Coupled post-consumer recycled polypropylene and methods of providing the same

By adding 4,4'-oxydiphenylsulfonyl azide to the polypropylene after consumption and melt blending, the problem of insufficient melt flow rate and strength of PCR-PP in blow molding applications is solved, and the problem of insufficient melt flow rate and strength of PCR-PP is achieved. More suitable application performance.

CN114127172BActive Publication Date: 2024-11-08DOW GLOBAL TECHNOLOGIES LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080051931.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2020-06-22
Publication Date
2024-11-08
Estimated Expiration
2040-06-22

AI Technical Summary

Technical Problem

The existing post-consumer recycled polymer (PCR) propylene-based fractions have insufficient melt flow rate and melt strength in blow molding applications, which have contamination problems, limiting their application range.

Method used

The melt flow rate (MFR I2) was formed by adding 4,4'-oxydiphenyl sulfonyl azide (DPO-BSA) to post-consumer recirculated polypropylene (PCR-PP) and melt blending DPO-BSA-coupled PCR-PP equal to or less than 5 g/10 minutes improves its melt strength.

Benefits of technology

The melt strength and flowability of DPO-BSA-coupled PCR-PP is significantly improved, making it suitable for blow molded products and other applications, overcoming the problem of high flow rate but insufficient strength of the original PCR-PP.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114127172B_ABST
    Figure CN114127172B_ABST
Patent Text Reader

Abstract

The present disclosure provides a method. The method includes (i) providing a post-consumer recycled polypropylene (PCR-PP) having a melt flow rate (MFR I2) equal to or greater than 7.0 g / 10 min; (ii) adding 4,4′-oxydiphenylsulfonyl azide (DPO-BSA) to the PCR-PP; (iii) melt blending the PCR-PP with the DPO-BSA; and (iv) forming a DPO-BSA-coupled PCR-PP having a melt flow rate (MFR I2) equal to or less than 5 g / 10 min.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art

[0001] There is a growing need to be able to utilize post-consumer recycled (PCR) polymers in a variety of applications. While modern sorting techniques for PCR sources enable the polymers to be sorted into propylene-based fractions and ethylene-based fractions, the sorting process is not perfect and contamination still exists in each fraction. Due to contamination, the applications in which each fraction can be successfully utilized are more limited than for the virgin polymer counterpart. In particular, PCR propylene-based polymer fractions do not exhibit suitable physical properties, such as melt flow rate and melt strength, for applications such as blow molded articles.

[0002] The art recognizes the need for PCR propylene-based polymers having melt strength suitable for molding applications, and particularly blow molding applications. Summary of the invention

[0003] The present disclosure provides a method. The method includes (i) providing a post-consumer recycled polypropylene (PCR-PP) having a melt flow rate (MFR I2) equal to or greater than 7.0 g / 10 min; (ii) adding 4,4′-oxydibenzenesulfonyl azide (DPO-BSA) to the PCR-PP; (iii) melt blending the PCR-PP and the DPO-BSA; and (iv) forming a DPO-BSA-coupled PCR-PP having a melt flow rate (MFR I2) equal to or less than 5 g / 10 min.

[0004] The present disclosure also provides a composition. The composition includes 4,4'-oxydibenzenesulfonyl azide coupled post-consumer recycled polypropylene (DPO-BSA coupled PCR-PP) having (i) a melt flow rate (MFR I2) equal to or less than 5 g / 10 min; and (ii) greater than 0 ppm to 350 ppm of sulfur.

[0005] The present disclosure also provides a molded article. The molded article includes a first surface layer comprising a polyolefin; an inner layer comprising a composition comprising 4,4′-oxydibenzenesulfonyl azide coupled post-consumer recycled polypropylene (DPO-BSA coupled PCR-PP) having a melt flow rate (MFR I2) equal to or less than 5 g / 10 min; and a second surface layer comprising a propylene-based polymer.

[0006] definition

[0007] Any reference to the Periodic Table of the Elements is to the Periodic Table as published by CRC Press, Inc., 1990-1991. Reference to a group of elements in the table is made by a new notation for numbering the groups.

[0008] For purposes of U.S. patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or their equivalent U.S. versions are so incorporated by reference), especially with respect to definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and common general knowledge in the art.

[0009] Numerical ranges disclosed herein include all values ​​from the upper and lower limits, and all values ​​include the upper and lower limits. For ranges containing explicit values ​​(e.g., 1 or 2 or 3 to 5 or 6 or 7 ranges), any subranges between any two explicit values ​​are included (e.g., above ranges 1-7 include subranges 1 to 2; 2 to 6; 5 to 7; 3 to 7; 5 to 6; etc.).

[0010] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all test methods are current as of the filing date of this disclosure.

[0011] "Alpha-olefin", "α-olefin" and similar terms refer to a hydrocarbon molecule or a substituted hydrocarbon molecule (i.e., a hydrocarbon molecule containing one or more atoms other than hydrogen and carbon, such as halogens, oxygen, nitrogen, etc.), the hydrocarbon molecule containing (i) only one olefinic unsaturated bond, which is located between the first and second carbon atoms, and (ii) at least 2 carbon atoms, preferably 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms in some cases, and preferably 4 to 8 carbon atoms in other cases. Non-limiting examples of α-olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-dodecene, and mixtures of two or more of these monomers.

[0012] "Blend", "polymer blend" and similar terms refer to a composition of two or more polymers. Such blends may or may not be miscible. Such blends may or may not be phase separated. Such blends may or may not contain one or more domain configurations, as determined by transmission electron spectroscopy, light scattering, x-ray scattering, and any other method for measuring and / or identifying domain configurations.

[0013] The term "composition" refers to a mixture of materials comprising the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0014] The terms "comprising", "including", "having" and their derivatives are not intended to exclude the presence of any additional components, steps or procedures, whether or not the components, steps or procedures are specifically disclosed. For the avoidance of any doubt, all compositions claimed through the use of the term "comprising" may include any additional additives, adjuvants or compounds, whether polymeric or otherwise, unless specified to the contrary. Conversely, the term "consisting essentially of excludes from the scope of any subsequent listing any other components, steps or procedures, except those that are not essential to operability. The term "consisting of excludes any component, step or procedure not specifically depicted or listed. Unless otherwise specified, the term "or" refers to the members of the list individually and in any combination. The use of the singular includes the use of the plural and vice versa.

[0015] "Ethylene-based polymers" are polymers containing more than 50 weight percent (wt%) of polymerized ethylene monomers (based on the total amount of polymerizable monomers) and optionally may contain at least one comonomer. Ethylene-based polymers include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). The terms "ethylene-based polymers" and "polyethylene" are used interchangeably. Non-limiting examples of ethylene-based polymers (polyethylene) include low-density polyethylene (LDPE) and linear polyethylene. Non-limiting examples of linear polyethylene include linear low-density polyethylene (LLDPE), ultra-low-density polyethylene (ULDPE), very low-density polyethylene (VLDPE), multi-component ethylene-based copolymers (EPE), ethylene / α-olefin multi-block copolymers (also known as olefin block copolymers (OBC)), substantially linear or linear plastomers / elastomers, and high-density polyethylene (HDPE). In general, polyethylene can be produced in a gas phase fluidized bed reactor, a liquid phase slurry reactor, or a liquid phase solution reactor using a heterogeneous catalyst system (such as a Ziegler-Natta catalyst), a homogeneous catalyst system comprising a Group 4 transition metal and a ligand structure (e.g., a metallocene, a non-metallocene metal center, a heteroaryl, an isovalent aryloxy ether, a phosphinimine, etc.). Combinations of heterogeneous and / or homogeneous catalysts can also be used in a single reactor or dual reactor configuration.

[0016] "Interpolymer" is a polymer prepared by polymerizing at least two different monomers. This general term includes copolymers, usually employed to refer to polymers prepared from two different monomers, and polymers prepared from more than two different monomers, for example, terpolymers, tetrapolymers, and the like.

[0017] "Low density polyethylene" (or "LDPE") is a polyethylene homopolymer or a polyethylene copolymer containing at least one C3-C6H2O2 having a density of 0.915 g / cc to less than 0.940 g / cc. 10 LDPE is composed of ethylene / α-olefin copolymers of α-olefins and contains long chain branches with broad MWD. ​​LDPE is usually produced by high pressure free radical polymerization (tubular reactor or autoclave with free radical initiator). Non-limiting examples of LDPE include MarFlex TM (Chevron Phillips), LUPOLEN TM (LyondellBasell), as well as LDPE products from Borealis, Ineos, ExxonMobil, etc.

[0018] As in 13 The term "not perceptible" used in the context of reporting alkyl branching in a C NMR analysis indicates that the branching is not detectable at a given signal-to-noise ratio.

[0019] "Olefin-based polymers" or "polyolefins" are polymers containing more than 50 weight percent polymerized olefin monomers (based on the total amount of polymerizable monomers) and optionally may contain at least one comonomer. A non-limiting example of an olefin-based polymer is an ethylene-based polymer.

[0020] "Polymer" is a polymeric compound prepared by polymerizing monomers, whether of the same type or different types. Thus, the general term polymer encompasses the term "homopolymer" (used to refer to polymers prepared from only one type of monomer, with the understanding that trace amounts of impurities can be incorporated into the polymer structure), as well as the term "interpolymer", which includes copolymers (used to refer to polymers prepared from two different types of monomers), terpolymers (used to refer to polymers prepared from three different types of monomers) and polymers prepared from more than three different types of monomers. Trace amounts of impurities, such as catalyst residues, can be incorporated into and / or within the polymer. It also encompasses all forms of copolymers, such as random, block, etc. It should be noted that although polymers are often referred to as being "made of" one or more specified monomers, "based on" a specified monomer or monomer type, "containing" a specified monomer content, etc., in this article, the term "monomer" should be understood to refer to the polymerized residue of the specified monomer rather than unpolymerized substances. In general, the polymer herein refers to a "unit" based on the corresponding monomer in polymerized form.

