Synthetic leather
By using high molecular weight polyester-based plasticizer and surface protective layer in the skin layer of vinyl chloride synthetic leather, combined with foam adhesive layer, the vinyl chloride synthetic leather is solved after cracks and oily substances are easily contacted by low temperature environment. Problems appear on the surface, which improves cold resistance and chemical resistance, enhances the feel and wear resistance.
Patent Information
- Application Number
- CN202110702687.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-18
- Filing Date
- 2021-06-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-06-24
AI Technical Summary
Vinyl chloride synthetic leather is prone to cracks in low temperature environments, and the surface plasticizer surfaces appear after contacting oily substances, resulting in poor feel and insufficient chemical resistance.
Polyester-based plasticizers with a number average molecular weight of 800 or more than 4000 are used in the skin layer. The proportion of polyester-based plasticizers to 100 mass% is 10% or more than 80%, and a surface protective layer is provided on the skin layer. and the foam adhesive layer, combined with vinyl chloride resin and polyurethane resin, optimize the ratio and acid value of the resin to the plasticizer.
It significantly improves the cold resistance and chemical resistance of vinyl chloride synthetic leather, inhibits the leakage of plasticizers, enhances wear resistance and feel, and is suitable for a variety of temperature environments and human contact scenarios.
Smart Images

Figure CN114108329B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a synthetic leather having a surface layer containing a vinyl chloride resin. Background Art
[0002] As shown in Patent Document 1, synthetic leather is composed of a base fabric and a skin layer laminated on the surface of the base fabric. The skin layer is a resin layer composed of a base resin. Examples of the base resin include vinyl chloride resins, polyurethane resins, and the like. Among them, vinyl chloride resins have the advantages of being cheap and easy to process, and are excellent as the base resin. Therefore, synthetic leather having a skin layer based on vinyl chloride resins is commonly used in various industrial fields. The skin layer based on the vinyl chloride resins usually contains a plasticizer in order to exhibit good softness.
[0003] For example, synthetic leather having a surface layer based on a vinyl chloride resin is used in various applications such as vehicle interior materials, furniture such as sofas, clothing such as shoes and clothes, small bags such as bags, and outdoor products such as tent canopies.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 9-228258 Summary of the invention
[0007] Problems to be solved by the invention
[0008] As described above, as the use of synthetic leather having a surface with a vinyl chloride resin as a base resin (hereinafter, also referred to as vinyl chloride synthetic leather or simply referred to as synthetic leather) expands, further improvement of the physical properties of the vinyl chloride synthetic leather is required. Specifically, when the vinyl chloride synthetic leather is used in a low temperature environment, there are problems such as cracks on the surface due to slight impact or bending. Therefore, improvement of cold resistance is required for the vinyl chloride synthetic leather.
[0009] On the other hand, it is understood that vinyl chloride synthetic leather is less likely to have the above-mentioned problems in a temperature environment above room temperature and can maintain a good condition. However, vinyl chloride synthetic leather has the following problems when in use.
[0010] That is, vinyl chloride synthetic leathers used for various purposes as described above have many opportunities to come into contact with people. Therefore, when in contact, oily substances such as human sebum, cosmetics, and sunscreens are easily attached to vinyl chloride synthetic leathers. When vinyl chloride synthetic leathers with oily substances attached are left for a long time at room temperature or a relatively high temperature atmosphere above that, there is sometimes an exudation phenomenon in which the plasticizer contained in the epidermis emerges on the surface of the synthetic leather. If the exudation phenomenon of the plasticizer occurs, the epidermis hardens, the feel of the synthetic leather deteriorates, and cracks are easily generated in the epidermis simply by impact or bending the synthetic leather. That is, vinyl chloride synthetic leathers have problems related to chemical resistance caused by oily substances, etc. This problem may occur even when a surface protective layer is formed on the surface side of the epidermis.
[0011] The present invention has been made in view of the above problems. That is, the problem of the present invention is to provide a vinyl chloride-based synthetic leather which is not prone to cracking even in a low-temperature environment, has good cold resistance, and has suppressed plasticizer bleeding and improved chemical resistance.
[0012] Means used to solve problems
[0013] The synthetic leather of the present invention is a synthetic leather having an epidermis layer and a base fabric, characterized in that the epidermis layer contains a vinyl chloride resin and a plasticizer, the plasticizer contains a polyester plasticizer having a number average molecular weight of 800 to 4000, and the polyester plasticizer accounts for 10% to 80% of the plasticizer contained in the epidermis layer.
[0014] Effects of the Invention
[0015] Since the synthetic leather of the present invention having the above-mentioned structure has improved cold resistance and chemical resistance, the temperature conditions of the use environment are substantially relaxed. Therefore, the synthetic leather of the present invention can be preferably used in various applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 It is a cross-sectional view of the first embodiment of the present invention.
[0017] Figure 2 It is a cross-sectional view of a second embodiment of the present invention.
[0018] Figure 3 It is a cross-sectional view of a modified example of the second embodiment of the present invention.
[0019] Description of Reference Numerals
[0020] 10: epidermis; 20: base fabric; 30: surface protection layer; 40: adhesive layer; 50: foam adhesive layer; 60: foam layer; 110, 120, 130: synthetic leather; 210: longitudinal line; 220: transverse line. DETAILED DESCRIPTION
[0021] The synthetic leather of the present invention comprises an epidermis layer and a base fabric. In the present invention, the epidermis layer contains a vinyl chloride resin and a plasticizer. The plasticizer contains a polyester plasticizer having a number average molecular weight of 800 to 4000, and the polyester plasticizer is contained in a range of 10% to 80% of the plasticizer contained in the epidermis layer.
