Constrained composite material, composite layer, preparation method thereof and composite damper for energy dissipation core material
By using a constrained composite layer structure in a metal composite damper and using zinc methacrylate and maleic anhydride to graft polybutadiene to improve the rubber material, the damper performance problems caused by uneven metal deformation are solved and the damper performance is improved. energy dissipation capacity and fatigue performance.
Patent Information
- Application Number
- CN202111002008.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-08-30
AI Technical Summary
In existing metal composite viscoelastic dampers, the metal deforms unevenly during the deformation process, resulting in an unsaturated envelope curve of the damper, large stress attenuation, and poor fatigue performance.
It adopts a constrained composite layer structure. The special rubber material contains zinc methacrylate and maleic anhydride grafted polybutadiene. It is superimposed with the skeleton material to form a constrained composite layer, which is wrapped around the low yield point metal core material to ensure uniform deformation. And prevent extrusion into the viscoelastic material layer.
It significantly improves the energy dissipation capacity, stability and fatigue recovery performance of the damper, ensures uniform deformation of the metal core material, reduces stress concentration, and extends the service life of the damper.
Smart Images

Figure CN114133634B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of building shock absorption and earthquake resistance, and in particular to a constrained composite material for energy-absorbing core material, a constrained composite layer, a preparation method of the constrained composite material, and a composite damper using the constrained composite layer. Background Art
[0002] The viscoelastic damper is a shock-absorbing and energy-dissipating device made of multiple layers of internal viscoelastic damping materials and multiple layers of internal steel plates laminated and vulcanized as a whole. The composite viscoelastic damper is formed by adding metals such as lead cores to the viscoelastic damper to form a metal composite damper, thereby increasing the energy dissipation capacity and effective stiffness of the damper.
[0003] Metal composite viscoelastic dampers are used in buildings to reduce wind vibration or earthquake effects. The above metal composite viscoelastic damper is obtained by assembling a viscoelastic damper with a lead core or other metal. However, the resilience provided by the rubber in the composite damper obtained by directly assembling and adding metals such as lead cores is not enough to make the metal in it deform evenly during the deformation process. At the same time, the metal in the damper will permanently squeeze the softer viscoelastic material into the steel plate interlayer due to uneven deformation. The envelope curve of the prepared metal composite damper is not full after reciprocating, the stress attenuation is large, and the fatigue performance is poor.
[0004] Compared with the traditional metal composite viscoelastic damper, the present invention provides a constrained composite damper, which adds a constraint layer to effectively constrain the uniform deformation of the metal in the damper, and significantly improves the energy dissipation capacity, stability and fatigue recovery. Summary of the invention
[0005] In order to solve the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a constrained composite layer rubber and a constrained composite layer structure for a composite damper, so as to solve the problem that the low yield point metal of the existing damper is subjected to uneven deformation by extrusion and is partially pressed into the softer viscoelastic rubber layer during the shear deformation process, resulting in an incomplete damper envelope curve, large stress attenuation and poor fatigue resistance. Specifically, the present invention is implemented as follows:
[0006] The first is a constrained composite material for energy-absorbing core material, which is used in the technical field of consuming kinetic energy and in equipment and devices. The constrained composite material includes a special rubber material, which contains zinc methacrylate and maleic anhydride grafted polybutadiene.
[0007] Furthermore, the special rubber material includes the following components by weight: 100 parts of diene rubber, 10-70 parts of white carbon black or carbon black, 0-30 parts of zinc methacrylate, 0-3 parts of antioxidant, 0-3 parts of bridging agent, 0-3 parts of sulfur, 1-3 parts of activation system, 0-10 parts of tackifying resin, and 0-15 parts of maleic anhydride grafted polybutadiene. The bridging agent includes a resin curing agent or a peroxide crosslinking agent.
[0008] Secondly, based on the above-mentioned constraint composite material, a constraint composite layer is formed, which includes a special rubber and a skeleton material laminated together, which is used to bond with the surface of the energy-consuming core material and form a partial or full wrapping of the energy-consuming core material, which can constrain the energy-consuming core material to deform uniformly and prevent it from deforming too much or being squeezed into the viscoelastic material layer during the deformation process. The skeleton material is a metal wire, a metal mesh or a metal tube.