[0021] A "propylene-based polymer" is a polymer containing more than 50 weight percent polymerized propylene monomer (based on the total amount of polymerizable monomers) and optionally may contain at least one comonomer. Propylene-based polymers include propylene homopolymers and propylene copolymers (meaning units derived from propylene and one or more comonomers). The terms "propylene-based polymer" and "polypropylene" are used interchangeably. Non-limiting examples of propylene-based polymers (polypropylenes) are polypropylenes having at least one C2 or C4-C 10 Propylene / α-olefin copolymers with α-olefin comonomers.

[0022] "Virgin polymer" is a polymer that has not been recycled industrially or through consumer waste streams. Virgin polymer refers to a polymer that has not been used in the manufacturing process of a plastic product or otherwise recycled or regenerated. Non-limiting examples of virgin polymers include virgin ethylene-based polymers and virgin propylene-based polymers.

[0023] Test Method

[0024] Charpy impact energy was measured according to ISO 179-1 at 23°C, 0°C and -20°C. The results are expressed in kJ / m 2 ) is recorded as a unit.

[0025] Density is measured according to ASTM D792 Method B. Results are reported in grams per cubic centimeter (g / cc).

[0026] Flexural modulus is measured according to ISO 178. Results are reported in megapascals (MPa).

[0027] The melt flow rate (MFR) of propylene-based polymers (such as PCR-PP) and compositions is measured according to ASTM D1238 and is reported in grams eluted per 10 minutes (g / 10 min). MFR is at 230°C under a load of 2.16 kg (MFR I2); and at 230°C under a load of 10.0 kg (MFR I 10 ) measured

[0028] The melt index (MI) of ethylene-based polymers is measured according to ASTM D1238 and is reported in grams eluted per 10 minutes (g / 10 min). MI is at 190°C under a load of 2.16 kg (MI I2); and at 190°C under a load of 10.0 kg (MI I 10 ) measured

[0029] Shore A hardness was measured according to ASTM D2240-05.

[0030] Differential Scanning Calorimetry (DSC)

[0031] Differential scanning calorimetry (DSC) can be used to measure the melting, crystallization and glass transition behavior of polymers over a wide range of temperatures. For example, a TA Instruments Q1000 DSC equipped with a refrigerated cooling system (RCS) and an autosampler is used to perform this analysis. During the test, a nitrogen purge gas flow of 50 ml / min is used. Each sample is melt pressed into a film at 190°C; the molten sample is then air cooled to room temperature (25°C). A 3-10 mg, 6 mm diameter sample is extracted from the cooled polymer, weighed, placed in a lightweight aluminum pan (50 mg), and crimped. Analysis is then performed to determine its thermal properties.

[0032] The thermal behavior of the sample is determined by ramping up and down the sample temperature to produce a heat flow versus temperature curve. First, the sample is quickly heated to 180°C and kept isothermal for 3 minutes to remove its thermal history. Next, the sample is cooled to -80°C at a cooling rate of 10 degrees Celsius / minute and kept isothermal at -80°C for 3 minutes. Next, the sample is heated to 180°C at a heating rate of 10°C / minute (this is the "second heating" ramp). The cooling and second heating curves are recorded. The determined value is the extrapolated melting start temperature T m and the extrapolated crystallization onset temperature T c The heat of fusion (H f ) (in Joules / gram) and calculated % crystallinity were performed using the following equation:

[0033] Crystallinity % = ((H f ) / 165J / g)×100.

[0034] Report the heat of fusion (H) from the second heating curve f ) and the peak melting temperature. The peak crystallization temperature is determined from the cooling curve.

[0035] The melting point T is determined from the DSC heating curve by first drawing a baseline between the beginning and end of the melting transition. m A tangent line is then drawn to the data on the low temperature side of the melting peak. The intersection of this line with the baseline is the extrapolated melting onset temperature (T m ). This is as described in Bernhard Wunderlich, The Basis of Thermal Analysis, in Thermal Characterization of Polymeric Materials, 92, 277-278 (Edith A. Turi, ed., 2nd edition, 1997).

[0036] Crystallization temperature T c Determined as above from the DSC cooling curve, except that a tangent line is drawn on the high temperature side of the crystallization peak. The point where this tangent line intersects the baseline is the crystallization (T c )’s extrapolation starting point.

[0037] Glass transition temperature T g The heat capacity is determined from the DSC heating curve in which half of the sample has reached liquid heat capacity, as described in Bernhard Wunderlich, Fundamentals of Thermal Analysis in Thermal Characterization of Polymeric Materials 92, 278-279 (Edith A. Turi, ed., 2nd ed. 1997). Base lines are drawn from above and below the glass transition region and through T g The temperature at which the sample heat capacity is in the middle of these baselines is T g .

[0038] 1 H NMR analysis - total unsaturation per mole of propylene

[0039] The sample was prepared by adding about 3.25 g of a 50 / 50 mixture of tetrachloroethane-d2 / tetrachloroethylene at 0.0015 M in chromium acetylacetonate (relaxant) to 0.130 g of sample in a 10 mm NMR tube. The sample was dissolved and homogenized by heating the tube and its contents to 110 ° C. Data was collected using a Bruker 400 MHz spectrometer equipped with a Bruker Dual DUL high temperature and low temperature probe. Unsaturation data were collected using 4 scans per data file and a 15.6 second pulse repetition delay, with a sample temperature of 120 ° C. The spectral width of 10,000 Hz and the file size of 16K data points were collected. Presaturation experiments were run with a modified pulse sequence lc1prf2.zz1 using 100 scans per data file.

[0040] Use the following calculation:

[0041] Number of moles of H from propylene: Propylene mole fraction* (integrated area δ3.5-0.2ppm)

[0042]

[0043] Mol% cis / trans unsaturation / mol propylene Mol% trisubstituted unsaturation / mol propylene

[0044]

[0045] Mol% vinylidene unsaturation / mol propylene

[0046]

[0047] Total mol% unsaturation / mol propylene

[0048] Mol% vinyl + cis and trans moles + Mol% trisubstituted + Mol+vinylidene DETAILED DESCRIPTION

[0049] The present disclosure provides a method. The method includes (i) providing a post-consumer recycled polypropylene (PCR-PP) having a melt flow rate (MFR I2) equal to or greater than 7.0 g / 10 min; (ii) adding 4,4′-oxydibenzenesulfonyl azide (DPO-BSA) to the PCR-PP; (iii) melt blending the PCR-PP and the DPO-BSA; and (iv) forming a DPO-BSA-coupled PCR-PP having a melt flow rate (MFR I2) equal to or less than 5 g / 10 min.

[0050] i. Provide post-consumer recycled polypropylene

[0051] The method comprises the steps of providing a post-consumer recycled polypropylene (PCR-PP) having a melt flow rate (MFR I2) equal to or greater than 7.0 g / 10 min.

[0052] "Post-consumer recycled polypropylene" or "PCR-PP" is a polymeric material that is extruded by a virgin material manufacturer after initial processing. In other words, PCR-PP is a polymeric material that was previously used, for example, as consumer packaging or industrial packaging. PCR-PP may be from a post-consumer source, or from a mixture of post-industrial and post-consumer sources. PCR-PP also includes residues from its original use, such as residues of paper, adhesives, inks, nylon, ethylene vinyl alcohol (EVOH) copolymers, polyethylene terephthalate (PET), and other odor-causing agents. Non-limiting examples of suitable sources of PCR-PP include food packaging, consumer packaging, blow molded bottles, films, syringe boxes, IV bags, tubing, tubing fittings, and combinations thereof. PCR-PP contains a majority amount or greater than 50 wt% of a propylene-based polymer, based on the total weight of the PCR-PP. PCR-PP does not include or exclude virgin polymers, such as virgin polypropylene. Non-limiting examples of suitable PCR-PPs include SYSTALEN PP-C32902 and SYSTALEN PP-C32900, each commercially available from Der Grune Punkt.

[0053] PCR-PP may include a small amount of post-consumer recycled polymers other than propylene-based polymers, such as post-consumer recycled ethylene-based polymers (PCR-PE). For example, if the source is a blow molded bottle having (i) a body formed of a propylene-based polymer and (ii) a cap formed of an ethylene-based polymer, then the PCR-PP formed by extruding the material from a material reprocessor contains a small amount or less than 50 wt% of PCR-PE based on the total weight of the PCR-PP.

[0054] The PCR-PP contains a majority amount or greater than 50 wt% of a propylene-based polymer based on the total weight of the PCR-PP. Non-limiting examples of suitable propylene-based polymers include propylene homopolymers, propylene / α-olefin copolymers, and combinations thereof. In one embodiment, the PCR-PP contains greater than 50 wt% to less than 100 wt%, or 60 wt% to less than 100 wt%, or 70 wt% to less than 100 wt% of a propylene-based polymer based on the total weight of the PCR-PP.

[0055] In one embodiment, the PCR-PP contains a small amount or less than 50 wt% of post-consumer recycled ethylene-based polymer (PCR-PE). The PCR-PE can be any ethylene-based polymer disclosed herein. Non-limiting examples of suitable ethylene-based polymers include ethylene homopolymers, ethylene / α-olefin copolymers, and combinations thereof.

[0056] In one embodiment, the PCR-PP contains 70 wt% to less than 100 wt% of a propylene-based polymer; and a complementary amount of PCR-PE, or greater than 0 wt% to 30 wt% of PCR-PE, based on the total weight of the PCR-PP.

[0057] PCR-PP is provided in solid form - for example as granules and / or pellets. PCR-PP pellets are not transparent and are not white. PCR-PP pellets have a non-white color because they contain pigment from a source (e.g., pigment from a container). In one embodiment, the PCR-PP pellets have a gray color. In contrast, conventional virgin polypropylene is white and / or transparent.