[0022] The synthetic leather of the present invention includes artificial leather using nonwoven fabric or special nonwoven fabric as a base fabric and other synthetic leathers that do not use nonwoven fabric or special nonwoven fabric in the base fabric. Here, the special nonwoven fabric refers to a base fabric formed by impregnating polyurethane or a substance similar thereto with a member having a fiber layer composed of a random three-dimensional structure as a base.
[0023] The synthetic leather of the present invention having the above-mentioned structure shows good cold resistance, and even when exposed to a relatively high temperature atmosphere above room temperature with oily substances such as human sebum attached to the surface side, the plasticizer oozing phenomenon can be suppressed. Therefore, the synthetic leather of the present invention can provide excellent quality even in the application fields such as vehicle interior materials, clothing products, and outdoor products, which are used in a wide range of temperature environments and are expected to come into contact with people. In addition, in the present invention, the fact that the plasticizer oozing phenomenon can be suppressed even when oily substances are attached is sometimes expressed as excellent chemical resistance.
[0024] Hereinafter, the present invention will be described in more detail with reference to embodiments.
[0025] <First Embodiment>
[0026] Figure 1 The synthetic leather 110 according to the first embodiment of the present invention is schematically cross-sectionally cut in the thickness direction. The synthetic leather 110 includes a skin layer 10 and a base fabric 20. In this embodiment, the skin layer 10 and the base fabric 20 are bonded together by an adhesive layer 40. A surface protection layer 30 is provided on the surface side of the skin layer 10.
[0027] (Epidermis 10)
[0028] The epidermis layer 10 contains a vinyl chloride resin and a plasticizer. The epidermis layer 10 is a layer constituting the surface of the synthetic leather 110, and may be appropriately given a texture and the like to present a leather-like appearance. In addition, the texture mentioned here refers to a pattern, a design, etc. decorated on the surface side of the component. The present invention includes any of a method in which the epidermis layer 10 is arranged on the outermost surface of the synthetic leather 110 and a method in which it is arranged at a position close to the outermost surface of the synthetic leather 110. That is, the present invention includes a method in which an arbitrary layer is arranged at a position closer to the surface side than the epidermis layer 10. In the present embodiment, specifically, a method in which a surface protection layer 30 is provided on the surface side of the epidermis layer 10 is shown. The synthetic leather 110 having the epidermis layer 10 containing a vinyl chloride resin includes a component so-called vinyl chloride leather.
[0029] Vinyl chloride resin:
[0030] The skin layer 10 contains a vinyl chloride resin, preferably a vinyl chloride resin as a base resin. Here, the base resin refers to a resin containing more than 50% by mass in 100% by mass of the resin constituting any layer (for example, the skin layer 10).
[0031] The vinyl chloride resin contained in the skin layer 10 is a resin containing a structural unit derived from vinyl chloride. Specific examples thereof include homopolymers of vinyl chloride, copolymers formed by using a vinyl chloride monomer and other monomers copolymerizable therewith, and blends of these resins.
[0032] Examples of other monomers copolymerizable with the vinyl chloride monomer include ethylene, propylene, vinyl acetate, vinylidene chloride, acrylic acid, acrylic acid esters, methacrylic acid, methacrylic acid esters, maleic acid, acrylonitrile fumarate, etc. The vinyl chloride resin contained in the skin layer 10 may be one type or two or more types.
[0033] The skin layer 10 may contain a vinyl chloride resin and other resins in combination, or may be substantially composed of only the vinyl chloride resin. The vinyl chloride resin contained in the skin layer 10 preferably accounts for more than 50% by mass, more preferably 70% by mass or more, further preferably 90% by mass or more, and particularly preferably substantially 100% by mass, of 100% by mass of the resin constituting the skin layer 10.
[0034] The thickness of the skin layer 10 is not particularly limited, but is preferably 10 μm or more, more preferably 100 μm or more from the viewpoint of durability, and preferably 400 μm or less from the viewpoint of hand feel and softness.
[0035] Plasticizer:
[0036] The skin layer 10 contains a plasticizer. In 100% by mass of the plasticizer, a polyester plasticizer is contained at a ratio of 10% by mass to 80% by mass. As the polyester plasticizer, a polyester plasticizer having a number average molecular weight of 800 to 4000 is selected. In this way, by containing the polyester plasticizer as a polymer plasticizer, the skin layer 10 not only more effectively exhibits softness similar to that of natural leather, but also exhibits the following excellent properties.
[0037] That is, by containing a polyester plasticizer having a number average molecular weight of 800 to 4000 at a predetermined ratio in the epidermis layer 10 formed of a vinyl chloride resin, even when the synthetic leather 110 with oily substances attached thereto is placed in a relatively high temperature atmosphere above room temperature for a long period of time, the plasticizer contained in the epidermis layer 10 can be effectively suppressed from oozing out on the surface of the synthetic leather 110. From the viewpoint of better suppressing the above-mentioned oozing out, the number average molecular weight of the polyester plasticizer used is preferably 1200 to 3000, and more preferably 1500 to 2000.