[0009] Furthermore, the surface bonding between the constraint composite layer and the energy consumption core material is vulcanization bonding; the special rubber and the skeleton material are crossed or at least one layer is laid flat to form a composite rubber layer; the special rubber contains zinc methacrylate and maleic anhydride grafted polybutadiene.
[0010] Then, a viscoelastic damper is constructed based on the above-mentioned constraint composite layer, including: an outer shear connecting plate, an intermediate shear connecting plate, a viscoelastic material, an energy-absorbing core material, and a constraint composite layer that is bonded and wrapped with the energy-absorbing core material, wherein the constraint composite layer is made of a special rubber and a skeleton material, and the special rubber includes zinc methacrylate and maleic anhydride grafted polybutadiene. The energy-absorbing core material is a low-yield point metal rod, the intermediate shear connecting plate is provided with a through hole of a corresponding diameter, and the outer shear connecting plate is provided with a blind hole of a corresponding diameter; the viscoelastic material is a rubber-like elastic material or a high-damping rubber; the low-yield point metal rod passes through the through hole and is placed in the corresponding blind hole; the skeleton material is a steel wire, fiber or metal mesh, and is cross- or flat-laid with a special rubber material to form a shape; the constraint composite layer wraps around the low-yield point metal rod, and is mainly vulcanized and bonded with the outer shear connecting plates and the viscoelastic material on both sides.
[0011] Finally, the present invention also provides a method for preparing a constrained composite material for an energy-consuming core material, comprising the following steps: preparing various components including zinc methacrylate and maleic anhydride grafted polybutadiene, and weighing them according to the proportions; first plasticizing the rubber in an internal mixer for 60 to 120 seconds to make its plasticity reach 0.3 to 0.4, and then sequentially adding an activation system, an antioxidant, a tackifying resin, carbon black, zinc methacrylate, and maleic anhydride grafted polybutadiene and mixing them for 120 to 180 seconds to make the various components evenly dispersed in the rubber, and then placing the mixed rubber on an open mixer, adding sulfur and a bridging agent, and mixing the rubber for 100 to 180 seconds before removing the rubber and parking it for standby use.
[0012] The working principle of the present invention is introduced as follows: the energy-consuming core material is a metal material used in the composite damper, and a constrained composite layer structure is added on its surface. The constrained composite layer is mainly composed of rubber, and a special hardening and reinforcing material zinc methacrylate is added, and the skeleton bonding material maleic anhydride grafted polybutadiene is strengthened. After being matched with conventional fillers, a special bridging agent is used to make it have higher hardness and strength. At the same time, the rubber material and the metal material have a certain bonding ability during the vulcanization process, so that the skeleton material therein is evenly stressed and deformed. The skeleton material is further added to the rubber of the constrained composite layer, which has a certain deformation ability and provides a higher elastic stiffness. The composite damper prepared by wrapping the constrained composite layer material and structure around the low yield point metal has full energy consumption and fatigue stability.
[0013] The beneficial effects of the present invention are introduced as follows: during vulcanization, the rubber of the constrained composite layer and the energy-consuming core material adhere to the energy-consuming core material, which effectively constrains the core material on the one hand, and makes the deformation process of the core material more uniform on the other hand, reduces stress concentration, and can effectively prevent the metal in the damper from permanently squeezing the softer viscoelastic material into the steel plate interlayer due to uneven deformation. Maleic anhydride forms a strong reaction with the polar groups on the fiber surface or the metal surface, while butadiene co-crosslinks with the polymer to play a bridging role. Therefore, the addition of zinc methacrylate and maleic anhydride grafted polybutadiene not only greatly improves the tear strength and hardness of the rubber, but also improves the adhesion between the rubber and the skeleton material, increases the strength and stiffness of the constrained composite layer, and at the same time, during vulcanization, the rubber of the partially constrained composite layer and the energy-consuming core material adhere to the energy-consuming core material, which effectively constrains the core material on the one hand, and makes the deformation process of the core material more uniform on the other hand, reduces stress concentration, and improves the performance of the viscoelastic damper as a whole.
