be formed by chemical vapor deposition. A photoresist layer is formed on the third dielectric layer 15, and then the photoresist layer is exposed and developed using a mask with a pattern to form a patterned photoresist layer, wherein the pattern in the patterned photoresist layer defines an initial opening K0; then the patterned photoresist layer is used as a mask to pattern the third dielectric layer 15 using an etching process to form an initial opening K0 penetrating the third dielectric layer 15, and then the patterned photoresist layer is removed.

[0048] In another embodiment, the first dielectric layer 13 is, for example, a silicon oxide layer, the second dielectric layer 14 is, for example, a silicon nitride layer, and the third dielectric layer 15 is, for example, a silicon oxide layer, forming an ONO (silicon oxide layer-silicon nitride layer-silicon oxide layer) stacked structure; the first dielectric layer 13, the second dielectric layer 14, and the third dielectric layer 15 can also be a combination of any other materials.

[0049] like Figure 3 and Figure 4 As shown, in step S2, a first deposition layer 16 is formed, and the first deposition layer 16 at least covers the side wall surface of the initial opening K0 to form a first mask layer with a first opening K1. The first deposition layer 16 with the first opening K1 and the patterned third dielectric layer together constitute the first mask layer; the cross-sectional width of the first opening K1 on the cross section perpendicular to the substrate 11 is D1, and the width D1 is the spacing of the first deposition layer 16 on the two side walls of the first opening K1. It should be understood that the cross-sectional width of the etching opening on the cross section perpendicular to the substrate after the second dielectric layer 14 to be etched is subsequently etched is also D1. In this step, the first deposition layer 16 is formed in the initial opening K0 to reduce the width D1 of the second dielectric layer 14 to be etched, so as to reduce the critical dimension (CD) of the groove finally formed. The first deposition layer 16 can also cover the surface of the second dielectric layer 14 exposed by the initial opening K0.

[0050] The first deposition layer 16 can be formed by a deposition process, the deposition gas includes C4F8, the source power is 800-1200W, and the bias voltage is 250-400V. The deposition gas containing C4F8 is flowed from the gas source into the plasma processing chamber. In one example, the deposition gas is composed of pure C4F8, and the flow rate of the deposition gas is 100-500sccm. The deposition gas is converted into a deposition plasma, and the deposition is provided for about 30 seconds. Then the deposition of the deposition layer is stopped, and the pressure of 90-150 mtorr is maintained. Preferably, the deposition is provided for at least 20 seconds. More preferably, the deposition is provided for at least 25 seconds. Most preferably, the deposition is provided for at least 30 seconds. Preferably, the first deposition layer on the sidewall is at least 200nm thick. More preferably, the first deposition layer on the sidewall is at least 300nm thick.

[0051] like Figure 4 As shown, in step S3, the first etching is performed using the first mask layer as a mask to remove the second dielectric layer 14 directly below the first opening K1 until the sidewall of the second dielectric layer 14 is exposed. Specifically, the second dielectric layer 14 directly below the first opening K1 is etched until the first dielectric layer 13 is exposed. The etching gas includes CF4, the source power is 600-800W, and the bias voltage is 250-400V.

[0052] like Figure 5 and Figure 6 As shown, in step S4, a second deposition layer 17 is formed, and the second deposition layer 17 at least covers the sidewalls of the first opening K1 and the exposed sidewalls of the second dielectric layer 14 to form a second mask layer with a second opening K2; specifically, the second dielectric layer 14, the third dielectric layer 15, the first deposition layer 16 and the second deposition layer 17 together constitute the second mask layer. In this step, the second deposition layer 17 is formed to reduce the width D2 of the first dielectric layer 13 to be etched, so as to reduce the critical dimension (CD) of the groove finally formed. The width D2 specifically refers to the cross-sectional width of the etched opening on the cross section perpendicular to the substrate after the first dielectric layer 13 to be etched is subsequently etched. The width D2 is also the cross-sectional width of the second opening K2, and the width D2 is also the spacing between the second deposition layers 17 on the two side walls of the second opening K2. The second deposition layer 17 can be formed by a deposition process, and the deposition gas includes C4F8, the source power: 800-1200W, and the bias voltage: 250-400V.

[0053] like Figure 6 and Figure 7As shown, in step S5, the second etching is performed using the second mask layer as a mask to remove the first dielectric layer 13 directly below the second opening K2 until the substrate 11 is exposed. Specifically, the first dielectric layer 13 and the oxide layer 12 directly below the second opening K2 are etched until the substrate 11 is exposed. The etching gas includes CO, O2, Ar2, the source power is 800-1500W, and the bias voltage is 200-400V.