[0038] The number average molecular weight of the plasticizer is measured by gel permeation chromatography (GPC) using tetrahydrofuran (THF) as an eluent, and can be obtained as a value converted into standard polystyrene.
[0039] In addition, by containing 10% by mass or more of the polyester plasticizer in 100% by mass of the plasticizer contained in the epidermis layer 10, the above-mentioned bleeding phenomenon can be well suppressed, and the synthetic leather 110 with excellent chemical resistance can be provided. In particular, the epidermis layer 10 has excellent chemical resistance when a higher fatty acid such as oleic acid is attached, so the above-mentioned bleeding phenomenon can be well suppressed even when sebum, cosmetics, sunscreen, etc. are attached. From the viewpoint of improving chemical resistance, the content of the polyester plasticizer is preferably 20% by mass or more, more preferably 40% by mass or more, and even more preferably 60% by mass or more.
[0040] On the other hand, by containing the polyester plasticizer in a range of 80% by mass or less in 100% by mass of the plasticizer contained in the epidermis layer 10, it is possible to provide a synthetic leather 110 having excellent cold resistance while maintaining good chemical resistance. From the viewpoint of improving cold resistance, the content of the polyester plasticizer is preferably 70% by mass or less. The synthetic leather 110 having the epidermis layer 10 is not easily damaged even when subjected to impact or bending in cold regions such as -30°C or below, and has excellent cold resistance.
[0041] Examples of the polyester plasticizer contained in the skin layer 10 include phthalic acid polyester plasticizers, adipic acid polyester plasticizers, sebacic acid polyester plasticizers, and maleic acid polyester plasticizers.
[0042] That is, examples of the polyester plasticizer used in the present invention include esters of polycarboxylic acids (dicarboxylic acids) such as phthalic acid, adipic acid, sebacic acid, or maleic acid, and polyhydric alcohols.
[0043] Examples of plasticizers other than polyester plasticizers contained in the skin layer 10 include trimellitic acid plasticizers, phthalic acid plasticizers, linear dibasic acid plasticizers, and phosphoric acid plasticizers. From the viewpoint of versatility, phthalic acid plasticizers are preferred, and more specifically, examples thereof include trimellitic acid plasticizers such as tri-n-octyl trimellitate, tri(2-ethylhexyl) trimellitate, tri-isooctyl trimellitate, tri-isodecyl trimellitate, and di-n-octyl-n-decyl trimellitate, and examples thereof include dibutyl phthalate, diisobutyl phthalate, dioctyl phthalate, and didodecyl phthalate. Phthalic acid plasticizers such as phthalate, butyl benzyl phthalate, diisodecyl phthalate, dihexyl phthalate, and diisononyl phthalate; linear dibasic acid plasticizers such as dioctyl adipate, diisodecyl adipate, dibutyl sebacate, and dioctyl sebacate; and phosphoric acid plasticizers such as tributyl phosphate, tricresyl phosphate, triphenyl phosphate, trichloroethyl phosphate, trioctyl phosphate, and diphenylcresyl phosphate.
[0044] In the present invention, a plasticizer having an ester bond and a number average molecular weight of less than 800 is recognized as a plasticizer other than the polyester plasticizer used in the present invention.
[0045] The plasticizer other than the polyester plasticizer contained in the skin layer 10 is 20 mass % to 90 mass % and preferably 30 mass % to 80 mass % in 100 mass % of the plasticizer contained in the skin layer 10 .
[0046] The average acid value (KOH mg / g) of all plasticizers contained in the skin layer 10 is preferably 0.1 or more, and more preferably 0.15 or more.
[0047] In addition, with respect to the present invention, the acid value refers to the number of milligrams (mg) of potassium hydroxide equivalent to the hydroxyl group in 1 g of the sample, and the average acid value of the plasticizer refers to the sum of the values obtained by multiplying the acid value of each plasticizer used in the epidermis by the mixing ratio of each plasticizer (the mixing ratio in 100% by mass of all plasticizers).
[0048] The ratio of the vinyl chloride resin to the polyester plasticizer in the skin layer 10 is:
[0049] The mixing ratio of the vinyl chloride resin and the polyester plasticizer contained as the base resin in the epidermis layer 10 can be appropriately determined. For example, the polyester plasticizer having a number average molecular weight of 800 to 4000 as the plasticizer is preferably adjusted to a range of 10 to 120 parts by mass, and more preferably adjusted to a range of 30 to 100 parts by mass. In particular, by mixing the plasticizer in the above range in the epidermis layer 10 containing the vinyl chloride resin as the base resin, the elasticity and softness of the synthetic leather 110 can be made close to the elasticity and softness of natural leather.
[0050] When the polyester plasticizer is added in an amount of less than 10 parts by mass relative to 100 parts by mass of the base resin, there is a risk that the elasticity and flexibility of the skin layer 10 cannot be fully exerted. On the other hand, when the amount exceeds 120 parts by mass, no further improvement in the elasticity and flexibility of the skin layer 10 is observed, and there is a risk of causing a decrease in strength and deterioration in workability.
[0051] Other Additives:
[0052] In addition to the resin and the plasticizer, additives may be appropriately added to the skin layer 10 within the scope of the present invention. Examples of the additives include stabilizers, fillers, flame retardants, pigments, and the like.