[0058] The melt flow rate (MFR I2) of PCR-PP is equal to or greater than 7.0 g / 10 min; or equal to or greater than 8.0 g / 10 min. In one embodiment, the MFR I2 of PCR-PP is 7.0 g / 10 min, or 7.5 g / 10 min, or 8.0 g / 10 min, or 9.0 g / 10 min, or 10 g / 10 min, or 11 g / 10 min, or 12 g / 10 min, or 13 g / 10 min to 14 g / 10 min, or 15 g / 10 min, or 18 g / 10 min, or 20 g / 10 min. In another embodiment, the MFR I2 of the PCR-PP is 7.0 g / 10 min to 20 g / 10 min, or 8 g / 10 min to 20 g / 10 min, or 7.0 g / 10 min to 15 g / 10 min, or 7.5 g / 10 min to 15 g / 10 min, or 8 g / 10 min to 15 g / 10 min.

[0059] In one embodiment, the MFR of PCR-PP is 10 In another embodiment, the MFR of the PCR-PP is from 100 g / 10 min, or 110 g / 10 min, or 120 g / 10 min, or 150 g / 10 min, or 200 g / 10 min, or 250 g / 10 min, or 280 g / 10 min to 300 g / 10 min, or 350 g / 10 min, or 400 g / 10 min. 10 The amount of the mixture may be 100 g / 10 min to 400 g / 10 min, or 100 g / 10 min to 300 g / 10 min, or 120 g / 10 min to 300 g / 10 min, or 100 g / 10 min to 200 g / 10 min.

[0060] In one embodiment, the MFR of PCR-PP is 10 / I2 is 12, or 15 to less than 22, or 22, or 25, or 30, or 35. In another embodiment, the MFR I of PCR-PP is 10 / I2 is 12 to 35, or 12 to 25, or 12 to 22, or 12 to less than 22.

[0061] In one embodiment, the flexural modulus of PCR-PP is 1000 MPa, or 1050 MPa to 1200 MPa, or 1500 MPa. In another embodiment, the flexural modulus of PCR-PP is 1000 MPa to 1500 MPa, or 1000 MPa to 1300 MPa, or 1050 MPa to 1200 MPa.

[0062] In one embodiment, the Charpy impact energy of PCR-PP at 23°C is greater than 0 kJ / m 2 , or 1.0 kJ / m 2, or 5.0 kJ / m 2 Up to 6.5 kJ / m 2 , or less than 7.0 kJ / m 2 In another embodiment, the Charpy impact energy of the PCR-PP at 0°C is greater than 0 kJ / m 2 , or 1.0 kJ / m 2 , or 2.0 kJ / m 2 Up to 3.1 kJ / m 2 , or 3.5 kJ / m 2 , or 5.0 kJ / m 2 In another embodiment, the Charpy impact energy of the PCR-PP at -20°C is greater than 0 kJ / m 2 , or 0.8 kJ / m 2 , or 1.5 kJ / m 2 Up to 2.2 kJ / m 2 , or 2.3 kJ / m 2 or 5.0 kJ / m 2 .

[0063] In one embodiment, PCR-PP has at least two melting points. The first melting point (Tm1) is 145°C, or 155°C, or 160°C to 163°C, or 165°C. The second melting point (Tm2) is 115°C, or 120°C, or 122°C to 125°C, or 130°C. In one embodiment, Tm1 is 145°C to 165°C, and Tm2 is 115°C to 130°C.

[0064] In one embodiment, PCR-PP has at least two crystallization temperatures. The first crystallization temperature (Tc1) is 120°C, or 125°C to 130°C, or 135°C. The second crystallization temperature (Tc2) is 100°C to 115°C, or less than 120°C. In one embodiment, Tc1 is 120°C to 135°C, and Tc2 is 100°C to less than 120°C.

[0065] In one embodiment, the MFR I2 of the PCR-PP is 7.0 g / 10 min to 20 g / 10 min, or 8 g / 10 min to 20 g / 10 min, or 7.0 g / 10 min to 15 g / 10 min, or 7.5 g / 10 min to 15 g / 10 min, or 8 g / 10 min to 15 g / 10 min, and the PCR-PP has one, some or all of the following characteristics: (i) contains 70 wt% to less than 100 wt% of propylene-based polymer based on the total weight of the PCR-PP; and / or (ii) contains greater than 0 wt% to 30 wt% of PCR-PE based on the total weight of the PCR-PP; and / or (iii) MFR I 10and / or (iv) MFR I 10 / I2 is from 12 to 35, or from 12 to 25, or from 12 to 22, or from 12 to less than 22; and / or (v) a flexural modulus of from 1000 MPa to 1500 MPa, or from 1050 MPa to 1200 MPa; and / or (vi) a Charpy impact energy at 23°C greater than 0 kJ / m 2 To less than 7.0kJ / m 2 , or 1.0 kJ / m 2 Up to 6.5 kJ / m 2 , or 5.0 kJ / m 2 Up to 6.5 kJ / m 2 ; and / or (vii) a Charpy impact energy at 0°C greater than 0 kJ / m 2 Up to 5.0 kJ / m 2 , or greater than 0kJ / m 2 Up to 3.5 kJ / m 2 , or 2.0 kJ / m 2 Up to 3.1 kJ / m 2 ; and / or (viii) a Charpy impact energy at -20°C greater than 0 kJ / m 2 Up to 5.0 kJ / m 2 , or greater than 0kJ / m 2 Up to 2.3 kJ / m 2 , or 1.5 kJ / m 2 Up to 2.2 kJ / m 2 ; and / or (ix) Tm1 is 145°C to 165°C, or 155°C to 165°C, or 160°C to 163°C; and / or (x) Tm2 is 115°C to 130°C, or 120°C to 130°C, or 122°C to 125°C: and / or (xi) Tc1 is 120°C to 135°C, or 120°C to 130°C, or 125°C to 130°C; and / or (xii) Tc2 is 100°C to less than 120°C, or 100°C to 115°C.

[0066] The sum of the components in each of the PCR-PP disclosed herein, the compositions and layers including the aforementioned PCR-PP yields 100 weight percent (wt %).

[0067] A PCR-PP may comprise two or more embodiments disclosed herein.

[0068] ii. Add 4,4'-oxydibenzenesulfonyl azide

[0069] The method includes the step of adding 4,4'-oxydibenzenesulfonyl azide (DPO-BSA) to PCR-PP.

[0070] 4,4'-Oxydibenzenesulfonyl azide (DPO-BSA) is a compound having the following structure (I):

[0071]

[0072] As shown in structure (I), DPO-BSA contains two sulfur atoms.

[0073] In one embodiment, the method comprises adding 150 ppm, or 250 ppm, or 300 ppm, or 400 ppm, or 450 ppm, or 500 ppm, or 800 ppm to 1000 ppm, or 1200 ppm, or 1500 ppm, or 1800 ppm, or 2000 ppm of DPO-BSA to PCR-PP, based on the combined weight of DPO-BSA and PCR-PP. In another embodiment, the method comprises adding 150 ppm to 2000 ppm, or 250 ppm to 1800 ppm, or 250 ppm to 1500 ppm, or 300 ppm to 1500 ppm, or 450 ppm to 1500 ppm, or 800 ppm to 1500 ppm, or 1000 ppm to 1500 ppm, or 1100 ppm to 1500 ppm of DPO-BSA to PCR-PP, based on the combined weight of DPO-BSA and PCR-PP.

[0074] iii. Melt blending of PCR-PP and DPO-BSA

[0075] The method includes the step of melt blending the PCR-PP with the DPO-BSA. "Melt blending" is a process in which at least two components are combined or otherwise mixed together and at least one component is in a molten state. Melt blending can be accomplished by batch mixing, extrusion blending, extrusion molding, and any combination thereof. Melt blending can be performed sequentially prior to extrusion. Alternatively, melt blending can be performed simultaneously or substantially simultaneously with extrusion (i.e., melt blending and extrusion are performed in the same extruder).

[0076] Non-limiting examples of suitable melt blending equipment include internal batch mixers such as a Banbury TM or Boiling TM Internal mixers; and continuous single or twin screw mixers such as Farrel TM Continuous mixers, Werner and Pfleiderer TM Twin screw mixer or Buss TM Kneading continuous extruder.

[0077] Melt blending is performed at a temperature above the melting temperature of PCR-PP. In one embodiment, melt blending is performed at a temperature of 160°C, or 180°C, or 200°C, or 220°C to 240°C, or 250°C, or 260°C. In another embodiment, melt blending is performed at a temperature of 160°C to 260°C, or 180°C to 250°C, or 200°C to 250°C for a period of 1 minute to 10 minutes.

[0078] During melt blending, DPO-BSA reacts with the propylene-based polymer in PCR-PP by coupling with the propylene-based polymer in PCR-PP. Without wishing to be bound by any particular theory, it is believed that during the reaction, DPO releases nitrogen from the terminal azide group, subsequently forming free radicals on each side of the DOP molecule.

[0079] Surprisingly, it was found that DPO-BSA does not react or does not substantially react (ie, crosslink) with PCR-PE during melt blending. Crosslinking of ethylene-based polymers such as PCR-PE is disadvantageous because it renders PCR-PP more brittle, making it unsuitable for molded product applications.

[0080] Melt blending may include two or more embodiments disclosed herein.

[0081] iv. Formation of DPO-BSA coupled PCR-PP

[0082] The method includes the steps of forming a DPO-BSA coupled PCR-PP having a melt flow rate (MFR I2) equal to or less than 5 g / 10 min.

[0083] The DPO-BSA conjugated PCR-PP formed during melt blending is compositionally and physically different from the unconjugated PCR-PP.

[0084] The MFR I2 of the DPO-BSA coupled PCR-PP is equal to or less than 5 g / 10 min; or equal to or less than 4 g / 10 min; equal to or less than 3 g / 10 min; or equal to or less than 2 g / 10 min. An MFR I2 of 5 g / 10 min or less is beneficial for molded product applications such as blow molded products because the melt flow rate is inversely proportional to the melt strength. In other words, the DPO-BSA coupled PCR-PP having a melt flow rate (MFR I2) of at least 7 g / 10 min has a higher melt strength than the uncoupled PCR-PP having a melt flow rate (MFR I2) of at least 7 g / 10 min.

