A method for manufacturing a shingled battery and a component
By printing high-temperature silver paste on the battery cell to form a secondary gate and main gate, and using low-temperature silver paste in component production, the line loss and leakage problems caused by the overlapping of the main gate and the edge in the stacked tiling assembly are solved, and the utilization of the battery is improved rate and component safety and power.
Patent Information
- Application Number
- CN202111406881.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2041-11-24
AI Technical Summary
During the production process of stacked tiling components, the overlap between the main gate and the edge of the battery cell leads to line loss and waste of battery area, and excessive shortening of the distance between the main gate and the edge will lead to leakage risks, affecting the quality and reliability of the components.
By printing high-temperature silver paste on the front of the cell, it forms ohmic contact between the secondary gate and the N-type diffusion layer, and printing high-temperature silver paste at the main gate position, drying and annealing to shorten the distance between the main gate and the edge, while using it in component production Low-temperature silver paste replaces conductive glue. The low-temperature silver paste passes through the silicon nitride layer on the curing table to form ohmic contact, bypassing the high-temperature silver paste to avoid the risk of leakage.
It effectively shortens the distance between the main gate of the battery cell and the edge, improves the utilization rate of the battery and the safety of the components, reduces costs, and improves the conductivity and power between the battery cells.
Smart Images

Figure CN114122163B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solar photovoltaic cells, and in particular relates to a method for manufacturing a shingled cell and a component. Background Art
[0002] At present, with the continuous development of the photovoltaic industry, the battery conversion efficiency and the power of the module are constantly improving. In response to the development of the market, the shingled module version came into being, and its higher power density is welcomed by the market. The shingled module is a module formed by cutting the battery sheet (mother sheet) into battery cells of preset size according to a certain method, and then rearranging the battery cells in series and parallel. The shingled module does not use welding ribbons to stack the battery cells in the limited space of the module, which not only reduces the line loss of the module but also increases the power of the module.
[0003] With the development of shingled modules, on the one hand, the pursuit of higher module power is pursued, and on the other hand, the cost of modules is reduced.
[0004] Each cell after cutting contains a main grid and several auxiliary grids as the path for current collection and conduction. In the production process of shingled modules, the main grids at the edges of two cells, the front side (N side) of a cell and the back side (P side) of a cell overlap each other and are bonded with conductive glue. The area from the main grid to the edge of the cell will be overlapped and covered and no longer play a role. On the one hand, the current conductive glue uses organic matter in the colloid to bond the metal main grids on the two cells, and uses the metal in the conductive glue (usually silver) to reduce the resistance of the organic matter and improve the conductivity. Finally, the two cells are electrically connected. This bonding method still has high line loss, which becomes an obstacle to the power increase of the module. On the other hand, the parts from the main grid to the edge of the two cells overlap each other, wasting this part of the battery area. If you want to improve the effective utilization of the battery cell, you must continuously reduce the distance from the main grid to the edge. However, the distance from the main grid to the edge of the battery cell is constantly reduced. In the distribution of battery cells in the battery sheet (mother sheet), if the battery cells are to be arranged uniformly, the distance from the main grid on the front (N side) of one of the battery cells to the edge of the battery sheet (mother sheet) must be shortened. However, since the thickness of the passivation layer such as silicon nitride on the edge of the front (N side) of the battery sheet (mother sheet) decreases as it approaches the edge, if the distance between the main grid and the edge is excessively reduced, the main grid silver paste will not be protected by the passivation layer such as silicon nitride. After sintering, it will directly burn through the N-type area and connect to the P-type substrate to form conductivity. In this way, there is a risk of leakage at the edge of the battery cell, which will seriously affect the quality and reliability of the component. Summary of the invention
[0005] The present invention provides a method for manufacturing a shingled battery and a component, which shortens the distance between the main grid and the edge and improves the battery utilization rate.
[0006] To achieve the above object, a method for manufacturing a shingled battery according to the present invention comprises the following steps:
[0007] Step 1: Print multiple sub-grids on the front of the cell body with high-temperature silver paste, and then make the sub-grids and the N-type diffusion layer form ohmic contact;
[0008] Step 2: Print a main grid with high-temperature silver paste at the main grid position on the edge of the battery cell body;
[0009] Step 3: Dry and anneal the structure obtained in step 2, so that the main grid enters a part of the front passivation layer and does not form contact with the N-type diffusion layer, thereby obtaining a battery cell.