[0014] Instruction Manual
[0015] Figure 1 It is a schematic diagram of the cross-sectional structure of a composite damper;
[0016] Figure 2 is a schematic diagram of the structure of the constrained composite layer;
[0017] Figure 3 is the displacement-load curve of Experiment 5;
[0018] Figure 4 is the displacement-load curve of Experiment 6;
[0019] Figure 5 is the displacement-load curve of Experiment 7;
[0020] Figure 6 A schematic diagram of the unfolded structure of a metal mesh as a skeleton material;
[0021] Figure 7 This is a three-dimensional structural diagram of a composite damper.
[0022] Among them: 1—outer shear connecting plate, 2—middle shear connecting plate, 3—viscoelastic material, 4—energy dissipation core material, 5—constrained composite layer, 6—skeleton material. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0024] Example 1: Constrained composite material for energy dissipating core material
[0025] In the field of building shock absorption technology and equipment for dissipating kinetic energy, the constraint composite material includes a special rubber material, which contains zinc methacrylate and maleic anhydride grafted polybutadiene. The special rubber material includes the following components by weight: 100 parts of diene rubber, 10-70 parts of white carbon black or carbon black, 0-30 parts of zinc methacrylate, 0-3 parts of antioxidant, 0-3 parts of bridging agent, 0-3 parts of sulfur, 1-3 parts of activation system, 0-10 parts of tackifying resin, and 0-15 parts of maleic anhydride grafted polybutadiene. The bridging agent includes a resin curing agent or a peroxide crosslinking agent.
[0026] Preferably, the diene rubber is 60-100 parts of butadiene rubber and 40-0 parts of natural rubber; the mass ratio of white carbon or carbon black to stearic acid is 10-30:40-20; 15-25 parts of zinc methacrylate, 0-3 parts of antioxidant, 1-2 parts of bridging agent, 0.5-1.5 parts of sulfur, 1-3 parts of activation system, 5-10 parts of tackifying resin, and 5-15 parts of maleic anhydride grafted polybutadiene.
[0027] Among them, the positively charged divalent Zn2+ ions between the two carboxyl anions of zinc methacrylate can easily act as ionic bridge bonds, and at the same time, the metal surface ions and Zn2+ ions are attracted by electrostatic force to produce extremely strong adhesion. The surface of untreated synthetic fibers is smooth, the modulus is high, the polarity is far different from that of rubber, and the bonding affinity is extremely low. Therefore, in the process of bonding fibers with rubber, it is usually necessary to pre-treat the fiber surface. After the maleic anhydride in the maleic anhydride grafted polybutadiene is grafted with polybutadiene, the maleic anhydride reacts strongly with the polar groups on the fiber surface or the metal surface, and butadiene is cross-linked with the polymer to play a bridging role. Therefore, the addition of zinc methacrylate and maleic anhydride grafted polybutadiene can not only greatly improve the tear strength and hardness of the rubber, but also improve the adhesion between the rubber and the skeleton material, increase the strength and stiffness of the constrained composite layer, and at the same time, the rubber of the partially constrained composite layer and the energy-consuming core material adhere to the energy-consuming core material during vulcanization, which effectively constrains the core material on the one hand and makes the deformation process of the core material more uniform on the other hand, reducing stress concentration.
[0028] Example 2: A constrained composite layer for an energy dissipating core material
[0029] It is made of the special rubber and skeleton material described in Example 1, and is used to bond with the surface of the energy-consuming core material 4 and form a partial or full wrapping of the energy-consuming core material, which can constrain the uniform deformation of the energy-consuming core material and prevent it from deforming too much, or being squeezed into the viscoelastic material layer during the deformation process. The surface bonding of the constrained composite layer and the energy-consuming core material is vulcanization bonding; the special rubber and the skeleton material are cross-shaped, or at least one layer is laid flat to form a composite rubber layer; the special rubber contains zinc methacrylate and maleic anhydride grafted polybutadiene. The skeleton material 6 is a metal wire, a metal mesh or a metal tube.
[0030] In order to increase the bonding effect of zinc methacrylate, maleic anhydride grafted polybutadiene and the skeleton material and its reinforcing effect on the rubber, a bridging agent is preferably added to the rubber formula, and the bridging agent is preferably an organic peroxide such as diisopropylbenzene peroxide, benzoyl peroxide, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, etc. The addition of the bridging agent allows the acrylate and polybutadiene to form a CC cross-linking bond, providing higher bond energy and tensile strength.