[0054] In this embodiment, the steps of forming the first mask layer, performing the first etching, forming the second mask layer, and performing the second etching are all completed in the same etching machine, also known as in-situ etching, which avoids the problems of forming the mask layer and etching in different machines in the existing process, increasing the number of steps and increasing the process time due to the transfer of machines.

[0055] Continue as Figure 6 and Figure 7 As shown, in step S6, the second mask layer is removed, and the substrate 11 is etched using the first dielectric layer 13 having the second opening K2 as a mask to form a groove V. The second mask layer is removed to specifically remove the second dielectric layer 14, the third dielectric layer 15, the first deposition layer 16, and the second deposition layer 17. The second deposition layer 17, the first deposition layer 16, and the third dielectric layer 15 can be removed by O2 plasma ashing or stripping solution immersion. The first deposition layer 16 and the second deposition layer 17 are both organic polymers formed by C4F8, and O2 plasma ashing or stripping solution immersion can remove the organic polymer. The O2 plasma ashing process parameters are: processing time 60-120s, power supply power 300-400W, O2 flow rate 300-500sccm, pressure 10-30mt, temperature 30-50°C. The stripping solution can be selected to be soaked in NMP stripping solution for 120-240s. N-Methylpyrrolidone, English name N-Methyl pyrrolidone, namely NMP, is an important chemical raw material and a polar solvent with strong selectivity and good stability. The second dielectric layer 14 can be removed by wet etching. For example, the second dielectric layer 14 is removed by wet etching with oxalic acid, the wet etching time is 20-50s, and the oxalic acid concentration is 2-10wt%.

[0056] like Figure 8 and Fig. 9As shown, the substrate 11 is etched with the first dielectric layer 13 having the second opening K2 as a mask to form a groove V. In the cross section perpendicular to the substrate, the cross-sectional width of the groove V is D, and the cross-sectional width of the groove V is D, which is approximately equal to the cross-sectional width D2 of the second opening K2. A small amount of lateral etching causes a deviation between the two during the etching process. The cross-sectional width D of the groove V can be used as a critical dimension of the groove. The etching substrate 11 can be etched using the Bosch process, and the etching gas includes SF6 and the passivation gas includes C4F8. The Bosch process refers to a process in which a layer of etching film is deposited on the lateral sidewall of the etching in order to prevent or weaken lateral etching in the manufacture of integrated circuits. First, silicon is etched using a fluorine-based active group, and then the sidewall is passivated. The etching and passivation processes are performed alternately. Etching and sidewall passivation are achieved by alternately switching the etching gas and the passivation gas. C4F8 can form a fluorinated carbon polymer in plasma, and deposition on the silicon surface can prevent the reaction of fluoride ions with silicon. Etching and passivation are switched every 5 to 10 seconds. After a short period of isotropic etching, the silicon surface that has just been etched is passivated. Due to the physical sputtering bombardment of ions in the depth direction, the passivation film can be retained, so that no lateral etching will occur in the next cycle of etching. Through this periodic "etching-passivation-etching", etching is only carried out along the depth direction, and finally a groove V is formed. The groove is, for example, a deep groove, and an isolation layer is filled in the deep groove to form a deep trench isolation (DPI). The depth of groove V is at least 500nm. More preferably, the depth of groove V is at least 1000nm. Preferably, the aspect ratio of the depth to the width of groove V is at least 5:1. More preferably, the aspect ratio of groove V is at least 10:1.

[0057] In the process of etching the substrate 11 to form the groove V, the deposition (passivation) process parameters specifically include, for example, deposition gas C4F8, deposition time 10-30s, power supply power 450-600W, C4F8 flow rate 10-20sccm, pressure 3-10mtor, temperature 30-50°C, bias voltage: 60-100V. In the Bosch process, C4F8 is mainly used to form a sidewall protection polymer to protect the sidewall from damage. The etching process parameters specifically include: etching gas SF6, etching time 30-50s, power supply power 300-400W, SF6 flow rate 30-50sccm, pressure 3-10mtor, temperature 30-50°C.

[0058] like Fig. 9As shown, the first dielectric layer 13 can be removed by dry etching process. Etching gases include CO, O2, Ar2, source power: 800-1500W, bias voltage: 200-400V. So far, a small-sized deep trench isolation (DTI) semiconductor device is formed in the substrate, which can be used as an image sensor and other devices requiring trench isolation. More photosensitive elements can be made in the same area, thereby increasing the pixels and improving the imaging quality of the semiconductor device.