[0053] (Base fabric 20)
[0054] Next, the base fabric 20 will be described. The base fabric 20 is a layer for supporting the epidermis layer 10. The base fabric 20 can be any base fabric used as a base fabric for general synthetic leather or artificial leather, and examples thereof include woven fabrics, woven fabrics, nonwoven fabrics, etc., made of single fibers selected from synthetic fibers such as polyester, polyamide, polyacrylonitrile, nylon, natural fibers such as cotton, linen, and regenerated fibers such as rayon and acetate, or blended fibers thereof. Figure 1 In the figure, as the base fabric 20, a woven fabric composed of longitudinal threads 210 and transverse threads 220 is exemplified. The base fabric 20 may be a raised base fabric or a non-raised base fabric.
[0055] The thickness of the base fabric 20 is not particularly limited, and for example, a thickness within a range of 400 μm to 1000 μm is appropriate.
[0056] (Surface protection layer 30)
[0057] The synthetic leather 110 of the present embodiment is provided with a surface protection layer 30 on the surface of the skin layer 10 on the side opposite to the base fabric 20 .
[0058] The surface protection layer 30 is composed of a properly selected resin or the like. For example, the surface protection layer 30 is composed of a polyurethane resin and a cross-linking agent. The surface protection layer 30 is a layer for protecting the surface of the epidermis layer 10, and can improve the wear resistance of the synthetic leather 110. The polyurethane resin refers to a resin containing a urethane bond in the molecule, and more specifically, refers to a resin having a urethane bond in the repeating unit of the main chain.
[0059] The polyurethane resin constituting the surface protection layer 30 can be any polyurethane resin that is formed by reacting a polyol component with a polyisocyanate component and that can constitute a layer suitable for protecting the surface side of the synthetic leather 110. For example, as an example, a water-based polyurethane resin can be cited. A water-based polyurethane resin refers to a polyurethane resin having a hydrophilic group and being soluble or emulsified in water. As the water-based polyurethane resin, for example, a polyurethane having a hydrophilic group (anionic hydrophilic group, cationic hydrophilic group or nonionic hydrophilic group) in the molecule, or a polyurethane having a hydrophilic segment. Among the water-based polyurethane resins, polycarbonate-based polyurethane resins are preferred from the viewpoints of durability, wear resistance and hydrolysis resistance. Polycarbonate-based polyurethanes are obtained, for example, by carrying out a polyaddition reaction using polycarbonate-based diols and polyisocyanates.
[0060] The crosslinking agent may be any crosslinking agent that can improve the physical properties of the polyurethane resin by self-crosslinking or three-dimensionally crosslinking the polyurethane resin, and examples thereof include carbodiimide crosslinking agents, isocyanate crosslinking agents, and oxazoline crosslinking agents.
[0061] One of the more preferred aspects of the present embodiment having the surface protection layer 30 is that the average acid value (KOHmg / g) of the plasticizer contained in the epidermis layer 10 is 0.1 or more, and the surface protection layer 30 composed of a polyurethane resin contains an isocyanate crosslinking agent as a crosslinking agent.
[0062] According to the above method, a synthetic leather 110 having particularly excellent wear resistance can be provided. The reason for the improvement of the wear resistance is not clear, but it is speculated that the hydroxyl contained in the epidermis 10 and the isocyanate contained in the surface protection layer 30 react with each other near the interface between the surface protection layer 30 and the epidermis 10 to enhance the adhesion between the epidermis 10 and the surface protection layer 30. From the viewpoint of improving the above wear resistance, in the above method, the average acid value of the plasticizer contained in the epidermis 10 is more preferably 0.15 or more. For example, synthetic leather used for vehicle seats, etc. is repeatedly rubbed by the user's skin and clothes, so the synthetic leather of this method with good wear resistance can be appropriately used in vehicle seats. Of course, the synthetic leather of this method can be appropriately used in various other technical fields.
[0063] The ratio of the crosslinking agent to be added is not particularly limited, but is preferably 2 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the polyurethane resin contained in the surface protection layer 30. If the crosslinking agent is less than 2 parts by mass, the wear resistance may be insufficient, and if it exceeds 20 parts by mass, the surface protection layer 30 may become hard and the feel may be impaired.
[0064] (Adhesive layer 40)
[0065] The skin layer 10 and the base fabric 20 of the present embodiment described above are bonded together by the adhesive layer 40 .
[0066] The adhesive layer 40 is another layer (on one side of the base fabric 20) provided on the base fabric 20. Figure 1 The adhesive layer 40 is a layer for bonding the skin layer 10). The resin constituting the adhesive layer 40 can be selected from resins that can be used as adhesives, such as polyurethane resins, vinyl chloride resins, or polyolefin resins. In particular, in the present embodiment, since the skin layer 10 containing vinyl chloride resin is bonded to the base fabric 20, the adhesive layer 40 is also preferably a layer containing vinyl chloride resin.
[0067] In other embodiments, the adhesive layer 40 may be omitted as appropriate. For example, a foaming layer may be formed on the surface of one of the base fabric 20 and the skin layer 10, and the other member may be quickly laminated while the foaming layer is in a semi-cured state, thereby bonding the two. The foaming adhesive layer, which is a foaming layer also serving as an adhesive layer, will be further described in the second embodiment described later. In addition, as another method, the skin layer 10 may be first formed on the release paper, and the base fabric 20 may be laminated on the semi-cured skin layer 10, thereby omitting the adhesive layer 40 and bonding the two.