[0031] Preferably, in order to improve the deformation resistance and resilience of the constrained composite layer, the constrained composite layer is preferably a steel wire or a metal wire mesh and a rubber composite constrained composite layer, the steel wire preferably has a wire diameter of 0.3mm to 1.2mm and is made of 0Cr18Ni9Ti, 1Cr18Ni9Ti, and the metal mesh is preferably made of 0Cr18Ni9Ti, 1Cr18Ni9Ti, 06Cr19Ni10 and processed into a mesh tube with a thickness of less than 1.5mm. The selected metal material has high tensile strength and an elongation of more than 60%. In particular, after it is processed into metal rubber and pressed into a metal mesh, its elastic deformation is greatly improved. The combination of the two makes the entire constrained composite layer have greater deformation capacity and resilience.
[0032] Example 3: A composite damper
[0033] like Figure 1 As shown, the composite damper includes: an outer shear connection plate 1, an intermediate shear connection plate 2, a viscoelastic material 3, an energy-absorbing core material 4, and a constrained composite layer 5 bonded and wrapped with the energy-absorbing core material 4; the constrained composite layer is the constrained composite structure in Examples 1 and 2, and is made by laminating a special rubber and a skeleton material 6, wherein the special rubber includes zinc methacrylate and maleic anhydride grafted polybutadiene. The energy-absorbing core material is a low-yield point metal rod, the intermediate shear connection plate is provided with a through hole of a corresponding diameter, and the outer shear connection plate is provided with a blind hole of a corresponding diameter; the viscoelastic material is a rubber-like elastic material or a high-damping rubber; the low-yield point metal rod passes through the through hole and is placed in the corresponding blind hole; the skeleton material is a steel wire, fiber or metal mesh, and is cross-laid or flatly laminated with a special rubber material to form a shape; the constrained composite layer wraps around the low-yield point metal rod, and is mainly vulcanized and bonded with the outer shear connection plates and the viscoelastic material on both sides.
[0034] Specifically: the shear steel plate and the viscoelastic material are superimposed into a sandwich structure, and the constraint composite layer is wrapped around the low-yield point metal rod and is vulcanized and bonded to the connecting steel plate, the viscoelastic material and the main body. The shear connecting plate is carbon structural steel, the middle shear connecting plate is equipped with a through hole of corresponding diameter, and the outer connecting steel plate is equipped with a blind hole of corresponding diameter; the viscoelastic material is a rubber elastic material or a high-damping rubber; the low-yield point metal is a low-yield point metal such as lead and tin. The constraint composite layer is wrapped around the low-yield point metal rod, vertically penetrates the middle connecting steel plate and the viscoelastic material, and is embedded in the blind hole of the outer connecting steel plate.
[0035] The addition of zinc methacrylate and maleic anhydride grafted polybutadiene can not only greatly improve the tear strength and hardness of the rubber, but also improve the adhesion between the rubber and the skeleton material, increase the strength and stiffness of the constrained composite layer, while at the same time, the rubber of the partially constrained composite layer and the energy-consuming core material adhere to the energy-consuming core material during vulcanization, which can effectively constrain the core material on the one hand and make the deformation process of the core material more uniform on the other hand, thereby reducing stress concentration.
[0036] Example 4: Preparation method of constrained composite material for energy dissipation core material
[0037] The method comprises the following steps: preparing various components including zinc methacrylate and maleic anhydride grafted polybutadiene, and weighing them according to the proportion; firstly plasticizing the rubber in an internal mixer for 60 to 120 seconds to make its plasticity reach 0.3 to 0.4, then sequentially adding an activation system, an antioxidant, a tackifying resin, carbon black, zinc methacrylate, and maleic anhydride grafted polybutadiene, and mixing them for 120 to 180 seconds to make various components evenly dispersed in the rubber, then placing the mixed rubber on an open mixer, adding sulfur and a bridging agent, mixing the rubber in reverse for 100 to 180 seconds, and then removing the rubber from the mixer and parking it for standby use.