[0010] Furthermore, in step 1, an ohmic contact is formed between the auxiliary gate and the N-type diffusion layer by sintering.
[0011] Furthermore, the sintering temperature is 500°C to 800°C.
[0012] Furthermore, in step 2, the distance from the main grid to the edge of the cell is less than 0.mm.
[0013] Furthermore, in step 3, drying and annealing are performed below °C.
[0014] Furthermore, in step 3, the main grid is dried using a photothermal furnace.
[0015] A method for manufacturing a shingled assembly comprises the following steps:
[0016] S1, manufacturing a battery cell according to the above-mentioned shingled battery manufacturing method;
[0017] S2, dicing and cutting the battery sheet to form a plurality of battery cells, wherein the cutting line is parallel to the main grid;
[0018] S3, printing low-temperature silver paste at the main grid position of the battery cell;
[0019] S4. Arrange a plurality of battery cells printed with low-temperature silver paste, and then cure them on a curing station. During the curing process, the low-temperature silver paste forms an ohmic contact with the front side of the battery cell to obtain a shingled assembly.
[0020] Furthermore, in S4, when arranging the cells, the overlapping width of two adjacent cells is 0.25 mm.
[0021] Compared with the prior art, the present invention has at least the following beneficial technical effects:
[0022] The manufacturing method of the battery cell described in the present invention only prints the edge main grid on the front side during battery cell production, and the main grid does not form ohmic contact with the N-type diffusion layer, thereby reducing the risk of high-temperature silver paste penetrating the N-type diffusion layer, shortening the distance between the main grid and the edge, improving battery utilization, and reducing battery costs.
[0023] Furthermore, the temperature of the drying furnace is maintained below 300°C to avoid the risk of the main grid at the edge of the cell penetrating the silicon nitride and N-type layer and directly electrically connecting with the P-type layer under high temperature conditions, thereby improving the safety of the shingled module.
[0024] Furthermore, some existing production lines are equipped with a photothermal furnace behind the sintering furnace, and the temperature is generally below 300°C. The photothermal furnace can be used as a drying furnace for the edge main grid of the final battery cell (mother cell), which is easy to operate and improves production efficiency.
[0025] The manufacturing method of the shingled assembly described in the present invention uses low-temperature silver paste to replace the conductive glue during the production of the shingled assembly. During the curing stage, for the battery cell without the front main grid, the low-temperature silver paste as the main grid will pass through the battery passivation layer such as the front silicon nitride on the curing table with a lower temperature to form an ohmic contact and form a good electrical connection with the back of another battery cell. On the battery cell with the front main grid, the high-temperature silver paste protects the N-type diffusion layer from being penetrated by the low-temperature silver paste while forming an ohmic contact. The low-temperature silver paste must bypass the high-temperature silver paste and pass through the battery passivation layer such as silicon nitride to form an ohmic contact with the battery cell. At this time, the high-temperature silver paste, as part of the passivation layer, hinders the penetration of the low-temperature silver paste, so that the low-temperature silver paste can only bypass the high-temperature silver paste to increase the stroke and form an ohmic contact with the battery cell, avoiding the risk of the low-temperature silver paste penetrating the N-type area, and forming good adhesion and conductivity. In this way, the distance from the printed main grid of the battery to the edge of the battery cell can be shortened, the utilization rate of the battery can be improved, and the battery cost can be reduced; the conductivity between the battery cells can be improved, the line resistance can be reduced, and the power can be increased. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a schematic diagram of an existing battery cell;
[0027] Figure 2 is a schematic diagram of an existing battery unit;
[0028] Figure 3 A schematic diagram of the overlap width of battery cells in the existing process;
[0029] Figure 4 This is a front view of the battery cell of the present invention after completion;
[0030] Figure 5 A schematic diagram of the overlapping width of the battery cells of the present invention;
[0031] Figure 6 This is a cross-sectional structural diagram of a battery containing a main grid after front printing of the present invention;
[0032] Figure 7 The cross-sectional structure diagram after printing low-temperature silver paste for a battery cell without a main grid;
[0033] Figure 8 A schematic diagram of a battery cell after dicing and cutting according to the present invention;
[0034] Fig. 9 This is a cross-sectional structural diagram of the battery unit containing the main grid of the present invention after printing low-temperature silver paste.