[0085] In one embodiment, the MFR I2 of the DPO-BSA coupled PCR-PP is greater than 0 g / 10 min, or 0.1 g / 10 min, or 0.5 g / 10 min, or 0.9 g / 10 min to 1.7 g / 10 min, or 1.8 g / 10 min, or 1.9 g / 10 min, or 2.0 g / 10 min, or 2.3 g / 10 min, or 2.5 g / 10 min, or 2.9 g / 10 min, or 3.0 g / 10 min, or 3.2 g / 10 min, or 4.0 g / 10 min, or 4.4 g / 10 min, or 5.0 g / 10 min. In another embodiment, the MFR I2 of the DPO-BSA coupled PCR-PP is greater than 0 g / 10 min to 5 g / 10 min, or greater than 0 g / 10 min to 4 g / 10 min, or greater than 0 g / 10 min to 3 g / 10 min, or greater than 0 g / 10 min to 2 g / 10 min, or 0.1 g / 10 min to 4.5 g / 10 min, or 0.9 g / 10 min to 4.4 g / 10 min.

[0086] In one embodiment, the MFR of DPO-BSA coupled PCR-PP is 10 In another embodiment, the MFR of the DPO-BSA coupled PCR-PP is greater than 0 g / 10 min, or 1 g / 10 min, or 10 g / 10 min, or 20 g / 10 min to 90 g / 10 min, or less than 100 g / 10 min. 10 It is greater than 0 g / 10 minutes to less than 100 g / 10 minutes, or 1 g / 10 minutes to 90 g / 10 minutes, or 20 g / 10 minutes to 90 g / 10 minutes.

[0087] In one embodiment, the MFR of DPO-BSA coupled PCR-PP is 10 / I2 is 12, or 15, or 18, or 19, or 20 to 29, or 30, or 35. In another embodiment, the MFR I of the DPO-BSA coupled PCR-PP is 10 / I2 is 12 to 35, or 15 to 30, or 18 to 30.

[0088] In one embodiment, the flexural modulus of the DPO-BSA-coupled PCR-PP is 800 MPa, or 850 MPa, or 1000 MPa, or 1100 MPa, or 1200 MPa to 1300 MPa, or 1500 MPa. In another embodiment, the flexural modulus of the DPO-BSA-coupled PCR-PP is 800 MPa to 1500 MPa, or 850 MPa to 1300 MPa, or 1000 MPa to 1500 MPa.

[0089] In one embodiment, the Charpy impact energy of the DPO-BSA coupled PCR-PP at 23°C is greater than 6.5 kJ / m 2 , or 7.0 kJ / m 2 Up to 16kJ / m 2 , or 20.0 kJ / m 2 , or 70.0 kJ / m 2 In another embodiment, the Charpy impact energy of the DPO-BSA coupled PCR-PP at 0°C is 2.0 kJ / m 2 , or 2.4 kJ / m 2 Up to 6.0 kJ / m 2 , or 7.0 kJ / m 2 , or 20 kJ / m 2 In another embodiment, the Charpy impact energy of the DPO-BSA coupled PCR-PP at -20°C is 1.5 kJ / m 2 , or 1.6 kJ / m 2 Up to 3.0 kJ / m 2 , or 4.0 kJ / m 2 The increase in Charpy impact energy at 23°C, 0°C and -20°C is advantageous as it indicates that the DPO-BSA coupled PCR-PP has improved ductility, which is beneficial in molding applications.

[0090] In one embodiment, the DPO-BSA coupled PCR-PP contains greater than 0 ppm, or 25 ppm, or 42 ppm, or 50 ppm, or 67 ppm, or 75 ppm, or 84 ppm, or 134 ppm to 168 ppm, or 202 ppm, or 252 ppm, or 301 ppm, or 336 ppm, or 350 ppm of sulfur based on the total weight of the DPO-BSA coupled PCR-PP. In another embodiment, the DPO-BSA coupled PCR-PP contains greater than 0 ppm to 350 ppm, or 42 ppm to 301 ppm, or 42 ppm to 252 ppm, or 50 ppm to 252 ppm, or 75 ppm to 252 ppm, or 84 ppm to 252 ppm, or 168 ppm to 252 ppm, or 184 ppm to 252 ppm of sulfur based on the total weight of the DPO-BSA coupled PCR-PP.

[0091] In one embodiment, the MFR I2 of the DPO-BSA coupled PCR-PP is greater than 0 g / 10 min to 5 g / 10 min, or greater than 0 g / 10 min to 4 g / 10 min, or greater than 0 g / 10 min to 3 g / 10 min, or greater than 0 g / 10 min to 2 g / 10 min, or 0.1 g / 10 min to 4.5 g / 10 min, or 0.9 g / 10 min to 4.4 g / 10 min; and the DPO-BSA coupled PCR-PP has one, some or all of the following properties: (i) MFR I 10 (ii) MFR I is from greater than 0 g / 10 min to less than 100 g / 10 min, or from 1 g / 10 min to 90 g / 10 min, or from 20 g / 10 min to 90 g / 10 min; and / or (ii) MFR I 10 / I2 is from 12 to 35, or from 15 to 30, or from 18 to 30; and / or (iii) a flexural modulus of from 800 MPa to 1500 MPa, or from 850 MPa to 1300 MPa, or from 1000 MPa to 1500 MPa; and / or (iv) a Charpy impact energy at 23°C greater than 6.5 kJ / m 2 Up to 70.0kJ / m 2 , or greater than 6.5 kJ / m 2 Up to 20.0kJ / m 2 , or 7.0 kJ / m 2 Up to 16kJ / m 2 ; and / or (v) a Charpy impact energy of 2.0 kJ / m at 0°C 2 Up to 20.0kJ / m 2 , or 2.0 kJ / m 2 Up to 7.0 kJ / m 2 , or 2.4 kJ / m 2 Up to 6.0 kJ / m 2 and / or (vi) a Charpy impact energy of 1.5 kJ / m at -20°C 2 Up to 4.0 kJ / m 2 , or 1.6 kJ / m 2 Up to 3.0 kJ / m 2 and / or (vii) contains greater than 0 ppm to 350 ppm, or 42 ppm to 301 ppm, or 42 ppm to 252 ppm, or 50 ppm to 252 ppm, or 75 ppm to 252 ppm, or 84 ppm to 252 ppm, or 168 ppm to 252 ppm, or 184 ppm to 252 ppm of sulfur, based on the total weight of the DPO-BSA coupled PCR-PP.

[0092] The DPO-BSA coupled PCR-PP may comprise two or more embodiments disclosed herein.

[0093] v. Optional melt blending with virgin polymer

[0094] In one embodiment, the method includes melt blending the DPO-BSA coupled PCR-PP with a virgin polymer to form a composition. In other words, the virgin polymer is added to the DPO-BSA coupled PCR-PP and melt blended with the DPO-BSA coupled PCR-PP. The melt flow rate (MFR I2) of the composition is equal to or less than 5 g / 10 min.

[0095] In one embodiment, the method includes adding a pristine polymer to a PCR-PP, and melt blending the pristine polymer with the DPO-BSA and the PCR-PP to form a composition containing a DPO-BSA-coupled pristine polymer and a DPO-BSA-coupled PCR-PP. The melt flow rate (MFR I2) of the composition is equal to or less than 5 g / 10 min.

[0096] In one embodiment, the virgin polymer is a virgin polyolefin. Non-limiting examples of suitable virgin polyolefins include ethylene-based polymers, propylene-based polymers, and combinations thereof.

[0097] A. Original ethylene-based polymers

[0098] In one embodiment, the original polyolefin is an ethylene-based polymer. In addition to PCR-PE, the ethylene-based polymer can be any ethylene-based polymer disclosed herein. In one embodiment, the original ethylene-based polymer is an ethylene / α-olefin multi-block copolymer.

[0099] The term "ethylene / α-olefin multi-block copolymer" refers to an ethylene / C4-C8 α-olefin multi-block copolymer consisting of or otherwise composed of ethylene and a copolymerizable C4-C8 α-olefin comonomer (and optional additives) in polymerized form, the polymer being characterized in that multiple blocks or segments of two polymerized monomer units differ in chemical or physical properties, the blocks being linked (or covalently bonded) in a linear manner, i.e., a polymer comprising chemically distinguishable units linked end-to-end with respect to polymerized olefinic functionality. Ethylene / α-olefin multi-block copolymers include block copolymers having two blocks (diblocks) and more than two blocks (multiblocks). The C4-C8 α-olefin is selected from butene, hexene and octene. The ethylene / α-olefin multi-block copolymer does not have or otherwise excludes styrene (i.e., does not contain styrene), and / or does not have vinyl aromatic monomers, and / or does not have conjugated dienes. When the amount of "ethylene" or "comonomer" is mentioned in the copolymer, it should be understood that this refers to its polymerized units. In some embodiments, the ethylene / α-olefin multi-block copolymer can be represented by the following formula: (AB)n; wherein n is at least 1, preferably an integer greater than 1, such as 2, 3, 4, 5, 10, 15, 20, 30, 40, 50, 60, 70, 80, 90, 100 or more, "A" represents a hard block or segment, and "B" represents a soft block or segment. Preferably, A and B are connected or covalently bonded in a substantially linear manner, or in a linear manner, relative to a substantially branched or substantially star-shaped manner. In other embodiments, the A blocks and B blocks are randomly distributed along the polymer chain. In other words, the block copolymer generally does not have the following structure: AAA-AA-BBB-BB. In one embodiment, the ethylene / α-olefin multi-block copolymer does not have a third type of block, which contains one or more different comonomers. In another embodiment, block A and block B each have monomers or comonomers that are substantially randomly distributed within the block. In other words, neither block A nor block B comprises two or more sub-segments (or sub-blocks) having unique compositions, such as an end segment having a substantially different composition than the remainder of the block.