[0038] More specifically: prepare the special rubber material raw materials described in Examples 1 and 2, weigh various materials according to the above-mentioned constrained composite layer rubber composition ratio components, first plasticize the rubber in an internal mixer for 60 to 120 seconds to make its plasticity reach 0.3 to 0.4, then add the activation system, antioxidant, tackifying resin, carbon black, zinc methacrylate, maleic anhydride grafted polybutadiene in sequence and mix for 120 to 180 seconds to make each component evenly dispersed in the rubber, then put the mixed rubber on an open mill, add sulfur and bridging agent, turn the rubber over and mix for 100 to 180 seconds, then put the sheet down and park for standby use. On the open mill, calender, and wire traction machine, cross the skeleton metal wire and the constrained layer rubber according to the corresponding design requirements, flatten and preform them into a composite rubber layer, preferably, the metal wire can be prefabricated into a metal mesh tube with rubber attached to its inner and outer surfaces to form a constrained composite layer. The above-mentioned constraint composite layer is coated on the outside of the low-yield point metal, passes through the middle shear connecting plate and the viscoelastic material, and is inserted into the blind hole of the outer constraint plate. After a period of heat preservation and pressure preservation, it is cross-linked and formed into a metal composite damper.
[0039] Experimental Example 1
[0040] Special rubber materials in restrained composite materials for energy dissipating core materials, counted by weight, including:
[0041] 100 parts of diene rubber, 15 parts of white carbon black, 20 parts of carbon black, 5 parts of zinc methacrylate, 3 parts of antioxidant, 2 parts of sulfur, 3 parts of activation system, and 5 parts of tackifying resin.
[0042] Experimental Example 2
[0043] Special rubber materials in restrained composite materials for energy dissipating core materials, counted by weight, including:
[0044] 100 parts of diene rubber, 15 parts of white carbon black, 20 parts of carbon black, 10 parts of zinc methacrylate, 3 parts of antioxidant, 2 parts of sulfur, 3 parts of activation system, 5 parts of tackifying resin, and 1 part of bridging agent.
[0045] Experimental Example 3
[0046] Special rubber materials in restrained composite materials for energy dissipating core materials, counted by weight, including:
[0047] 100 parts of diene rubber, 15 parts of white carbon black, 20 parts of carbon black, 15 parts of zinc methacrylate, 3 parts of antioxidant, 2 parts of sulfur, 3 parts of activation system, 5 parts of tackifying resin, 5 parts of maleic anhydride grafted polybutadiene, 1 part of bridging agent
[0048] Experimental Example 4
[0049] Special rubber materials in restrained composite materials for energy dissipating core materials, counted by weight, including:
[0050] 100 parts of diene rubber, 15 parts of white carbon black, 20 parts of carbon black, 15 parts of zinc methacrylate, 3 parts of antioxidant, 2 parts of sulfur, 3 parts of activation system, 5 parts of tackifying resin. 10 parts of maleic anhydride grafted polybutadiene, 1.5 parts of bridging agent
[0051] Among them, when the amount of zinc methacrylate exceeds 20 parts, there will be problems such as sticking to the roller and difficulty in processing, so the amount is recommended to be no more than 20 parts; and when the amount of maleic anhydride grafted polybutadiene exceeds 20 parts, there will be problems such as decreased hardness and strength of the vulcanized rubber, so the amount is recommended to be no more than 20 parts.
[0052] The constrained composite rubber material provided in Experimental Examples 1 to 4 was used. The tensile strength of the vulcanized specimens was tested using a universal testing machine in accordance with GB / T528-1998, with a test speed of 500 mm / min; the Shore A hardness of the specimens was tested in accordance with GB / T531-1999. The mechanical properties of the materials are shown in Table 1.
[0053] Table 1 Mechanical properties of the constrained composite rubber layer
[0054]
[0055] The restrained composite layer rubber materials provided in Experimental Examples 1 to 4 were used to test the tensile shear strength of the bond between the vulcanized rubber and the metal using a universal testing machine in accordance with GB-T 13936. The bond strength between the restrained rubber and the metal is shown in Table 2.
[0056] Table 2 Bond strength of restrained rubber and metal
[0057] Adhesion strength / Mpa Experimental Example 1 1.2 Experimental Example 2 2.1 Experimental Example 3 3.3 Experimental Example 4 4.3
[0058] Experimental Example 5 used the restraining material of Experimental Example 1 without adding the skeleton material;
[0059] Experimental Example 6 uses the constraint material of Experimental Example 4 without adding the skeleton material.