[0035] In the attached figure: 1. battery cell, 2. battery unit, 3. main grid, 4. auxiliary grid, 5. back passivation layer, 6. substrate, 7. N-type diffusion layer, 8. front passivation layer, 9. low-temperature silver paste. DETAILED DESCRIPTION
[0036] In order to make the purpose and technical solution of the present invention clearer and easier to understand, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0037] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more. In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0038] Reference Figure 1 and Figure 2In the manufacturing process of the existing battery cell 1, a P-type silicon wafer is used as the substrate 6, and an N-type diffusion layer 7 with a thickness of 200 to 400 nm is formed on the substrate by diffusing phosphorus to form a PN junction. In addition, a 60 to 100 nm thick front passivation layer is plated on the substrate forming the PN junction, such as silicon nitride, silicon oxide, etc., with different thicknesses depending on the process. Finally, a high-temperature silver paste is printed on the front side (N side) by screen printing. At 500°C to 800°C, the high-temperature silver paste passes through the silicon nitride layer and forms an ohmic contact with the N-type diffusion layer 7. The high-temperature silver paste is a silver paste that is sintered at 500 to 800°C to form an ohmic contact.
[0039] Reference Figure 3 Under the existing process, the minimum distance between the main grid 3 on the front side (N side) of the battery cell (mother cell) and the edge is 0.5 mm, the width of the main grid 3 is generally 0.5 mm, and the minimum width of the two battery cells 2 covered after overlapping is 1.5 mm.
[0040] Example 1
[0041] A method for manufacturing a shingled battery provided by the present invention comprises the following steps:
[0042] Step 1: The main grid at the edge of the front side (N side) of the cell (mother cell) is no longer printed and sintered according to the existing process scheme. First, the secondary grid is printed on the front side (N side) of the cell with high-temperature silver paste, and then sintered at 500°C to 800°C in a sintering furnace to form an ohmic contact;
[0043] Step 2: Print a main grid 3 at the main grid 3 position at the edge of the battery cell (mother cell) with high-temperature silver paste. At this time, the main grid is only printed near the edge of the front side of each battery cell;
[0044] Step 3: Dry and anneal the cell 2 obtained in step 2 in a photothermal furnace. During drying and annealing, the temperature of the drying furnace is kept below 300°C to avoid the main grid 3 at the edge of the cell 1 (mother sheet) from penetrating the silicon nitride and N-type layer to directly connect electrically with the P-type layer and cause leakage under high temperature conditions, thereby improving the safety of the shingled component. Figure 4 The cell shown. Some existing production lines even have a photothermal furnace behind the sintering furnace, and the temperature is generally below 300°C. The photothermal furnace can be used as a drying furnace for the edge main grid of the final cell (mother cell). The distance from the front (N side) edge main grid to the edge of the cell is greatly reduced, which improves the battery utilization rate and reduces production costs. The distance from the front (N side) main grid 3 to the edge is reduced to 0.25mm, and the overlap width is reduced by 0.5mm, as shown in the figure. Figure 5 As shown in the figure, taking a 158mm battery sheet (mother sheet) containing 6 battery cells as an example, if the overlap width is reduced by 0.5mm, the utilization area of the battery can be increased by 2.01%.
[0045] For the finished cell (mother) sheet, the secondary grid 4 on the front side (N side) has formed an ohmic contact with the N-type diffusion layer 7, and the main grid 3 has only been dried and entered into a part of the front passivation layer 8, and does not form contact with the N-type diffusion layer 7. In addition, the main grid is only printed at the edge of the front side (N side) of the cell (mother) sheet, and there is no main grid at other positions. The distance D from the main grid 3 to the edge of the cell can be controlled at 0.25mm, which is mainly limited by the printing accuracy of the existing machine.
[0046] Example 2
[0047] Reference Figures 6 to 8 , a method for manufacturing a shingled assembly, comprising the following steps:
[0048] S1. Prepare a battery cell according to the method described in Example 1;
[0049] S2, the finished battery cell is sliced and cut, the cutting line is parallel to the main grid 3, and the slicing and cutting obtains a plurality of small battery cells 2, such as Figure 6 As shown;
[0050] S3. Print low-temperature silver paste at the main grid position of the battery cell 2 after dicing to replace the existing main grid and conductive glue. The low-temperature silver paste generally has an operating temperature of 120-200°C, such as Shanren AS9100. At the position where the high-temperature silver paste is not printed on the front side (N side), the low-temperature silver paste 9 can directly penetrate the front passivation layer 8 to form an ohmic contact. The high-temperature silver paste at the position where the high-temperature silver paste has been printed can prevent the low-temperature silver paste from penetrating the N-type diffusion layer 7 to form an ohmic contact with the N-type diffusion layer 7 and destroy the PN junction, and can ensure efficient conduction of current.