[0100] Preferably, ethylene accounts for most of the mole fraction of the entire ethylene / α-olefin multi-block copolymer, that is, ethylene accounts for at least 50wt% of the entire ethylene / α-olefin multi-block copolymer. More preferably, ethylene comprises at least 60wt%, at least 70wt%, or at least 80wt%, and the basic remainder of the entire ethylene / α-olefin multi-block copolymer comprises C4-C8α-olefin comonomers. In one embodiment, the ethylene / α-olefin multi-block copolymer contains 50wt%, or 60wt%, or 65wt% to 80wt%, or 85wt%, or 90wt%, or 95wt% of ethylene. For a variety of ethylene / octene multi-block copolymers, the composition comprises an ethylene content greater than 80wt% of the entire ethylene / octene multi-block copolymer and an octene content of 5wt%, or 10wt% to 15wt%, or 15wt% to 20wt% of the entire multi-block copolymer.

[0101] Ethylene / alpha-olefin multi-block copolymers include various amounts of "hard" segments and "soft" segments. "Hard" segments are blocks of polymerized units, wherein ethylene is present in an amount of greater than 90wt% or 95wt% or greater than 95wt% or greater than 98wt%, up to 100wt%, based on the weight of the polymer. In other words, by the weight of the polymer, the comonomer content (excluding the monomer content of ethylene) in the hard segments is less than 10wt%, or 5wt%, or less than 5wt%, or less than 2wt%, and can be as low as zero. In some embodiments, the hard segments include all or substantially all units derived from ethylene. "Soft" segments are blocks of polymerized units, wherein by the weight of the polymer, the comonomer content (the content of monomers other than ethylene) is greater than 5wt%, or greater than 8wt%, greater than 10wt%, or greater than 15wt%. In one embodiment, the comonomer content in the soft segments is greater than 20 wt%, greater than 25 wt%, greater than 30 wt%, greater than 35 wt%, greater than 40 wt%, greater than 45 wt%, greater than 50 wt%, or greater than 60 wt% and can be as high as 100 wt%.

[0102] The soft segment can be present in the ethylene / α-olefin multi-block copolymer by 1wt%, or 5wt%, or 10wt%, or 15wt%, or 20wt%, or 25wt%, or 30wt%, or 35wt%, or 40wt%, or 45wt% to 55wt%, or 60wt%, or 65wt%, or 70wt%, or 75wt%, or 80wt%, or 85wt%, or 90wt%, or 95wt%, or 99wt% of the total weight of the ethylene / α-olefin multi-block copolymer. On the contrary, the hard segment can exist in a similar range. The soft segment weight percentage and the hard segment weight percentage can be calculated based on the data obtained from DSC or NMR. This method and calculation are disclosed in, for example, USP 7,608,668, the disclosure of which is incorporated herein by reference in its entirety. Specifically, the hard segment weight percent and the soft segment weight percent and the comonomer content may be determined as described in columns 57 to 63 of USP 7,608,668.

[0103] The ethylene / α-olefin multi-block copolymer comprises two or more chemically distinct regions or segments (referred to as "blocks") joined (or covalently bonded) in a linear manner, i.e., a polymer containing chemically distinguishable units joined end-to-end in terms of polymerized olefinic functionality rather than joined in a pendant or grafted manner. In one embodiment, the blocks differ in the amount or type of comonomer incorporated, density, crystallinity, crystallite size attributable to polymers of such composition, type or degree of stereoisomerism (isotactic or syndiotactic), regioregularity or regio-irregularity, amount of branching (including long chain branching or hyperbranching), uniformity, or any other chemical or physical attribute. Compared to prior art block interpolymers, including those produced by sequential monomer addition, stereolabile catalysts, or anionic polymerization techniques, the inventive ethylene / α-olefin multi-block copolymers are characterized by a unique distribution of polymer polydispersity (PDI or Mw / Mn or MWD), polydisperse block length distribution, and / or polydisperse block number distribution, which, in one embodiment, is due to the effect of one or more shuttling agents in combination with various catalysts used in their preparation.

[0104] In one embodiment, the ethylene / α-olefin multi-block copolymer is produced in a continuous process and has a polydispersity index (Mw / Mn) of 1.7 to 3.5, or 1.8 to 3, or 1.8 to 2.5, or 1.8 to 2.2. When prepared in a batch or semi-batch process, the ethylene / α-olefin multi-block copolymer has a Mw / Mn of 1.0 to 3.5, or 1.3 to 3, or 1.4 to 2.5, or 1.4 to 2.

[0105] In addition, the ethylene / α-olefin multi-block copolymer has a PDI (or Mw / Mn) that fits the Schultz-Flory distribution rather than the Poisson distribution. The ethylene / α-olefin multi-block copolymer of the present invention has both a polydisperse block distribution and a polydisperse distribution of block sizes. This results in the formation of polymer products with improved and distinguishable physical properties. This has been previously described in Potemkin, Physical Review E (Physical ... hysical Review E ) (1998) 57(6), pp. 6902-6912 and Dobrynin, Journal of Chemical Physics ( J.Chem.Phvs. The theoretical benefits of polydisperse block distributions are modeled and discussed in ) (1997) 107(21), pp. 9234-9238.

[0106] In one embodiment, the ethylene / α-olefin multi-block copolymers of the present invention have a most probable distribution of block lengths.

[0107] Non-limiting examples of suitable ethylene / α-olefin multi-block copolymers are disclosed in U.S. Patent No. 7,608,668, which is incorporated herein by reference in its entirety.

[0108] In one embodiment, the ethylene / α-olefin multi-block copolymer has hard segments and soft segments, is free of styrene, consists only of (i) ethylene and (ii) C4-C8 α-olefins (and optional additives), and is defined as having a Mw / Mn of 1.7 to 3.5, at least one melting point Tm in degrees Celsius, and a density d in grams per cubic centimeter, wherein the numerical values ​​of Tm and d correspond to the following relationship: Tm>-2002.9+4538.5(d)-2422.2(d) 2 ,

[0109] wherein the density d is from 0.860 g / cc, or 0.865 g / cc, or 0.869 g / cc to 0.875 g / cc, or 0.877 g / cc, or 0.880 g / cc, or 0.890 g / cc; and the melting point Tm is from 110°C, or 115°C, or 118°C to 122°C, or 125°C, or 130°C, or 135°C.

[0110] The ethylene / α-olefin copolymer contains, consists essentially of, or consists of: (i) ethylene and (ii) a C4-C8 α-olefin comonomer. In one embodiment, the α-olefin comonomer is selected from hexene and octene. In another embodiment, the α-olefin is octene.

[0111] In one embodiment, the ethylene / α-olefin multi-block copolymer contains, consists essentially of, or consists of (i) ethylene and (ii) a C4-C8 α-olefin comonomer, and the ethylene / α-olefin multi-block copolymer has one, some, or all of the following properties: (i) a density of 0.860 g / cc to 0.890 g / cc, or 0.865 g / cc to 0.880 g / cc; and / or (ii) a melting point of 110° C. to 135° C., or 115°C to 130°C; and / or (iii) a melt index (I2) of 0.1 g / 10 min to 10 g / 10 min, or 0.1 g / 10 min to 5 g / 10 min, or 0.1 g / 10 min to 1 g / 10 min; and / or (iv) a glass transition temperature (Tg) of -80°C to -50°C, or -70°C to -60°C; and / or (v) a Shore A hardness of 30 to 70, or 40 to 70, or 40 to 60, or 50 to 60.

[0112] In one embodiment, the ethylene / α-olefin multi-block copolymer is an ethylene / octene multi-block copolymer. The ethylene / octene multi-block copolymer is marketed under the trade name INFUSE TM Sold and available from The Dow Chemical Company, Midland, Michigan, USA.

[0113] An ethylene / α-olefin multi-block copolymer may comprise two or more embodiments disclosed herein.

[0114] The original ethylene-based polymer may comprise two or more embodiments disclosed herein.

[0115] B. Original Propylene-Based Polymers

[0116] In one embodiment, the original polyolefin is a propylene-based polymer. In addition to PCR-PP, the propylene-based polymer can be any propylene-based polymer disclosed herein. In one embodiment, the original propylene-based polymer is a propylene / α-olefin copolymer. In another embodiment, the propylene / α-olefin copolymer is a propylene / ethylene copolymer.

[0117] In one embodiment, the propylene / ethylene copolymer comprises, consists essentially of, or consists of propylene, ethylene, optional diene comonomer, and optional additives.

[0118] In one embodiment, the propylene / ethylene copolymer contains propylene and from greater than 0 wt%, or 0.5 wt%, or 1 wt%, or 2 wt% to 5 wt%, or 10 wt%, or 15 wt%, or 20 wt%, or 25 wt% ethylene comonomer, based on the total weight of the propylene / ethylene copolymer.

[0119] In one embodiment, the propylene / ethylene copolymer comprises, consists essentially of, or consists of less than 100 wt%, or 99 wt%, or 98 wt% to 97 wt%, or 96 wt%, or 95 wt% units derived from propylene and complementary amounts, or greater than 0 wt%, or 1 wt%, or 2 wt% to 3 wt%, or 4 wt%, or 5 wt% units derived from ethylene, based on the total weight of the propylene / ethylene copolymer.

[0120] In one embodiment, the propylene / ethylene copolymer has a density from 0.860 g / cc, or 0.863 g / cc to 0.870 g / cc, or 0.880 g / cc, or 0.890 g / cc, or 0.900 g / cc, or 0.905 g / cc.

[0121] In one embodiment, the propylene / ethylene copolymer has an MFR I2 from 0.3 g / 10 min, or 2.0 g / 10 min, or 3.0 g / 10 min, or 4.0 g / 10 min to 5.0 g / 10 min, or 6.0 g / 10 min, or 7.0 g / 10 min, or 8.0 g / 10 min, or 10.0 g / 10 min, or 15.0 g / 10 min, or 20.0 g / 10 min, or 25.0 g / 10 min, or 50 g / 10 min, or 70 g / 10 min.

[0122] In one embodiment, the propylene / ethylene copolymer has a total unsaturation per mole of propylene of 0.01%, or 0.015% to 0.025%, or 0.03%. As described above in the Test Methods section, the total unsaturation per mole of propylene is determined by 1 Measured by H NMR analysis.

[0123] In one embodiment, the propylene / ethylene copolymer has a crystallinity of 1 wt%, or 10 wt%, or 14 wt% to 20 wt%, or 25 wt%, or 30 wt%, or 40 wt%, or 50 wt%, or 60 wt%, or 70 wt%.