[0068] The thickness of the adhesive layer 40 is not particularly limited, but is preferably in the range of 50 μm to 250 μm from the viewpoint of achieving sufficient adhesion without impairing the flexibility of the skin layer 10 .
[0069] <Second Embodiment>
[0070] Hereinafter, a second embodiment of the present invention will be described.
[0071] Figure 2 FIG. 2 shows a schematic cross-sectional view of a synthetic leather 120 according to a second embodiment cut along the thickness direction. Figure 3 A schematic cross-sectional view showing a synthetic leather 130 which is a modified example of the synthetic leather 120 according to the second embodiment and is cut along the thickness direction is shown.
[0072] The synthetic leather 120 includes a foam adhesive layer 50 between the surface layer 10 and the base fabric 20. In the present embodiment, the surface layer 10 and the base fabric 20 are bonded to each other via the foam adhesive layer 50, and a surface protective layer 30 is provided on the surface side of the surface layer 10. The synthetic leather 120 is configured similarly to the synthetic leather 110 except that the foam adhesive layer 50 is provided instead of the adhesive layer 40 in the synthetic leather 110. Therefore, the synthetic leather 120, especially the foam adhesive layer 50, will be described, and the description related to the first embodiment will be appropriately referred to for other configurations.
[0073] The foam adhesive layer 50 is a foam resin layer having adhesiveness, which can bond the skin layer 10 to the base fabric 20 and impart impact absorption and flexibility to the synthetic leather 120. That is, the synthetic leather 120 has impact absorption and flexibility in addition to excellent cold resistance and chemical resistance, which are desired by the present invention, and is therefore very suitable for surface components of vehicle seats, for example.
[0074] The foaming adhesive layer 50 is a resin layer having a plurality of bubbles inside. The bubbles may be independent bubbles, or may partially or entirely constitute continuous bubbles. The resin constituting the foaming adhesive layer 50 is not particularly limited, and may be appropriately selected from foamable resins. For example, a foaming polyurethane resin layer or a foaming vinyl chloride resin layer is suitable as the foaming adhesive layer 50.
[0075] In particular, it is preferred that the foam adhesive layer 50 provided between the skin layer 10 containing vinyl chloride resin and plasticizer and the base fabric 20 is constituted to contain vinyl chloride resin and plasticizer. In this embodiment, the plasticizer contained in the foam adhesive layer 50 more preferably contains a polyester plasticizer having a number average molecular weight of 800 to 4000, and the polyester plasticizer accounts for 10% to 80% of the plasticizer contained in the foam adhesive layer 50.
[0076] By making the foam adhesive layer 50 and the adjacent skin layer 10 mutually contain vinyl chloride resin and plasticizer, it is possible to provide a synthetic leather 120 with further improved cold resistance and chemical resistance and better impact absorption and flexibility.
[0077] In addition, regarding the details of the vinyl chloride resin and the plasticizer that can be used for the foam adhesive layer 50, the description related to the vinyl chloride resin and the plasticizer used for the skin layer 10 in the first embodiment is appropriately referred to, and the detailed description is omitted here.
[0078] The forming method of the foaming adhesive layer 50 is not particularly limited. In the case of forming the foaming adhesive layer 50 as a foaming polyurethane resin layer, for example, a skin layer 10 is pre-formed on a release paper, and a coating liquid containing a foaming agent (water) and a polyurethane resin forming composition is applied on the skin layer 10. Then, heating is performed at a suitable temperature, so that the isocyanate group in the polyurethane resin forming composition reacts with water to produce carbon dioxide, and the isocyanate reacts with a polyol and solidifies. Thus, a foaming polyurethane resin layer having bubbles formed by allowing carbon dioxide to enter a carbamate polymer can be formed. By pasting a base fabric 20 during the period when the foaming polyurethane resin layer is not solidified, a laminate having a skin layer 10, a foaming adhesive layer 50 composed of a foaming polyurethane resin layer, and a base fabric 20 can be formed. By forming a surface protective layer 30 on the surface side of the skin layer 10 in the laminate, a synthetic leather 120 can be obtained.
[0079] In the case of forming the foamed adhesive layer 50 as a foamed vinyl chloride resin layer, for example, the skin layer 10 may be formed in advance on release paper, a coating liquid containing a foaming agent and a vinyl chloride resin may be applied to the skin layer 10, and then the foaming agent may be foamed by heating to form a foamed vinyl chloride resin layer containing fine bubbles. By attaching the base fabric 20 while the foamed vinyl chloride resin layer is not cured, a laminate including the skin layer 10, the foamed adhesive layer 50 composed of the foamed vinyl chloride resin layer, and the base fabric 20 can be formed. By forming the surface protective layer 30 on the surface side of the skin layer 10 in the laminate, the synthetic leather 120 can be obtained.
[0080] The thickness of the foam adhesive layer 50 is not particularly limited, but is preferably in the range of 50 μm to 500 μm. If the thickness is less than 50 μm, the adhesive strength may be deteriorated, and if it exceeds 500 μm, the texture may be deteriorated.