[0060] Experimental Example 7 uses the restraining material of Experimental Example 4 plus a metal mesh.
[0061] Composite dampers containing four lead rods with a diameter of 75 mm were prepared. The test was carried out using GJ / T 209-2012 Building Energy Dissipation Damper. The test results are shown in Table 3.
[0062] Table 3 Composite damper performance test
[0063]
[0064] As shown in Table 3, the composite damper was prepared by using the constrained composite layer structure provided by Experimental Examples 5 to 7, and its yield force increased with the increase of the hardness of the constrained composite layer rubber and the increase of the skeleton material.
[0065] like Figures 3 to 5 As shown, the load-displacement curves of the composite damper under different displacements were prepared by using the constrained composite layer provided in Experimental Examples 5 to 7.
[0066] Example 7 Displacement-Load Curve
[0067] Figures 3 to 5 Displacement load curves of composite dampers in examples 5 to 7
[0068] The composite damper prepared by using the constrained composite layer structure provided in Experimental Examples 5 to 7 has a hysteresis curve that gradually becomes fuller and a more stable fatigue energy consumption.
[0069] It should be understood that the above specific experimental methods of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A composite damper, comprising: The outer shear connecting plate, the middle shear connecting plate, the viscoelastic material, and the energy dissipation core material are characterized in that they also include a constrained composite layer that is bonded to and wraps the energy dissipation core material. The constrained composite layer is made of a special rubber material and a skeleton material, and is used to bond with the surface of the energy-consuming core material and form a partial or full wrapping of the energy-consuming core material, which can constrain the energy-consuming core material to deform uniformly and prevent it from deforming too much or being squeezed into the viscoelastic material layer during the deformation process; the bonding between the constrained composite layer and the surface of the energy-consuming core material is vulcanization bonding; The special rubber material comprises zinc methacrylate and maleic anhydride grafted polybutadiene; The energy dissipation core material is a low-yield point metal rod, the middle shear connection plate is provided with a through hole of corresponding diameter, and the outer shear connection plate is provided with a blind hole of corresponding diameter; the viscoelastic material is a rubber-like elastic material; the low-yield point metal rod passes through the through hole and is placed in the corresponding blind hole; the skeleton material is steel wire, fiber or metal mesh, and is cross- or flat-laid with a special rubber material to form a mold; the constraint composite layer wraps around the low-yield point metal rod, and is vulcanized and bonded to the outer shear connection plates and viscoelastic materials on both sides; The special rubber material comprises the following components by weight: 100 parts of diene rubber, wherein the diene rubber is 60-100 parts of butadiene rubber and 40-0 parts of natural rubber; 10-70 parts of white carbon black or carbon black; 15-25 parts of zinc methacrylate, 0-3 parts of antioxidant, 1-2 parts of bridging agent, 0.5-1.5 parts of sulfur, 1-3 parts of activation system, 5-10 parts of tackifying resin, and 5-15 parts of maleic anhydride grafted polybutadiene; the bridging agent comprises a resin curing agent or a peroxide crosslinking agent.
2. The composite damper according to claim 1, characterized in that: The constrained composite layer is prepared by the following steps: preparing various components including zinc methacrylate and maleic anhydride grafted polybutadiene, and weighing them according to the proportion; firstly plasticizing the rubber in an internal mixer for 60 to 120 seconds to make its plasticity reach 0.3 to 0.4, then adding an activation system, an antioxidant, a tackifying resin, carbon black, zinc methacrylate, and maleic anhydride grafted polybutadiene in sequence and mixing for 120 to 180 seconds to make the various components uniformly dispersed in the rubber, then placing the mixed rubber on an open mixer, adding sulfur and a bridging agent, and mixing the rubber for 100 to 180 seconds before removing the rubber and parking it for standby use.
Citation Information
Patent Citations
Energy-consumption shear wall made of composite material
CN104060724A
Constraint composite layer for energy consumption core material and composite damper using constraint composite layer
CN216007380U
Laminated rubber bearing device and its manufacturing method
JP2003214493A
Rubber composition for seismic isolation laminate and seismic isolation laminate using the same
JP2005320376A