[0059] In summary, the present invention provides a method for manufacturing a semiconductor, including: providing a substrate, sequentially forming a first dielectric layer, a second dielectric layer and a third dielectric layer on the substrate, wherein the third dielectric layer has an initial opening; forming a first deposition layer, wherein the first deposition layer at least covers the sidewall surface of the initial opening; etching the second dielectric layer directly below the first opening until the sidewall of the second dielectric layer is exposed; forming a second deposition layer, wherein the second deposition layer at least covers the sidewall of the first opening and the exposed sidewall of the second dielectric layer; etching the first dielectric layer directly below the second opening until the substrate is exposed; etching the substrate to form a groove. The present invention separates the deposition and etching processes, forms a first deposition layer to reduce the width of the second dielectric layer to be etched; forms a second deposition layer to reduce the width of the first dielectric layer to be etched, and transfers layer by layer to reduce the critical size of the groove finally formed; forms a small-sized deep trench isolation (DTI) at a relatively low cost, thereby improving the imaging quality.

[0060] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the method disclosed in the embodiment, since it corresponds to the device disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part description.

[0061] The above description is only a description of the preferred embodiment of the present invention, and is not any limitation on the scope of rights of the present invention. Any technical personnel in this field can make possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. A method for manufacturing a semiconductor, characterized in that: include: Providing a substrate, and sequentially forming a first dielectric layer, a second dielectric layer, and a third dielectric layer on the substrate, wherein the third dielectric layer has an initial opening; forming a first deposition layer, wherein the first deposition layer at least covers the sidewall surface of the initial opening to form a first mask layer having a first opening; Performing a first etching process using the first mask layer as a mask to remove the second dielectric layer directly below the first opening until a side wall of the second dielectric layer is exposed; forming a second deposition layer, wherein the second deposition layer at least covers the sidewalls of the first opening and the exposed sidewalls of the second dielectric layer, so as to form a second mask layer having a second opening; Performing a second etching process using the second mask layer as a mask to remove the first dielectric layer directly below the second opening until the substrate is exposed; The second mask layer is removed, and the substrate is etched using the first dielectric layer having the second opening as a mask to form a groove; wherein the removal of the second mask layer comprises: the second deposition layer, the first deposition layer and the third dielectric layer are all removed by O2 plasma ashing or stripping solution immersion, and the second dielectric layer is removed by oxalic acid wet etching.

2. The method for manufacturing a semiconductor according to claim 1, wherein: The steps of forming the first mask layer, performing the first etching, forming the second mask layer and performing the second etching are all completed in the same etching machine.

3. The method for manufacturing a semiconductor according to claim 1, wherein: The process parameters for forming the first deposition layer are as follows: the deposition gas includes C4F8, the source power is 800-1200W, the bias voltage is 250-400V, and the flow rate of the deposition gas is 100-500sccm.

4. The method for manufacturing a semiconductor according to claim 1, wherein: The thickness of the first deposition layer formed on the sidewall of the initial opening is greater than or equal to 200 nm.

5. The method for manufacturing a semiconductor according to claim 1, wherein: Process parameters for etching the second dielectric layer directly below the first opening are as follows: etching gas includes CF4, source power: 600-800W, bias voltage: 250-400V.

6. The method for manufacturing a semiconductor according to claim 1, wherein: The process for forming the second deposition layer is as follows: the deposition gas includes C4F8, the source power is 800-1200W, the bias voltage is 250-400V, and the flow rate of the deposition gas is 200-600sccm.

7. The method for manufacturing a semiconductor according to claim 1, wherein: Process parameters for etching the first dielectric layer directly below the second opening are as follows: etching gases include CO, O2, Ar2, source power: 800-1500W, bias voltage: 200-400V.

8. The method for manufacturing a semiconductor according to claim 1, wherein: The substrate is etched by alternately etching and passivating, the etching gas includes SF6, and the passivating gas includes C4F8.

9. The method for manufacturing a semiconductor according to claim 8, wherein: In the process of etching the substrate, the passivation process parameters include: passivation gas C4F8, passivation time 10-30s, power supply power 450-600W, C4F8 flow rate 10-20sccm, pressure 3-10mtor, temperature 30-50°C, bias voltage: 60~100V; the etching process parameters specifically include: etching gas SF6, etching time 30-50s, power supply power 300-400W, SF6 flow rate 30-50sccm, pressure 3-10mtor, temperature 30-50°C.

10. The method for manufacturing a semiconductor according to any one of claims 1 to 9, characterized in that: The first dielectric layer is a bottom anti-reflection layer, the second dielectric layer is a low-temperature oxidation layer, and the third dielectric layer is a photoresist layer.

Citation Information

Patent Citations

  • Image sensor and manufacturing method of deep trench thereof

    CN112466900A

  • Method for fabricating semiconductor device

    KR1020070069971A