[0051] S4, arranging a plurality of battery cells 2 printed with low-temperature silver paste, and then curing them on a curing station to obtain a shingled assembly.
[0052] When arranging cells, the distance from the main grid 3 to the edge of the front side (N side) of the battery cell 2 is 0.25 mm. Figure 5 shown.
[0053] After the curing stage, refer to Figure 7 For battery cells without a front (N-side) main grid, the low-temperature silver paste will penetrate the front (N-side) silicon nitride and other battery passivation layers on a curing table with a relatively low temperature (200°C) to form an ohmic contact and form a good electrical connection with the back of another battery cell. Figure 8 and Fig. 9On the battery cell with the existing front (N-side) main grid, the low-temperature silver paste will bypass the high-temperature silver paste, pass through the battery passivation layer such as silicon nitride and form an ohmic contact with the battery cell. At this time, the high-temperature silver paste, as part of the passivation layer, hinders the penetration of the low-temperature silver paste, so that the low-temperature silver paste can only bypass the high-temperature silver paste to increase the stroke and form an ohmic contact with the battery cell, avoiding the risk of the low-temperature silver paste penetrating the N-type area, and forming good adhesion and conductivity. In this way, the distance from the printed main grid of the battery to the edge of the battery cell can be shortened, the battery utilization rate can be improved, and the battery cost can be reduced; the conductivity between battery cells can be improved, the line resistance can be reduced, and the power can be increased.
[0054] Since the low-temperature silver paste forms an ohmic contact with a battery cell 2, it can reduce the line resistance between two stacked battery cells, improve the current conduction efficiency, and thus increase the component power.
[0055] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for manufacturing a shingled assembly, characterized in that: The following steps are involved: S1, making a battery cell, including the following steps: S1.1, printing a plurality of auxiliary grids on the front side of the battery cell body using high temperature silver paste, and then forming an ohmic contact between the auxiliary grid (4) and the N-type diffusion layer (7); S1.2, printing a main grid (3) at the main grid (3) position at the edge of the battery cell body using high temperature silver paste; S1.3, drying and annealing the structure obtained in step S1.2, so that the main grid (3) enters a portion of the front passivation layer (8) and does not form contact with the N-type diffusion layer (7), thereby obtaining a battery cell; In the step S1.1, an ohmic contact is formed between the auxiliary gate (4) and the N-type diffusion layer (7) by a sintering method; In the step S1.3, drying and annealing are performed at a temperature below 300°C; S2, slicing and cutting the battery sheet to form a plurality of battery cells (2), with the cutting line being parallel to the main grid; S3, printing low-temperature silver paste (9) at the main grid position of the battery cell (2); S4, arranging a plurality of battery cells (2) printed with low-temperature silver paste (9), and then curing them on a curing station. During the curing process, the low-temperature silver paste (9) forms an ohmic contact with the front surface of the battery cell (2), thereby obtaining a shingled assembly.
2. A method for manufacturing a shingled assembly according to claim 1, characterized in that: In S4, when arranging the cells, the overlapping width of two adjacent cells is 0.25 mm.
3. The method for manufacturing a shingled assembly according to claim 1, characterized in that: The sintering temperature is 500°C to 800°C.
4. The method for manufacturing a shingled assembly according to claim 1, characterized in that: In step S1.2, the distance between the main grid (3) and the edge of the cell is less than 0.25 mm.
5. The method for manufacturing a shingled assembly according to claim 1, characterized in that: In the step S1.3, the main grid is dried using a photothermal furnace.
Citation Information
Patent Citations
Method for preparing crystalline silicon solar battery electrode by utilizing overprinting way
CN101656276A
Method for forming metal electrode on surface of solar battery
CN102468369A
Nanometer silicon phosphorus slurry, method for preparing same and application of same
CN103489932A
Battery piece, imbricate assembly and manufacturing method of battery piece
CN112582491A
Metal alloy series-connected imbricated photovoltaic module cell string and preparation method thereof