[0124] The term "B-value" is a measure of randomness, and measures the distribution of propylene and ethylene comonomers in the polymer chain of the entire propylene / ethylene copolymer. The range of B-value is 0 to 2. The higher the B-value, the more alternate the ethylene distribution in the propylene / ethylene copolymer. The lower the B-value, the more blocky or clustered the ethylene distribution in the propylene / ethylene copolymer. In one embodiment, the B-value of the propylene / ethylene copolymer is less than 1.0, or less than 0.99, or less than 0.98, or less than 0.97. In one embodiment, the B-value of the propylene / ethylene copolymer is 0.90, or 0.92, or 0.93, or 0.94 to 0.95, or 0.96, or 0.97, or 0.98, or 0.99.

[0125] The B-value as described by Koenig (Spectroscopy of Polymers, 2nd ed., 1999) is calculated as follows. For propylene / ethylene copolymers, B is defined as: Where f(EP+PE) = the sum of the EP and PE diad fractions; and Fe and Fp are equal to the mole fractions of ethylene and propylene in the copolymer, respectively. The diad fraction can be obtained from the triad data according to the following equation: f(EP+PE) = [EPE] + [EPP+PPE] / 2 + [PEP] + [EEP+PEE] / 2.

[0126] In one embodiment, the propylene / ethylene copolymer is characterized as having substantially isotactic propylene sequences. "Substantially isotactic propylene sequences" are propylene sequences having 13 A sequence having an isotactic triad (mm) greater than 0.85, or greater than 0.90, or greater than 0.92, or greater than 0.93 as measured by C NMR. An isotactic triad is defined by 13 C NMR spectroscopy determines the isotactic sequence with respect to the triad units in the copolymer molecular chains.

[0127] In one embodiment, the propylene / ethylene copolymer has one, some or all of the following properties: (i) a density of 0.860 g / cc to 0.905 g / cc, or 0.860 g / cc to 0.870 g / cc; and / or (ii) an MFR I2 of 0.3 g / 10 min to 70 g / 10 min, or 2.0 g / 10 min to 10 g / 10 min, or 2.0 g / 10 min to 8 g / 10 min; and / or (iii) a crystallinity of 1 wt% to 70 wt%, or 10% to 70%, or 10 wt% to 50 wt%, or 10 wt% to 20 wt%, or 14 wt% to 20 wt%; and / or (iv) less than 100 wt%, or 99 wt%, or 98 wt% to 97 wt%, or 96 wt%, or 98 wt% to 9 ...8 wt%, or 98 wt% to 5wt%, or 90wt%, or 85wt% units derived from propylene and complementary amounts, or greater than 0wt%, or 1wt%, or 2wt% to 3wt%, or 4wt%, or 5wt%, or 10wt%, or 15wt% units derived from ethylene; and / or (v) a total unsaturation per mole of propylene of 0.01% to 0.03%; and / or (vi) a glass transition temperature (Tg) of -50°C to -20°C, or -40°C to -30°C; and / or (vii) a B value of 0.90 to 0.99; and / or (viii) a 13 The sequence of isotactic triads (mm) measured by C NMR is greater than 0.85; and / or (ix) Shore A is from 60 to 90, or from 70 to 90, or from 70 to 80.

[0128] Propylene / ethylene copolymers may be prepared as described in International Publication No. WO 2009 / 067337, the entire contents of which are incorporated herein by reference.

[0129] In one embodiment, the propylene / ethylene copolymer is a propylene-based plastomer or elastomer. A non-limiting example of a suitable propylene / ethylene copolymer that is a propylene-based plastomer or elastomer is VERSIFY TM 3000 and VERSIFY TM 3401.

[0130] A propylene / ethylene copolymer may comprise two or more embodiments disclosed herein.

[0131] The original propylene-based polymer may comprise two or more embodiments disclosed herein.

[0132] A raw polymer may comprise two or more embodiments disclosed herein.

[0133] The composition comprises, consists essentially of or consists of: (i) DPO-BSA coupled PCR-PP; (ii) optionally, a pristine polymer; (iii) optionally, an additive. The MFR I2 of the composition is equal to or less than 5 g / 10 min.

[0134] In one embodiment, the composition contains 60wt%, or 70wt%, or 80wt%, or 85wt%, or 90wt%, or 95wt%, or 99wt% to less than 100wt%, or 100wt% of DPO-BSA coupled PCR-PP based on the total weight of the composition. In one embodiment, the composition contains 60wt% to 100wt%, or 80wt% to 100wt%, or 85wt% to 100wt%, or 90wt% to 100wt% of DPO-BSA coupled PCR-PP. In another embodiment, the composition consists of DPO-BSA coupled PCR-PP.

[0135] In one embodiment, the composition contains, consists essentially of, or consists of: 85 wt% to 99 wt%, or 90 wt% to 99 wt%, or 95 wt% to 99 wt% of DPO-BSA coupled PCR-PP; and a complementary amount of the original polymer, or 1 wt% to 15 wt%, or 1 wt% to 10 wt%, or 1 wt% to 5 wt% of the original polymer, based on the total weight of the composition.

[0136] In one embodiment, the composition contains one or more optional additives. Non-limiting examples of suitable optional additives include impact modifiers, pigments, processing aids, mold release additives, mineral oils, antioxidants, flame retardants, ultraviolet (UV) stabilizers, reinforcing fillers (e.g., glass fibers), anti-scratch additives, talc, calcium carbonate, mica, and combinations thereof. The composition contains 0 wt % to 40 wt %, or greater than 0 wt % to 25 wt % of the optional additives by the total weight of the composition.

[0137] The MFR I2 of the composition is equal to or less than 5 g / 10 min; or equal to or less than 4 g / 10 min; equal to or less than 3 g / 10 min; or equal to or less than 2 g / 10 min. In another embodiment, the MFR I2 of the composition is greater than 0 g / 10 min to 5 g / 10 min, or greater than 0 g / 10 min to 4 g / 10 min, or greater than 0 g / 10 min to 3 g / 10 min, or greater than 0 g / 10 min to 2 g / 10 min, or 0.1 g / 10 min to 4.5 g / 10 min, or 0.9 g / 10 min to 4.4 g / 10 min.

[0138] In one embodiment, the MFR of the composition is 10In another embodiment, the MFR of the DPO-BSA coupled PCR-PP is greater than 0 g / 10 min, or 1 g / 10 min, or 10 g / 10 min, or 20 g / 10 min to 90 g / 10 min, or less than 100 g / 10 min. 10 It is greater than 0 g / 10 minutes to less than 100 g / 10 minutes, or 1 g / 10 minutes to 90 g / 10 minutes, or 20 g / 10 minutes to 90 g / 10 minutes, or 20 g / 10 minutes to less than 90 g / 10 minutes.

[0139] In one embodiment, the MFR of the composition is 10 / I2 is 12, or 15, or 18, or 19, or 20 to 29, or 30, or 35. In another embodiment, the MFR I of the composition is 10 / I2 is 12 to 35, or 15 to 30, or 18 to 30.

[0140] In one embodiment, the flexural modulus of the composition is 800 MPa, or 850 MPa, or 1000 MPa, or 1100 MPa, or 1200 MPa to 1300 MPa, or 1500 MPa. In another embodiment, the flexural modulus of the composition is 800 MPa to 1500 MPa, or 850 MPa to 1300 MPa, or 1000 MPa to 1500 MPa.

[0141] In one embodiment, the composition has a Charpy impact energy of greater than 6.5 kJ / m at 23°C. 2 , or 7.0 kJ / m 2 Up to 16kJ / m 2 , or 20.0 kJ / m 2 , or 70.0 kJ / m 2 In another embodiment, the composition has a Charpy impact energy of 2.0 kJ / m at 0°C. 2 , or 2.4 kJ / m 2 Up to 6.0 kJ / m 2 , or 7.0 kJ / m 2 , or 20 kJ / m 2 In another embodiment, the composition has a Charpy impact energy of 1.5 kJ / m at -20°C. 2 , or 1.6 kJ / m 2 Up to 3.0 kJ / m 2 , or 4.0 kJ / m 2 .

[0142] In one embodiment, the composition contains greater than 0 ppm to 350 ppm, or 42 ppm to 301 ppm, or 42 ppm to 252 ppm, or 50 ppm to 252 ppm, or 75 ppm to 252 ppm, or 84 ppm to 252 ppm, or 168 ppm to 252 ppm, or 184 ppm to 252 ppm sulfur, based on the total weight of the composition.

[0143] In one embodiment, the composition contains, consists essentially of, or consists of: 60 wt% to 99 wt%, or 85 wt% to 99 wt%, or 90 wt% to 99 wt%, or 95 wt% to 99 wt% of DPO-BSA coupled PCR-PP; and 1 wt% to 40 wt%, or 1 wt% to 15 wt%, or 1 wt% to 10 wt%, or 1 wt% to 5 wt% of virgin polymer, based on the total weight of the composition; the MFR I2 of the composition is greater than 0 g / 10 min to 5 g / 10 min, or greater than 0 g / 10 min to 4 g / 10 min, or greater than 0 g / 10 min to 3 g / 10 min, or greater than 0 g / 10 min to 2 g / 10 min, or 0.1 g / 10 min to 4.5 g / 10 min, or 0.9 g / 10 min to 4.4 g / 10 min; and the composition has one, some or all of the following properties: (i) MFRI 10 (ii) MFR I is from greater than 0 g / 10 min to less than 100 g / 10 min, or from 1 g / 10 min to 90 g / 10 min, or from 20 g / 10 min to 90 g / 10 min; and / or (ii) MFR I 10 / I2 is from 12 to 35, or from 15 to 30, or from 18 to 30; and / or (iii) a flexural modulus of from 800 MPa to 1500 MPa, or from 850 MPa to 1300 MPa, or from 1000 MPa to 1500 MPa; and / or (iv) a Charpy impact energy at 23°C greater than 6.5 kJ / m 2 Up to 70.0kJ / m 2 , or greater than 6.5 kJ / m 2 Up to 20.0kJ / m 2 , or 7.0 kJ / m 2 Up to 16kJ / m 2 ; and / or (v) a Charpy impact energy of 2.0 kJ / m at 0°C 2 Up to 20.0kJ / m 2 , 2.0kJ / m 2 Up to 7.0 kJ / m 2 , or 2.4 kJ / m 2 Up to 6.0 kJ / m 2 ; and / or (vi) a Charpy impact energy of 1.5 kJ / m at -20°C2 Up to 4.0 kJ / m 2 , or 1.6 kJ / m 2 Up to 3.0 kJ / m 2 and / or (vii) contains from greater than 0 ppm to 350 ppm, or from 42 ppm to 301 ppm, or from 42 ppm to 252 ppm, or from 50 ppm to 252 ppm, or from 75 ppm to 252 ppm, or from 84 ppm to 252 ppm, or from 168 ppm to 252 ppm, or from 184 ppm to 252 ppm sulfur, based on the total weight of the composition.