[0081] The second embodiment is an embodiment in which a layer containing a foamed resin is provided between the skin layer 10 and the base fabric 20. Figure 3 As shown in FIG. 1 , the synthetic leather 120 can be modified to a synthetic leather 130 in which the foamed adhesive layer 50 is replaced with a foamed layer 60 and an adhesive layer 40. The foamed layer 60 is a foamed resin layer, and can impart impact absorption and softness to the synthetic leather 130. In addition, the adhesive layer 40 bonds the foamed layer 60 to the base fabric 20, and as a result, the skin layer 10 is bonded to the base fabric 20. In this way, by providing the foamed layer 60 and the substantially non-foamed adhesive layer 40 as different layers, the contact area between the adhesive layer 40 and the base fabric 20 can be increased compared to the synthetic leather 120 described above. As a result, the synthetic leather 130 can exhibit better wear resistance than the synthetic leather 120.
[0082] The foam layer 60 can be formed by the same method as the method for forming the foam adhesive layer 50. After the foam layer 60 is formed, an adhesive for forming the adhesive layer 40 is applied to the surface of the foam layer 60, and then the base fabric 20 is attached, thereby forming a laminate constituting the synthetic leather 130. The synthetic leather 130 can be obtained by forming the surface protection layer 30 on the surface side of the epidermis layer 10 in the laminate.
[0083] The thickness of the foam layer 60 is not particularly limited, but is preferably 100 μm or more from the viewpoint of exhibiting good impact absorption and flexibility, and is preferably 500 μm or less from the viewpoint of cost.
[0084] The adhesive layer 40 and the surface protection layer 30 in the synthetic leather 130 can be configured similarly to the adhesive layer 40 and the surface protection layer 30 in the synthetic leather 110 described in the first embodiment, and thus detailed descriptions thereof are omitted here.
[0085] In addition, the synthetic leather 130 preferably includes a skin layer 10 composed of a vinyl chloride resin and a plasticizer, a foam layer 60 composed of a foamed vinyl chloride resin, and an adhesive layer 40 containing a vinyl chloride resin. In particular, it is more preferred that each layer of the skin layer 10, the foam layer 60, and the adhesive layer 40 contains a vinyl chloride resin at a ratio of 90% by mass or more in 100% by mass of the resin constituting each layer. As a result, the resin layer portion of the synthetic leather 130 other than the surface protection layer 30 is entirely composed of a vinyl chloride resin, so that the adhesion between adjacent layers becomes good, and the wear resistance can be further improved.
[0086] (Method for producing synthetic leather)
[0087] Hereinafter, an example of a method for manufacturing the synthetic leather 130 will be described. However, the manufacturing method described below does not limit the synthetic leather of the present invention in any way, and the synthetic leather of the present invention can be manufactured by other manufacturing methods as appropriate within the scope of the present invention. Hereinafter, the embodiment in which the surface layer 10, the foaming layer 60, and the adhesive layer 40 all contain a vinyl chloride resin will be described as an example.
[0088] First, a coating liquid for forming the skin layer 10 containing a vinyl chloride resin and a polyester plasticizer is prepared, applied to release paper using a knife coater, a comma knife coater, or other common coating means, and appropriately heated and dried to obtain the skin layer 10 .
[0089] Thereafter, a coating liquid for forming the foam layer 60 containing a foaming agent, a vinyl chloride resin and a polyester plasticizer is applied to the exposed surface of the obtained skin layer 10 by the same coating means as described above, and heated appropriately to foam the liquid, thereby forming the foam layer 60 .
[0090] Then, the coating liquid for forming the adhesive layer 40 containing a vinyl chloride resin is applied to the exposed surface of the obtained foam layer 60 by the above-mentioned coating means, and appropriately heated and dried to form the adhesive layer 40. The fiber base material for constituting the base fabric 20 is laminated on the semi-cured adhesive layer 40, and then the release paper and the like are peeled off to obtain a laminate. Thereafter, a coating liquid for forming the surface protective layer 30 containing a composition for forming a polyurethane resin and a crosslinking agent such as isocyanate is applied to the surface of the epidermis layer 10 and appropriately heated to form the surface protective layer 30, thereby obtaining the synthetic leather 130. In addition, before forming the surface protective layer 30, the surface of the epidermis layer 10 may be embossed to give a leather-like appearance.
[0091] In the above, the present invention is described using the first embodiment and the second embodiment, but these are examples of the present invention and do not limit the present invention in any way. In addition, the above-mentioned manufacturing method does not limit the manufacturing method of the synthetic leather of the present invention in any way. For example, the manufacturing of the synthetic leather 110 only requires omitting the step of forming the above-mentioned foaming adhesive layer 50 and forming the adhesive layer 40 after the skin layer 10. In addition, the manufacturing of the synthetic leather 120 only requires forming the foaming adhesive layer 50 in the same manner as the above-mentioned foaming layer 60 and laminating the fiber base material constituting the base fabric 20 while the foaming adhesive layer 50 is in a semi-cured state.
[0092] [Example]
[0093] The following is an explanation of the embodiments of the present invention. The following is an example of a synthetic leather having a base fabric, an adhesive layer, a skin layer, and a surface protective layer as an example to illustrate the embodiments and comparative examples. However, the embodiments shown below do not limit the present invention in any way.
[0094] First, the materials constituting each layer were prepared as follows. Table 1 shows the composition and the mixing ratio contained in the coating liquid for forming the skin layer and the surface protection layer.
[0095] <Coating liquid for forming skin layer>
[0096] · Vinyl chloride resin (ZEST PQHPN, manufactured by Shin-First Vinyl Chloride Co., Ltd.)