[0144] A composition may comprise two or more embodiments disclosed herein.

[0145] Melt blending with a pristine polymer may comprise two or more embodiments disclosed herein.

[0146] A method may comprise two or more embodiments disclosed herein.

[0147] Composition

[0148] The present disclosure also provides a composition. The composition contains 4,4'-oxydibenzenesulfonyl azide coupled post-consumer recycled polypropylene (DPO-BSA coupled PCR-PP) having (i) an MFR I2 equal to or less than 5 g / 10 min; and (ii) greater than 0 ppm to 350 ppm of sulfur.

[0149] The composition and DPO-BSA-coupled PCR-PP may be any corresponding composition and DPO-BSA-coupled PCR-PP disclosed herein.

[0150] In one embodiment, the DPO-BSA conjugated PCR-PP contains greater than 0 wt % to 30 wt % PCR-PE based on the total weight of the PCR-PP.

[0151] In one embodiment, the composition contains, consists essentially of, or consists of: 60 wt% to 99 wt%, or 85 wt% to 99 wt%, or 90 wt% to 99 wt%, or 95 wt% to 99 wt% of DPO-BSA coupled PCR-PP, and 1 wt% to 40 wt%, or 1 wt% to 15 wt%, or 1 wt% to 10 wt%, or 1 wt% to 5 wt% of virgin polymer, and the MFR I2 of the composition is greater than 0 g / 10 min to 5 g / 10 min, or greater than 0 g / 10 min to 4 g / 10 min, or greater than 0 g / 10 min to 3 g / 10 min, or greater than 0 g / 10 min to 2 g / 10 min, or 0.1 g / 10 min to 4.5 g / 10 min, or 0.9 g / 10 min to 4.4 g / 10 min. The virgin polymer is selected from virgin ethylene-based polymers, virgin propylene-based polymers, and combinations thereof. The original polymer can be any original polymer disclosed herein.

[0152] A composition may comprise two or more embodiments disclosed herein.

[0153] Molding

[0154] The present disclosure also provides a molded article. In one embodiment, the molded article includes (i) a first surface layer comprising, consisting essentially of, or consisting of a polyolefin; (ii) an inner layer comprising, consisting essentially of, or consisting of a composition as described above; and (iii) a second surface layer comprising, consisting essentially of, or consisting of a propylene-based polymer.

[0155] In another embodiment, a molded article includes (i) a first surface layer comprising a polyolefin; (ii) an inner layer comprising a composition comprising 4,4′-oxydibenzenesulfonyl azide coupled post-consumer recycled polypropylene (DPO-BSA coupled PCR-PP) having an MFR I2 equal to or less than 5 g / 10 min, and (iii) a second surface layer comprising a propylene-based polymer.

[0156] The propylene-based polymer of the second surface layer is a pristine propylene-based polymer. The pristine propylene-based polymer of the second surface layer is compositionally and physically different from the PCR-PP, and is further different from the DPO-BSA coupled PCR-PP.

[0157] The molded article comprises three layers, or more than three layers. For example, the molded article may have three, four, five, six, seven, eight, nine, ten, eleven or more layers. In one embodiment, the molded article contains only three layers.

[0158] i. Surface layer

[0159] The molded article comprises two surface layers. A "surface layer" is a layer having an outer surface that is exposed or substantially exposed to the surrounding environment.

[0160] The first surface layer and the second surface layer (collectively referred to herein as "surface layers") are each a continuous layer having two opposing surfaces including an outer surface and an inner surface.

[0161] The first surface layer comprises, consists essentially of, or consists of a polyolefin. Non-limiting examples of suitable polyolefins include ethylene-based polymers, propylene-based polymers, and combinations thereof.

[0162] In one embodiment, the first surface layer comprises, consists essentially of, or consists of an ethylene-based polymer.

[0163] In one embodiment, the first surface layer comprises, consists essentially of, or consists of a propylene-based polymer.

[0164] The second surface layer contains, consists essentially of, or consists of a propylene-based polymer. The propylene-based polymer of the second surface layer may be the same or different from the propylene-based polymer of the first surface layer. In one embodiment, the second surface layer and the first surface layer contain the same propylene-based polymer.

[0165] In one embodiment, the propylene-based polymer in the second surface layer is compositionally and / or physically different from the propylene-based polymer in the first surface layer.

[0166] The ethylene-based polymer and the propylene-based polymer may be any corresponding ethylene-based polymer and propylene-based polymer, provided that the ethylene-based polymer and the propylene-based polymer are original polymers.

[0167] The surface layers may each individually optionally contain additives. The additives may be any optional additive disclosed herein.

[0168] A surface layer may comprise two or more embodiments disclosed herein.

[0169] ii. Inner layer

[0170] The molded article comprises an inner layer. The inner layer comprises a composition comprising 4,4'-oxydibenzenesulfonyl azide coupled post-consumer recycled polypropylene (DPO-BSA coupled PCR-PP) having an MFR I2 of equal to or less than 5 g / 10 min.

[0171] An "inner layer" is a layer that has no surface exposed or significantly exposed to the surrounding environment. In other words, the inner layer is sandwiched between surface layers.

[0172] The inner layer is a continuous layer having two opposing surfaces including two inner surfaces.

[0173] The composition and DPO-BSA-coupled PCR-PP may be any corresponding composition and DPO-BSA-coupled PCR-PP disclosed herein.

[0174] The molded article includes at least one inner layer containing the composition. In one embodiment, the molded article includes one inner layer, or more than one inner layer. For example, the molded article may have one, two, three, four, five, six, seven, eight, nine, ten, eleven or more inner layers. In one embodiment, the molded article contains only one inner layer. Each inner layer may be the same or different, provided that at least one inner layer contains the composition.

[0175] The inner layer is in contact with both surface layers. The inner layer may be in direct contact or indirect contact with one or both surface layers. In one embodiment, the inner layer is in direct contact with one or both of the first surface layer and the second surface layer. As used herein, the term "direct contact" is a layer configuration whereby the inner layer is positioned adjacent to the surface layer and there is no intermediate layer or intermediate structure between the inner layer and the surface layer.

[0176] In another embodiment, the inner layer indirectly contacts one or both of the first surface layer and the second surface layer, and there is no intermediate layer. As used herein, the term "indirect contact" is a layer configuration whereby there is an intermediate layer, intermediate coating or intermediate structure between the inner layer and one or both of the first surface layer and the second surface layer.

[0177] The inner layer may comprise two or more embodiments disclosed herein.

[0178] In one embodiment, the molded article has the following structure (II):

[0179] First surface layer / inner layer / second surface layer structure (II).

[0180] In one embodiment, in Structure (II), the first surface layer comprises, consists essentially of, or consists of a propylene-based polymer.

[0181] In one embodiment, the molded article has the following structure (III):

[0182] First surface layer / first inner layer / second inner layer / second surface layer structure (III).

[0183] In one embodiment, in Structure (III), the first inner layer contains, consists essentially of, or consists of a propylene / ethylene copolymer; and the second inner layer contains, consists essentially of, or consists of a composition comprising DPO-BSA coupled PCR-PP. The first surface layer contains an ethylene-based polymer.

[0184] In one embodiment, the molded article includes an inner layer composed of 100 wt % of DPO-BSA coupled PCR-PP, based on the total weight of the inner layer.

[0185] Non-limiting examples of suitable molded articles include blow molded articles, injection molded articles, and rotational molded articles.

[0186] In one embodiment, the molded article is a blow molded article. Non-limiting examples of suitable blow molded articles include containers such as for toiletries (e.g., shampoo bottles, conditioner bottles, shower gel bottles), household cleaners (e.g., detergent bottles, bathroom cleaner bottles), and hazardous waste; signs; wheels for products such as toys, garden products, and utility containers; fuel tanks; and furniture such as chairs.

[0187] In one embodiment, the molded article is a blow molded article, and the inner layer

[0188] In one embodiment, the molded article includes an inner layer, the inner layer containing, consisting essentially of, or consisting of a composition, the composition containing, consisting essentially of, or consisting of: 60 wt% to 99 wt%, or 80 wt% to 99 wt%, or 90 wt% to 99 wt%, or 95 wt% to 99 wt% of DPO-BSA coupled PCR-PP; and 1 wt% to 40 wt%, or 1 wt% to 20 wt%, or 1 wt% to 10 wt%, or 1 wt% to 5 wt% of the original polymer, based on the total weight of the composition; and the MFR of the composition I2 is greater than 0 g / 10 min to 5 g / 10 min, or greater than 0 g / 10 min to 4 g / 10 min, or greater than 0 g / 10 min to 3 g / 10 min, or greater than 0 g / 10 min to 2 g / 10 min, or 0.1 g / 10 min to 4.5 g / 10 min, or 0.9 g / 10 min to 4.4 g / 10 min. The original polymer is selected from original ethylene-based polymers, original propylene-based polymers, and combinations thereof. The original polymer can be any original polymer disclosed herein. The original polymer of the inner layer can be the same or different from the original polymer of the surface layer. In one embodiment, the inner layer and the composition contain sulfur greater than 0 ppm to 350 ppm by the total weight of the corresponding inner layer and the composition. In another embodiment, the molded article is a blow molded article.