[0097] Polyester plasticizer (adipic acid polyester plasticizer, number average molecular weight 1500, acid value 0.2KOHmg / g)
[0098] Non-polyester plasticizer (phthalate plasticizer, number average molecular weight 450, acid value 0.07KOHmg / g)
[0099] In addition, the ratio of the polyester plasticizer was calculated based on the sum of the blending amounts of the polyester plasticizer and the non-polyester plasticizer in the coating liquid, that is, the total plasticizer being 100% by mass, and the results are shown in Table 1. In addition, the average acid value of the plasticizer in the coating liquid was calculated as the sum of the values obtained by multiplying the acid value of each plasticizer by each blending ratio, and the results are shown in Table 1.
[0100] <Coating liquid for forming foaming layer>
[0101] 100 parts by mass of vinyl chloride resin (ZEST PQHPN, manufactured by Shin-First Vinyl Chloride Co., Ltd.)
[0102] ·Polyester plasticizer (adipic acid polyester plasticizer, number average molecular weight 1500, acid value 0.2KOHmg / g) 45 parts by mass
[0103] · Non-polyester plasticizer (phthalate plasticizer, number average molecular weight 450, acid value 0.07 KOHmg / g) 20 parts by mass
[0104] · Foaming agent (azodicarbonamide) 1 part by mass
[0105] <Adhesive Layer Forming Coating Liquid>
[0106] 100 parts by mass of vinyl chloride resin (ZEST PQHPN, manufactured by Shin-First Vinyl Chloride Co., Ltd.)
[0107] ·Polyester plasticizer (adipic acid polyester plasticizer, number average molecular weight 1500, acid value 0.2KOHmg / g) 45 parts by mass
[0108] Non-polyester plasticizer (phthalate plasticizer, number average molecular weight 450, acid value 0.07 KOHmg / g) 20 parts by mass
[0109] (Base fabric)
[0110] Fiber base material (polyester knitted fabric, organic mass = 110g / m 2 , density = hole / row = 25 / 22)
[0111] <Surface protection layer forming coating liquid>
[0112] · Aqueous polyurethane resin composition (polycarbonate polyurethane composition, solid content: 25% by mass)
[0113] ·Crosslinking agent (carbodiimide)
[0114] ·Crosslinking agent (isocyanate)
[0115] In addition, the mixing ratio (mass parts) of the polycarbonate polyurethane composition shown in Table 1 is a mixing ratio including the mass of the solvent.
[0116] (Example 1)
[0117] The coating liquid for forming a skin layer prepared in the composition ratio shown in Table 1 was applied to release paper (manufactured by Dai Nippon Printing Co., Ltd., trade name "DE-73") to a thickness of 200 μm after drying, and dried in an oven at 180° C. for 1 minute to obtain a skin layer.
[0118] Next, the adhesive layer-forming coating liquid prepared as described above was applied to the exposed surface of the obtained skin layer to a thickness of 100 μm after drying, and a base fabric was laminated and dried at 200° C. for 3 minutes. The release paper was peeled off to obtain a laminate.
[0119] Then, the exposed surface of the skin layer of the laminate was coated with a coating having an amount of 30 g / m 2 The coating liquid for forming a surface protective layer prepared as described above was applied so that the thickness after drying would be 10 μm, and dried in an oven at 120° C. for 2 minutes to form a surface protective layer, thereby obtaining a synthetic leather as Example 1.
[0120] (Examples 2 to 6, Comparative Examples 1 to 3)
[0121] Examples 2 to 4, Example 6, and Comparative Examples 1 to 3 were carried out in the same manner as in Example 1, except that the composition ratios were changed to those shown in Table 1, to produce synthetic leathers.
[0122] Example 5 A synthetic leather was produced in the same manner as in Example 1 except that a foamed layer having a thickness of 300 μm was provided between the adhesive layer and the surface layer.
[0123] The examples and comparative examples obtained as described above were evaluated as follows. The evaluation results are shown in Table 1.
[0124] <Chemical Resistance Evaluation (Condition 1)>
[0125] The obtained synthetic leather was cut into 210×297 mm (A4 size in ISO 216) and prepared as a test piece. Next, a glass plate was placed on a tray, and the test piece was placed on the glass plate with the surface protection layer on top. A cotton white cloth (muslin cloth No. 3, kanakin) was placed on the test piece, and 15 ml of oleic acid was dripped onto the white cloth from above. Next, a glass plate was further placed on the white cloth, and in this state, the test piece was dried at 80°C for 72 hours. After drying, the glass plate and the white cloth were removed, and the surface of the test piece was wiped with a paper towel, and further dried at room temperature for 24 hours. After drying, the test piece was cut into φ130 mm (circle with a diameter of 130 mm) from the center of the test piece. According to the DuPont drop impact test based on JIS K5600-5-3, the cut φ130 mm test piece was set on the DuPont impact tester, and a drop ball test was performed. The ball drop test was carried out at room temperature. The load of the ball used for the ball drop was 800 g, and the drop distance of the ball was 15 cm. After the ball drop test, the surface (surface protection layer side) of the synthetic leather was visually observed and evaluated based on the following evaluation criteria.
[0126] <Chemical Resistance Evaluation (Condition 2)>
[0127] The test was conducted in the same manner as in the above-mentioned chemical resistance evaluation (Condition 1) except that the drying time in the 80° C. environment was set to 120 hours, and evaluation was performed based on the following evaluation criteria.
[0128] [Evaluation criteria]
[0129] ○: No cracks were observed on the surface of the test piece.
[0130] △: Fine cracks were observed on the surface of the test piece.
[0131] ×: Cracks were observed on the surface of the test piece, and the fabric (base fabric) on the back side was exposed.
[0132] <Cold resistance evaluation (condition 1)>
[0133] The obtained synthetic leather was cut into a φ130 mm (circle with a diameter of 130 mm) to prepare a test piece. Then, the test piece was placed in an atmosphere of -30°C for 60 minutes for cooling. After cooling, the DuPont drop impact test based on JIS K 5600-5-3 was immediately carried out under the same conditions as the above-mentioned chemical resistance evaluation. Then, after the drop ball test, the surface (surface protection layer side) of the synthetic leather was visually observed and evaluated based on the following evaluation criteria.
[0134] <Cold resistance evaluation (condition 2)>
[0135] The test was conducted in the same manner as in the above-mentioned cold resistance evaluation (condition 1) except that the test piece placement atmosphere was set to -40°C, and evaluation was performed based on the following evaluation criteria.
[0136] [Evaluation criteria]
[0137] ○: No cracks were observed on the surface of the test piece.
[0138] △: Fine cracks were observed on the surface of the test piece.
[0139] ×: Cracks were observed on the surface of the test piece, and the fabric (base fabric) on the back side was exposed.
[0140] <Abrasion resistance evaluation>
[0141] Using the obtained synthetic leather, abrasion resistance was evaluated as follows.
[0142] That is, using the Gakushin type friction tester specified in JIS-L-0823 (friction tester for color fastness test), collect the No. 6 cotton canvas of JIS-L-0823 with a width of 30 mm and a length of 250 mm, and fix it with a clamp in a way that no wrinkles are generated on the sample table of the tester. Prepare a test piece obtained by cutting the obtained synthetic leather into a width of 20 mm and a length of 50 mm, and firmly mount the test piece on the friction part with the surface protection layer side located on the outside. Then, set the pressing load of the friction part to 1000 gf (9.8N), the stroke to 100 mm, and the speed to 30 reciprocations / minute, and conduct a test of rubbing the friction part against the canvas set on the test table. Then, visually observe the surface state of the test piece after 30,000 reciprocations, and evaluate based on the following evaluation criteria.
[0143] [Evaluation criteria]
[0144] ○: No damage to the surface protection layer was observed.
[0145] △: Damage to the surface protection layer was slightly observed.
[0146] ×: The surface protective layer is obviously damaged.
[0147]
[0148] The above-mentioned embodiments include the following technical concepts.
[0149] (1) A synthetic leather comprising a skin layer and a base fabric, characterized in that:
[0150] The skin layer contains vinyl chloride resin and plasticizer.
[0151] The plasticizer contains a polyester plasticizer having a number average molecular weight of 800 to 4000.
[0152] The polyester plasticizer accounts for 10% to 80% by mass of 100% by mass of the plasticizer contained in the skin layer.
[0153] (2) The synthetic leather according to (1) above, wherein the average acid value (KOH mg / g) of the plasticizer is 0.1 or more.
[0154] (3) The synthetic leather according to (1) or (2) above, wherein:
[0155] A surface protection layer is provided on the surface of the epidermis layer on the side opposite to the base fabric.
[0156] The surface protection layer contains a polyurethane resin and a cross-linking agent.
[0157] The cross-linking agent contains isocyanate.
[0158] (4) The synthetic leather according to any one of (1) to (3) above, wherein
[0159] A foaming layer or a foaming adhesive layer is provided between the skin layer and the base fabric.
[0160] The foam layer or the foam adhesive layer contains a vinyl chloride resin and a plasticizer.
[0161] The plasticizer contains a polyester plasticizer having a number average molecular weight of 800 to 4000.
[0162] The polyester plasticizer accounts for 10% by mass or more and 80% by mass or less of 100% by mass of the plasticizer contained in the foam layer or the foam adhesive layer.
Claims
1. A synthetic leather comprising an epidermis layer and a base fabric, characterized in that: The skin layer contains vinyl chloride resin and plasticizer. The plasticizer contains a polyester plasticizer having a number average molecular weight of 800 to 4000. In 100% by mass of the plasticizer contained in the skin layer, the polyester plasticizer accounts for 10% by mass or more and 80% by mass or less, The average acid value (KOHmg / g) of the plasticizer contained in the skin layer is 0.15 or more, A surface protection layer is provided on the surface of the epidermis layer on the side opposite to the base fabric. The surface protection layer contains a polyurethane resin and a cross-linking agent. The cross-linking agent contains isocyanate, The ratio of the cross-linking agent to be added is 2 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the polyurethane resin.
2. The synthetic leather according to claim 1, characterized in that A foaming layer or a foaming adhesive layer is provided between the skin layer and the base fabric. The foam layer or the foam adhesive layer contains a vinyl chloride resin and a plasticizer. The plasticizer contains a polyester plasticizer having a number average molecular weight of 800 to 4000. The polyester plasticizer accounts for 10% by mass or more and 80% by mass or less of 100% by mass of the plasticizer contained in the foam layer or the foam adhesive layer.