[0189] A molded article may include one or more embodiments disclosed herein.

[0190] By way of example and not limitation, some embodiments of the present disclosure will now be described in detail in the following examples.

[0191] Examples

[0192] The materials used in the Examples are provided in Table 1 below.

[0193] Table 1. Starting materials for the compositions

[0194]

[0195] The sample compositions were prepared by adding the individual components to a Haake PolyLab co-rotating twin screw extruder and extruding the composition at an output of 2.5 to 3 kg / hour. Melt blending of the components was performed in the extruder at 240°C.

[0196] The composition and properties of each sample composition are provided in Table 2 below.

[0197] Figure 1 is the DSC curve of CS 1. In other words, Figure 1 SYSTALEN PP-C32902 is a DSC curve. As shown in the figure, the heating test (i.e., melting temperature) curve has two peaks - one at about 125°C and one at about 160°C. The peak at 125°C indicates that SYSTALEN PP-C32902 contains post-consumer recycled ethylene-based polymer (PCR-PE), and the peak at 160°C indicates that SYSTALEN PP-C32902 contains propylene-based polymer. The cooling test (i.e., crystallization temperature) curve also has two peaks - one at about 120°C and one at about 125°C. The peak at 120°C indicates that SYSTALEN PP-C32902 contains PCR-PE, and the peak at 125°C indicates that SYSTALEN PP-C32902 contains propylene-based polymer. SYSTALEN PP-C32902 contains a majority amount (greater than 50 wt%) of propylene-based polymer based on the total weight of SYSTALEN PP-C32902.

[0198] Figure 2 is the DSC curve of CS 3. In other words, Figure 2SYSTALEN PP-C32900 is a DSC curve. As shown in the figure, the heating test (i.e., melting temperature) curve has two peaks - one at about 125°C and one at about 160°C. The peak at 125°C indicates that SYSTALEN PP-C32900 contains PCR-PE, and the peak at 160°C indicates that SYSTALEN PP-C32900 contains a propylene-based polymer. The cooling test (i.e., crystallization temperature) curve also has two peaks - one at about 115°C and one at about 125°C. The peak at 115°C indicates that SYSTALEN PP-C32900 contains PCR-PE, and the peak at 125°C indicates that SYSTALEN PP-C32900 contains a propylene-based polymer. SYSTALEN PP-C32900 contains a majority amount (greater than 50 wt%) of a propylene-based polymer based on the total weight of SYSTALEN PP-C32900.

[0199] As shown in Table 2, CS 1 and CS 3 each contain PCR-PP (SYSTALEN PP-C32902 or SYSTALEN PP-C32900) that is not coupled to DPO-BSA. As shown in Table 2, CS 1 and CS 2 each exhibit an MFR I2 greater than 2 g / 10 min (13.2 g / 10 min and 7.8 g / 10 min, respectively). Therefore, both CS 1 and CS 3 are not suitable for blow molding applications.

[0200] CS 2 contains PCR-PP (SYSTALEN PP-C32902), PCR-PE (SYSTALEN 32104) and a virgin ethylene-based polymer (INFUSE 9077) not coupled with DPO-BSA. CS 2 exhibits an MFR I2 greater than 2 g / 10 min (7 g / 10 min). Therefore, CS 2 is not suitable for blow molding applications.

[0201] Table 2

[0202]

[0203] 1 Based on total combined weight of DPO-BSA, PCR-PP and optional pristine polymer.

[0204] 2 Based on the total weight of the composition containing DPO-BSA coupled PCR-PP.

[0205] The applicant unexpectedly discovered that coupling a PCR-PP (SYSTALEN PP-C32902 or SYSTALEN PP-C32900) having an MFR I2 greater than 7 g / 10 min (13.2 g / 10 min and 7.8 g / 10 min, respectively) with DPO-BSA produced coupled PCR-PP (Examples 1-3, Examples 5-7) having an MFR I2 equal to or less than 5 g / 10 min, as shown in Table 2. Therefore, Examples 1-3 and Examples 5-7 are each suitable for use in blow molded article applications.

[0206] Example 4 is a composition containing (i) a pristine ethylene-based polymer (INFUSE 9077) and (ii) a PCR-PP (SYSTALEN PP-C32902) having an MFR I2 greater than 7 g / 10 min (13.2 g / 10 min) that has been coupled with DPO-BSA. The resulting coupled PCR-PP of Example 4 exhibits an MFR I2 equal to or less than 5 g / 10 min. The composition of Example 4 also exhibits a melt flow rate equal to or less than 5 g / 10 min (2.9 g / 10 min). Therefore, Example 4 is suitable for blow molding applications.

[0207] Example 8 is a composition containing (i) a pristine propylene-based polymer (VERSIFY 3401) and (ii) a PCR-PP (SYSTALEN PP-C32900) having an MFR I2 greater than 7 g / 10 min (7.8 g / 10 min) that has been coupled with DPO-BSA. The resulting coupled PCR-PP of Example 8 exhibits an MFR I2 equal to or less than 5 g / 10 min. The composition of Example 8 also exhibits a melt flow rate equal to or less than 5 g / 10 min (3.2 g / 10 min). Therefore, Example 8 is suitable for blow molding applications.

[0208] It is particularly intended that the present disclosure is not limited to the embodiments and descriptions contained herein, but includes modifications of those embodiments including parts of the embodiments and combinations of elements of different embodiments as appear within the scope of the following claims.

Claims

1. A method comprising: (i) providing a post-consumer recycled polypropylene (PCR-PP) having a melt flow rate MFRI2 equal to or greater than 7.0 g / 10 min; wherein the PCR-PP comprises equal to or greater than 70 wt% of a propylene-based polymer and a post-consumer recycled ethylene-based polymer (PCR-PE); (ii) adding 150 ppm to 2000 ppm of 4,4'-oxydibenzenesulfonyl azide (DPO-BSA) to the PCR-PP; (iii) melt-blending the PCR-PP and the DPO-BSA; and (iv) forming a DPO-BSA coupled PCR-PP having a melt flow rate MFR I2 equal to or less than 5 g / 10 min; The melt flow rate MFR I2 is measured according to ASTM D1238 at 230° C. under a load of 2.16 kg.

2. The method of claim 1, comprising providing a PCR-PP having a melt flow rate MFRI2 equal to or greater than 8.0 g / 10 min.

3. The method of claim 1, comprising melt blending the DPO-BSA coupled PCR-PP with a virgin polymer selected from the group consisting of a virgin ethylene-based polymer, a virgin propylene-based polymer, and combinations thereof to form a composition having a melt flow rate (MFR I2) equal to or less than 5 g / 10 min.

4. The method of claim 2, comprising melt blending the DPO-BSA coupled PCR-PP with a virgin polymer selected from the group consisting of a virgin ethylene-based polymer, a virgin propylene-based polymer, and combinations thereof to form a composition having a melt flow rate (MFR I2) equal to or less than 5 g / 10 min.

5. The method according to any one of claims 1 to 4, comprising forming the DPO-BSA coupled PCR-PP having a melt flow rate MFRI2 equal to or less than 2 g / 10 min.

6. A composition comprising: 4,4'-oxydibenzenesulfonyl azide coupled post-consumer recycled polypropylene (DPO-BSA coupled PCR-PP) having (i) a melt flow rate MFR I2 equal to or less than 5 g / 10 min; and (ii) greater than 0 ppm to 350 ppm of sulfur, The DPO-BSA coupled PCR-PP is prepared by the following method: (a) providing a post-consumer recycled polypropylene (PCR-PP) having a melt flow rate MFR I2 equal to or greater than 7.0 g / 10 min; wherein the PCR-PP comprises equal to or greater than 70 wt% of a propylene-based polymer and a post-consumer recycled ethylene-based polymer (PCR-PE); (b) adding 150 ppm to 2000 ppm of 4,4'-oxydibenzenesulfonyl azide (DPO-BSA) to the PCR-PP; (c) melt-blending the PCR-PP and the DPO-BSA to form the DPO-BSA-coupled PCR-PP; The melt flow rate MFR I2 is measured according to ASTM D1238 at 230° C. under a load of 2.16 kg.

7. The composition of claim 6, wherein the DPO-BSA coupled PCR-PP comprises From greater than 0 wt% to 30 wt% post-consumer recycled ethylene-based polymer (PCR-PE), based on the total weight of the DPO-BSA coupled PCR-PP.

8. The composition of claim 6 or 7, further comprising from greater than 0 wt% to 5 wt% of a virgin polymer selected from the group consisting of a virgin ethylene-based polymer, a virgin propylene-based polymer, and combinations thereof.

9. A molded product comprising a first surface layer comprising a polyolefin; An inner layer comprising a composition according to any one of claims 6 to 8; and A second surface layer comprises a propylene-based polymer.

10. A molded product comprising a first surface layer comprising a polyolefin; an inner layer comprising a composition comprising 4,4'-oxydibenzenesulfonyl azide coupled post-consumer recycled polypropylene (DPO-BSA coupled PCR-PP) having a melt flow rate MFR I2 equal to or less than 5 g / 10 min; and a second surface layer comprising a propylene-based polymer; The melt flow rate MFR I2 is measured according to ASTM D1238 at 230° C. under a load of 2.16 kg. 11 . The molded article of claim 10 , wherein the first surface layer comprises a polyolefin selected from the group consisting of an ethylene-based polymer, a propylene-based polymer, and combinations thereof. 12 . The molded article according to claim 10 , wherein the inner layer consists of 100 wt % of the DPO-BSA coupled PCR-PP based on the total weight of the inner layer.

13. The molded article according to any one of claims 10 to 11, wherein the inner layer composition comprises (i) the DPO-BSA coupled PCR-PP and (ii) from greater than 0 wt% to 5 wt% of a virgin polymer selected from the group consisting of a virgin ethylene-based polymer, a virgin propylene-based polymer, and a combination thereof.

14. The molded article according to any one of claims 10 to 11, wherein the inner layer comprises from greater than 0 ppm to 350 ppm of sulfur.